Polyethylene compositions and uses thereof, and polyolefin microporous breathable films prepared therefrom
The introduction of maleic anhydride copolymer microspheres as organic porogens in polyethylene breathable films addresses the issues of inorganic porogens, achieving uniform micropore formation and improved breathability and mechanical properties without the need for dispersants or surfactants.
Patent Information
- Application Number
- JP2024525480
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-31
AI Technical Summary
Inorganic porogens used in the production of polyethylene breathable films tend to aggregate, have large particle sizes, uneven particle size distribution, poor surface modification, and poor compatibility with the matrix, leading to non-uniform breathability and mechanical weakness in the films.
Employing maleic anhydride copolymer microspheres as organic porogens with uniform particle size distribution and suitable compatibility with the polyethylene matrix, eliminating the need for dispersants and surfactants, to achieve uniform micropore formation and improved mechanical properties.
The use of maleic anhydride copolymer microspheres results in a breathable film with uniform air permeability, enhanced water vapor transmission rate, and stable physical properties, overcoming the limitations of inorganic porogens.
Smart Images

Figure 2024540130000001_ABST
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present invention relates to the field of polyolefin compositions, in particular to polyethylene compositions and their uses, as well as polyolefin microporous breathable films prepared therefrom, and further to breathable composite articles comprising the polyolefin microporous breathable films.
[0002] [Background technology] The breathable film, also called "water-impermeable breathable microporous film", has the characteristic of being permeable to gas (air, water vapor, etc.) and impermeable to water (water droplets, sweat and other liquids). The breathable film in the prior art is generally a composite material with a thermoplastic matrix and a certain percentage of solid particles (such as calcium carbonate, barium sulfate, titanium dioxide, talc powder and other mineral fillers). This composite material is prepared into a thin film through methods such as blow molding, calendar molding, or casting molding. This thin film is then uniaxially or biaxially stretched under appropriate conditions to obtain a microporous thin film material with smaller pores. The microporous breathable film can allow gases such as water vapor and air to pass while blocking liquids, and can be widely used in medical supplies such as medical protective clothing, wound care bandages and dressings, hygiene products such as baby diapers and adult care products, food packaging and daily necessities, and other fields, and is a new material that has developed rapidly in the past 20 years.
[0003] Theoretically, any thermoplastic resin can be used as the matrix resin of breathable film materials, but in terms of the total market value of microporous breathable films, polyethylene breathable films account for the largest proportion. Polyethylene has the advantages of abundant starting materials, easy processing and molding, good film forming effect, and soft and comfortable touch, and is widely used as the matrix resin of breathable film materials.
[0004] Since the hygiene industry is the largest end market for polyethylene breathable film, the safety and comfort of the breathable film must be taken into consideration. Therefore, the porogen used in the preparation process of polyethylene breathable film must have high quality requirements. Inorganic fillers, especially calcium carbonate, have become the preferred material as porogens due to their abundant resources, low price, and good overall properties. However, inorganic porogens have hydrophilic and oleophobic and highly polar surfaces, which make them poorly compatible with the polymer matrix and difficult to disperse uniformly in the matrix. At the same time, the dispersion uniformity of the porogen in the matrix affects the mechanical properties, surface uniformity, micropore pore size uniformity, porosity and other parameters of the breathable film. In the traditional manufacturing process, the inorganic filler is often pretreated with a surfactant to increase its compatibility with the matrix, and at the same time, a coupling agent and a dispersing agent are added to solve the problem of dispersing the inorganic filler.
[0005] CN102336940A discloses a composition for a breathable film with low permeability and its preparation method. The composition includes a polyolefin resin mixture, a permeability regulator, surface-modified micro-scale inorganic particles, an antioxidant, a lubricant and a coupling agent. The advantage of this composition is that the micron-scale inorganic filler can improve the mechanical properties of the breathable film, and at the same time, the coupling modification of the surface of the inorganic particles can improve the compatibility with the polyolefin resin, but the disadvantage is that the micron-scale inorganic particles cannot be uniformly dispersed in the matrix resin, thus affecting the uniformity of the breathability of the film.
[0006] CN1176986C discloses a special resin for polyolefin high breathability cast film and a method for preparing the film. This special resin is obtained by using polyolefin resin (composed of three polymers of LDPE, LLDPE, and propylene copolymer) and ultrafine mineral filler (such as calcium carbonate, talc powder, particle size 3μm-10μm) as the main starting materials, adding Ti-Al composite coupling agent, POE modifier, and OPE dispersant, and subjecting to coupling treatment, compatibilization dispersion and dispersion, internal mixing and processing by extrusion granulation. Through the casting and stretching process, this special resin forms uniform and fine pores between the mineral filler particles and the two phases of polyolefin in the thin film, and then after cooling and crystallization, a polyolefin high breathability cast film is formed. This method cannot effectively form pores and control the pore size, and further uses an internal mixer, which makes the process cumbersome and complicated.
[0007] CN101747548A discloses a compound for preparing high-strength polyolefin breathable film and its preparation method. The compound includes polyolefin resin, micron-scale inorganic filler and nano-scale inorganic filler, antioxidant, processing aid, and coupling agent. The nano-scale inorganic filler can improve the mechanical properties of the polyolefin breathable film and reduce the thickness of the breathable film. In addition, by adjusting the processing conditions, a breathable film with high strength and high breathability can be prepared. However, the poor compatibility between the nano-inorganic filler and the polyolefin resin will cause the breathability of the material to be non-uniform, thus affecting the use of the breathable film.
[0008] Currently, inorganic porogens used in the production of commercially available breathable films have the following problems: (1) they are prone to aggregation; (2) their particle size is large and their particle size distribution is non-uniform, resulting in poor pore size uniformity in the breathable film or the occurrence of numerous pinhole defects; (3) the surface modification effect of the filler particles is low and their compatibility with the matrix is poor, thereby affecting the strength of the film; and (4) the dispersibility of the filler particles is poor, leading to migration to the surface of the breathable film, causing color differences or spots on the breathable film.
[0009] In recent years, some publications have reported the use of organic porogens in breathable films. For example, Bo Shi et al. ("New Breathable Films Using a Themoplastic Cross-Linked Starch as a Porogen", J. Appl. Polym. SCI, 2014, 41016, pp. 1-8) disclose a biodegradable breathable film prepared by using natural corn and chemically cross-linked starch as organic porogens and poly(butylene adipate terephthalate) as the matrix resin. This film does not use polyolefin as the matrix resin. In addition, no inorganic porogens are used, but monoglycerides and diglycerides need to be used as surfactants to convert the two starch porogens into thermoplastic starch or thermoplastic cross-linked starch before mixing with the copolyester during film preparation.
[0010] Summary of the Invention In order to overcome the shortcomings existing in the prior art, one object of the present invention is to provide a polyethylene composition for preparing a polyolefin microporous breathable film, which can achieve good dispersion of porogen in a polyethylene matrix resin without aggregation when no coupling agent, dispersant and / or surfactant is used, and thus can avoid the shortcomings of inorganic porogen such as non-uniform pore size distribution, poor dispersion, poor compatibility, etc. When the breathable film is prepared using this composition, uniform breathability and improved water vapor transmission rate can be achieved.
[0011] Another object of the present invention is to provide a polyolefin microporous breathable film and a breathable composite article comprising the film, which has the characteristics of widely adjustable physical properties and breathability, wide applicability, easy operation, and stable product performance.
[0012] In the present invention, it has been unexpectedly found that the above object is achieved by using maleic anhydride copolymer microspheres as organic porogens in polyethylene matrix resins. The copolymer microspheres have suitable compatibility and binding strength with the polyethylene matrix resins, in particular, the copolymer microspheres have even a uniform particle size distribution (monodisperse particle size distribution) and preferably have a spherical shape. This allows the porogens to be well and uniformly dispersed in the polyethylene matrix resin, not aggregate therein, and properly bonded therewith without the use of coupling agents, dispersants and / or surfactants. Thus, micropores permeable to air and water vapor but impermeable to liquid water can be generated in the film during the film preparation process by casting and stretching, and such micropores even have a uniform pore size.
[0013] Thus, according to a first aspect, the present invention provides a polyethylene composition comprising a polyethylene matrix resin and a porogen, the porogen being used in an amount of 30 parts by weight to 110 parts by weight based on 100 parts by weight of the polyethylene matrix resin, the porogen comprising maleic anhydride copolymer microspheres, the copolymer in said microspheres comprising structural units A from maleic anhydride, structural units B from a vinyl-containing comonomer M and, optionally, crosslinking structural units from a crosslinker, and the maleic anhydride copolymer microspheres having an average particle size of 500 nm to 2000 nm.
[0014] According to a second aspect, the present invention provides the use of the polyethylene composition of the present invention for preparing a polyolefin microporous breathable film.
[0015] According to a third aspect, the present invention provides a polyolefin microporous breathable film prepared from the polyethylene composition according to the present invention.
[0016] According to a fourth aspect, the present invention provides a breathable composite article comprising a polyolefin microporous breathable film according to the present invention.
[0017] Description of the drawings FIG. 1 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-1; FIG. 2 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-3; [Figure 3] Figure 3 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-5; FIG. 4 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-6; [Figure 5] Figure 5 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-1; [Figure 6] Figure 6 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-2; [Figure 7] Figure 7 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-3; FIG. 8 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-1; FIG. 9 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-3; FIG. 10 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-4; FIG. 11 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-6; FIG. 12 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example II-1; FIG. 13 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example II-2; FIG. 14 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example II-3.
[0018] Detailed Description of the Invention According to a first aspect, the present invention provides a polyethylene composition comprising a polyethylene matrix resin and a porogen, the porogen having a content of 30 parts by weight to 110 parts by weight based on 100 parts by weight of the polyethylene matrix resin, the porogen comprising maleic anhydride copolymer microspheres, the copolymer in the microspheres comprising structural units A from maleic anhydride and structural units B from a vinyl-containing comonomer M, and an average particle size of the maleic anhydride copolymer microspheres being 500 nm to 2000 nm.
[0019] In this specification, porogen refers to an additive added to a composition for preparing a breathable film, which can generate micropores in the film during the process of preparing the film by orientation, the micropores being large enough to allow gases, including air and water vapor, to pass through, but not allow liquids, such as water droplets and sweat, to pass through.
[0020] As used herein, microspheres refer to particles having a size on the micron scale and may be in the form of spherical, near-spherical, or non-spherical particles.
