Electrodeposition coating composition and method for preparing same
Self-emulsifying blocked polyisocyanates with neutralized amines in cathodic electrodeposition coatings address the challenge of low-temperature curing, ensuring stability and improved coating film properties, particularly in automotive applications.
Patent Information
- Application Number
- JP2024526855
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-04
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-31
AI Technical Summary
Existing cathodic electrodeposition coating materials face challenges in achieving low-temperature curing while maintaining stability and coating film properties, particularly in automotive applications, leading to issues such as decreased storage and operational stability, and deterioration in coating appearance and performance.
The use of self-emulsifying blocked polyisocyanates with neutralized amines in cathodic electrodeposition coating materials, comprising a cationic amino-containing epoxy resin and a blocked polyisocyanate with neutralized amines, which are prepared by reacting polyurethane prepolymers with blocking agents and neutralizing the amine-containing blocked polyisocyanate, eliminating the need for emulsifiers.
This approach enables curing at temperatures below 160°C with improved stability and enhanced coating film properties, including corrosion resistance, while maintaining desirable application performance and reducing volatile organic compounds (VOC) and improving throw power.
Smart Images

Figure 2024540363000001 
Figure 2024540363000002 
Figure 2024540363000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a cathodic electrodeposition coating material containing a self-emulsifying blocked polyisocyanate, and to a method for using the self-emulsifying blocked polyisocyanate. [Background technology]
[0002] Cationic electrodeposition coating materials are widely used in various fields due to their excellent application performance and the excellent properties of the resulting coating films. Cationic electrodeposition coating materials generally contain a binder dispersion containing a resin component (e.g., a cationic amino-containing epoxy resin) and a curing agent component (e.g., a blocked polyisocyanate) in an aqueous medium, and a pigment paste in a pigment paste. The binder dispersion is generally prepared by mixing the resin component and the curing agent component, followed by neutralization and dispersion in an aqueous medium. The neutralized resin component and the curing agent exist together in the binder dispersion in the form of charged micelles. During storage of the cationic electrodeposition coating composition and during long-term circulation of the electrodeposition coating bath, there is a good chance that the two components will react with each other.
[0003] During electrodeposition coating, the substrate to be coated is used as the cathode. An electric current is applied between the cathode and the anode, causing micelles containing the neutralized resin component and the curing component in the coating bath to precipitate on the metal substrate, forming a coating film. To cure the coating film, the coated substrate is then heated, usually at temperatures above 160°C.
[0004] In recent years, there has been an increasing demand from original equipment manufacturers, particularly in the automotive field, for cathodic electrodeposition coating materials that can be cured at low temperatures (i.e., low-temperature-curing cathodic electrodeposition coating materials). Generally, low-temperature-curing cathodic electrodeposition coating materials containing curing agents that can exhibit reactivity at low temperatures are known in the art. The curing agent is, for example, an oxime-blocked polyisocyanate as described in JPH10120947A and JPH07300698A.
[0005] However, improved reactivity of electrodeposition coating materials can result in reduced stability, for example, long-term storage stability and / or working stability during electrodeposition coating. The appearance and properties of the resulting coating film can also be impaired. Solutions to this problem have been proposed. For example, EP3415574B describes a method for producing an electrodeposition coating composition that can be cured at low temperatures. The electrodeposition coating composition in this patent document is prepared by mixing an aqueous dispersion (A) of an amino group-containing epoxy resin, an aqueous dispersion (B) of a blocked polyisocyanate compound, and a pigment dispersion paste (C), where an emulsifier is required to provide the aqueous dispersion (B) of the blocked polyisocyanate compound.
[0006] There is still a need for low-temperature curable cationic electrodeposition coating materials with improved storage stability and working stability. It is also desirable for low-temperature curable cationic electrodeposition coating materials to have improved application performance, such as slow power and VOC, and to be able to produce coating films with excellent properties, such as corrosion resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JPH10120947A [Patent Document 2] JPH07300698A [Patent Document 3] EP3415574B Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a cathodic electrodeposition coating material that can be cured at temperatures below 160°C, has improved stability, preferably improved application performance, and can provide excellent coating film properties such as corrosion resistance. [Means for solving the problem]
[0009] Surprisingly, it has now been found that this object is achieved by using self-emulsifying blocked polyisocyanates with neutralized amines in cathodic electrodeposition coating materials.
[0010] Therefore, the present invention provides (A) a cationic amino-containing epoxy resin, (B) a blocked polyisocyanate having a neutralized amine, the process comprising the steps of: (i) reacting a polyurethane prepolymer containing isocyanate groups as a polyisocyanate with a blocking agent selected from oximes, pyrazoles, and active methylene compounds to provide a partially blocked polyisocyanate; (ii) reacting the remaining isocyanate groups in the partially blocked polyisocyanate with an amine compound having an active hydrogen to provide an amine-containing blocked polyisocyanate; (iii) neutralizing the amine-containing blocked polyisocyanate with an acid; a blocked polyisocyanate having a neutralized amine, obtainable or obtained by a process comprising: (C) Curing catalyst A cathodic electrodeposition coating composition is provided, comprising:
[0011] In another aspect, the present invention provides a method for preparing a cathodic electrodeposition coating composition comprising mixing (A) an aqueous dispersion comprising a cationic amino-containing epoxy resin with (B) an aqueous dispersion comprising a blocked polyisocyanate having a neutralized amine.
[0012] In a further aspect, the present invention provides a coating bath for cathodic electrodeposition comprising the cathodic electrodeposition coating composition of the present invention or a cathodic electrodeposition coating composition prepared by the method of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0013] Detailed Description of the Invention The present invention will be described in detail below. It should be understood that the present invention may be embodied in many different ways and should not be construed as being limited to the embodiments set forth herein. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs.
[0014] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0015] The terms "comprise", "comprises", and the like are used interchangeably with "contain", "include", and the like, and are to be interpreted in an open and non-limiting manner. That is, for example, additional components or elements may be present. The phrase "consisting of" or "consisting essentially of" or synonyms may be encompassed by "comprise" or synonyms.
[0016] As used herein, the term "self-emulsifying" in the context of blocked polyisocyanates is intended to mean that the blocked polyisocyanates are capable of forming stable dispersions without the need for added surfactants, such as emulsifiers or dispersants.
[0017] As used herein, the term "prepolymer" refers to a monomer or system of monomers that has been reacted through reactive groups to an intermediate molecular weight state that can be further polymerized to a fully cured, high molecular weight state.
[0018] Cationic electrodeposition coating composition (A) Cationic amino-containing epoxy resin Cationic amino-containing epoxy resins, which have the positive charge necessary for electrodeposition, are used as binders in cathodic electrodeposition coating compositions. The positive charge can be generated by neutralizing the amino-containing epoxy resin with a water-soluble acid.
[0019] Suitable amino-containing epoxy resins may be adducts of unmodified or modified polyepoxides with primary or secondary amines, as described, for example, in EP 1171530 A1, US 5236564 A, US 5236564 A and US 6274649 B.
[0020] Examples of suitable polyepoxides include polyglycidyl ethers derived from polyphenols and epihalohydrins, more particularly epichlorohydrin. Preferred polyphenols are, more particularly, bisphenol A and bisphenol F. Suitable polyphenols also include, but are not limited to, 4,4'-dihydroxybenzophenone, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)isobutane, 2,2-bis(4-hydroxy-tert-butylphenyl)propane, bis(2-hydroxynaphthyl)methane, 1,5-dihydroxynaphthalene, and phenol novolac resins.
[0021] Suitable polyepoxides also include, but are not limited to, polyglycidyl ethers of polyhydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,4-propylene glycol, 1,5-pentanediol, 1,2,6-hexanetriol, glycerol, and 2,2-bis(4-hydroxycyclohexyl)propane; polyglycidyl esters of polycarboxylic acids such as oxalic acid, succinic acid, glutaric acid, terephthalic acid, hexahydrophthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid; hydantoin epoxide, epoxidized polybutadiene, and polyepoxide compounds obtained by epoxidizing olefinically unsaturated aliphatic compounds.
