Copolymer of (meth)acrylic acid and cyclic ketene acetal

A copolymer of (meth)acrylic acid and cyclic ketene acetal monomers addresses the biodegradability issue of PAA by forming effective dispersants and scale inhibitors through controlled copolymerization and deprotection, ensuring environmental compatibility.

JP2024540140AInactive Publication Date: 2024-10-31ROHM & HAAS CO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024525524
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-04
Filing Date
2022-11-01
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing low molecular weight polyacrylic acid (PAA) dispersants and scale inhibitors are difficult to biodegrade due to their inert carbon-carbon skeleton, and biodegradable alternatives like MDO-AA copolymers are not effectively formed by existing methods.

Method used

A copolymer composition is developed comprising (meth)acrylic acid and cyclic ketene acetal monomers, with a mole-to-mole ratio of 2:1 to 15:1, where at least 80% of the copolymer consists of (meth)acrylic acid and cyclic ketene acetal units, prepared through a multi-step process involving copolymerization and deprotection to create biodegradable dispersants.

Benefits of technology

The copolymer effectively functions as a biodegradable dispersant and scale inhibitor, demonstrated by NMR spectroscopy and biodegradation simulations, achieving molecular weights suitable for environmental compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540140000001
    Figure 2024540140000001
  • Figure 2024540140000002
    Figure 2024540140000002
  • Figure 2024540140000003
    Figure 2024540140000003
Patent Text Reader

Abstract

The present invention relates to compositions comprising aqueous solutions of copolymers of (meth)acrylic acid and cyclic ketene acetal monomers, which copolymers are useful as biodegradable dispersants.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to aqueous solutions of copolymers of (meth)acrylic acid and cyclic ketene acetals, more specifically copolymers of acrylic acid and 2-methylene-1,3-dioxepane (MDO). [Background technology]

[0002] Low molecular weight (MW) polyacrylic acid (PAA) is widely used as a dispersant and antiscalant in the home care and oil and gas industries. In these applications, PAA typically enters municipal wastewater treatment plants or is at least partially released into the environment after use. Increasing scrutiny from governments, regulatory agencies, companies, and consumers regarding the fate of polymers in the environment has created a need to find new biodegradable materials. Previous studies have established that PAA is difficult to biodegrade, due in part to the inert nature of its carbon-carbon backbone. On the other hand, PAA oligomers with molecular weights below 1000 g / mol are susceptible to biodegradation. (Kawai, F., Bacterial Degradation of Acrylic Oligomers and Polymers, Applied Microbiology and Biotechnology 1993, 39(3), 382-385; Hayashi, T.; Mukouyama, M.; Sakano, K.; Tani, Y., Degradation of a Sodium Acrylate Oligomer by an Arthrobacter sp. Appl Environ Microbiol 1993,59(5),1555-9;Larson,RJ;Bookland,EA;Williams,RT;Yocom,KM;Saucy,DA;Freeman,MB;Swift,G., Biodegradation of Acrylic Acid Polymers and Oligomers by Mixed Microbial Communities in Activated Sludge,Journal of environmental polymer degradation 1997, 5(1), 41-48). Nevertheless, these biodegradable oligomers are unsuitable as dispersants and scale inhibitors.Strategies for incorporating labile bonds into PAA polymers have been reported.For example, US Patent No. 4,923,941 (Bailey) discloses an aqueous preparation of biodegradable MDO-AA copolymer by reacting sodium acrylate with MDO in water containing tetrabutylammonium bromide. Similarly, Guo et al. (Guo) report the preparation of MDO-AA copolymer by reacting incompletely neutralized acrylic acid with MDO in water containing tetrabutylammonium bromide (see Acta Polymerica Sinica 2012, 12, 958-964). Bailey claims that evidence of copolymer formation can be confirmed by the "presence of ester bonds in the copolymer chain." Similarly, Guo assigns the triplet peak at δ=4.00 ppm in the disclosed proton NMR spectrum of the polymer product to the methylene protons associated with the MDO structural unit. However, despite the assertions of Bailey and Guo, the present inventors have confirmed that no detectable amount of MDO-AA copolymer can be formed by the similar method disclosed by Bailey and Guo.