[0021] In this specification, the average particle size means the number average particle size, and is measured using a scanning electron microscope. Specifically, 500 microspheres are selected from a scanning electron microscope photograph, their diameters are measured, and the average particle size is calculated using the arithmetic mean method. In the case of spherical particles, the diameter is the diameter of the sphere. In the case of nearly spherical particles, the diameter is the diameter of the sphere that corresponds to the nearly spherical object. In the case of non-spherical particles, the diameter refers to the vertical axis of the particle (the distance between the two furthest points on the particle profile).
[0022] As used herein, the terms "spherical" and "near spherical" mean that the particle has an aspect ratio substantially in the range of 1 to 2.
[0023] [Porogen] In the polyethylene composition of the present invention, the porogen can be used in an amount of 30 parts by weight to 110 parts by weight, preferably 35 parts by weight to 110 parts by weight, more preferably 50 parts by weight to 100 parts by weight, and even more preferably 50 parts by weight to 90 parts by weight, based on 100 parts by weight of the polyethylene matrix resin.
[0024] The polyethylene composition of the present invention comprises maleic anhydride copolymer microspheres as the organic porogen, and preferably comprises only maleic anhydride copolymer microspheres as the porogen.
[0025] The average particle size of the maleic anhydride copolymer microspheres used in the present invention is smaller than the average particle size of inorganic porogens (e.g., calcium carbonate) used in the prior art, and may be 500nm to 2000nm, preferably 500nm to 1700nm, preferably 500nm to 1600nm, preferably 500nm to 1500nm, more preferably 600nm to 1300nm, more preferably 800nm to 1300nm, more preferably 900nm to 1200nm.
[0026] The maleic anhydride copolymer microspheres are preferably spherical or near spherical.
[0027] The maleic anhydride copolymer microspheres preferably have a uniform particle size distribution. Preferably, the copolymer microspheres are monodisperse copolymer microspheres, in particular having a particle size distribution coefficient of 1.05 to 1.0001, preferably 1.035 to 1.002, more preferably 1.028 to 1.002.
[0028] The particle size distribution coefficient (U) is measured by the following method: a sample is taken from the polymer dispersion and the morphology of the polymer microspheres is observed using a scanning electron microscope. The size of the microspheres is determined by the average particle size (D n ) and the particle size distribution is expressed by the dispersion coefficient. The formula is as follows:
[0029] [ka]
[0030] In the formula, D i i th is the particle diameter (nm), N is the sample size, and D n is the defined mathematical mean diameter, and D w is the defined weight average diameter.
[0031] Such a uniform particle size distribution allows for a more uniform distribution of pores in the prepared breathable film.
[0032] The molar ratio of structural units A from maleic anhydride to structural units B from vinyl-containing comonomer M in the maleic anhydride copolymer microspheres may range from (0.5:1) to (1:0.5), preferably from (0.75:1) to (1:0.75).
[0033] Based on the total molar amount of the structural units A and B in the copolymer, the molar content of the structural unit A may be 48% to 55%, preferably 48% to 53%, and the molar content of the structural unit B may be 45% to 52%, preferably 47% to 52%. More preferably, the molar content of the structural unit A is 49% to 51%, and the molar content of the structural unit B is 49% to 51%, i.e., the copolymer preferably has an alternating copolymerization structure.
[0034] The vinyl-containing comonomer M is preferably at least one selected from the group consisting of styrene, alpha-methylstyrene, vinyl acetate, mixed C4 and mixed C5.
[0035] In the present invention, mixed C4 refers to a general term for hydrocarbon compounds having 4 carbon atoms (mainly including butene). Generally, C4 contains a variety of butenes with different structures (such as trans-2-butene, cis-2-butene, n-butene, and isobutene), as well as a certain amount of alkanes (e.g., n-butane) and other possible impurities. In the present invention, the content of olefins in mixed C4 is in the range of 60% by weight to 75% by weight.
[0036] In the present invention, mixed C5 refers to a general term for hydrocarbon compounds having 5 carbon atoms (mainly including pentene). In general, C5 contains various different structures of pentenes (dienes (isopentadiene, cyclopentadiene, 1,4-pentadiene, and piperylene), and monoolefins (1-pentene, 2-pentene, cyclopentene, 2-methyl-1-butene, and 2-methyl-2-butene), as well as a certain amount of alkanes (n-pentane, isopentane, cyclopentane, and 2-methylbutane), alkynes (butyne-2, and 3-penten-1-yne, etc.), and other possible impurities. In the present invention, the content of olefins in mixed C5 is 55% by weight to 65% by weight.
[0037] Mixed C4 and mixed C5 can be derived from petroleum refining or petrochemical manufacturing processes (C4 and C5 fractions obtained from ethylene cracking processes, liquefied fuels produced in petroleum refining processes, cracked gas produced from naphtha cracking, gas produced by preparing olefins from methanol, etc.).
[0038] In one embodiment, the maleic anhydride copolymer microspheres may be maleic anhydride copolymer microspheres crosslinked by a crosslinking agent. The copolymer in said microspheres further comprises crosslinked structural units from the crosslinking agent. The crosslinking degree of the copolymer microspheres may be ≧65%, more preferably ≧70%. The crosslinking degree is determined by an extraction method using tetrahydrofuran.
[0039] Structural units A and B in the crosslinked maleic anhydride copolymer microspheres are also as described above.
[0040] The crosslinking agent described herein can be various common vinyl-containing monomers having difunctionality or higher functionality capable of free radical polymerization. Preferably, the crosslinking agent is at least one selected from the group consisting of divinylbenzene and an acrylate crosslinking agent containing at least two acrylate groups. The structural formula of the acrylate group is preferably -OC(O)-C(R')=CH2, where R' is H or C1-C4 alkyl (e.g., methyl). More preferably, the crosslinking agent is divinylbenzene, propylene glycol bis(meth)acrylate (such as 1,3-propanediol dimethacrylate, 1,2-propanediol dimethacrylate, 1,3-propanediol diacrylate, and 1,2-propanediol diacrylate), ethylene glycol bis(meth)acrylate (such as ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, tri ... acrylate, tetraethylene glycol dimethacrylate, and tetraethylene glycol diacrylate), trimethylolpropane tri(meth)acrylate, bistrimethylolpropane tetra(meth)acrylate, polyethylene glycol bis(meth)acrylate, diethylene glycol diacrylate phthalate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and at least one selected from the group consisting of ethoxylated multifunctional acrylates. More preferably, the crosslinking agent is divinylbenzene.
[0041] In the crosslinked maleic anhydride copolymer microspheres, the molar ratio of the structural unit A to the structural unit B to the crosslinked structural unit may be 100:(100-120):(1-40), preferably 100:(100-105):(10-30).
[0042] Maleic anhydride copolymer microspheres can be prepared by methods known in the art, particularly the two methods mentioned below.
[0043] In a first preparation method, the maleic anhydride copolymer microspheres can be prepared by a process comprising the steps of: (1) dissolving maleic anhydride, a comonomer and an initiator in an inert atmosphere in a reaction medium to form a homogeneous solution, the comonomer may be at least one selected from the group consisting of styrene, α-methylstyrene and vinyl acetate; (2) subjecting the homogeneous solution to a polymerization reaction to obtain a copolymer emulsion suspension, and then obtaining maleic anhydride copolymer microspheres by solid-liquid separation.
[0044] Based on the total weight of maleic anhydride and comonomer, maleic anhydride is used in an amount of 50% to 90% by weight and the comonomer is used in an amount of 10% to 50% by weight; preferably, maleic anhydride is used in an amount of 50% to 60% by weight and the comonomer is used in an amount of 40% to 50% by weight.
[0045] In step (1) of this method, the combined mass concentration of maleic anhydride and comonomer may be 5% to 25% by weight, preferably 5% to 20% by weight, based on the total weight of the homogeneous solution, and the mass concentration of initiator may be 0.01% to 5% by weight, preferably 1% to 4% by weight, based on the total weight of the homogeneous solution.
[0046] The reaction medium can be selected from ketones and mixtures thereof with alkanes, and is preferably a mixture of a compound of formula (1) with an alkane:
[0047] [ka]
[0048] In the formula, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, and more preferably methyl or ethyl.
[0049] The alkane is preferably an alkane having 6 to 12 carbon atoms, preferably at least one selected from the group consisting of hexane, heptane and octane, more preferably hexane. Based on the total volume of the reaction medium, the amount of the alkane may be 50% by volume to 90% by volume, preferably 60% by volume to 80% by volume.
[0050] In this method, by using a mixture of the compound represented by formula (1) and an alkane (which can interact with a certain amount of maleic anhydride and comonomer) as a reaction medium, a self-stabilizing precipitation polymerization reaction between maleic anhydride and comonomer can be achieved, and this polymerization reaction system does not require the addition of stabilizers and co-stabilizers and has a self-stabilizing dispersion effect. The obtained polymer microspheres have a uniform particle size and a clean surface without contamination (as can be seen by observing the surface with SEM photographs).
[0051] The polymerization reaction in step (2) can be carried out under an inert atmosphere, which can be provided by a conventional inert gas (e.g., nitrogen) in the prior art. The polymerization reaction conditions can include a polymerization temperature of 61°C to 100°C, preferably 70°C to 90°C; and a polymerization time of 1 hour to 24 hours, preferably 2 hours to 12 hours.
[0052] The solid-liquid separation may be a conventional solid-liquid separation mode in the technical field (for example, centrifugation or flash separation). When centrifugation is employed, the centrifugal rotation speed can be 1500 rad / min to 5000 rad / min, and the centrifugation time can be 5 minutes to 60 minutes. When flash separation is employed, it can be performed in a flash separator, the flash temperature can be 10°C to 40°C, and the flash pressure can be about 0 MPa.
[0053] In this preparation method, maleic anhydride monomer and comonomer are copolymerized in a certain ratio, so that the prepared maleic anhydride copolymer takes microspheres with excellent uniformity, the copolymer features clean surface, disperses well in the medium, and does not aggregate. Especially, when the amount of maleic anhydride is 50wt%-60wt% and the amount of comonomer is 40wt%-50wt% based on the total weight of polymerizable monomers, the prepared maleic anhydride copolymer microspheres have uniform particles, excellent particle morphology, and clean particle surface, and the copolymer microspheres have better comprehensive performance.