[0022] A modified polyepoxide is a polyepoxide in which some of the reactive groups have been reacted with a modifying compound. Examples of modifying compounds include, for example, i) compounds containing carboxyl groups, such as saturated or unsaturated monocarboxylic acids, for example benzoic acid, 2-ethylhexanoic acid, versatic acid; aliphatic, cycloaliphatic and / or aromatic dicarboxylic acids of different chain lengths, for example (meth)acrylic acid or poly(meth)acrylic acid, adipic acid, sebacic acid, isophthalic acid, fatty acids or dimer fatty acids; hydroxyalkylcarboxylic acids, for example lactic acid, dimethylolpropionic acid; and carboxyl-containing polyesters, or ii) compounds containing amino groups, such as diethylamine, ethylhexylamine, diamines having secondary amino groups, such as N,N'-dialkylalkylenediamines (e.g., dimethylethylenediamine), N,N'-dialkylpolyoxyalkylenediamines (e.g., N,N'-dimethylpolyoxypropylenediamine), cyanoalkylated alkylenediamines (e.g., N,N'-bis(cyanoethyl)ethylenediamine), cyanoalkylated polyoxyalkylenediamines (e.g., N,N'-bis(cyanoethyl)polyoxypropylenediamine), polyaminoamides, such as amino-terminated reaction products of diamines, polycarboxylic acids, and monocarboxylic acids, or reaction products of one mole of diaminohexane with two moles of monoglycidyl ethers or monoglycidyl esters, in particular glycidyl esters of α-branched fatty acids such as Versatic acid, or iii) compounds containing hydroxyl groups, such as neopentyl glycol, bisethoxylated neopentyl glycol, neopentyl glycol hydroxypivalate, dimethylhydantoin-N,N'-diethanol, hexane-1,6-diol, hexane-2,5-diol, 1,4-bis(hydroxymethyl)cyclohexane, 1,1-isopropylidenebis(p-phenoxy)-2-propanol, trimethylolpropane, pentaerythritol, or aminoalcohols, such as triethanolamine, methyldiethanolamine, or hydroxyl-containing alkyl ketimines, such as aminomethylpropane-1,3-diol methylisobutylketimine or tris(hydroxymethyl)aminomethanecyclohexanone ketimine, and also polyglycol ethers, polyester polyols, polyether polyols, polycaprolactone polyols, and polycaprolactam polyols of different functionality and molecular weight, or iv) saturated or unsaturated fatty acid methyl esters that are transesterified with the hydroxyl groups of the epoxy resin in the presence of sodium methoxide Includes:
[0023] Suitable primary and / or secondary amines for forming adducts with polyepoxides include, but are not limited to, mono- and dialkylamines such as methylamine, ethylamine, propylamine, butylamine, dimethylamine, diethylamine, dipropylamine, and methylbutylamine; alkanolamines such as methylethanolamine and diethanolamine; dialkylaminoalkylamines such as dimethylaminoethylamine, diethylaminopropylamine, and dimethylaminopropylamine; alkylenepolyamines such as ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine.
[0024] The amine may contain other groups, provided that they do not interfere with the reaction of the amine with the epoxide groups and do not cause gelation of the reaction mixture. Secondary amines are particularly suitable for forming adducts with polyepoxides.
[0025] In the present invention, an amino-containing epoxy resin modified with a modifier selected from polyols, polyether polyols, and polyester polyols is particularly suitable. The amount of the modifier is not particularly limited, and may be, for example, preferably 0.1% by mass to 30% by mass, more preferably 1% by mass to 20% by mass, based on the solid content of the amino-containing epoxy resin.
[0026] Suitable acids for neutralizing the amino-containing epoxy resins may be inorganic acids, such as hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, boric acid, perchloric acid, etc. Suitable acids may also be organic acids, such as mono- or polycarboxylic acids optionally substituted with hydroxyl groups. In particular, organic acids may be C1-C 10 -Monocarboxylic acids, C1-C 10 -Dicarboxylic acids, C1-C 10 -Tricarboxylic acids, C1-C 10 -Hydroxymonocarboxylic acids, C1-C 10 -Hydroxydicarboxylic acids, C1-C 10 hydroxytricarboxylic acids, and any combination thereof. Examples of organic acids include formic acid, acetic acid, propanoic acid, butanoic acid, lactic acid, glycolic acid, 3-hydroxybutanoic acid, 2-hydroxyisobutanoic acid, malic acid, oxalic acid, malonic acid, methylmalonic acid, succinic acid, methylsuccinic acid, adipic acid, pimelic acid, suberic acid, glutaric acid, and citric acid. Tartaric acid, fumaric acid, benzoic acid, and any combination thereof are not limited thereto. Suitable organic acids may be selected from formic acid, acetic acid, propionic acid, lactic acid, oxalic acid, glycolic acid, citric acid, malic acid, adipic acid, succinic acid, fumaric acid, benzoic acid, and any combination thereof.
[0027] The cationic amino-containing epoxy resin may be introduced into the cathodic electrodeposition coating composition according to the present invention in the form of an aqueous dispersion.
[0028] The cathodic electrodeposition coating composition according to the present invention may contain 30% to 85% by mass, preferably 40% to 70% by mass, of the cationic amino-containing epoxy resin (A) based on the solids content of the cathodic electrodeposition coating composition.
[0029] (B) Blocked polyisocyanate with neutralized amine The blocked polyisocyanate having a neutralized amine is used in the cathodic electrodeposition coating composition, which is introduced into the cathodic electrodeposition coating composition of the present invention in the form of an aqueous dispersion. The aqueous dispersion is prepared by the following steps: (i) reacting a polyurethane prepolymer containing isocyanate groups as a polyisocyanate with a blocking agent selected from oximes, pyrazoles, and active methylene compounds to provide a partially blocked polyisocyanate; (ii) reacting the remaining isocyanate groups in the partially blocked polyisocyanate with an amine compound having an active hydrogen to provide an amine-containing blocked polyisocyanate; (iii) neutralizing the amine-containing blocked polyisocyanate with an acid and dispersing it in water; It is prepared by a process comprising:
[0030] The polyurethane prepolymer containing an isocyanate group as the polyisocyanate in step (i) may be derived from a polyisocyanate compound and a polyol.
[0031] Polyisocyanate compounds useful for deriving polyurethane prepolymers containing isocyanate groups include aliphatic, cycloaliphatic, and aromatic diisocyanates, and polyisocyanates containing three or more isocyanate groups per molecule.
[0032] Examples of aliphatic diisocyanates include, but are not limited to, 1,3-trimethylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,2-propylene diisocyanate, ethylethylene diisocyanate, 1-methyltrimethylene diisocyanate, 2-methylpentane diisocyanate, 2,2,4-trimethylhexane diisocyanate, isomers and oligomers thereof.
[0033] Examples of cycloaliphatic diisocyanates include, but are not limited to, isophorone diisocyanate, 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, dicyclohexylmethane diisocyanate, isomers and oligomers thereof.
[0034] Examples of aromatic diisocyanates include, but are not limited to, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,4-naphthylene diisocyanate, 1,5-naphthylene diisocyanate, biphenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2,2-diphenylpropane-4,4'-diisocyanate, isomers and oligomers thereof.
[0035] Examples of triisocyanates include, but are not limited to, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, 1,8-diisocyanato-4-(isocyanatomethyl)octane, lysine triisocyanate, isomers and oligomers thereof.
[0036] The oligomers may be, for example, dimers, trimers, and higher order oligomers such as tetramers, pentamers, hexamers, or mixtures thereof.
[0037] In accordance with the present invention, particularly suitable polyisocyanate compounds for deriving polyurethane prepolymers include one or more oligomers of 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,4-naphthylene diisocyanate, 1,5-naphthylene diisocyanate, biphenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, and 2,2-diphenylpropane-4,4'-diisocyanate.
[0038] Preferably, the isocyanate group-containing polyurethane prepolymer is derived from a polyisocyanate compound containing one or more oligomers of 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 2,2'-diphenylmethane diisocyanate.
[0039] To derive the isocyanate group-containing polyurethane prepolymer, the polyisocyanate compounds can be used alone or in a mixture of two or more kinds.
[0040] Examples of polyols for deriving the isocyanate group-containing polyurethane prepolymer include polyhydric alkanols, polyhydric phenols, (poly)ether polyols, (poly)ester polyols, and polycarbonate polyols.
[0041] Examples of polyhydric alkanols include glycols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentyl glycol, 1,4-hexanediol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,8-octanediol, 1,9-nonanediol, 2,2-diethyl-1,3- These include, but are not limited to, propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2-n-hexadecane-1,2-ethylene glycol, 2-n-eicosane-1,2-ethylene glycol and 2-n-octacosane-1,2-ethylene glycol, hydrogenated bisphenol A; and trihydric or higher polyhydric alkanols such as glycerol, trimethylolethane, trimethylolpropane, 1,2,6-hexanetriol, pentaerythritol, sorbitol and mannitol.
[0042] Examples of polyhydric phenols include polyphenols. Suitable polyphenols include, but are not limited to, bisphenol A, bisphenol F, and their polyalkoxylated derivatives, such as polyethoxylated bisphenol A. Suitable polyphenols also include, but are not limited to, 4,4'-dihydroxybenzophenone, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)isobutane, 2,2-bis(4-hydroxy-tert-butylphenyl)propane, bis(2-hydroxynaphthyl)methane, 1,5-dihydroxynaphthalene, and their polyalkoxylated derivatives.