[0003] Thus, there remains a need in the art of biodegradable dispersants to find methods for preparing PAAs that are biodegradable yet remain effective as dispersants and scale inhibitors. Summary of the Invention

[0004] The present invention provides a composition comprising an aqueous solution of a copolymer comprising a) structural units of (meth)acrylic acid, and b) structural units of a cyclic ketene monomer, wherein the molar to molar ratio of the (meth)acrylic acid structural units to the cyclic ketene monomer structural units is in the range of 2:1 to 15:1, and at least 80 weight percent of the copolymer comprises structural units of (meth)acrylic acid and a cyclic ketene acetal monomer, the cyclic ketene acetal monomer having the following structure:

[0005] [ka] (Wherein, n is 0, 1, or 2; R is H or C 1 ~C 6 -alkyl, R 1 and R 2 are independently H, C 1 ~C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 ~C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 ~C 12 -alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’ are independently H, C 1 ~C 12 -alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, if n is 2, Each R 3 are independently H, C 1 ~C 12 -alkyl or, together with the carbon atom to which they are attached, an internal double bond, a fused benzene ring, or a fused C 3 ~C 7 -forming an alicyclic ring; The present invention addresses a need in the art by providing:

[0006] The compositions of the present invention provide copolymers of acrylic acid that are biodegradable yet effective as dispersing agents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention provides a composition comprising an aqueous solution of a copolymer comprising a) structural units of (meth)acrylic acid, and b) structural units of a cyclic ketene acetal monomer, wherein a molar to molar ratio of structural units of acrylic acid to structural units of the cyclic ketene acetal monomer is in the range of 2:1 to 15:1, and at least 80 weight percent of the copolymer comprises structural units of (meth)acrylic acid and the cyclic ketene acetal monomer; The cyclic ketene acetal monomer has the following structure:

[0008] [ka] (Wherein, n is 0, 1, or 2; R is H or C 1 ~C 6 -alkyl, R 1 and R 2 are independently H, C 1 ~C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 ~C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 ~C 12 -alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, if n is 1, R 3 and R 3’are independently H, C 1 ~C 12 -alkyl, phenyl, or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, if n is 2, Each R 3 are independently H, C 1 ~C 12 -alkyl or, together with the carbon atom to which they are attached, an internal double bond, a fused benzene ring, or a fused C 3 ~C 7 -forming an alicyclic ring; It is.

[0009] As used herein, the term "structural unit of (meth)acrylic acid" refers to the following repeat unit:

[0010] [ka] (In the formula, R 4 is H or CH 3 , preferably H) or a salt thereof.

[0011] Reference to structural units of (meth)acrylic acid and its salts does not imply that these units result as a residue from the copolymerization of (meth)acrylic acid (i.e., methacrylic acid or acrylic acid). Indeed, the structural units of (meth)acrylic acid present in the copolymers of the invention advantageously result from the deprotection of t-butyl groups.

[0012] The term "cyclic ketene acetal monomer structural unit" refers to a polymer backbone containing the following repeat units:

[0013] [ka]

[0014] Structural units of cyclic ketene acetal monomers (wherein R, R 1 , R 2 , R 3 , R 1’ , R 2’ , R 3’ , and n are as previously defined).

[0015] Examples of cyclic ketene acetal monomers include:

[0016] [ka]

[0017] A preferred cyclic ketene acetal monomer is 2-methylene-1,3-dioxepane (MDO).

[0018] [ka]

[0019] The copolymer of cyclic ketene acetal monomer and acrylic acid is advantageously prepared in multiple stages. In a first step, a mixture of cyclic ketene acetal monomer and t-butyl (meth)acrylate, preferably t-butyl acrylate, is gradually added from a monomer container (monomer container) to a reaction vessel in the presence of an organic solvent. At the same time, an initiator, advantageously diluted with the same organic solvent as used for the monomer, is gradually added from an initiator container (initiator container) to the reaction vessel. It may be desirable to gradually add the mixture of monomer and initiator to a reaction vessel containing a solvent and a small amount of monomer (generally on the order of 10-30 weight percent of the total monomer used to prepare the copolymer).