[0054] In a second preparation method, maleic anhydride copolymer microspheres can be prepared by a method comprising the steps of: A process for subjecting maleic anhydride, comonomer M and optionally crosslinking agent to copolymerization reaction in the presence of an initiator in an organic solvent under an inert atmosphere to obtain optionally crosslinked maleic anhydride copolymer microspheres, said comonomer M being at least one selected from the group consisting of styrene, α-methylstyrene, vinyl acetate, mixed C4 and mixed C5. In the present specification, when non-crosslinked maleic anhydride copolymer microspheres are prepared, comonomer M is preferably selected from mixed C4 and / or mixed C5.
[0055] In this preparation method, the copolymerization reaction may be a one-step reaction by precipitation polymerization. The copolymerization reaction can be carried out at a temperature of 50°C to 100°C, preferably 60°C to 90°C, more preferably 70°C to 90°C, under a pressure of 0.1 MPa to 2 MPa, preferably 0.2 MPa to 2 MPa, preferably 0.5 MPa to 1 MPa, for a reaction time of 3 hours to 15 hours, preferably 5 hours to 12 hours, more preferably 5 hours to 10 hours, preferably 6 hours to 9 hours.
[0056] Unless otherwise specified, pressures stated herein refer to gauge pressures.
[0057] The weight ratio of maleic anhydride to the comonomer may be 1:(0.2-3), preferably 1:(0.8-3), or the amount of the comonomer M may be 50-150 mol, more preferably 75-100 mol, relative to 100 mol of maleic anhydride.
[0058] The organic solvent may include an organic acid alkyl ester, for example, selected from an organic acid alkyl ester, or a mixture of an organic acid alkyl ester and an alkane, or a mixture of an organic acid alkyl ester and an aromatic hydrocarbon. The organic acid alkyl ester includes, but is not limited to, at least one of methyl formate, ethyl formate, propyl formate, butyl formate, isobutyl formate, amyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, amyl acetate, isoamyl acetate, benzyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate, isobutyl butyrate, isoamyl butyrate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate, and ethyl phenylacetate, preferably at least one selected from isoamyl acetate, butyl acetate, isopropyl acetate, and ethyl acetate. Alkanes include, but are not limited to, n-hexane and / or n-heptane. Aromatic hydrocarbons include, but are not limited to, at least one of benzene, toluene, and xylene.
[0059] The amount of organic solvent is not particularly limited as long as it can provide a medium for the reaction. Preferably, the amount of organic solvent can be 50L to 150L, more preferably 75L to 100L, for 100 moles of maleic anhydride; or, based on the total weight of the organic solvent, the concentration of maleic anhydride can be 5% by weight to 25% by weight, preferably 10% by weight to 20% by weight.
[0060] In these two preparation methods, the amount of the initiator is not particularly required. Preferably, based on the total amount of maleic anhydride, the amount of the initiator may be 0.05 mol% to 20 mol%, preferably 0.05 mol% to 10 mol%, more preferably 1 mol% to 1.5 mol%.
[0061] The initiator may be a common reagent in the art used to initiate the polymerization reaction of maleic anhydride with vinyl-containing monomers, such as α-methylstyrene (or styrene), or may be a pyrolytic initiator, such as an organic peroxide and / or an azo compound. The organic peroxide may be at least one selected from the group consisting of dibenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, dodecanoyl peroxide, tert-butyl peroxybenzoate, diisopropyl peroxydicarbonate, and dicyclohexyl peroxydicarbonate. The azo compound may be selected from azobisisobutyronitrile and / or azobisisoheptanitrile.
[0062] A water bath and / or an oil bath can be used to provide the heat required for the polymerization.
[0063] In the preparation method of crosslinked maleic anhydride copolymer microspheres, the amount of comonomer M can be 50 mol-150 mol, preferably 75 mol-100 mol, based on 100 mol of maleic anhydride; the amount of crosslinker can be 1 mol-40 mol, preferably 10 mol-20 mol, more preferably 15 mol-20 mol; and the amount of initiator can be 0.05 mol-10 mol, preferably 1 mol-1.5 mol, based on 100 mol of maleic anhydride.
[0064] In the method for preparing crosslinked maleic anhydride copolymer microspheres, the reaction conditions may include carrying out the reaction in an inert atmosphere at a reaction temperature of 50°C to 90°C, preferably 60°C to 70°C, for a reaction time of 3 hours to 15 hours, preferably 5 hours to 12 hours, under a reaction pressure of 0.1 MPa to 1 MPa, preferably 0.1 MPa to 0.5 MPa. The product (suspension) obtained by the polymerization reaction is subjected to post-treatment steps such as separation, washing, and drying to obtain crosslinked maleic anhydride copolymer microspheres.
[0065] The copolymer emulsion suspension obtained by the polymerization reaction can be separated by solid-liquid separation to obtain composite microspheres. Conventional solid-liquid separation methods in the prior art can be used, and centrifugal separation is preferred. When centrifugal separation is used, the centrifugal rotation speed is 1500 rad / min to 5000 rad / min, and the centrifugal time is 5 minutes to 60 minutes.
[0066] By adding maleic anhydride copolymer microspheres as a porogen to the composition of the present invention, the porogen can be uniformly dispersed in the polyethylene matrix without using coupling agents, dispersing agents and / or surfactants, and the micropores have a suitable and uniform pore size; by adjusting the maleic anhydride copolymer microspheres, the physical properties and breathability can be widely adjusted, and a breathable film characterized by wide applicability, simple operation and stable product performance can be realized.
[0067] Furthermore, by adding maleic anhydride copolymer microspheres as an organic porogen, the melting enthalpy ΔH of the polyethylene matrix resin, which satisfies the following relationship, mPE and the fusion enthalpy ΔH of the polyethylene composition. m 組成物 and in particular can be achieved: ΔH m PE and ΔH m 組成物 The difference between the above is in the range of 8 J / g to 48 J / g, preferably 10 J / g to 45 J / g, and more preferably 20 J / g to 45 J / g.
[0068] When the difference between the fusion enthalpy of the polyethylene and the fusion enthalpy of the polyethylene composition is sufficiently within the above range, the maleic anhydride copolymer microspheres are uniformly distributed in the polyethylene composition and the phenomenon in which the fusion enthalpy of the composition is significantly reduced due to aggregation of the maleic anhydride copolymer microspheres does not occur, so that a breathable film prepared from the composition has both excellent physical properties and breathability.
[0069] In the present invention, the enthalpy of fusion of the polyethylene and polyethylene compositions is measured by differential scanning calorimetry.
[0070] Furthermore, the density ρ 組成物 and the density of polyethylene, ρ PE The relation can be satisfied: ρ 組成物 and ρ PE The difference is 0.045g / cm 3 ~0.155g / cm 3 In the case where the maleic anhydride copolymer microspheres are non-crosslinked maleic anhydride copolymer microspheres, the difference is preferably in the range of 0.055 g / cm 3 ~0.155g / cm 3 , more preferably 0.068 g / cm 3 ~0.145g / cm 3 When the maleic anhydride copolymer microspheres are crosslinked maleic anhydride copolymer microspheres, the difference is preferably 0.045 g / cm 3 ~0.120g / cm 3 , more preferably 0.050 g / cm 3 ~0.110g / cm 3 It is.
[0071] The density of polyethylene is measured using a density gradient column method according to the method specified in GB / T 1033.2-2010.
[0072] The density of the polyethylene composition is measured in accordance with the method specified in GB / T 3682-2000 by using a melt flow rate meter to extrude a bubble-free molten test piece at 190°C under a load of 2.16 kg, and then by a mass volume method using a balance, a 25 mL volumetric flask and absolute ethanol.
[0073] [Polyethylene matrix resin] The composition of the present invention uses polyethylene as matrix resin.The polyethylene matrix resin can be selected from ethylene homopolymers (such as low density polyethylene (LDPE), high density polyethylene (HDPE) and ultra-high molecular weight polyethylene (UHMWPE)), ethylene copolymers (such as linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), high density polyethylene (HDPE), medium density polyethylene (MDPE), ethylene-vinyl acetate copolymer and ethylene-methyl acrylate copolymer), and mixtures thereof or mixtures with other polyolefins (such as propylene homopolymers, propylene-based copolymers, polyolefin plastomers, polyolefin elastomers and polybutylene).
[0074] The polyethylene matrix resin is preferably selected from a mixture of linear low density polyethylene and low density polyethylene, and the amount of the linear low density polyethylene can be 60 to 99 parts by weight, preferably 70 to 95 parts by weight, based on 100 parts by weight of polyethylene, and the amount of the low density polyethylene can be 1 to 40 parts by weight, preferably 5 to 30 parts by weight, based on 100 parts by weight of polyethylene.
[0075] The linear low density polyethylene may be a copolymer of ethylene and an α-olefin. Preferably, the α-olefin is at least one selected from the group consisting of butene, hexene, and octene.
[0076] Linear low density polyethylene is 0.905 g / cm 3 ~0.935g / cm3 Preferably, the linear low density polyethylene has a melt flow rate of 0.5 g / 10 min to 10 g / 10 min, preferably 2 g / 10 min to 6 g / 10 min, at 190° C. under a load of 2.16 kg. Preferably, the linear low density polyethylene has a molecular weight distribution of 2 to 12, preferably 2 to 10.
[0077] The density of low density polyethylene is 0.913 g / cm 3 ~0.934g / cm 3 The melt flow rate of the low-density polyethylene under a load of 2.16 kg at 190° C. is preferably 0.1 g / 10 min to 12 g / 10 min, preferably 2 g / 10 min to 9 g / 10 min. The molecular weight distribution of the low-density polyethylene is preferably 5 to 11, more preferably 6 to 10.
[0078] In this specification, the melt flow rate MFR is measured at 190° C. under a load of 2.16 kg according to the method specified in GB / T 3682-2000; the density is measured using a density gradient column method according to the method specified in GB / T 1033.2-2010; and the molecular weight distribution is measured by GPC.
[0079] Ethylene homopolymers and copolymers are commercially available or can be prepared by methods known in the art. Linear low density polyethylene is preferably prepared by catalytic polymerization using Ziegler-Natta and / or metallocene catalysts.
[0080] [Antioxidants] The polyethylene composition may further contain an antioxidant. The amount of the antioxidant is preferably 0.1 to 2.5 parts by weight, preferably 0.1 to 2 parts by weight, more preferably 0.1 to 1.5 parts by weight, and further preferably 0.2 to 1.5 parts by weight, based on 100 parts by weight of the polyethylene matrix resin.