[0043] Examples of (poly)ether polyols include, but are not limited to, oligomeric ether polyols such as diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, diglycerol, triglycerol, and dipentaerythritol, polyether polyols such as polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetrahydrofuran (polyTHF), wherein the polyether polyol preferably has an average molecular weight (Mn) of 1000 or less, more preferably 800 or less, and most preferably 700 or less.
[0044] Examples of (poly)ester diols include, but are not limited to, (poly)condensates of polyhydric alcohols such as ethylene glycol, propylene glycol, neopentyl glycol, 1,4-butanediol, 1,4-butenediol, 1,6-hexanediol, furandiethanol, and cyclohexanedimethanol with polycarboxylic acids such as maleic acid, fumaric acid, itaconic acid, succinic acid, glutaric acid, adipic acid, isophthalic acid, terephthalic acid, phthalic anhydride, dimethyl terephthalate, dimer acid, and derivatives thereof.
[0045] Examples of polycarbonate polyols include C2 to C 20 - include, but are not limited to, reaction products of polyols with diaryl or dialkyl carbonates, such as diphenyl carbonate and dimethyl carbonate, or phosgene. 20Examples of polyols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, neopentyl glycol, 1,4-bishydroxymethylcyclohexane, 2-methyl-1,3-propanediol, 2,2,4-trimethylpentane-1,3-diol, bisphenol A, diethylene glycol, tetraethylene glycol, glycerol, trimethylolethane, trimethylolpropane, 1,2,6-hexanetriol, pentaerythritol, and combinations thereof.
[0046] Examples of commercially available polycarbonate polyols include products from Bayer Material Science AG available under the trade names Desmophen® C 2100, Desmophen® C 2200, Desmophen® C XP 2613, Desmophen® C 3100 XP, Desmophen® C 3200 XP, and Desmophen® C XP 2716.
[0047] The isocyanate group-containing polyurethane prepolymers described herein may be commercially available or may be prepared in situ prior to reaction with the blocking agent in step (i).
[0048] A suitable isocyanate group-containing polyurethane prepolymer may have an isocyanate group content in the range of 70 mol % to 90 mol %, preferably 70 mol % to 80 mol %, based on the total amount of isocyanate groups and urethane groups in the polyurethane prepolymer.
[0049] In some embodiments, an isocyanate group-containing polyurethane prepolymer prepared in situ is used to react with a blocking agent in step (i). In particular, the polyurethane prepolymer can be prepared by adding a polyol as described above to a polyisocyanate compound over a certain period of time. Known catalysts and organic solvents for preparing polyurethanes can be used without particular limitations.
[0050] In this case, the step (i) includes a substep (i-1) of preparing an isocyanate group-containing polyurethane prepolymer from a polyisocyanate compound and a polyol, and a substep (i-2) of reacting the isocyanate group-containing polyurethane prepolymer from the substep (i-1) as the polyisocyanate with a blocking agent selected from an oxime, a pyrazole, and an active methylene compound to provide a partially blocked polyisocyanate.
[0051] Thus, in a preferred embodiment, the blocked polyisocyanate having a neutralized amine is prepared by the following steps: (i-1) preparing an isocyanate group-containing polyurethane prepolymer from a polyisocyanate compound and a polyol; (i-2) reacting the isocyanate group-containing polyurethane prepolymer from step (i-1) as a polyisocyanate with a blocking agent selected from oximes, pyrazoles, and active methylene compounds to provide a partially blocked polyisocyanate; (ii) reacting the remaining isocyanate groups in the partially blocked polyisocyanate with an amine compound having an active hydrogen to provide an amine-containing blocked polyisocyanate; (iii) neutralizing the amine-containing blocked polyisocyanate with an acid and dispersing it in water; The compound is obtained by a process including:
[0052] Preferably, in step (i-1), the polyol is added to the polyisocyanate compound over a certain period of time. Any known catalyst and organic solvent for preparing polyurethane can be used in step (i-1) without any particular limitation. The polyol and polyisocyanate compound used in step (i-1) are as described above in this specification.
[0053] The isocyanate group-containing polyurethane prepolymer obtained in step (i-1) can have an isocyanate group content in the range of 70 mol % to 90 mol %, preferably 70 mol % to 80 mol %, based on the total amount of isocyanate groups and urethane groups in the polyurethane prepolymer.
[0054] The blocking agent in step (i) or (i-2) can be selected from oximes. Examples of useful oximes include, but are not limited to, formamide oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, diethyl ketoxime, diacetyl monooxime, benzophenoxime, cyclopentanone oxime, cyclohexanone oxime, or a combination thereof. Preferably, methyl ethyl ketoxime is used as the blocking agent.
[0055] The blocking agent in step (i) or (i-2) can be selected from pyrazoles. Examples of useful pyrazoles include, but are not limited to, pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-bromo-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-benzyl-3,5-dimethylpyrazole, methyl 5-methylpyrazole-3-carboxylate, 3-methyl-5-phenylpyrazole, and 3,5-dimethylpyrazole-4-carboxanilide.
[0056] The blocking agent in step (i) or (i-2) can be selected from active methylene compounds. Examples of useful active methylene compounds include, but are not limited to, dimethyl malonate, diethyl malonate, diisopropyl malonate, ethyl acetoacetate, isopropyl acetoacetate, methyl acetoacetate, isopropyl acetoacetate, and acetylacetone.
[0057] The reaction of the polyisocyanate with the blocking agent is typically carried out by dosing the blocking agent to the polyisocyanate over a period of time, and heat may be applied to the reaction mixture, for example, after dosing of the blocking agent is complete, to accelerate the reaction between the polyisocyanate and the blocking agent.
[0058] Preferably, the partially blocked polyisocyanate obtained from step (i) or (i-2) may have a content of remaining isocyanate groups in the range of 10 mol % to 25 mol %, preferably 10 mol % to 20 mol %, based on the total amount of isocyanate groups, blocked polyisocyanate groups, and urethane groups in the partially blocked polyisocyanate.
[0059] The amine compound having an active hydrogen used in step (ii) is a C3-C 20-amine compounds, such as diethanolamine, methyldiethanolamine (MDEA), triethanolamine (TEA), dimethylethanolamine (DMEA), diethylethanolamine (DEEA), 3-dimethylaminopropane-1,2-diol (DMAPD), 3-diethylaminopropane-1,2-diol (DEAPD), 2-dimethylaminopropane-1,3-diol, 2-diethylaminopropane-1,3-diol, 2-(hydroxyethyl)-2-dimethylaminopropane-1,3-diol (DMTA), 2-(hydroxyethyl)-2-diethylaminopropane-1,3-diol (DETA), N,N-dimethyl-N-(2-hydroxyethyl)- The amine compound having an active hydrogen atom may be selected from the group consisting of diethanolamine, methyldiethanolamine (MDEA), 2-[2-(dimethylamino)ethyl]methylamino]ethanol (DMAEA), N,N,N'-trimethylaminoethylethanolamine (TMAEEA), tetra(2-hydroxypropyl)ethylenediamine, N,N'-bis(2-hydroxyethyl)ethylenediamine, tetramethylhexamethylenediamine (TMHMDA), 2-(2-aminoethylamine)ethanol, 3-(N,N-dimethylamino)propylamine (DMAPA), bis-(3-dimethylaminopropylamine) (BDMAPA), and combinations thereof. Preferably, the amine compound having an active hydrogen atom is selected from the group consisting of diethanolamine, methyldiethanolamine (MDEA), 2-[2-(dimethylamino)ethyl]methylamino]ethanol (DMAEA), 3-(N,N-dimethylamino)propylamine (DMAPA), bis-(3-dimethylaminopropylamine) (BDMAPA), and combinations thereof.
[0060] The reaction of the partially blocked polyisocyanate with the amine compound having active hydrogen can usually be carried out by dosing the partially blocked polyisocyanate with the amine compound having active hydrogen over a period of time, and, for example, after dosing is complete, heat may be applied to the reaction mixture to promote the reaction between the partially blocked polyisocyanate and the amine compound having active hydrogen.
[0061] The amine-containing blocked polyisocyanate obtained in step (ii) is substantially free of isocyanate groups, and in particular free of detectable isocyanate groups.
[0062] In step (ii), any suitable organic solvent and, optionally, a catalyst known in the art for the reaction of a partially blocked polyisocyanate with an amine compound having an active hydrogen can be used.
[0063] The reactions in step (i) (or steps (i-1) and (i-2)) and step (ii) can be carried out in the same or different organic solvents or solvent mixtures. In particular, the reactions in step (i) (or steps (i-1) and (i-2)) and step (ii) are carried out in the same organic solvent or solvent mixture. Suitable solvents may be, for example, acetone, butanone, methyl isobutyl ketone (MIBK), cyclohexanone, N-methyl-2-pyrrolidone (NMP), acetonitrile, dimethyl sulfoxide (DMSO), tetrahydrofuran (THF), 1,4-dioxane, and C1-C4-alkyl-C1-C4-alkanoates, and combinations thereof. The organic solvent or solvent mixture, if used in step(s), may not be removed from the reaction mixture obtained from step(s) and is therefore included in the aqueous dispersion of the blocked polyisocyanate having a neutralized amine.