[0020] Suitable organic solvents include aliphatic esters such as ethyl acetate, ethers such as tetrahydrofuran and 1,4-dioxane, alkanes such as pentane, hexane, and isododecane, and aromatic solvents such as benzene, toluene, and xylene. Examples of suitable initiators include t-amyl peroxypivalate (commercially available as Trigonox-125-C75 initiator), t-butyl peroxypivalate (commercially available as Trigonox-25-C75), t-amyl peroxy-2-ethylhexanoate, 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate).

[0021] A chain transfer agent such as n-dodecyl mercaptan may also be added simultaneously with the monomers and initiator to control the molecular weight of the intermediate and final copolymers.

[0022] The contents of the reaction vessel are heated to a temperature sufficient to promote copolymerization of the cyclic ketene acetal monomer and t-butyl (meth)acrylate, generally in the range of from 40° C., or from 50° C. to 150° C., or to 100° C., or to 80° C., to provide a solution of an intermediate copolymer of the cyclic ketene acetal monomer and t-butyl (meth)acrylate.

[0023] In a second step, the intermediate copolymer is reacted under deprotection conditions to convert the t-butyl pendant groups of the copolymer to carboxylic acid groups or salts thereof, thereby forming a solution of a copolymer of cyclic ketene acetal monomer and (meth)acrylic acid, preferably acrylic acid or a salt thereof. The deprotection conditions preferably convert the intermediate copolymer to a pK ranging from -2 or -1 to 2 or 1. aThe deprotection step includes contacting the cyclic ketene acetal monomer with an organic acid having a formula: embedded image Examples of suitable acids for deprotection include trifluoroacetic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, and methanesulfonic acid. The organic solution of the copolymer of the cyclic ketene acetal monomer and acrylic acid can then be converted to an aqueous solution of the copolymer of the cyclic ketene acetal monomer and acrylic acid by conventional means, such as removing the solvent in vacuum followed by dissolving in water, or removing the solvent in vacuum followed by dissolving in water, lyophilizing, and then redissolving in water.

[0024] When the cyclic ketene acetal monomer is MDO, the MDO-AA copolymer is found to contain two types of structural units of MDO, one of which is degradable by treatment with base and the other of which is not readily degradable by treatment with base, as described.

[0025] [ka]

[0026] For the copolymers to be useful for the purposes of this invention, they must contain degradable structural units of cyclic ketene acetal monomers; although the formation of non-degradable structural units is undesirable, it has proven difficult to prepare copolymers without some residual concentration of the non-degradable forms.

[0027] The molar to molar ratio of (meth)acrylic acid structural units to cyclic ketene acetal monomer (both degradable and non-degradable), preferably MDO structural units, ranges from 2:1, or 3:1, or 4:1, to 15:1, or 10:1, or 8:1, to 7:1. At least 80, more preferably at least 90, weight percent of the copolymer comprises structural units of (meth)acrylic acid and cyclic ketene acetal monomer. Preferably, the M of the desired copolymer is 0.01 to 0.01. nranges from 1500 g / mole to 20,000, or 15,000, or 10,000 g / mole. Statistically, the polymer backbone is expected to contain 2 to 15 structural units of (meth)acrylic acid (preferably fragments of acrylic acid groups) anchored at each end by a single degradable structural unit of a cyclic ketene acetal monomer, as illustrated:

[0028] [ka] (In the formula, R 4 is H or CH 3 , preferably H, x ranges from 2, or 3, or 4 to 15, or 10, or 8, or 7, and the dotted line represents the attachment of a structural unit of MDO to another fragment of the acrylic acid group).

[0029] In accelerated aging studies, the ester groups are hydrolyzed with a strong base such as KOH to give a distribution of oligomers, including, in part, an oligomer predicted to have the following structure:

[0030] [ka]

[0031] The presence of non-degradable structural units of cyclic ketene acetal monomers is predicted to form copolymers that are hydrolyzable to the following oligomers:

[0032] [ka]

[0033] Although the exact structure of the oligomers can be deduced, the number average molecular weight (M) of the hydrolyzed copolymers as determined by gel permeation chromatography according to the method detailed in the Examples section. n) can be identified with greater confidence as being in the range of 144, or 200, or 400, or 500 g / mole to 1000, or 800, or 750 g / mole.