[0081] The antioxidant may be any antioxidant known in the art suitable for polyolefin compositions, such as at least one, preferably at least two, of the following antioxidants: hindered phenols, phosphites and thioesters, preferably at least one selected from the group consisting of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite, octadecyl propionate (e.g., n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and alkylated polyphenols.
[0082] In a preferred embodiment, the antioxidant is an antioxidant complex additive comprising an antioxidant and an acid acceptor. The weight ratio of the antioxidant to the acid acceptor may be 1-6:1, preferably 2-5:1. The acid acceptor may be a stearate, preferably at least one selected from the group consisting of calcium stearate, zinc stearate, and sodium stearate.
[0083] Preferably, the antioxidant complex additive is a mixture of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate, wherein the weight ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate can be (1-3):(1-3):1, preferably (1-2):(1-2):1.
[0084] [Other additives] By using maleic anhydride copolymer microspheres as the organic porogen, the polyethylene composition of the present invention can be free of coupling agents, dispersing agents or surfactants, or free of two or three of them (e.g., free of coupling agents and dispersing agents).
[0085] Coupling agents refer to additives commonly used in the art to improve the interfacial properties between the matrix resin and inorganic fillers or reinforcing materials in plastic compounds, such as stearic acid, zinc stearate, calcium stearate, magnesium stearate, titanate ester coupling agents, aluminate ester coupling agents, silane coupling agents, lanthanum stearate and other rare earth carboxylate coupling agents, and Ti-Al and Al-Zr complex coupling agents (used in the prior art in polyethylene breathable films using inorganic porogens).
[0086] Dispersants refer to additives that can enhance and improve the dispersion performance of solid or liquid materials in a medium, thereby reducing the aggregation of solid or liquid particles in the dispersion system. For example, paraffin oil, PE wax, polyethylene oxide (OPE) dispersant, higher alcohol (C 16 -C 18 ) (used in the prior art in polyethylene breathable films using inorganic porogens).
[0087] Surfactants refer to compounds that can reduce the surface tension (or interfacial tension) between two liquids, between a gas and a liquid, or between a liquid and a solid, such as the mono- and diglycerides that have been used in the prior art in polyester breathable films using starch as a porogen.
[0088] However, the composition of the present invention may further comprise an inorganic porogen selected from calcium carbonate, barium sulfate, titanium dioxide, talc, clay, etc. as a second porogen, and may also comprise other conventional additives suitable for breathable films.
[0089] Preparation of Polyethylene Composition and Product Morphology The polyethylene composition of the present invention may be in the form of a powder or pellets.
[0090] The powder can be prepared by mixing the various components. Any suitable mixing device can be used here.
[0091] The pellets can be obtained by melt compounding, extruding, pelletizing and drying the polyethylene composition. Any suitable extruder, preferably a twin screw extruder, can be used here. The pellets can be prepared using conventional processing conditions.
[0092] Specifically, the pellets can be prepared by a method comprising the steps of: (1) mixing a polyethylene matrix resin, a porogen, and optionally other additives to obtain a mixture; and (2) A step of melt-kneading the mixture in a twin-screw extruder, extruding, granulating, and drying to obtain polyethylene composition pellets.
[0093] The rotation speed of the twin-screw extruder can be 150 r / min to 400 r / min, preferably 180 r / min to 350 r / min. The temperatures of the feed section, melt section, homogenization section, and die of the twin-screw extruder can be 150°C to 180°C, 165°C to 200°C, 180°C to 215°C, and 175°C to 210°C, respectively. Preferably, the temperatures of the feed section, melt section, homogenization section, and die of the twin-screw extruder are 160°C to 175°C, 175°C to 190°C, 190°C to 210°C, and 180°C to 205°C, respectively.
[0094] [Breathable films and their applications] According to a second aspect, the present invention provides the use of the above polyethylene composition in a polyolefin microporous breathable film.
[0095] The polyethylene composition of the present invention can be used to prepare polyolefin microporous breathable film.The obtained breathable film has significantly improved physical properties and breathability, so it can be used as the water-proof and moisture-permeable material of various breathable composite articles, especially hygiene articles, medical articles, food packaging or building articles (such as disposable medical and hygiene products, baby diapers, adult care products, medical protective clothing, wound care bandages, dressings, food packaging films, industrial protective clothing, etc.).
[0096] According to a third aspect, the present invention provides a polyolefin microporous breathable film prepared from the polyethylene composition described above.
[0097] The method for preparing the polyolefin microporous breathable film is not particularly limited. An appropriate method can be selected as necessary, and it can be preferably prepared by extrusion casting and stretching. For example, a polyethylene composition is added to an extrusion casting machine, and a cast sheet is melted and cast at an extrusion temperature of 210°C to 240°C and a cooling roller temperature of 20°C to 60°C, thereby producing a polyethylene cast film. The cast film is then uniaxially stretched 2 to 5 times to obtain a polyethylene microporous breathable film having an average thickness of 25 μm to 35 μm. The heat setting temperature at this time is 70°C to 120°C.
[0098] The polyolefin microporous breathable film of the present invention has at least one of the following characteristics: 1)Thickness of 25μm~35μm; 2) 3060g / (m 2 Water vapor transmission rate of at least 24h; 3) porosity of 38% or more; 4) tensile strength in the longitudinal direction ≥ 25MPa, tensile strength in the transverse direction ≥ 5MPa, elongation at break in the longitudinal direction ≥ 125%, elongation at break in the transverse direction ≥ 355%; and 5) 24.5g / m 2 Surface density of the following breathable films (measured on a sample having a thickness of 30 microns):
[0099] The polyolefin microporous breathable film prepared from the above polyethylene composition not only maintains the excellent physical properties of the polyethylene composition, but more importantly, the polyolefin microporous breathable film has high breathability and can be used as a water-proof and moisture-permeable material for use in various breathable composite articles.
[0100] Thus, according to a fourth aspect, the present invention provides a breathable composite article comprising a polyolefin microporous breathable film, in particular a hygiene article, a medical article, a food packaging or a building article (such as disposable medical and hygiene products, baby diapers, adult care products, medical protective clothing, wound care bandages, dressings, food packaging films, industrial protective clothing, etc.).
[0101] The end points of the ranges and any values disclosed herein are not limited to the exact ranges or values, but these ranges or values are understood to include the values close to these ranges or values.For numerical ranges, the end points of each range and the individual point values of each range and the individual point values can be combined with each other to obtain one or more new numerical ranges.This numerical range is considered to be specifically disclosed herein.
[0102] [Example] The present invention will be described in detail below with reference to examples. It should be understood that the specific examples described here are used to explain the present invention and do not limit the present invention.
[0103] The relevant data in the present invention and examples were obtained according to the following test methods: 1. The content of each structural unit in maleic anhydride copolymer microspheres was measured using an Avance 300 nuclear magnetic resonance spectrometer from Bruker, Switzerland. 1 The compound was tested by H NMR.1 The content of each structural unit is calculated based on the ratio of the peak area corresponding to the characteristic hydrogen of the corresponding structural unit in H NMR.
[0104] 2. Polymerization yield of maleic anhydride copolymer (Cp): Cp = Mp x 100% / Mm where Mp was the mass of the resulting polymer and Mm was the total mass of monomers added.
[0105] 3. Test method for particle size of copolymer microspheres: After gold spraying under vacuum, the morphology of the copolymer microsphere powder was observed with a Hitachi S4800 field emission scanning electron microscope. 500 microspheres were selected from the electron microscope photograph, their diameters were measured, and the average particle size was calculated using the arithmetic mean method. For spherical particles, the diameter was taken as the diameter of the sphere. For near-spherical particles, the diameter was taken as the diameter of the sphere corresponding to the near-spherical object. For particles of other shapes, the diameter refers to the length of the vertical axis of the particle (the distance between the two furthest points on the particle profile).
[0106] 4. Particle size distribution of maleic anhydride copolymer microspheres: The particle size and particle size distribution of the polymer microspheres were calculated by measuring and calculating at least 500 microspheres in a scanning electron micrograph using Nano Measurer 1.2 software. The particle size and particle size distribution of the polymer microspheres were calculated according to Equations (1) to (3):
[0107] [ka]
[0108] In the formula, D i i th is the particle diameter (nm), N is the sample size, and D n is the defined mathematical mean diameter, and D w was the defined weight average diameter.
[0109] 5. Specific surface area of copolymer microspheres: Measured by nitrogen physical adsorption BET method in accordance with the international test standard ISO-9277 using an ASAP2020C+M fully automatic specific surface / porosity analyzer from Micromeritics, USA.
[0110] 6. Conversion efficiency of mixed C4: The polymer after the reaction was weighed; conversion efficiency (%) = [(4 x mass of polymer actually obtained) / (11 x mass of C4 actually used)] x 100%.
[0111] 7. Molecular weight of copolymer microspheres: The molecular weight of the samples was measured using a Waters 2410 gel permeation chromatograph manufactured by WATERS, USA. Here, the chromatography column used was three WATERS Styragel columns in series, the standard substance was polystyrene (PS), the DMF solvent system was used, and the flow rate was 1.0 mL / min.
[0112] 8. Cross-sectional morphology and porogen dispersion of polyethylene composition sample sheet: The sample was immersed in liquid nitrogen for 15 minutes, and then subjected to brittle fracture. The fractured cross section was then subjected to a gold spray treatment. The characteristics of the fractured cross section of the material were evaluated using a Hitachi S4800 field emission scanning electron microscope manufactured by Hitachi, Ltd., and a microscopic morphology photograph was obtained.
[0113] 9. Melt flow rate (MFR): Measured at 190° C. under a load of 2.16 kg using a melt flow rate meter UPXRZ-400C manufactured by Ceast of Italy in accordance with the method specified in GB / T 3682-2000.
[0114] 10. Density of polyethylene: Measured using a density gradient column method according to the method specified in GB / T 1033.2-2010.
[0115] 11. Tensile properties: The tensile properties of the polyethylene composition were measured using a 5966 universal material testing machine from INSTRON, USA, in accordance with the method specified in GB / T 1040.2-2006; the tensile properties of the breathable film were measured using an XLW intelligent electronic tensile testing machine from Labthink Instruments Co., Ltd., Jinan, China, in accordance with the method specified in GB / T 1040.3-2006.
[0116] 12.Tc, Tm and △Hm: A differential scanning calorimeter DSC25 from TA Instruments, USA was used to analyze the melting and crystallization processes of the material. The specific operation involves measuring 5mg-10mg samples (diameter 5.4mm, thickness 1mm-1.5mm) in three-step heating / cooling measurement procedures from 20℃ to 200℃ under nitrogen protection. The change in heat flow reflects the melting and crystallization processes of the material. Calculate the crystallization temperature Tc, melting temperature Tm, and melting enthalpy △Hm according to GB / T 19466.3-2004.