[0064] The amine-containing blocked polyisocyanate obtained in step (ii) can contain 30 to 200, preferably 50 to 180 millimoles (mmol) of amine constitutional units per 100 g of the amine-containing blocked polyisocyanate, calculated based on the solid content.
[0065] The amine-containing blocked polyisocyanate can be neutralized in step (iii) with any inorganic or organic acid as a neutralizing agent. Suitable inorganic acids include, for example, hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, boric acid, and perchloric acid. Suitable organic acids include, for example, mono- or polycarboxylic acids optionally substituted with hydroxyl groups. In particular, organic acids include C1-C 10 -Monocarboxylic acids, C1-C 10 -Dicarboxylic acids, C1-C 10 -Tricarboxylic acids, C1-C 10 -Hydroxymonocarboxylic acids, C1-C 10 -Hydroxydicarboxylic acids, C1-C 10 hydroxytricarboxylic acids, and combinations thereof. Examples of organic acids include, but are not limited to, formic acid, acetic acid, propanoic acid, butanoic acid, lactic acid, glycolic acid, 3-hydroxybutanoic acid, 2-hydroxyisobutanoic acid, malic acid, oxalic acid, malonic acid, methylmalonic acid, succinic acid, methylsuccinic acid, adipic acid, pimelic acid, suberic acid, glutaric acid, citric acid, tartaric acid, fumaric acid, benzoic acid, and combinations thereof. Suitable organic acids may be selected from, in particular, formic acid, acetic acid, propanoic acid, lactic acid, glycolic acid, malic acid, oxalic acid, adipic acid, citric acid, succinic acid, fumaric acid, benzoic acid, and combinations thereof.
[0066] Neutralization can be carried out in the presence of water, for example, by introducing an acid as neutralizing agent in the form of its aqueous solution.
[0067] Neutralization can be carried out using an equivalent amount of acid in the range of 20% to 125%, preferably 30% to 100%, more preferably 30% to 90%, based on the molar amount of amino groups in the amine-containing blocked polyisocyanate.
[0068] Dispersion in water in step (iii) can typically be carried out, for example, by stirring. It should be understood that dispersion may take place during or after neutralization. Preferably, neutralization is followed by a separate dispersion operation.
[0069] According to the present invention, it is not necessary to use an emulsifier or dispersant for dispersion.
[0070] In some embodiments, the dispersion in step (iii) is carried out by mixing the neutralized mixture with water in the absence of added emulsifiers or dispersants.
[0071] The added emulsifier or dispersant is believed to improve the stability of the dispersion, and therefore the dispersion in step (iii) may be carried out in the presence of an added emulsifier or dispersant, but an emulsifier or dispersant is not required, in which case the aqueous dispersion of the neutralized amine-bearing blocked polyisocyanate according to the present invention will contain an emulsifier or dispersant.
[0072] Any conventional emulsifier or dispersant for preparing an aqueous dispersion of a blocked polyisocyanate can be used, including nonionic, anionic, cationic, or zwitterionic emulsifiers or dispersants. In particular, nonionic emulsifiers or dispersants can be mentioned. Suitable nonionic emulsifiers or dispersants can be selected from polyalkylene oxides, such as polyethylene oxide and polypropylene oxide, ethoxylated or propoxylated fatty alcohols, ethoxylated or propoxylated alkylphenols, ethoxylated or propoxylated fatty acids, ethoxylated or propoxylated fatty esters, sorbitan derivatives, sucrose esters and derivatives, ethylene oxide-propylene oxide block copolymers, fluorinated alkyl polyoxyethylene ethanols, and combinations thereof.
[0073] The aqueous dispersion of the blocked polyisocyanate with neutralized amine according to the present invention may further comprise additional components such as organic solvents, colorants or pigments, viscosity modifiers, leveling agents, gel-forming inhibitors, light stabilizers, antioxidants, ultraviolet absorbers, heat resistance improvers, inorganic or organic fillers, plasticizers, lubricants, softeners, antistatic agents, reinforcing agents, and combinations thereof.
[0074] If included, additional components may be introduced into the aqueous dispersion of neutralized amine-bearing blocked polyisocyanate according to the present invention after step (ii), for example, before neutralization in step (iii), between neutralization and dispersing in step (iii), or during dispersing in step (iii).
[0075] The aqueous dispersions of blocked polyisocyanates with neutralized amines according to the present invention may have one or more of the following properties: i) a pH in the range of 3.0 to 8.0, preferably 3.5 to 8.0, more preferably 4.0 to 8.0, measured at 20°C according to DIN 55659-1; ii) a conductivity in the range of 2 to 10 mS / cm, preferably 3 to 8 mS / cm, measured at 20°C according to DIN EN ISO 15091; iii) a Z-average particle size measured according to DIN ISO 13321 in the range of 60 to 200 nm, preferably 60 to 160 nm; iv) a polydispersity index (PDI), a measure of particle size distribution, of less than 0.2, measured according to DIN ISO 13321; v) a solids content of 10% to 40% by weight, preferably 15% to 35% by weight, measured according to DIN EN ISO 3251 at 130°C for 60 minutes; vi) a molar equivalent of acid (MEQ-A), measured according to DIN EN ISO 15880, ranging from 20 to 150 mmol / 100 g, preferably from 30 to 120 mmol / 100 g; and vii) Molar equivalents of base (MEQ-B), measured according to DIN EN ISO 15880, in the range of 30 to 200 mmol / 100 g, preferably 50 to 180 mmol / 100 g.
[0076] Component (B), i.e., the blocked polyisocyanate having a neutralized amine, can account for 100% by weight of the curing agent in the cathodic electrodeposition coating composition of the present invention. Alternatively, the cathodic electrodeposition coating composition of the present invention may contain a curing agent (D) other than the blocked polyisocyanate having a neutralized amine.
[0077] (C) Curing catalyst A curing catalyst is required to promote the reaction between the cationic amino-containing epoxy resin (A) and the blocked polyisocyanate (B) having neutralized amine building blocks. Any curing catalyst commonly used in electrodeposition coating can be used. Preferably, metal catalysts such as triphenyltin hydroxide, butyl stannoate, dioctyltin oxide, dibutyltin dilaurate, dibutyltin diacetate, dibutyltin oxide, and oxides of titanium, hafnium, zirconium, niobium, zinc, bismuth, lead, indium, tin, copper, and yttrium can be used.
[0078] The curing catalyst can be introduced into the cathodic electrodeposition coating composition of the present invention in the form of a paste containing a ground resin, a pigment, a filler, and a catalyst. The paste can be prepared, for example, by mixing a pigment with a ground resin for dispersing the pigment and a neutralizing agent. Examples of suitable ground resins for dispersing the pigment include, but are not limited to, epoxy resins having hydroxyl groups and cationic groups, acrylic resins having hydroxyl groups and cationic groups, tertiary amine-type, quaternary ammonium salt-type, and tertiary sulfonium salt-type epoxy resins, and tertiary amine-type, quaternary ammonium salt-type, and tertiary sulfonium salt-type acrylic resins.
[0079] Examples of suitable pigments include, but are not limited to, white pigments such as titanium dioxide, aluminum silicate, silicon dioxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, magnesium carbonate, and magnesium silicate; black pigments such as carbon black; or colored pigments. Examples of colored pigments include, for example, inorganic colored pigments such as iron oxide or chromium oxide, organic colored pigments such as azo pigments, triphenylmethane pigments, indigoid pigments, metal complex pigments, isoindolinone pigments, anthraquinone pigments, perylene and perinone pigments, dioxazine pigments, quinophthalone pigments, diketopyrrolopyrrole or pyrazoloquinazolone pigments.
[0080] The curing catalyst may be present separately from the cationic amino-containing epoxy resin (A), the neutralized amine-containing blocked polyisocyanate (B), and the optional curing agent (D), and is mixed with components (A), (B), and optional (D) immediately prior to application in a cathodic electrodeposition coating process.
[0081] Generally, the cathodic electrodeposition coating composition according to the present invention can contain the curing catalyst (C) in an amount of 0.01% to 2% by weight, preferably 0.05% to 1% by weight, based on the total weight of the cathodic electrodeposition coating composition.
[0082] (D) Hardener Optionally, the cathodic electrodeposition coating composition may contain an additional curing agent. There are no particular restrictions on the optional curing agents that may be used in combination with the neutralized amine-containing blocked polyisocyanate.
[0083] As the optional curing agent in the cathodic electrodeposition coating composition according to the present invention, any conventional blocked polyisocyanate, for example, a reaction product of a polyisocyanate compound with a blocking agent, and optionally an active hydrogen-containing compound other than the blocking agent, can be used.