[0034] The compositions of the present invention are ostensibly disclosed in U.S. Pat. No. 4,923,941 (Bailey), however, repeating the procedure and proton NMR spectroscopy of Bailey's only example demonstrates that Bailey's interpretation of the data is incorrect and, in fact, the disclosed example does not permit the preparation of copolymers of MDO and AA.

[0035] Bailey's example was repeated as described and the proton NMR spectrum of the reaction mixture of sodium acrylate and MDO was recorded after 30 minutes of reaction at 90° C. Triplets were observed at 4.02 ppm and 3.52 ppm, consistent with 4-hydroxybutyl acetate, the hydrolysis product of MDO.

[0036] [ka]

[0037] A small triplet at the same resonance was also observed in the proton NMR spectrum of the isolated product. Diffusion-edited proton NMR spectroscopy, which suppresses the chemical shifts of small molecules and reveals only those associated with the polymer, confirmed that these residual peaks could not be attributed to ester formation of the copolymer. Importantly, no chemical shifts were observed near 4 ppm, confirming that Bailey was unable to form detectable levels of copolymers of AA and MDO by the method disclosed. Moreover, proton NMR spectroscopy further confirmed that MDO was hydrolyzed to 4-hydroxybutyl acetate (among other by-products) under the initial reaction conditions reported by Bailey at room temperature.

[0038] Similarly, in Acta Polymerica Sinica 2012,12,958-964, Guo claims to have prepared MDO-AA copolymers by reacting incompletely neutralized acrylic acid with MDO in water containing tetrabutylammonium bromide. Guo's method was repeated as described, and additional experiments were performed using acrylic acid at various degrees of neutralization. The method described by Guo could not be reproduced to obtain proton NMR spectroscopy patterns consistent with those reported by Guo. In contrast, NMR spectroscopy did not show detectable amounts of MDO-AA copolymers. Proton NMR and diffusion NMR spectroscopy did not indicate the formation of structural units of MDO (as concluded by Guo), but rather revealed a small, sharp triplet resonance at 4.0 ppm characteristic of MDO hydrolysis products such as 4-hydroxybutyl acetate.

[0039] In contrast, copolymers prepared by the process of the present invention and analyzed by diffusion-edited proton NMR spectroscopy reveal a strong and broad chemical shift near 4 ppm, consistent with the expected profile for copolymers containing structural units of cyclic ketene acetal monomers. The compositions of the present invention are useful as biodegradable dispersants and scale inhibitors. EXAMPLES

[0040] M n Decision Aqueous samples for gel permeation chromatography (GPC) were prepared at a concentration of approximately 2 mg / mL in aqueous 20 mM phosphate buffer at pH 7. Separation was performed on a Waters UPLC system equipped with a refractive index detector, using the same phosphate buffer as the mobile phase. An APC column set consisting of a TOSOH Bioscience TSKgel G2500PWxl 7.8 mm ID x 30 cm, 7 μm column and a TOSOH Bioscience TSKgel GMPWxl 7.8 mm ID x 30 cm, 13 μm column was used. The flow rate was maintained at 1.0 mL / min and the column temperature was maintained at 35 °C. Peak molecular weights (M) of 216 g / mol to 1,100,000 g / mol were obtained.p The results were calibrated using narrow pAA standards and fitted to a quadratic calibration curve. Standards 1–15 were obtained from American Polymer Standards, and standard 16 (M p The peak molecular weights (M = 216 g / mol AA trimer) were prepared in-house. The flow rate was 1.0 mL / min and the column temperature was maintained at 35 °C. p The results were calibrated using narrow pAA standards of 0.01 and fitted to a quadratic calibration curve. The M of the copolymers in the examples was calculated using Empower Version 3 software (Waters Corporation). n was calculated.

[0041] A GPC calibration table showing the retention times of the 16 standards is shown in Table 1.