[0117] 13. Density of polyethylene composition: The polyethylene composition was pressed under a load of 2.16 kg at 190°C by a UPXRZ-400C melt flow rate meter manufactured by Ceast, Italy, according to the method specified in GB / T 3682-2000 to obtain a bubble-free molten sample, which was cooled and cut into pieces, and then baked in a vacuum oven at 100°C for 8 hours to obtain a composition sample for density testing.
[0118] A 25 mL volumetric flask was placed on a balance and the tar was removed to clear it. A polyethylene composition sample was placed on it and the weight was recorded as M1. Anhydrous ethanol was slowly added to the volumetric flask with a dropper so that the polyethylene composition sample was completely immersed in the anhydrous ethanol. After the dropping was completed, the product was left to stand for 2 hours, the liquid level was kept at the same height as the graduation line of the volumetric flask, and the weight M2 was recorded. The volume of anhydrous ethanol in the volumetric flask was V エタノール =(M2-M1) / ρ エタノールThe volume of the polyethylene composition is V = 25 - V エタノール The density of the sample was ρ 組成物 =M1 / V.
[0119] 14. Water vapor transmission rate (WVTR): Measured according to the method specified in GB / T 12704-1991.
[0120] 15. Porosity of breathable film: Measured using ASTM-D2873-1994. The breathable film was immersed in n-hexadecane for 1 hour, then removed, the n-hexadecane remaining on the surface was wiped off with filter paper, the mass change of the breathable film before and after immersion was weighed, and the porosity was calculated according to formula (4).
[0121] [ka]
[0122] In the formula, m a is the mass of n-hexadecane in the breathable film after absorption, and m b is the mass of the breathable film before liquid absorption, and ρ a is the density of n-hexadecane, and ρ b was the density of a particular material.
[0123] 16. Surface density of breathable film: Measured according to GB / T 31729-2015, with the sample thickness set at 30μm.
[0124] 17. Crosslinking degree of crosslinked maleic anhydride copolymer: The crosslinking degree was characterized by the gel content. 2g-3g of polymer microspheres were weighed (the weight was recorded as w1), wrapped in medium speed qualitative filter paper, placed in a Soxhlet extractor, and extracted with tetrahydrofuran for 24 hours, the extracted polymer was dried and weighed (the weight was recorded as w2), and the crosslinking degree was calculated by w2 / w1.
[0125] 18. Content of each structural unit in crosslinked copolymer: For crosslinked maleic anhydride-α-methylstyrene copolymer microspheres, the amount of monomer or crosslinker that did not participate in the reaction was analyzed using LC-MC (Waters 2695 liquid chromatograph and Q-Tof Micro mass spectrometer, USA), and the molar ratio of structural unit A, structural unit B, and crosslinked structural unit was calculated based on the amount of feed. For crosslinked mixed C4-maleic anhydride copolymer microspheres, the carbon and oxygen contents in the polymer were measured by X-ray fluorescence spectrometry. The transparent liquid after centrifugation was analyzed by Agilent 7890A gas chromatograph, and the contents of remaining maleic anhydride and crosslinker were measured. The results were comprehensively analyzed, and the molar ratio of structural unit A, structural unit B, and crosslinked structural unit in the polymer was calculated.
[0126] Starting materials used in the examples and comparative examples were commercially available products unless otherwise specified.
[0127] Solvents and liquid monomers were treated to be free of oxygen and water.
[0128] The pressure was gauge pressure.
[0129] Preparation Example 1 Preparation of Porogen A1 302.5g maleic anhydride, 51.3g azobisisobutyronitrile, 299.9g styrene, 1.462L acetone, and 4.614L hexane (amount of hexane: 75.9% by volume) were added to a 20L reaction vessel (the amount of maleic anhydride was 50.2% by weight, and the amount of styrene was 49.8% by weight, relative to the polymerizable monomer). After the materials were mixed uniformly (in the homogeneous solution, the mass concentrations of maleic anhydride and styrene were both 6.2% by weight, and the mass concentration of the initiator was 1.1% by weight), nitrogen was introduced for 20 minutes, the temperature of the reaction vessel was raised to 70°C, and the reaction was carried out for 6 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged for 20 minutes at a rotation speed of 2000 rad / min using a centrifuge to obtain 542g of maleic anhydride-styrene copolymer microspheres A1 as the porogen, and the corresponding polymerization yield was 90%.
[0130] The copolymer microspheres A1 1 Analysis by H NMR showed that the molar content of structural unit A derived from maleic anhydride was 49.5% and the molar content of structural unit B derived from styrene was 50.5%, based on the total molar amount of the various structural units in the polymer.
[0131] The maleic anhydride copolymer microspheres A1 as the porogen have an average particle size of about 1000 nm, a particle size distribution U of 1.0026, and a molecular weight Mw of 3.52×10 4 , BET specific surface area is 6.39m 2 / g.
[0132] Preparation Example 2 Preparation of Porogen A2 The mass percentages of various components in the mixed C4 (manufactured by SINOPEC Beijing Yanshan Company, China) were as follows: 1,3-butadiene: 0.06%, trans-2-butene: 12.67%, isobutane: 37.09%, isobutene: 19.48%, cis-2-butene: 27.79%, 1-butene: 1.02%, others: 1.89%. 13.5 kg of the mixed C4 having the above composition was introduced into a 200 L reaction kettle containing an organic reaction liquid consisting of 10 kg maleic anhydride, 4 kg dibenzoyl peroxide, and 100 L isoamyl acetate, and subjected to a free radical copolymerization reaction (concentration of maleic anhydride in the organic solvent: 10.2 wt%). The copolymerization reaction pressure was 1 MPa, the copolymerization reaction temperature was 80°C, and the copolymerization reaction time was 6 hours. The weight ratio of maleic anhydride to the mixed C4 was 1:1.35.
[0133] The copolymerization reaction product was passed through a flash separator and gas-liquid separation was performed under the conditions of 30°C and 0 MPa. The obtained liquid-solid mixture was then centrifuged in a centrifuge at 4000 rad / min for 20 minutes to separate the liquid and solid, obtaining a solid product, which was returned to the reaction vessel. The solid product was washed with hexane and suction-filtered through a fritted glass funnel to obtain a filter cake, which was vacuum-dried at 90°C for 8 hours to obtain 20.5 kg of maleic anhydride-mixed C4 copolymer microspheres A2.
[0134] Maleic anhydride-mixed C4 copolymer microspheres A2 as porogen 1 Analysis by H NMR showed that the molar content of structural unit A from maleic anhydride was 49 mol %, the molar content of structural unit B from the C4 mixture was 51 mol %, based on the total molar amount of the various structural units in the polymer, and the conversion efficiency of the C4 mixture calculated by gravimetry was 55 wt %.
[0135] Maleic anhydride-mixed C4 copolymer microspheres A2 have an average particle size of about 1200 nm, a particle size distribution U of 1.0048, and a molecular weight Mw of 3.06×10 4 , BET specific surface area is 3.57m 2 / g.
[0136] Preparation Example 3 Preparation of Porogen A3 Into a 20L reactor, 376.4g of maleic anhydride, 48.8g of azobisisobutyronitrile, 256.6g of styrene, 1.165L of acetone, and 4.614L of hexane (amount of hexane: 79.8% by volume) were charged (the amount of maleic anhydride was 59.5% by weight and the amount of styrene was 40.5% by weight relative to the polymerizable monomer). After the materials were uniformly mixed (in the homogeneous solution, the mass concentration of maleic anhydride was 8.1% by weight, the mass concentration of styrene was 5.5% by weight, and the mass concentration of the initiator was 1.1% by weight), nitrogen was introduced for 20 minutes, the temperature of the reactor was raised to 70°C, and the reaction was carried out for 8 hours. After the reaction was completed, the resulting polymer emulsion suspension was centrifuged at a rotation speed of 2000 rad / min for 20 min using a centrifuge to obtain 493 g of maleic anhydride-styrene copolymer microspheres A3 as the porogen, with a corresponding polymerization yield of 78%.
[0137] Polymer microspheres 1 Analysis by H NMR showed that the molar content of structural unit A derived from maleic anhydride was 48% and the molar content of structural unit B derived from styrene was 52%, based on the total molar amount of the various structural units in the polymer.
[0138] The maleic anhydride copolymer microspheres A3 as the porogen have an average particle size of about 1200 nm, a particle size distribution U of 1.0034, and a molecular weight Mw of 3.89×10 4 , BET specific surface area is 5.67m 2 / g.
[0139] Preparation Example 4 Preparation of Porogen A4 Into a 20L reactor, 262.6g of maleic anhydride, 51.3g of azobisisobutyronitrile, 235.1g of styrene, 1.253L of acetone, and 4.614L of hexane (amount of hexane: 78.6% by volume) were charged (relative to the polymerizable monomer, the amount of maleic anhydride was 52.8% by weight, and the amount of styrene was 47.2% by weight). After the materials were mixed uniformly (in the homogeneous solution, the mass concentration of maleic anhydride was 5.7% by weight, the mass concentration of styrene was 5.1% by weight, and the mass concentration of the initiator was 1.1% by weight, respectively), nitrogen was introduced for 20 minutes, and the temperature of the reactor was raised to 70°C to react for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged for 20 minutes at a rotation speed of 2000 rad / min using a centrifuge to obtain 438g of maleic anhydride copolymer microspheres A4 as a porogen, and the corresponding polymerization yield was 88%.
[0140] The copolymer microspheres 1 Analysis by H NMR showed that the molar content of structural unit A derived from maleic anhydride was 49% and the molar content of structural unit B derived from styrene was 51%, based on the total molar amount of the various structural units in the polymer.
[0141] The maleic anhydride copolymer microspheres A4 as the porogen have an average particle size of about 700 nm, a particle size distribution U of 1.0038, and a molecular weight Mw of 3.18×10 4 , BET specific surface area is 7.98m 2 / g.
[0142] Preparation Example 5 Preparation of Porogen A5 Into a 20L reactor, 124.6g of maleic anhydride, 51.3g of azobisisobutyronitrile, 129.9g of styrene, 2.307L of acetone, and 2.645L of hexane (amount of hexane: 53.4% by volume) were charged (relative to the polymerizable monomer, the amount of maleic anhydride was 49.0% by weight, and the amount of styrene was 51.0% by weight). After the materials were mixed uniformly (in the homogeneous solution, the mass concentration of maleic anhydride was 3.2% by weight, the mass concentration of styrene was 3.4% by weight, and the mass concentration of the initiator was 1.3% by weight), nitrogen was introduced for 20 minutes, and the temperature of the reactor was raised to 70°C to react for 4 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged for 20 minutes at a rotation speed of 2000 rad / min using a centrifuge to obtain 191g of maleic anhydride copolymer microspheres A5 as a porogen, and the corresponding polymerization yield was 75%.
[0143] The copolymer microspheres 1 Analysis by H NMR showed that the molar content of structural unit A derived from maleic anhydride was 47% and the molar content of structural unit B derived from styrene was 53%, based on the total molar amount of the various structural units in the polymer.
[0144] The maleic anhydride copolymer microspheres A5 as the porogen have an average particle size of about 460 nm, a particle size distribution U of 1.0098, and a molecular weight Mw of 2.03×10 4 , BET specific surface area is 9.67m 2 / g.
[0145] Preparation Example 6 Preparation of porogen B1 In a 20L reactor, 400g of maleic anhydride, 472g of α-methylstyrene, 95g of divinylbenzene, and 8g of azobisisobutyronitrile were dissolved in 4L of isoamyl acetate, and reacted for 5 hours at 0.1MPa and 70°C under a nitrogen atmosphere. The amount of α-methylstyrene was 97.9mol, the amount of divinylbenzene was 17.9mol, and the amount of initiator was 1.2mol, relative to 100mol of maleic anhydride. The system after the reaction was centrifuged at 5000rad / min for 30 minutes to obtain crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B1, which were washed and purified with n-hexane and dried under vacuum.
[0146] The crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B1 had a crosslinking degree of 82%, and the molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit was 100:101:25. The copolymer microspheres B1 had an average particle size of 1200 nm, a particle size distribution U of 1.0134, and a BET specific surface area of 5.97 m 2 / g.
[0147] Preparation Example 7 Preparation of Porogen B2 In a 20L reactor, 400g of maleic anhydride, 472g of α-methylstyrene, 104g of divinylbenzene, and 8g of azobisisobutyronitrile were dissolved in 4L of isoamyl acetate, and reacted for 5 hours at 0.1MPa and 70°C under a nitrogen atmosphere. The amount of α-methylstyrene was 97.9mol, the amount of divinylbenzene was 19.6mol, and the amount of initiator was 1.2mol, relative to 100mol of maleic anhydride. The system after the reaction was centrifuged at 5000rad / min for 30 minutes to obtain crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B2, which were washed and purified with n-hexane and dried under vacuum.
[0148] The crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B2 have a crosslinking degree of 84%, a molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit of 100:101:28, and a mean particle size of 900 nm, a particle size distribution U of 1.0228, and a BET specific surface area of 6.58 m 2 / g.
[0149] Preparation Example 8 Preparation of Porogen B3 In a 20L reactor, 1000g of maleic anhydride, 1200g of α-methylstyrene, 200g of divinylbenzene, and 20g of azobisisobutyronitrile were dissolved in 10L of isoamyl acetate, and reacted for 5 hours at 0.1MPa and 70°C under a nitrogen atmosphere. The amount of α-methylstyrene was 99.6 moles, the amount of divinylbenzene was 15.1 moles, and the amount of initiator was 1.2 moles, relative to 100 moles of maleic anhydride. The system after the reaction was centrifuged at 5000rad / min for 30 minutes to obtain crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B3, which were washed and purified with n-hexane and dried under vacuum.
[0150] The crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B3 had a crosslinking degree of 70%, and the molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit was 100:101:23. The copolymer microspheres B3 had an average particle size of 1500 nm, a particle size distribution U of 1.0304, and a BET specific surface area of 4.94 m 2 / g.
[0151] Preparation Example 9 Preparation of Porogen B4 The gas composition of mixed butenes (manufactured by SINOPEC Beijing Yanshan Company, China) was as follows: trans-2-butene: 40.83 wt%, cis-2-butene: 18.18 wt%, n-butane: 24.29 wt%, n-butene: 9.52 wt%, isobutene: 2.78 wt%, others: 4.4 wt%. In a 20L reactor, the weighed mixed butene (molar ratio of maleic anhydride to the active ingredient (terminal olefin) in the mixed olefin: 1:1) was introduced into 1L of isoamyl acetate solution containing 1 mol / L concentration of maleic anhydride, 0.05 mol / L concentration of azobisisobutyronitrile, and 0.2 mol / L concentration of divinylbenzene under nitrogen atmosphere (the amount of mixed butene (active ingredient) was 100 mol, the amount of divinylbenzene was 20 mol, and the amount of initiator was 5 mol for 100 mol of maleic anhydride), charged with nitrogen, pressurized to a relative pressure of 0.5 MPa, and reacted at 70°C for 6 hours. The system after the reaction was centrifuged at 5000 rad / min for 30 minutes to obtain crosslinked mixed butene-maleic anhydride copolymer microspheres B4, which were washed and purified with n-hexane and dried under vacuum.
[0152] The crosslinked mixed C4-maleic anhydride copolymer microspheres B4 had a crosslinking degree of 76%, and the molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit was 100:100:25. The copolymer microspheres B4 had an average particle size of 1100 nm, a particle size distribution U of 1.0415, and a BET specific surface area of 3.46 m 2 / g.
[0153] Preparation Example 10 Preparation of Porogen B5 Crosslinked copolymer microspheres were prepared according to the method of Preparation Example 1, except that the amount of divinylbenzene was 155 g, to obtain crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B5. Relative to 100 mol of maleic anhydride, the amount of α-methylstyrene was 97.9 mol, the amount of divinylbenzene was 29.2 mol, and the amount of initiator was 1.2 mol.
[0154] The crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B5 have a crosslinking degree of 89%, a molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit of 100:102:31, and have an average particle size of 400 nm, a particle size distribution U of 1.0676, and a BET specific surface area of 9.14 m / g. 2 It was.
[0155] Preparation Example 11 Preparation of Porogen B6 In a 20L reactor, 600g of maleic anhydride, 722g of α-methylstyrene, 110g of divinylbenzene, and 12g of azobisisobutyronitrile were dissolved in 6L of isoamyl acetate, and reacted for 5 hours at 0.1MPa and 70°C under a nitrogen atmosphere. The amount of α-methylstyrene was 99.8mol, the amount of divinylbenzene was 13.8mol, and the amount of initiator was 1.2mol, relative to 100mol of maleic anhydride. The system after the reaction was centrifuged at 5000rad / min for 30 minutes to obtain crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B6, which were washed and purified with n-hexane and dried under vacuum.
[0156] The crosslinked maleic anhydride-α-methylstyrene copolymer microspheres B6 had a crosslinking degree of 67%, and the molar ratio of the structural unit A, the structural unit B, and the crosslinked structural unit was 100:101:19. The copolymer microspheres B6 had an average particle size of 2150 nm, a particle size distribution U of 1.0688, and a BET specific surface area of 4.02 m 2 / g.
[0157] Preparation of Polyethylene Composition Example I-1 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 370 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0158] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 1 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 1 that the porogen has a uniform particle size (the particle size of the porogen in the polyethylene composition is close to the particle size of the porogen itself) and is uniformly distributed in the polyethylene matrix.
[0159] Example I-2 Linear low-density polyethylene 99 parts by weight (MFR 3.5 g / 10 min, density 0.927 g / cm 3 , molecular weight distribution 2.7; M2735 from ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 70 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis (β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris (2,4-di-tert-butylphenyl) phosphite and calcium stearate in a weight ratio of 2:2:1.
[0160] After uniform mixing, the resultant was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm.
[0161] Example I-3 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 100 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0162] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min, and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 2 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 2 that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0163] Example I-4 75 parts by weight of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 25 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 1C7A from SINOPEC Beijing Yanshan Company, China), 85 parts by weight of Porogen A2, and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0164] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0165] Example I-5 75 parts by weight of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 25 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 100 parts by weight of Porogen A3 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0166] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min, and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 3 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 3 that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0167] Example I-6 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 31C7A from SINOPEC Beijing Yanshan Company, China), 45 parts by weight of Porogen A4, and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0168] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min, and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 4 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 4 that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0169] Example I-7 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 70 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and calcium stearate in a weight ratio of 4:1.
[0170] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0171] Comparative example I-1 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd.), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 25 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0172] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min, and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 5 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 5 that the porogen has a uniform particle size, but the amount is small and distributed non-uniformly.
[0173] Comparative example I-2 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 , molecular weight distribution 7.2; 1C7A from SINOPEC Beijing Yanshan Company, China), 100 parts by weight of nano CaCO3 powder (Shanghai Yuanjiang Chemical Co., Ltd., China, 10000 mesh, BET specific surface area 4.41 m 2 / g) and 1 part by weight of an antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0174] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 6 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from FIG. 6 that the porogen is significantly aggregated.
[0175] Comparative example I-3 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3, molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 , molecular weight distribution 7.2; 1C7A from SINOPEC Beijing Yanshan Company, China), 100 parts by weight of nano BaSO4 powder (Sachtleben, Blanc Fixe Micro, organic coating, d50=0.7 μm, BET specific surface area 3.55 m 2 / g) and 1 part by weight of an antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0176] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 120 μm to 160 μm. FIG. 7 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen is significantly aggregated.
[0177] Comparative example I-4 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3140 parts by weight of Porogen A1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0178] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0179] Comparative example I-5 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 , molecular weight distribution 7.2; 1C7A from SINOPEC Beijing Yanshan Company, China), 70 parts by weight of Porogen A5 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0180] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0181] Comparative example I-6 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 70 parts by weight of crosslinked starch (National 4302 from Ingredion Food Ingredients Co, Ltd.) and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0182] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0183] Example II-1 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3, molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 1C7A from SINOPEC Beijing Yanshan Company, China), 70 parts by weight of Porogen B1, and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0184] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 160 μm to 200 μm. FIG. 8 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0185] Example II-2 Linear low-density polyethylene 82 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 38 parts by weight of random copolymer polypropylene (MFR 2.5g / 10min, molecular weight distribution 4.9, GM250E from Sinopec Shanghai Petrochemical Co., Ltd., China), 70 parts by weight of Porogen B1, and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0186] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0187] Example II-3 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 1C7A from SINOPEC Beijing Yanshan Company, China), 30 parts by weight of Porogen B2 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0188] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min, and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 160 μm to 200 μm. FIG. 9 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0189] Example II-4 75 parts by weight of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 25 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 1C7A from SINOPEC Beijing Yanshan Company, China), 50 parts by weight of Porogen B3 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0190] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 160 μm to 200 μm. FIG. 10 is an SEM photograph of the cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0191] Example II-5 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 90 parts by weight of Porogen B4 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0192] After uniform mixing, the resultant mixture was added to a twin-screw extruder, and melt-kneaded, extruded and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed zone, melt zone, homogenization zone and die of 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.
[0193] Example II-6 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 100 parts by weight of Porogen B1 and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0194] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 160 μm to 200 μm. FIG. 11 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen has a uniform particle size and is uniformly distributed in the polyethylene matrix.
[0195] Comparative Example II-1 A polyethylene composition was prepared according to the method of Example II-1, except that the amount of porogen B1 was 15 parts by weight. The properties of the polyethylene composition are shown in Table 1. Fig. 12 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. Fig. 12 shows that the porogen has a uniform particle size, but the amount is small and non-uniformly distributed.
[0196] Comparative Example II-2 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 100 parts by weight of nano-CaCO3 powder (10000 mesh, manufactured by Shanghai Yuanjiang Chemical Co., Ltd., China) were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite, and calcium stearate in a weight ratio of 2:2:1.
[0197] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and pressed into a sheet, and the thickness of the sample sheet was 160 μm to 200 μm. FIG. 13 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen is significantly aggregated.
[0198] Comparative Example II-3 Linear low-density polyethylene 90 parts by weight (MFR 3.5 g / 10 min, density 0.917 g / cm 3, molecular weight distribution 4; M2330 manufactured by ZhongKe (Guangdong) Refinery & Petrochemical Co. Ltd., China), 10 parts by weight of low-density polyethylene (MFR 7.5 g / 10 min, density 0.919 g / cm 3 100 parts by weight of nano BaSO4 powder (Blanc Fixe Micro, organic coating, d50=0.7μm, manufactured by Sachtleben) and 1 part by weight of antioxidant complex additive were mixed in a high-speed mixer. The antioxidant complex additive was a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate in a weight ratio of 2:2:1.
[0199] After uniform mixing, the obtained mixture was added to a twin-screw extruder, and melt-kneaded, extruded, and pelletized at a screw rotation speed of 200 r / min and temperatures of the feed section, melt section, homogenization section, and die of 170°C, 180°C, 200°C, and 190°C, respectively, to obtain a polyethylene composition. The prepared polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. This polyethylene composition was melted at 200°C and press-molded into a film having a thickness of 160 μm to 200 μm. FIG. 14 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition. It can be seen from the figure that the porogen is significantly aggregated.
[0200] Comparative Example II-4 A polyethylene composition was prepared according to the method of Example II-1, except that the amount of Porogen B1 was 135 parts by weight. The properties of the polyethylene composition are shown in Table 1.
[0201] Comparative Example II-5 A polyethylene composition was prepared according to the method of Example II-1, except that the porogen used was Porogen B5. The properties of the polyethylene composition are shown in Table 1.
[0202] Comparative Example II-6 A polyethylene composition was prepared according to the method of Example II-1, except that the porogen used was Porogen B6. The properties of the polyethylene composition are shown in Table 1.
[0203] [Table 1] JPEG2024540130000007.jpg37169
[0204] As can be seen from Table 1, the melt flow rate (MFR) of the polyethylene composition provided by the present invention meets the requirements of the casting process, especially ΔH m PE and △H m 組成物 When the difference between the density ρ and the density ρ is within a certain range, the maleic anhydride copolymer microspheres are uniformly distributed in the composition without aggregation. At the same time, the compositions of the examples according to the present invention also have good mechanical properties, thereby meeting the requirements of the stretch ratio of the breathable film. 組成物 and the density of polyethylene, ρ PE The difference between the porogen content and the matrix resin content was advantageously within a certain range. The composition of the present invention could achieve good dispersion of the porogen in the matrix resin without additionally using coupling agents, dispersants and surfactants.
[0205] Test Example The polyethylene compositions of the Examples and Comparative Examples were added to an extrusion cast machine, and melted and cast at an extrusion temperature of 210°C to 240°C and a cooling roller temperature of 20°C to 60°C to prepare a cast sheet, thereby obtaining a polyethylene cast film. This cast film was then uniaxially stretched three times to obtain a polyethylene microporous breathable film having an average thickness of 30 μm. The heat setting temperature at this time was 85°C. The properties of this polyethylene microporous breathable film are shown in Table 2.
[0206] [Table 2] JPEG2024540130000009.jpg4169
[0207] As can be seen from Table 2 and the SEM photographs in the drawings, in the examples according to the present invention, by using maleic anhydride copolymer microspheres as organic porogen in polyethylene matrix resin, the porogen can be well dispersed in the matrix resin without using coupling agents, dispersing agents and surfactants, which can generate a large number of uniformly distributed micropores with suitable sizes in the resulting film, and therefore the resulting breathable film has higher breathability.
[0208] In the comparative examples using inorganic porogens or crosslinked starch as organic porogens without adding dispersants, coupling agents and surfactants, both the properties of the compositions and the properties of the breathable films prepared were worse than those of the examples according to the invention, and the obtained films had fewer and non-uniformly distributed micropores and therefore lower water vapor transmission rates.
[0209] As can be seen from the comparison between Example I-1 and Comparative Example I-5 and between Example II-1 and Comparative Example II-5, when maleic anhydride copolymer microspheres having an average particle size of less than 500 nm were used, the pores were too small, and both the properties of the polyethylene composition and the properties of the resulting film were deteriorated, and the water vapor transmission rate was less than 3000 g / (m 2 -24h) was lower.
[0210] As can be seen from the comparison between Example II-1 and Comparative Example II-6, when the porogen was large (average particle size >2000 nm), the pores were large, the amount of pores was small, the water vapor permeability was poor, and the mechanical properties were adversely affected.
[0211] As can be seen from the comparison between Example I-1 and Example I-2, compared with the case where LLDPE is used alone as the matrix resin, the use of a combination of LLDPE and LDPE as the matrix resin not only improves the processing performance, but also promotes the dispersion of the porogen to a certain extent, and therefore achieves an improvement in the water vapor transmission rate.
[0212] The results show that the polyethylene breathable films produced by the examples according to the present invention have high breathability and good mechanical properties, and therefore can be widely used in the fields of breathable composite articles, such as water-proof and moisture-permeable materials, hygiene articles, medical articles, food packaging or building articles.
[0213] Although the present invention has been described in detail and illustrated by examples, it will be apparent to those skilled in the art that other modifications and variations are possible within the spirit and scope of the present invention. It should be further understood that the various aspects described in the present invention, various parts of the different embodiments, and various features listed may be combined or interchanged in whole or in part. Furthermore, those skilled in the art will appreciate that the foregoing description is illustrative only and is not intended to limit the present invention. [Brief description of the drawings]
[0214] [Figure 1] FIG. 1 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-1; [Diagram 2] FIG. 2 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-3; [Diagram 3] FIG. 3 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-5; [Figure 4] FIG. 4 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example I-6; [Diagram 5] FIG. 5 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-1; [Figure 6] FIG. 6 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-2; [Figure 7] FIG. 7 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example I-3; [Figure 8] FIG. 8 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-1; [Figure 9] FIG. 9 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-3; [Figure 10] FIG. 10 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-4; [Figure 11] FIG. 11 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Example II-6; [Figure 12] FIG. 12 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example II-1; [Figure 13] FIG. 13 is an SEM photograph of a cross section of a sample sheet of the polyethylene composition prepared in Comparative Example II-2; [Figure 14] FIG. 14 is an SEM photograph of a cross section of the sample sheet of the polyethylene composition prepared in Comparative Example II-3.
Claims
1. 1. A polyethylene composition comprising a polyethylene matrix resin and a porogen, The content of the porogen is 30 parts by weight to 110 parts by weight based on 100 parts by weight of the polyethylene matrix resin, 1. A polyethylene composition comprising: a porogen comprising maleic anhydride copolymer microspheres, the copolymer in the microspheres comprising structural units A from maleic anhydride and structural units B from a vinyl-containing comonomer M; and an average particle size of the maleic anhydride copolymer microspheres is from 500 nm to 2000 nm.
2. The melting enthalpy ΔH of the polyethylene matrix resin m PE and the melting enthalpy ΔH of the polyethylene composition. m 組成物 and satisfy the following relationship: ΔH m PE and ΔH m 組成物 The difference between the above is 8 J / g to 48 J / g, preferably 10 J / g to 45 J / g, and more preferably 20 J / g to 45 J / g.
3. The density ρ of the polyethylene composition 組成物 and the density of polyethylene, ρ PE satisfies the relation: ρ 組成物 and ρ PE The difference is 0.045 g / cm 3 ~0.155g / cm 3 and When the maleic anhydride copolymer microspheres are non-crosslinked maleic anhydride copolymer microspheres, the difference is preferably 0.055 g / cm 3 ~0.155g / cm 3 , more preferably 0.068 g / cm 3 ~0.145g / cm 3 and When the maleic anhydride copolymer microspheres are crosslinked maleic anhydride copolymer microspheres, the difference is preferably 0.045 g / cm 3 ~0.120g / cm 3 , more preferably 0.050 g / cm 3 ~0.110g / cm 3 3. The polyethylene composition according to claim 1 or 2,
4. The polyethylene composition according to any one of claims 1 to 3, wherein the content of the porogen is 35 to 110 parts by weight, preferably 50 to 100 parts by weight, and more preferably 50 to 90 parts by weight, based on 100 parts by weight of the polyethylene matrix resin.
5. said maleic anhydride copolymer microspheres have an average particle size of 500 nm to 1700 nm, preferably 500 nm to 1600 nm, more preferably 600 nm to 1300 nm, more preferably 800 nm to 1300 nm; 5. The polyethylene composition according to any one of claims 1 to 4, wherein the copolymer microspheres are preferably monodisperse copolymer microspheres, in particular having a particle size dispersion coefficient of 1.05 to 1.0001, preferably 1.035 to 1.002, more preferably 1.028 to 1.
002.
6. The polyethylene composition according to any one of claims 1 to 5, wherein the maleic anhydride copolymer microspheres are spherical or near-spherical.
7. the molar ratio of the structural unit A to the structural unit B is in the range of (0.5:1) to (1:0.5), preferably (0.75:1) to (1:0.75); Preferably, based on the total molar amount of structural units A and B in said copolymer, the molar content of structural units A is 48% to 55% and the molar content of structural units B is 45% to 52%; More preferably, the molar content of structural units A is from 49% to 51% and the molar content of structural units B is from 49% to 51%.
8. The polyethylene composition according to any one of claims 1 to 7, wherein said comonomer M is at least one selected from the group consisting of styrene, α-methylstyrene, vinyl acetate, mixed C4 and mixed C5, said mixed C4 and mixed C5 being preferably the C4 and C5 fractions obtained from said ethylene cracking process.
9. the porogen is a crosslinked maleic anhydride copolymer microsphere, the copolymer in the microsphere further comprising crosslinked structural units from a crosslinker; The crosslinking degree of said copolymer microspheres is preferably ≧65%, preferably ≧70%; The crosslinking agent is preferably selected from di- or higher functionality vinyl-containing monomers capable of free radical polymerization; Preferably, the crosslinker is at least one selected from the group consisting of divinylbenzene and an acrylate crosslinker containing at least two acrylate groups; More preferably, the crosslinking agent is at least one selected from the group consisting of divinylbenzene, propylene glycol bis(meth)acrylate, ethylene glycol bis(meth)acrylate, trimethylolpropane tri(meth)acrylate, bistrimethylolpropane tetra(meth)acrylate, polyethylene glycol bis(meth)acrylate, diethylene glycol phthalate diacrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ethoxylated multifunctional acrylates; The polyethylene composition according to any one of claims 1 to 8, wherein a molar ratio of the structural unit A to the structural unit B to the crosslinking structural unit is 100:(100-120):(1-40), preferably 100:(100-105):(10-30).
10. The maleic anhydride copolymer microspheres of the polyethylene composition according to any one of claims 1 to 8 are prepared by a process comprising the steps of: (1) dissolving maleic anhydride, a comonomer and an initiator in a reaction medium under an inert atmosphere to form a homogeneous solution, said comonomer being preferably at least one selected from the group consisting of styrene, α-methylstyrene and vinyl acetate; (2) subjecting the homogeneous solution to a polymerization reaction to obtain a copolymer emulsion suspension, and then obtaining the maleic anhydride copolymer microspheres by solid-liquid separation, the polymerization being preferably carried out at a polymerization temperature of 61° C. to 100° C. for a polymerization time of 1 hour to 24 hours; Preferably, the maleic anhydride is used in an amount of 50% by weight to 90% by weight, and the comonomer is used in an amount of 10% by weight to 50% by weight, based on the total weight of the maleic anhydride and the comonomer; The reaction medium is preferably a mixture of a compound of formula (1) and an alkane: 【Chemistry 1】 In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 6 carbon atoms, preferably methyl or ethyl; The alkane is preferably an alkane having from 6 to 12 carbon atoms.
11. The maleic anhydride copolymer microspheres of the polyethylene composition according to any one of claims 1 to 8 are prepared by a process comprising the steps of: subjecting maleic anhydride and comonomer M to a copolymerization reaction in an inert atmosphere, in an organic solvent, in the presence of an initiator; next, separating the product obtained by the polymerization reaction to obtain maleic anhydride copolymer microspheres; wherein said comonomer M is preferably selected from mixed C4 and / or mixed C5; The copolymerization reaction is preferably carried out at a temperature of 50° C. to 100° C., under a pressure of 0.2 MPa to 2 MPa, and for a reaction time of 5 hours to 10 hours; Preferably, the weight ratio of said maleic anhydride to said comonomer is 1:(0.2-3); Preferably, the organic solvent is selected from an organic acid alkyl ester, a mixture of an organic acid alkyl ester and an alkane, or a mixture of an organic acid alkyl ester and an aromatic hydrocarbon, preferably at least one selected from the group consisting of isoamyl acetate, butyl acetate, isopropyl acetate, and ethyl acetate.
12. 10. The polyethylene composition of claim 9, wherein the crosslinked maleic anhydride copolymer microspheres are prepared by a process comprising the steps of: contacting maleic anhydride, a comonomer M and a crosslinking agent in an inert atmosphere in an organic solvent in the presence of an initiator to copolymerize to obtain crosslinked maleic anhydride copolymer microspheres, wherein the comonomer M is at least one selected from the group consisting of styrene, α-methylstyrene, vinyl acetate, mixed C4 and mixed C5; Preferably, the amount of said crosslinker is 1 mol to 40 mol, the amount of said comonomer M is 50 mol to 150 mol, and the amount of said initiator is 0.05 mol to 10 mol, based on 100 mol of maleic anhydride; The copolymerization reaction is preferably carried out at a temperature of 50° C. to 90° C., under a pressure of 0.1 MPa to 1 MPa, and for a reaction time of 3 hours to 15 hours; Preferably, the organic solvent is selected from an organic acid alkyl ester, a mixture of an organic acid alkyl ester and an alkane, or a mixture of an organic acid alkyl ester and an aromatic hydrocarbon, preferably at least one selected from the group consisting of isoamyl acetate, butyl acetate, isopropyl acetate, and ethyl acetate.
13. The polyethylene matrix resin is selected from ethylene homopolymers (such as low density polyethylene, high density polyethylene and ultra-high molecular weight polyethylene), ethylene copolymers (such as linear low density polyethylene, very low density polyethylene, high density polyethylene, medium density polyethylene, ethylene-vinyl acetate copolymer and ethylene-methyl acrylate copolymer), and mixtures thereof or mixtures with other polyolefins (such as propylene homopolymer, propylene-based copolymer, polyolefin plastomer, polyolefin elastomer and polybutylene), preferably selected from mixtures of linear low density polyethylene and low density polyethylene, preferably the amount of the linear low density polyethylene is 60 parts by weight to 99 parts by weight, preferably 70 parts by weight to 95 parts by weight; the amount of the low density polyethylene is 1 part by weight to 40 parts by weight, preferably 5 parts by weight to 30 parts by weight, based on 100 parts by weight of the polyethylene matrix resin; wherein the linear low density polyethylene is preferably a copolymer of ethylene and an α-olefin; preferably, the α-olefin is at least one selected from the group consisting of butene, hexene and octene; and preferably, the linear low density polyethylene has at least one of the following properties: 3 ~0.935g / cm 3 a melt flow rate at 190° C. under a load of 2.16 kg of from 0.5 g / 10 min to 10 g / 10 min, preferably from 2 g / 10 min to 6 g / 10 min; and a molecular weight distribution of from 2 to 12, preferably from 2 to 10; The polyethylene composition according to any one of claims 1 to 12, wherein the low density polyethylene preferably has at least one of the following properties: 3 ~0.934g / cm 3 a melt flow rate at 190° C. and under a load of 2.16 kg of 0.1 g / 10 min to 12 g / 10 min, preferably 2 g / 10 min to 9 g / 10 min; and a molecular weight distribution of 5-11, preferably 6-10.
14. The composition further comprises an antioxidant, and the content of the antioxidant is preferably 0.1 to 2.5 parts by weight, preferably 0.1 to 2 parts by weight, more preferably 0.1 to 1.5 parts by weight, and even more preferably 0.2 to 1.5 parts by weight, based on 100 parts by weight of the polyethylene matrix resin; Preferably, the antioxidant is at least one selected from the group consisting of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite, octadecylpropionate and alkylated polyphenol, more preferably an antioxidant complex additive comprising an antioxidant and an acid acceptor, wherein preferably, the weight ratio of the antioxidant to the acid acceptor is 1-6:1; the acid acceptor is preferably a stearate, preferably selected from the group consisting of calcium stearate, zinc stearate and sodium stearate. The polyethylene composition according to any one of claims 1 to 13, wherein the antioxidant complex additive is at least one selected from the group consisting of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate, and more preferably, the weight ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite and calcium stearate is preferably (1-3):(1-3):
1.
15. The polyethylene composition according to any one of the preceding claims, wherein the polyethylene composition does not comprise a coupling agent, a dispersing agent or a surfactant, or a combination of two or three thereof.
16. The polyethylene composition according to any one of claims 1 to 15, wherein the composition is in the form of powder or pellets, and the pellets are obtained by melt blending, extruding, pelletizing and drying the polyethylene composition, preferably, the melt blending and extruding are performed in a twin-screw extruder.
17. The polyethylene composition according to any one of the preceding claims, wherein the composition further comprises, as a second porogen, an inorganic porogen selected from the group consisting of calcium carbonate, barium sulfate, titanium dioxide, silica and talc.
18. Use of the polyethylene composition according to any one of claims 1 to 17 for the preparation of a polyolefin microporous breathable film.
19. 18. A polyolefin microporous breathable film prepared from the polyethylene composition according to any one of claims 1 to 17, preferably by extrusion casting and stretching, wherein preferably said polyethylene composition is added to an extrusion cast machine, melted and cast into a cast sheet, the extrusion temperature is 210°C to 240°C, and the cooling roller temperature is 20°C to 60°C, thereby producing a polyethylene cast film, and said cast film is uniaxially stretched 2 to 5 times to obtain a polyethylene microporous breathable film, wherein the heat setting temperature is 70°C to 120°C.
20. 20. The polyolefin microporous breathable film of claim 19, wherein the film has at least one of the following characteristics: 1) a thickness of 25 μm to 35 μm; 2) 3060g / (m 2 - Water vapor transmission rate of at least 24 hours; 3) a porosity of 38% or more; 4) tensile strength in the longitudinal direction ≧25 MPa, tensile strength in the transverse direction ≧5 MPa, elongation at break in the longitudinal direction ≧125%, and elongation at break in the transverse direction ≧355%; and 5) 24.5 g / m2, measured on a sample having a thickness of 30 μm 2 a surface density of said breathable film which is:
21. 21. A breathable composite article comprising the polyolefin microporous breathable film according to claim 19 or 20, in particular a hygiene article, a medical article, a food packaging or a building article, such as disposable medical and hygiene products, baby diapers, adult care products, medical protective clothing, wound care bandages, dressings, food packaging films, and industrial protective clothing.
Citation Information
Patent Citations
Production of polyolefin composition
JP2000159826A
Porous film
JP2005112905A
Stretched porous film
JP2019142992A
Porous membrane for water treatment and method for manufacturing same
JP2021505358A
Cited By
Polyolefin composition using ionomer cavity filler
JP2026512551A