[0084] Examples of suitable polyisocyanate compounds include those described above for the blocked polyisocyanates with neutralized amines.
[0085] Examples of suitable blocking agents may be selected from aliphatic alcohols such as methanol, ethanol, chloroethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, 3,5,5-trimethylhexanol, decanol, and lauryl alcohol; alicyclic alcohols such as cyclopentanol and cyclohexanol; and aromatic alkyl alcohols such as phenylcarbinol and methylphenylcarbinol. Other suitable blocking agents include, for example, hydroxylamines such as ethanolamine, oximes such as methyl ethyl ketone oxime, acetone oxime, and cyclohexanone oxime, or amines such as dibutylamine and diisopropylamine.
[0086] The cathodic electrodeposition coating composition according to the present invention may comprise a curing agent comprising a neutralized amine-containing blocked polyisocyanate (B) and an optional curing agent (D) in a total amount of 10% to 40% by mass, preferably 15% to 35% by mass, based on the solids content of the cathodic electrodeposition coating composition.
[0087] The neutralized amine-containing blocked polyisocyanate (B) can account for at least 10% by weight, preferably at least 20% by weight, of the total amount of the neutralized amine-containing blocked polyisocyanate (B) and optional curing agent (D).
[0088] Thus, the blocked polyisocyanate (B) having a neutralized amine can be present in the cathodic electrodeposition coating composition according to the present invention in an amount of 2% to 40% by mass, more preferably 3% to 35% by mass, based on the solids content of the cathodic electrodeposition coating composition.
[0089] The curing agent (D) may be present in the cathodic electrodeposition coating composition according to the invention in an amount of up to 38% by weight, preferably up to 32% by weight, based on the solids content of the cathodic electrodeposition coating composition.
[0090] The cathodic electrodeposition coating composition according to the invention may contain further additives such as pigments, plasticizers, fillers, wetting agents and catalysts. In particular, the cathodic electrodeposition coating composition may contain a pigment.
[0091] Method for preparing cathodic electrodeposition coating compositions The present invention provides a method for preparing a cathodic electrodeposition coating composition, which comprises mixing an aqueous dispersion containing a cationic amino-containing epoxy resin (A) with an aqueous dispersion containing a neutralized amine-containing blocked polyisocyanate (B) and a curing catalyst (C).
[0092] The cationic amino-containing epoxy resin (A) is as described above. An aqueous dispersion containing the cationic amino-containing epoxy resin (A) can be prepared by neutralizing the amino-containing epoxy resin with an acid and dispersing the resultant in water. Optionally, the aqueous dispersion may contain additives such as a neutralizing agent, an emulsifier, a catalyst, and resin components other than the cationic amino-containing epoxy resin (A).
[0093] The aqueous dispersion containing the neutralized amine-containing blocked polyisocyanate (B) can be prepared by the process described herein for obtaining the neutralized amine-containing blocked polyisocyanate. The above-mentioned explanations and preferences regarding the aqueous dispersion of the neutralized amine-containing blocked polyisocyanate are applicable here.
[0094] The curing catalyst (C) is as described above.
[0095] The method for preparing the cathodic electrodeposition coating composition may optionally include a curing agent other than the neutralized amine-containing blocked polyisocyanate. The additional curing agent is as described above for curing agent (D). For example, the additional curing agent can be incorporated into the cathodic electrodeposition coating composition together with the cationic amino-containing epoxy resin (A).
[0096] In particular, the additional curing agent may be mixed with the unneutralized amino-containing epoxy resin, neutralized, and dispersed. In this case, the aqueous dispersion containing the cationic amino-containing epoxy resin (A) also contains the additional curing agent, and if the additional curing agent contains a basic group, it may be neutralized.
[0097] In some embodiments, the present invention provides a method for producing a pharmaceutical composition comprising the steps of: (1) mixing an amino-containing epoxy resin with a curing agent other than a blocked polyisocyanate having a neutralized amine (B), neutralizing, and dispersing in water to provide an aqueous dispersion comprising a cationic amino-containing epoxy resin (A) and additional curing agent; (2) mixing the resulting aqueous dispersion containing the cationic amino-containing epoxy resin (A) and additional curing agent with an aqueous dispersion containing the neutralized amine-containing blocked polyisocyanate (B); (3) immediately prior to application in a cathodic electrodeposition coating process, mixing an aqueous dispersion containing a cationic amino-containing epoxy resin (A) and an aqueous dispersion containing a neutralized amine-containing blocked polyisocyanate (B) with a curing catalyst (C); The present invention provides a method for preparing a cathodic electrodeposition coating composition, comprising:
[0098] The curing catalyst may be introduced into the cathodic electrodeposition coating composition according to the present invention in the form of a paste containing ground resin, pigment, filler and catalyst.
[0099] The present invention further provides a coating bath for cathodic electrodeposition coating, which comprises the cathodic electrodeposition coating composition of the present invention or the cathodic electrodeposition coating composition prepared by the method of the present invention.
[0100] Embodiment Various embodiments are listed below, and it will be understood that the listed embodiments can be combined with all aspects and other embodiments in accordance with the scope of the present invention.
[0101] Embodiment 1 (A) a cationic amino-containing epoxy resin, (B) a blocked polyisocyanate having a neutralized amine, the process comprising the steps of: (i) reacting a polyurethane prepolymer having isocyanate groups with at least one blocking agent selected from oximes, pyrazoles, and active methylene compounds to provide a partially blocked polyisocyanate; (ii) reacting the remaining isocyanate groups in the partially blocked polyisocyanate with an amine compound having an active hydrogen to provide an amine-containing blocked polyisocyanate; (iii) neutralizing the amine-containing blocked polyisocyanate with an acid; a blocked polyisocyanate having a neutralized amine, obtainable or obtained by a process comprising: (C) Curing catalyst A cathodic electrodeposition coating composition comprising:
[0102] Embodiment 2 2. The cathodic electrodeposition coating composition according to embodiment 1, wherein the polyurethane prepolymer having isocyanate groups is obtainable or obtained by reaction of a polyisocyanate with a polyol.
[0103] Embodiment 3 The partially blocked polyisocyanate is subjected to the following steps: (i-1) a step of preparing a polyurethane prepolymer having an isocyanate group by reacting a polyisocyanate with a polyol; and (i-2) a step of reacting the polyurethane prepolymer having an isocyanate group obtained in the step (i-1) with at least one blocking agent selected from the group consisting of oxime, pyrazole, and active methylene compound; 3. The cathodic electrodeposition coating composition of embodiment 1 or 2, obtainable or obtained by a process comprising:
[0104] Embodiment 4 4. The cathodic electrodeposition coating composition according to any one of embodiments 1 to 3, wherein the blocking agent is at least one selected from the group consisting of formamide oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, diethyl ketoxime, diacetyl monooxime, benzophenoxime, cyclopentanone oxime, and cyclohexanone oxime.
[0105] Embodiment 5 5. The cathodic electrodeposition coating composition of any one of embodiments 2 to 4, wherein the polyisocyanate is at least one selected from aliphatic, cycloaliphatic, and aromatic diisocyanates, and polyisocyanates having at least three isocyanate groups per molecule.
[0106] Embodiment 6 6. The cathodic electrodeposition coating composition of embodiment 5, wherein the polyisocyanate is at least one selected from the group consisting of monomers, isomers, and oligomers of 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,4-naphthylene diisocyanate, 1,5-naphthylene diisocyanate, biphenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, and 2,2-diphenylpropane-4,4'-diisocyanate.
[0107] Embodiment 7 7. The cathodic electrodeposition coating composition according to any one of embodiments 1 to 6, wherein the polyurethane prepolymer having isocyanate groups has an isocyanate group content in the range of 70 mol % to 90 mol %, preferably 70 mol % to 80 mol %, based on the total amount of isocyanate groups and urethane groups in the polyurethane prepolymer.
[0108] Embodiment 8 8. The cathodic electrodeposition coating composition according to any one of embodiments 1 to 7, wherein the partially blocked polyisocyanate has a content of remaining isocyanate groups in the range of 10 mol % to 25 mol %, preferably 10 mol % to 20 mol %, based on the total amount of remaining blocked polyisocyanate groups and urethane groups contained in the partially blocked polyisocyanate.
[0109] Embodiment 9 9. The cathodic electrodeposition coating composition according to any one of embodiments 1 to 8, wherein the curing catalyst is preferably a metal catalyst, more preferably at least one selected from the group consisting of triphenyltin hydroxide, butyl stannoate, dioctyltin oxide, dibutyltin dilaurate, dibutyltin diacetate, dibutyltin oxide, oxides of titanium, hafnium, zirconium, niobium, zinc, bismuth, lead, indium, tin, copper, and yttrium.
[0110] Embodiment 10 10. The cathodic electrodeposition coating composition of embodiment 9, wherein the curing catalyst is provided in the form of a paste comprising ground resin, pigment, filler, and catalyst.