[0042] [Table 1]

[0043] Proton NMR Spectroscopic Analysis Proton NMR spectra were obtained using a Bruker NEO 600 MHz spectrometer equipped with a 5 mm BBO CryoProbe using a Bruker zg30 pulse sequence. The relaxation delay was 12 seconds. Pulsed-field gradient NMR spectroscopy experiments were performed using a Bruker ledbpgp2s1d pulse sequence with a gradient pulse length of 2 ms and a delay time of 20 ms.

[0044] Example 1 - Preparation of MDO-AA Copolymer A copolymer of MDO and acrylic acid was prepared with approximately a 1:4 mole:mol ratio of MDO:AA building blocks using the following procedure.

[0045] A. Preparation of MDO-t-butyl acrylate copolymer (1:4 mole ratio of MDO:t-butyl acrylate) A 250 mL three-neck round-bottom flask equipped with a condenser, stir bar, thermocouple, and a Y-shaped glass adapter for two polyethylene feed tubes was charged with ethyl acetate (18.0 g) and placed on an Opti-chem hotplate stirrer heated to 75 °C. 2 A blanket of 100 g was applied and agitation was set at 300 rpm. The first vessel was charged with t-butyl acrylate (24.55 g), MDO (5.45 g), and n-dodecyl mercaptan (0.90 g), and the second vessel was charged with Trigonox 125-C75 initiator (0.40 g, 75% active in mineral spirits) in ethyl acetate (7.50 g). A portion of the contents of the first vessel (6.18 g) was added to the reaction flask over 2 minutes. After a few minutes, the remainder of the contents of the first vessel and the contents of the second vessel were metered into the reaction flask at rates of 0.275 g / min and 0.088 g / min, respectively, such that the addition of the contents of the second vessel and the remainder of the first vessel was completed after 90 minutes. The first vessel was rinsed with ethyl acetate (4.50 g), which was added to the reaction flask. After 15 minutes, a portion of Trigonox 125-C75 initiator (0.60 g) in ethyl acetate (2.25 g) was metered into the reaction flask over 30 minutes, followed by a 15 minute hold, followed by a second addition of the same amount of initiator also metered into the reaction flask over 30 minutes. Heating and stirring of the reaction flask was continued for an additional 30 minutes, after which the reaction was cooled to room temperature. The resulting copolymer was transferred to a glass container for storage without further purification. The solids content was found to be 41.4 wt.%. The conversions of both t-butyl acrylate and MDO were determined to be quantitative by proton NMR spectroscopy.

[0046] B. Deprotection of MDO-t-butyl acrylate copolymer A portion (5.0 g) of the copolymer prepared from Part A was transferred to a 1 oz. glass vial equipped with a stir bar. The volatiles were removed by vacuum distillation, and then the dried polymer was dissolved in methylene chloride (CH 2 Cl 2The hexanes were redissolved in 1,2-dichloromethane (HCl, 8.0 g). Trifluoroacetic acid (TFA, 4.4 g) was added dropwise to the stirred contents of the vial. After the addition was complete, the vial was capped and the reaction mixture was stirred at ambient temperature for 18 hours. A slightly yellow opaque mixture was obtained.

[0047] The volatiles were removed in vacuum, and then anhydrous tetrahydrofuran (THF, 5.0 g) was added to redissolve the reaction mixture. The volatiles were once again removed in vacuum, and the resulting crude product (2.68 g) was dissolved in deionized water (10.26 g) and neutralized with 1N NaOH solution (5.73 g) to obtain a clear solution with a pH of 5.86. The neutralized polymer was dialyzed against deionized water using a dialysis membrane with a molecular weight cut-off (MWCO) of 100-500 g / mol to remove low molecular weight impurities. The dialyzed solution was freeze-dried to obtain a fluffy white polymer as the final product. The M of the product by GPC as described above was n was 2060 g / mol (polydispersity 4.66). Using proton NMR spectroscopy, the ester content was found to be 18 wt%, the ester retention in the polymer backbone was found to be 80 wt%, and the residual t-butyl groups in the backbone were found to be 3 mol%.