[0111] Embodiment 11 11. The cathodic electrodeposition coating composition of any one of the preceding embodiments, further comprising a curing agent (D) other than the blocked polyisocyanate having a neutralized amine.
[0112] Embodiment 12 10. The cathodic electrodeposition coating composition according to claim 9, wherein the content of the neutralized amine-containing blocked polyisocyanate is at least 10% by mass, preferably at least 20% by mass, based on the total amount of the neutralized amine-containing blocked polyisocyanate and the curing agent (D).
[0113] Embodiment 13 13. A method of preparing the cathodic electrodeposition coating composition of any one of claims 1 to 12, comprising combining an aqueous dispersion comprising the cationic amino-containing epoxy resin, an aqueous dispersion comprising the neutralized amine-containing blocked polyisocyanate, and a catalyst.
[0114] Embodiment 14 14. The method of embodiment 13, wherein the aqueous dispersion comprising the cationic amino-containing epoxy resin is prepared by neutralizing an amino-containing epoxy resin with an acid and dispersing it in water.
[0115] Embodiment 15 15. The method of embodiment 13 or 14, wherein a curing agent (D) is added to the aqueous dispersion comprising the cationic amino-containing epoxy resin.
[0116] Embodiment 16 13. A coating bath for cathodic electrodeposition comprising the cathodic electrodeposition coating composition of any one of embodiments 1 to 12.
[0117] Embodiment 17 A coating bath for cathodic electrodeposition comprising a cathodic electrodeposition coating composition prepared by the method of any one of claims 13 to 15. [Example]
[0118] The present invention is further illustrated by the following examples which set forth particularly advantageous embodiments. The examples are provided to illustrate the invention but are not intended to limit the invention.
[0119] Description of materials and measurements material: Lupranate® M20S: a solvent-free polymer product based on 4,4'-diphenylmethane diisocyanate (MDI) containing oligomers and isomers, with an average functionality of about 2.7 and an NCO content of 31.5 g / 100 g according to ASTM D 5155, available from BASF; CathodGuard® 800: a set of electrocoat paints comprising two separate packages, namely a first package of pigment paste with a solids content of 65% by weight and a second package of an aqueous binder dispersion of cationic amino-containing epoxy resin and hardener with a solids content of 37.5% by weight, available from BASF; Pluriol® C 1651: dibutoxyethoxyformal, available from BASF; BE-188EL: liquid bisphenol A epoxy resin with an epoxy equivalent weight of approximately 188 g / mol, available from Chang Chun Group; PPG 900: Pluriol® P 900 available from BASF; Bisphenol A 6EO: bisphenol A ethoxylate with 3 EO / phenol, available from Sigma-Alrdrich; MIBK: methyl isobutyl ketone, solvent; MEKO: Methyl ethyl ketoxime, blocking agent; MDEA: N-methyldiethanolamine; DMAPA: N,N-dimethylaminopropylamine.
[0120] measurement: The methods and equipment described in the table below were used to measure the examples.
[0121] [Table 1]
[0122] I. Preparation example Example 1: Preparation of butyl glycol blocked polyisocyanate (conventional product) 494.8 parts by weight of methyl isobutyl ketone (MIBK), 789.1 parts by weight of butyl glycol, and 0.90 parts by weight of dibutyltin dilaurate (DBTL) were charged into a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. The initial charge was heated to 50°C, and 933.8 parts by weight of Lupranate® M20S was slowly added to the reactor over 60 minutes with continuous stirring. After the addition was completed, 175.2 parts by weight of phenoxypropanol (POP) was added to the reactor as a solvent. A butyl glycol-blocked polyisocyanate curing agent was obtained.
[0123] Example 2: Preparation of MEKO Blocked Polyisocyanates Containing Amine Building Blocks (Unneutralized) 900 parts by weight of Lupranate® M20S, 218.6 parts by weight of MIBK, and 0.18 parts by weight of DBTL were charged into a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. The initial charge was heated to 30°C, and 56.2 parts by weight of 1,2-propanediol was added to the reactor at a uniform rate over 60 minutes with continuous stirring. 546.5 parts by weight of MIBK was then added to the reactor, and the contents of the reactor were cooled to 30°C. At 30°C, 343.4 parts by weight of MEKO was slowly added to the reactor over 20 minutes. After the MEKO addition was completed, the reaction was ramped up to 60°C and continued for an additional 30 minutes. The resulting intermediate was immediately transferred to a dropping funnel and then attached to a second, clean reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. 120.8 parts by weight of DMAPA was initially charged to the second reactor and heated to 30°C. The intermediate in the dropping funnel was then added to the reactor at a uniform rate over 60 minutes with continuous stirring. 30 minutes after the end of addition, the reaction mixture was heated to 60°C and stirred for an additional 15 minutes. A MEKO-blocked polyisocyanate curing agent containing unneutralized amine building blocks was obtained.
[0124] Example 3: Preparation of MEKO Blocked Polyisocyanates Containing Self-Emulsifying Hardener-Neutralized Amine Building Blocks 150.9 parts by weight of MEKO, 19.7 parts by weight of 1,2-propanediol, 408 parts by weight of methyl isobutyl ketone (MIBK), and 0.18 parts by weight of dibutyltin dilaurate (DBTL) were charged to a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. This initial charge was heated to 30°C. Then, over a period of 60 minutes, 400 parts by weight of Lupranate® M20S was added to the reactor at a uniform rate with continuous stirring. After the addition was complete, the reaction temperature was cooled to 60°C and stirred for an additional 60 minutes. After cooling to 30°C, 41.3 parts by weight of MDEA was added to the reactor at a rate such that the temperature did not exceed 80°C. Thirty minutes after the addition was complete, the reaction mixture was raised to 80°C and stirred for an additional 60 minutes to obtain an organic system containing an amine-containing MEKO-blocked polyisocyanate. A mixture of 510 parts by weight of water and 23.1 parts by weight of formic acid (86%) was then added to the organic system with vigorous stirring to obtain an aqueous dispersion of blocked polyisocyanate with neutralized amine. The properties of the resulting aqueous dispersion are shown in Table 1 below.
[0125] Example 4: Preparation of MEKO Blocked Polyisocyanates Containing Self-Emulsifying Hardener-Neutralized Amine Building Blocks 500 parts by weight of Lupranate® M20S, 121.4 parts by weight of MIBK, and 0.23 parts by weight of DBTL were charged to a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. This initial charge was heated to 30°C. 31.2 parts by weight of 1,2-propanediol were then uniformly charged to the reactor over a period of 60 minutes with continuous stirring. 303.6 parts by weight of MIBK were then added to the reactor, and the contents of the reactor were cooled to 30°C. At 30°C, 190.8 parts by weight of MEKO were slowly charged to the reactor over a period of 20 minutes. After the MEKO charge was completed, the reaction was heated to 60°C and continued for an additional 30 minutes. The resulting intermediate was immediately transferred to a dropping funnel and attached to a second, clean reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. 67.1 parts by weight of DMAPA were initially charged to the second reactor and heated to 30°C. The intermediate in the dropping funnel was then added to the reactor at a uniform rate over 60 minutes with continuous stirring. Thirty minutes after the end of addition, the reaction mixture was heated to 60°C and stirred for an additional 15 minutes. The resulting organic system was transferred to a plastic container. A mixture of 36.9 parts by weight of water and 19.9 g of formic acid (86%) was then slowly added to the organic system to create a water-in-oil phase. An additional 1,700 parts by weight of water was then added to effect phase inversion to an oil-in-water phase. The properties of the resulting aqueous dispersion are shown in Table 1 below.
[0126] Example 5: Preparation of MEKO Blocked Polyisocyanates Containing Self-Emulsifying Hardener-Neutralized Amine Building Blocks 450 parts by weight of Lupranate® M20S, 131.6 parts by weight of MIBK, and 0.20 parts by weight of DBTL were charged to a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. The initial charge was heated to 30°C. Then, 309.0 parts by weight of bisphenol A 6EO were uniformly charged into the reactor over 60 minutes with continuous stirring. Subsequently, 328.9 parts by weight of MIBK were added to the reactor, and the contents of the reactor were cooled to 30°C. At 30°C, 171.0 parts by weight of MEKO were slowly charged into the reactor over 20 minutes. After the MEKO charge was completed, the reaction was heated to 60°C and continued for an additional 30 minutes. The resulting intermediate was immediately transferred to a dropping funnel and attached to a second, clean reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. 60.2 parts by weight of DMAPA was initially charged into the second reactor and heated to 30°C. The intermediate in the dropping funnel was then added to the reactor at a uniform rate over 60 minutes with continuous stirring. 30 minutes after the end of addition, the reaction mixture was again heated to 60°C and stirred for an additional 15 minutes. The resulting organic system was transferred to a plastic container. A mixture of 35.8 parts by weight of water and 18.9 parts by weight of formic acid (86%) was then slowly added to the organic system to create a water-in-oil phase. An additional 2050 parts by weight of water was then added to effect phase inversion to an oil-in-water phase. The properties of the resulting aqueous dispersion are shown in Table 1 below.
[0127] Example 6: Preparation of MEKO Blocked Polyisocyanates Containing Self-Emulsifying Hardener-Neutralized Amine Building Blocks 500 parts by weight of Lupranate® M20S, 112.3 parts by weight of MIBK, and 0.23 parts by weight of DBTL were charged into a reactor equipped with a condenser, a nitrogen gas inlet, and a nitrogen gas outlet. The initial charge was heated to 30°C, and 30.9 parts by weight of 1,2-propanediol was rapidly added to the reactor. The reaction was continued for 60 minutes at 60°C with continuous stirring. Next, 224.7 parts by weight of MIBK was added to the reactor, and the contents of the reactor were cooled to 30°C. At 30°C, 188.8 parts by weight of MEKO was slowly added to the reactor over 20 minutes. After the MEKO addition was completed, the reaction was again heated to 60°C and continued for another 30 minutes. After cooling to 30°C, 66.4 parts by weight of DMAPA was rapidly added to the reactor. 20 minutes after the addition was completed, the reaction mixture was heated to 60°C and stirred for an additional 30 minutes. The resulting organic system was transferred to a plastic container. A mixture of 38.9 parts by weight of water and 20.9 parts by weight of formic acid (86%) was then slowly added to the organic system to create a water-in-oil phase. An additional 1960.5 parts by weight of water was then added to effect phase inversion to an oil-in-water phase. The properties of the resulting aqueous dispersion are shown in Table 1 below.
[0128] [Table 2]
[0129] Example 7: Preparation of an aqueous dispersion of a cationic amino-containing epoxy resin An amino-containing epoxy resin was prepared according to US Pat. No. 6,274,649 B1, column 9, lines 15-35. 1128 parts by weight of liquid bisphenol A epoxy resin (BE-188EL), 262 parts by weight of dodecylphenol, 31.4 parts by weight of xylene, and 228 parts by weight of bisphenol A were charged into a reactor equipped with a stirrer, reflux condenser, thermometer, and inert gas inlet. The reactor was heated to 127°C, and 1.6 g of triphenylphosphine was added thereto with stirring under nitrogen to initiate an exothermic reaction, which was then heated to 160°C. The mixture was cooled again to 130°C, and the epoxide content was then confirmed. When the epoxide content indicated that more than 98% of the phenolic OH groups had reacted, 297.5 parts by weight of PPG 900 was added while simultaneously cooling. After 5 minutes, 131.25 parts by weight of diethanolamine (DEOLA) was added at 120°C with further cooling. When the temperature dropped to 110°C, 63.75 parts by weight of N,N-dimethylaminopropylamine (DMAPA) was added. After a short exotherm (Tmax of 140°C), the mixture was further reacted at 130°C for 2 hours until the viscosity became constant, yielding an organic system containing an amino-containing epoxy resin.
[0130] The organic system containing the amino-containing epoxy resin was then immediately transferred with stirring to a plastic container containing a mixture of 3840 parts by weight of water and 48.8 parts by weight of formic acid (86%) to obtain an aqueous dispersion of cationic amino-containing epoxy resin. The properties of the resulting dispersion are shown in Table 2 below.
[0131] [Table 3]
[0132] Example 8: Preparation of binder dispersion with conventional hardener To 1353 parts by weight of the organic system containing the amino-containing epoxy resin intermediate prepared in Example 7, 470.6 parts by weight of the butyl glycol-blocked polyisocyanate curing agent prepared in Example 1 was added and stirred for 20 minutes to achieve uniform mixing. The resulting organic mixture was then immediately transferred to a plastic container containing a mixture of 2609.1 parts by weight of water and 30.4 parts by weight of formic acid (86%). A binder dispersion containing the resin component and a conventional curing agent component was obtained. The properties of this dispersion are shown in Table 3 below.
[0133] Example 9: Preparation of binder dispersion with conventional hardener To 1353 parts by weight of the organic system containing the amino-containing epoxy resin intermediate prepared in Example 7, 294.1 parts by weight of the butyl glycol-blocked polyisocyanate curing agent prepared in Example 1 was added and stirred for 20 minutes to achieve uniform mixing. The resulting organic mixture was immediately transferred to a plastic container containing a mixture of 2475.1 parts by weight of water and 30.9 parts by weight of formic acid (86%). A binder dispersion containing the resin component and a conventional curing agent component was obtained. The properties of this dispersion are shown in Table 3 below.
[0134] Example 10: Preparation of binder dispersion with conventional hardener To 1353 parts by weight of the organic system containing the amino-containing epoxy resin intermediate prepared in Example 7, 117.6 parts by weight of the butyl glycol-blocked polyisocyanate curing agent prepared in Example 1 was added and stirred for 20 minutes to achieve uniform mixing. The resulting organic mixture was immediately transferred to a plastic container containing a mixture of 2341.6 parts by weight of water and 31.8 parts by weight of formic acid (86%). A binder dispersion containing the resin component and a conventional curing agent component was obtained. The properties of this dispersion are shown in Table 3 below.
[0135] Example 11: Preparation of a binder dispersion containing a MEKO-blocked polyisocyanate curing agent containing non-neutralized amine building blocks To 680.8 parts by weight of the organic system containing the amino-containing epoxy resin prepared in Example 7, 111.1 parts by weight of MIBK was added along with 413.9 parts by weight of the MEKO-blocked polyisocyanate curing agent containing unneutralized amine building blocks prepared in Example 2 at 75°C, and the mixture was stirred for 20 minutes to achieve uniform mixing. The resulting organic mixture was immediately transferred to a plastic container containing a mixture of 1632.8 parts by weight of water and 15.3 parts by weight of formic acid (86%). A binder dispersion containing a resin component and a non-inventive curing agent component was obtained. The properties of this dispersion are shown in Table 3 below.
[0136] [Table 4]
[0137] Examples 12 to 14: Preparation of binder dispersions containing self-emulsifying hardener components The self-emulsifying curing agent dispersions prepared in Examples 3 to 5 and the aqueous dispersion of cationic amino-containing epoxy resin (i.e., resin dispersion) prepared in Example 7 were mixed with moderate stirring to obtain a uniform mixture. In this way, a 1K binder dispersion was obtained. The formulation and properties of the 1K binder dispersion are shown in Tables 4 and 5 below.
[0138] [Table 5]
[0139] [Table 6]
[0140] Examples 15-20: Preparation of binder dispersions containing self-emulsifying hardeners and conventional hardeners A portion of the self-emulsifying hardener dispersion was mixed with a portion of the dispersion containing the resin and conventional hardener prepared in Examples 8 to 10 under moderate stirring to obtain a uniform mixture. A 1K binder dispersion was thus obtained. The formulation and properties of this 1K binder dispersion are shown in Tables 6 and 7 below.
[0141] [Table 7]
[0142] [Table 8]
[0143] II. Application Examples II.a Formulation Examples B1 to B5 Comparative and inventive cathodic electrodeposition coating (E-coat) materials were prepared by combining the aqueous binder dispersion, aqueous pigment paste, and deionized water according to the formulations shown in Table 8. The combination was carried out by first diluting the binder dispersion with deionized water while stirring, and then introducing the pigment paste. E-coat materials B1 to B5 were obtained.
[0144] [Table 9]
[0145] Examples B6 and B7 Comparative and inventive cathodic electrodeposition coating (E-coat) materials were prepared by combining the aqueous binder dispersion, aqueous pigment paste, and deionized water according to the formulations shown in Table 9. The combination was carried out by first diluting the binder dispersion with deionized water under stirring, then introducing the pigment paste, and then introducing Pluriol® C 1651. E-coat materials B6 and B7 were obtained.
[0146] [Table 10]
[0147] Examples B8 to B11 Comparative and inventive cathodic electrodeposition coating (E-coat) materials were prepared by combining the aqueous binder dispersion, aqueous pigment paste, and deionized water according to the formulations shown in Table 10. The combination was carried out by first diluting the binder dispersion with deionized water under stirring, then introducing the pigment paste, and then introducing Pluriol® C 1651. E-coat materials B8 to B11 were obtained.
[0148] [Table 11]
[0149] Examples B12 to B17 Comparative and inventive cathodic electrodeposition coating (E-coat) materials were prepared by combining the aqueous binder dispersion, aqueous pigment paste, and deionized water according to the formulations shown in Table 11. The combination was carried out by first diluting the binder dispersion with deionized water while stirring, and then introducing the pigment paste. E-coat materials B12 to B17 were obtained.
[0150] [Table 12]
[0151] II.b Measurement (1) General procedure for cathodic electrodeposition coating Unless otherwise specified, the E-coat materials as coating baths were aged at room temperature with stirring for 1 day. Films were deposited on cathodically connected zinc phosphate-treated steel test panels (26S / 6800 / OC or 26 / 1 / 6800 MBZ) at a deposition voltage of 260 volts for 2 minutes at a bath temperature of approximately 30°C. For general testing, the deposited films were rinsed with deionized water and then baked at 175°C (substrate temperature for 15 minutes) unless otherwise specified.
[0152] (2) Dynamic Mechanical Analysis (DMA) Test E-coat materials B1-B5 were tested on a TA Instruments DMA Q800 Dynamic Mechanical Analyzer. The test setup is summarized below and the results are shown in Table 12.
[0153] Onset Temperature Test Settings: Film / fiber tension clamp; Sample size: 10mm(L) x 6.5mm(W); Distortion: 0.05%, Frequency: 1Hz; and Ramp to 110°C at 2°C / min; Ramp to 205°C at 1.3°C / min.
[0154] Offset Time Test Settings: Film / fiber tension clamp; Sample size: 10mm(L) x 6.5mm(W); Distortion: 0.05%, Frequency: 1Hz; and Ramp(T-25) / 10°C / min, then isothermal at the given temperature for 60 min.
[0155] [Table 13]
[0156] As shown in Table 12, for all samples B2, B3, B4 and B5 containing self-emulsifying curing agents, gelation of the E-coat films occurred at temperatures below 120°C, and the films could be successfully cured within 36.03 minutes, 22.13 minutes, 18.73 minutes and 16.88 minutes, respectively, at 140°C. In contrast, sample B1, which did not contain a self-emulsifying curing agent, could not be cured at 140°C.
[0157] (3) Stability test by differential scanning calorimetry (DSC) Sample B5 was tested for aging stability. Fresh Sample B5, Sample B5 after 2 weeks aging, and Sample B5 after 4 weeks aging were used as coating baths to prepare E-coated films according to the general procedure described above. The E-coated films were baked at different temperatures and for different periods, as summarized in Table 13 below. The Tg of the baked E-coated films was tested, and the results are shown in Table 13.
[0158] [Table 14]
[0159] Apparently, under low curing temperature conditions, there is no significant increase in the Tg of the baked E-coat films from the fresh bath, the 2-week aged bath, and the 4-week aged bath, which means that gelation does not occur during long-term aging of the bath. In other words, the E-coat material according to the present invention has good aging stability for at least 4 weeks.
[0160] (4) Stability test by roughness measurement The aging stability of E-coat materials can also be monitored by the change in appearance of the E-coat film. Better aging stability results in less change in roughness, while worse aging stability results in greater change in roughness. Using Sample B6 and Sample B7 as coating baths, E-coat films were prepared on 26 / 1 / 6800 MBZ panels according to the general procedure described above. The change in roughness of the film was measured, and the test results are shown in Table 14.
[0161] [Table 15]
[0162] Clearly, the film prepared from Sample B6 after 2 weeks of aging has a significantly higher Ra value than the film from Sample B6 in the fresh state. In contrast, the films prepared from Sample B7 in the fresh state and after 2 weeks of aging have no significant change in Ra value. The E-coat material according to the present invention has improved aging stability compared to the E-coat material containing an amino-containing epoxy resin and a curing agent (neutralized and dispersed together).
[0163] (5) Other performance tests The application performance was also tested for E-coat films prepared from samples B8-B17 according to the general procedure described above, and the test results are shown in Tables 15 and 16.
[0164] [Table 16]
[0165] [Table 17]
[0166] It has been found that cathodic electrodeposition coating compositions according to the present invention have improved stability while at the same time providing desirable film properties, such as higher or equal flexibility, higher corrosion resistance, and desirable application performance such as significantly reduced VOC and higher throw power.
Claims
1. (A) a cationic amino-containing epoxy resin, (B) a blocked polyisocyanate having a neutralized amine, comprising the steps of: (i) reacting a polyurethane prepolymer having isocyanate groups with at least one blocking agent selected from oximes, pyrazoles, and active methylene compounds to provide a partially blocked polyisocyanate; (ii) reacting the remaining isocyanate groups in the partially blocked polyisocyanate with an amine compound having an active hydrogen to provide an amine-containing blocked polyisocyanate; (iii) neutralizing the amine-containing blocked polyisocyanate with an acid; a blocked polyisocyanate having a neutralized amine, which is obtainable or obtained by a process comprising: (C) Curing catalyst 1. A cathodic electrodeposition coating composition comprising:
2. 2. A cathodic electrodeposition coating composition according to claim 1, wherein said polyurethane prepolymer having isocyanate groups is obtainable or obtained by reaction of a polyisocyanate with a polyol.
3. The partially blocked polyisocyanate of step (i) is subjected to the following steps: (i-1) reacting a polyisocyanate with a polyol to prepare a polyurethane prepolymer having an isocyanate group; and (i-2) a step of reacting the polyurethane prepolymer having an isocyanate group obtained in the step (i-1) with at least one blocking agent selected from oxime, pyrazole and active methylene compounds; 3. A cathodic electrodeposition coating composition according to claim 1 or 2, obtainable or obtained by a process comprising:
4. 3. The cathodic electrodeposition coating composition according to claim 1, wherein the blocking agent is at least one selected from the group consisting of formamide oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, diethyl ketoxime, diacetyl monoxime, benzophenoxime, cyclopentanone oxime and cyclohexanone oxime.
5. 3. The cathodic electrodeposition coating composition of claim 2, wherein the polyisocyanate is at least one selected from aliphatic, cycloaliphatic and aromatic diisocyanates, and polyisocyanates having at least three isocyanate groups per molecule.
6. The cathodic electrodeposition coating composition according to claim 5, wherein the polyisocyanate is at least one selected from the group consisting of 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,4-naphthylene diisocyanate, 1,5-naphthylene diisocyanate, biphenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, and 2,2-diphenylpropane-4,4'-diisocyanate monomers, isomers, and oligomers.
7. The cathodic electrodeposition coating composition according to claim 1 or 2, wherein the polyurethane prepolymer having an isocyanate group has a content of isocyanate groups in the range of 70 mol% to 90 mol%, preferably 70 mol% to 80 mol%, based on the total amount of isocyanate groups and urethane groups in the polyurethane prepolymer.
8. 3. The cathodic electrodeposition coating composition according to claim 1 or 2, wherein the partially blocked polyisocyanate has a content of remaining isocyanate groups in the range of 10 mol % to 25 mol %, preferably 10 mol % to 20 mol %, based on the total amount of remaining blocked polyisocyanate groups and urethane groups contained in the partially blocked polyisocyanate.
9. 3. The cathodic electrodeposition coating composition according to claim 1 or 2, wherein the curing catalyst is preferably a metal catalyst, more preferably at least one selected from the group consisting of triphenyltin hydroxide, butyl stannate, dioctyltin oxide, dibutyltin dilaurate, dibutyltin diacetate, dibutyltin oxide, titanium, hafnium, zirconium, niobium, zinc, bismuth, lead, indium, tin, copper and yttrium oxide.
10. 10. The cathodic electrodeposition coating composition of claim 9, wherein the curing catalyst is provided in the form of a paste comprising ground resin, pigment, filler and catalyst.
11. 3. The cathodic electrodeposition coating composition of claim 1, further comprising a curing agent (D) other than the blocked polyisocyanate having a neutralized amine.
12. 10. The cathodic electrodeposition coating composition according to claim 9, wherein the neutralized amine-containing blocked polyisocyanate has a content of at least 10% by weight, preferably at least 20% by weight, based on the total amount of the neutralized amine-containing blocked polyisocyanate and the curing agent (D).
13. 3. A method for preparing the cathodic electrodeposition coating composition of claim 1 or 2, comprising the step of mixing an aqueous dispersion containing the cationic amino-containing epoxy resin, an aqueous dispersion containing the blocked polyisocyanate with a neutralized amine, and a catalyst.
14. 14. The method of claim 13, wherein the aqueous dispersion containing the cationic amino-containing epoxy resin is prepared by neutralizing an amino-containing epoxy resin with an acid and dispersing it in water.
15. 14. The method of claim 13, wherein a curing agent (D), a blocked polyisocyanate with a neutralized amine, is added to the aqueous dispersion containing the cationic amino-containing epoxy resin.
16. A coating bath for cathodic electrodeposition comprising the cathodic electrodeposition coating composition according to claim 1 or 2.
17. A coating bath for cathodic electrodeposition comprising a cathodic electrodeposition coating composition prepared by the method of claim 13.
Citation Information
Patent Citations
Aqueous coating composition
JP1983113264A
Coating material containing curing agent dispersible in the absence of solvent
JP1996041422A
Method for producing cationic electrodeposition coating composition
EP3415574A1
Formation of electrodeposition coated film
JP1995300698A
Cationic electrodeposition coating composition and prevention of foaming by using the same
JP1998120947A