[0048] Example 2 - Preparation of MDO-AA Copolymer The procedure used to prepare the MDO-AA copolymer of Example 2 varied the amounts of t-butyl acrylate (26.62 g), MDO (3.38 g), and n-dodecyl mercaptan (0.34 g) for Part A to give a final molar ratio of MDO:AA of about 1:7, with M n The procedure was essentially the same as that described for the preparation of the MDO-AA copolymer in Example 1, except that the copolymer produced an MDO-AA copolymer with a molecular weight of 4080 g / mol (polydispersity 4.61).

[0049] Biodegradation Simulation The MDO-t-butyl acrylate copolymer of Example 1A was subjected to exhaustive hydrolysis to simulate the biodegradable potential of the MDO-AA copolymer as follows: A general-purpose acid-digestion Parr bomb with a 23 mL PTFE cup was charged with 4-5 KOH pellets, polymer solution (1 g, approximately 41.4 wt % solids), and ethanol (10 g). The Parr bomb was sealed and transferred to a 150° C. oven and equilibrated for 3 days. The bomb was removed from the oven and cooled to ambient temperature. Disassembly of the bomb revealed the presence of liquid and solid portions. The liquid portion was separated and discarded, and the solid portion was diluted with approximately 5 g of water. The resulting polymer solution was analyzed by GPC as described above, revealing an M of the hydrolyzed polymer. n was found to be 677 g / mol. Hydrolysis studies predict a dramatic reduction in molecular weight from the useful MDO-AA copolymer to biodegradable oligomers.

Claims

1. 1. A composition comprising an aqueous solution of a copolymer comprising: a) structural units of (meth)acrylic acid; and b) structural units of a cyclic ketene acetal monomer, wherein a molar to molar ratio of structural units of acrylic acid to structural units of cyclic ketene acetal monomer is in the range of 2:1 to 15:1, and at least 80 weight percent of the copolymer comprises structural units of (meth)acrylic acid and structural units of cyclic ketene acetal monomer, and the cyclic ketene acetal monomer has the following structure: [Case 1] (wherein n is 0, 1, or 2; R is H or C 1 ~C 6 - alkyl, R 1 and R 2 are each independently H, C 1 ~C 12 - alkyl, phenyl, or vinyl, or R 1 and R 2 together with the carbon atom to which they are attached form a fused benzene ring or a fused C 3 ~C 7 - forms an alicyclic ring, R 1’ and R 2’ are each independently H or C 1 ~C 12 - alkyl or R 1 and R 1’ and / or R 2 and R 2’ forms an exocyclic double bond, However, when n is 1, R 3 and R 3’ are each independently H, C 1 ~C 12 - alkyl, phenyl or R 3 and R 3’ forms an exocyclic double bond or a spirocycloaliphatic group or a spiro-2-methylene-1,3-dioxepane group, Further, when n is 2, Each R 3 are independently H, C 1 ~C 12 - alkyl or, together with the carbon atom to which they are attached, an internal double bond, a fused benzene ring, or a fused C 3 ~C 7 - forming an alicyclic ring.

2. 2. The composition of claim 1, wherein the cyclic ketene acetal monomer is selected from the group consisting of: [chemical 2]

3. 2. The composition of claim 1, wherein the cyclic ketene monomer is 2-methylene-1,3-dioxepane (MDO), the (meth)acrylic acid structural units are acrylic acid structural units, and the molar to molar ratio of acrylic acid structural units to MDO structural units ranges from 3:1 to 8:

1.

4. The copolymer has a number average molecular weight (M) in the range of 200 g / mol to 800 g / mol as determined by gel permeation chromatography. n 4. The composition of claim 3, wherein the aryl group is aryl, and the aryl group is aryl.

5. The copolymer has an M in the range of 400 g / mol to 800 g / mol by gel permeation chromatography. n The composition of claim 3, which is hydrolyzable to one or more oligomers having the formula:

6. The copolymer has an M in the range of 500 g / mol to 750 g / mol by gel permeation chromatography. n The composition of claim 3, which is hydrolyzable to one or more oligomers having the formula:

7. The copolymer has an M in the range of 1500 g / mol to 10,000 g / mol. n The composition of claim 3 having the formula: