Polymer powders for producing high-resolution, low-roughness parts
Thermoplastic polymer powders with a specific particle size distribution improve the resolution and surface finish of 3D printed parts, addressing the limitations of existing methods by optimizing melting and reducing roughness without increasing production time or cost.
Patent Information
- Application Number
- JP2024527170
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-09
- Filing Date
- 2022-11-08
- Publication Date
- 2024-10-31
AI Technical Summary
Existing 3D printing methods using thermoplastic polymer powders for selective melting produce parts with unsatisfactory resolution and surface roughness, and existing treatments to improve these properties increase production time and cost.
The use of thermoplastic polymer powders with a specific particle size distribution, characterized by a volume average diameter less than 55 μm, a span less than 1.2, and a d ratio of 0.40 to 0.55, which optimizes melting and reduces surface roughness while maintaining good productivity.
The proposed polymer powders enhance the resolution and reduce surface roughness of 3D printed parts, avoiding structural defects and maintaining mechanical properties, without requiring additional treatments.
Smart Images

Figure 2024540414000001_ABST
Abstract
Description
[Technical field]
[0001] This patent application relates to thermoplastic polymer powders for additive manufacturing of high resolution, low roughness parts. [Background technology]
[0002] 3D printing by selective melting of thermoplastic polymer powders (SLS, MJF, HSS, etc.) allows the creation of parts with complex geometries. However, the resolution of parts printed in this way as well as their surface roughness are still not entirely satisfactory.
[0003] Selective melting by physical and / or chemical treatments is known to improve the surface condition of the fabricated parts, but these treatments significantly increase the production time, thus increasing the cost of manufacturing the parts.
[0004] Several methods of processing polymer powders used in 3D printing have also been described. Thus, EP 1 742 986 B1 discloses that polyamide powders with melting enthalpy and melting temperature far away from the crystallization temperature can improve the resolution of parts made by selective melting.
[0005] EP 1 413 595 B1 describes a method for increasing at least one of two parameters of a polyamide: (i) the melting point and (ii) the enthalpy of fusion ΔHf, by contacting the polyamide in the solid state with water or water vapor at a temperature close to the crystallization temperature Tc for a time sufficient to effect said increase, then separating the water (or water vapor) from the polyamide and drying the polyamide.
[0006] Furthermore, EP 2115043 B1 and EP 2627687 B1 disclose that heat treatment of PAEK (polyaryletherketone) powders can improve the resolution of the produced parts.
[0007] However, these methods are specific to particular polymers and are not always completely satisfactory. Summary of the Invention
[0008] It is therefore an object of the present invention to provide a polymer powder that allows improving the resolution and surface appearance of parts produced by selective melting.
[0009] Indeed, the invention is based on the finding that powders with the right morphology and appropriate grain size improve part resolution and reduce the surface roughness of articles produced by 3D printing methods through selective melting.
[0010] In particular, it has been determined that powders with low fines and narrow particle size distribution allow for optimized fusion of targeted particles in that they reduce the risk of fusion of neighboring particles, thus improving the resolution of the produced parts. Furthermore, the low concentration of large particles limits surface texturing and, therefore, the loss of resolution and surface roughness that this may cause.
[0011] It was also found that the resolution of the parts can be optimized by using powders with a ratio of the apparent density of the material corresponding to 0.40 to 0.55. The apparent density of the powder depends in particular on the powder morphology, but also on the crystallinity. Moreover, such powders make it possible to avoid structural defects of the parts, especially of round or tilted parts, while maintaining good productivity.
[0012] Thus, according to a first aspect, the present invention is directed to a composition of a thermoplastic polymer powder suitable for additive manufacturing by selective melting, said polymer powder comprising: - has a grain size characterized by: 〇Volume mean diameter Dv<55μm, and ○Span is less than 1.2, -d ratio is 0.40 to 0.55, and this d ratio is expressed by the following formula: [Number 1] TIFF2024540414000002.tif13170, where d p is the apparent density of the powder measured according to the ISO 787-11:1981 standard, d m is the density of the material measured on the powder after melting according to the ISO 1183-1 standard.
[0013] According to one embodiment, the thermoplastic polymer comprises or consists of a thermoplastic polymer selected from the group consisting of polyesters, polyvinyl chloride, polyacetals, polyolefins such as polypropylene and polyethylene, polystyrene, polycarbonate, poly-(N-methylmethacrylate, PMMI), polymethylmethacrylate (PMMA), thermoplastic elastomers such as ionomers, polyamides, polyether block amides, PAEKs, and mixtures thereof, and in particular semi-aromatic polyamides such as PA11, PA12, PA11 / 10T, PEBA or PAEKs such as PEKK, PEEK, PEEK-PEDEK and PEEK-PEmEK.
[0014] According to one embodiment, the composition further comprises a flow aid.
[0015] Advantageously, the polymer powder has a span of less than 1.00, preferably less than 0.90.
[0016] Preferably, the polymer powder has a d ratio of 0.45 to 0.55, in particular 0.47 to 0.51.
[0017] Advantageously, the polymer powder also has an intrinsic viscosity ranging from 0.65 to 1.50, preferably from 0.85 to 1.40 and even better from 1.00 to 1.30.
[0018] According to a second aspect, the present invention is directed to a method for producing the powder composition as defined above, the method comprising the steps of: (i) a prepolymerization step of one or more monomers of a thermoplastic polymer followed by a granulation step; (ii) grinding to a powder; (iii) if necessary, thereafter sieving the resulting prepolymer powder; and (iv) A step of subjecting the obtained prepolymer powder to solid-phase polycondensation to obtain a polymer powder. Includes.
[0019] According to a third aspect, the present invention is directed to the use of a composition described or obtained according to the method described above for producing an article by additive manufacturing by selective melting, in particular selected among SLS, MJF and HSS.
[0020] Finally, according to a fourth aspect, the invention is directed to an article obtained by additive manufacturing by selective melting of the composition described or of a composition obtained according to the method described.
[0021] The present invention will be better understood with reference to the following description and drawings. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 shows a 3D printing apparatus with SLS-type sintering (acronym for the English "Selective Laser Sintering"). [Diagram 2] This graph shows the calculated change in thickness e of the powder deposited after irradiation melting as a function of the number of layers n, each of which is 100 μm when produced by laser sintering, for powders with d ratios of 0.3 (●), 0.5 (■), and 0.7 (◆). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Definition of Terms The term "thermoplastic polymer" is understood to denote a polymer having the property of softening when sufficiently heated and becoming hard again when cooled, said polymer having a molar mass, as measured by CES (size exclusion chromatography), of more than 5000 g / mol.
[0024] The term "volume mean diameter" or "Dv" also means the mean diameter by volume of a powder material, measured, for example, with a Coulter Counter-Multisizer 3 (Beckman Coulter) particle counter according to the ISO 13319-1:2021 standard. Various diameters are distinguished. More specifically, Dv50 denotes the median diameter by volume, while Dv10 and Dv90 denote the diameters below which 10% or 90% by volume of the particles lie, respectively.
[0025] The term "span" refers to a ratio that represents the width of the particle size distribution of a powder, [Number 2] TIFF2024540414000003.tif13170 where: Dv10 is the diameter below which 10% by volume of the particles of the polymer powder lie; Dv50 is the diameter below which 50% by volume of the particles of the polymer powder lie (by definition, Dv50 is also the median diameter), and Dv90 indicates the diameter below which 90% by volume of the particles of the polymer powder lie. These diameters are measured as described above.
[0026] Furthermore, the term "3D printing by sintering" refers to a method in which a layer of polymer powder is irradiated with electromagnetic radiation (e.g. laser beam, infrared radiation, UV radiation) to selectively melt the powder particles affected by the radiation. The molten particles coalesce and solidify to form a solid mass. In this way, 3D articles can be produced by repeatedly irradiating successive newly applied layers of powder.
[0027] The term "surface roughness" is understood to denote the arithmetic mean deviation Ra of the surface profile of a sample according to the ISO 4287:1997 standard, for example with a PERTHOMETER S8P device. In the case of 3D printing, the build orientation can have an influence on the roughness, so it may be useful to distinguish between a top and a bottom of the article, the bottom corresponding to the first build layer and the top corresponding to the last build layer.
[0028] The term "viscosity" refers to the intrinsic viscosity measured with an Ubbelohde viscometer according to the ISO 307:2019 standard, except for the use of m-cresol as the solvent at a temperature of 20 °C. The dimension of intrinsic viscosity is the reciprocal of concentration and is equal to the natural logarithm of the relative viscosity divided by the concentration of the polymer dissolved in the solvent.
[0029] The nomenclature used to describe polyamides follows the ISO 1874-1 standard. In particular, in the PA (polyamide) X designation, X represents the number of carbon atoms in the polyamide unit resulting from the condensation of amino acids or lactams. In the PA XY designation, which describes polyamides resulting from the condensation of diamines with dicarboxylic acids or difunctional acid derivatives, X represents the number of carbon atoms in the diamine and Y represents the number of carbon atoms in the dicarboxylic acid or acid derivative. Designations such as PA X / Y, PA X / Y / Z refer to copolyamides, where X, Y, Z, etc. represent homopolyamide units as described above.
[0030] In a broad sense, the present invention proposes a suitable thermoplastic polymer powder composition for additive manufacturing by selective melting, the polymer powder being characterized by a specific particle size distribution with a mean diameter Dv<55 μm, a span of less than 1.2 and a d ratio between the density of the powder and the density of the material of 0.40-0.55.
[0031] The use of powders with a low d ratio often impairs the properties of the built article, especially in terms of mechanical strength. Moreover, such powders are difficult to deform due to the powder behavior of the particles. Furthermore, such powder beds cannot support the weight of the article being built. The article would then collapse during printing and would not be able to be completed. Better mechanical properties can be achieved by using powders with a high d ratio. However, such powders contain large grain particles and the built articles often show a large roughness. The d ratio defined above therefore turns out to constitute a good compromise between the two requirements of roughness and mechanical properties.
[0032] Moreover, it was found that powders with such d-ratios are able to more quickly absorb differences in the powder layer thickness at the start of the build, which are related to the powder shrinkage at the sintering position. Such thickness differences can cause various constraints on the part and can also affect the part quality if the laser power is not sufficient to melt the polymer and ensure complete coalescence. These defects can result in porosity that risks degrading the mechanical properties.
[0033] Furthermore, it was confirmed that the surface roughness Ra of the 3D structured built article, while directly related to the granularity characteristics of the powder used, in particular the mean diameter Dv, is likewise dependent on the span of the build layer, its thickness ep and the ratio d of the powder density to the material density. For several polyamides, the following correlations were found: [Number 3] TIFF2024540414000004.tif13170
[0034] The effect of d-ratio on roughness was particularly unexpected.
[0035] Overall, the thermoplastic polymer powder composition according to the invention allows parts to be obtained with low roughness and, moreover, makes it possible to avoid structural defects, especially for round or inclined parts, while maintaining good productivity.
[0036] A. Thermoplastic Polymer Powder Composition The thermoplastic polymer powder composition proposed by the present invention comprises - Grain size characterized by: 〇Volume mean diameter Dv<55μm, and ○The span is less than 1.20, and -d ratio is 0.40 to 0.55, and this d ratio is expressed by the following formula: [Number 4] TIFF2024540414000005.tif13170, where d p is the apparent density of the powder measured according to the ISO 787-11:1981 standard, d m is the material density measured on the powder after melting by vertical thrust in water (21°C) according to the ISO1183-1 standard.
[0037] According to the invention, the thermoplastic polymer powder has a specific particle size.
[0038] In fact, the thermoplastic polymer powder of the invention has a volume mean diameter Dv of less than 55 μm. According to a particular embodiment, the thermoplastic polymer powder has a volume mean diameter Dv of 30 to 55 μm, in particular 35 to 50 μm, in particular 40 to 45 μm.
[0039] In addition to the average diameter, the particle size distribution of thermoplastic polymer powders can have a significant impact on the performance of 3D printing by sintering.
[0040] Thus, according to the invention, the thermoplastic polymer powder has a span as defined above of less than 1.2, in particular less than 1, in particular less than 0.9. According to one embodiment, the span of the thermoplastic polymer powder is between 0.20 and 1.20, or between 0.30 and 1.10, or between 0.35 and 1.00, or between 0.40 and 0.90.
[0041] According to one embodiment, it is preferred that the powder has a volume diameter Dv10 of more than 15 μm.According to a particular embodiment, the thermoplastic polymer powder has a volume diameter Dv10 of 15 to 50 μm, or 25 to 45 μm, or 30 to 40 μm.
[0042] According to one embodiment, the powder preferably has a volume diameter Dv50 of 30 to 60 μm. According to a particular embodiment, the thermoplastic polymer powder has a volume diameter Dv50 of 35 to 55 μm, or 40 to 50 μm.
[0043] According to one embodiment, the thermoplastic polymer powder has a volume diameter Dv90 of less than 120 μm, in particular less than 100 μm, in particular 90 μm. According to a particular embodiment, the thermoplastic polymer powder has a volume diameter Dv90 of 40 to 120 μm, or 45 to 100 μm, or 50 to 80 μm.
[0044] The thermoplastic polymer powder in the composition according to the invention is also characterized by a specific d ratio between 0.40 and 0.55. The d ratio is expressed by the following formula: [Number 5] TIFF2024540414000006.tif13170
[0045] As mentioned before, the d-ratios specified represent a compromise proposed by the present invention between the pursuit of maximum powder density, and therefore a high d-ratio, on the one hand, and the fact that such powders produce articles with high roughness, which require more layers to absorb the thickness difference resulting from density differences at the start of the build (8-10 layers in the built article, i.e. approximately 1 mm, see FIG. 2). It was therefore found that a d-ratio between 0.40 and 0.55 best reconciles the advantages of obtaining a high density powder for good mechanical properties of the printed article, and a less dense powder to limit constraints and defects at the start of the build.
[0046] Apparent density d of thermoplastic polymer powder pIn addition to the particle size, it depends in particular on the shape, porosity and crystal structure of the particles. The thermoplastic polymer powder has an apparent density d p It is preferred that the compound has the formula:
[0047] Density d of thermoplastic polymer m depends on the polymer under consideration and is generally between 0.850 and 1.850, preferably between 0.900 and 1.450, and very preferably between 0.950 and 1.150.
[0048] Thermoplastic polymers that can be used within the scope of the present invention can be chosen in particular from among polyesters, polyvinyl chloride, polyacetals, polyolefins such as polypropylene and polyethylene, polystyrene, polycarbonates, thermoplastic elastomers such as poly-(N-methylmethacrylate, PMMI), polymethylmethacrylate (PMMA), ionomers, polyamides, polyether block amides (PEBA), PAEKs, and copolymers and mixtures thereof.
[0049] Among the polyamides, particular mention may be made of aliphatic polyamides such as PA6, PA6.6, PA11 and PA12, and their copolymers, and also semi-aromatic polyamides, for example PA11 / 10T.
[0050] Among the PAEK polymers, mention may in particular be made of polyetherketoneketone (PEKK), polyetheretherketone (PEEK) and their copolymers, such as polyetheretherketone-polyetherdiphenyletherketone (PEEK-PEDEK) and polyetheretherketone-polyethermetaetherketone (PEEK-PEmEK).
[0051] According to one embodiment, the polymer comprises or consists of a polyamide, in particular a semi-aromatic polyamide such as PA11, PA12, PEBA or PA11 / 10T, or a PAEK such as PEKK, and mixtures or copolymers thereof.
[0052] The thermoplastic polymer powder generally comprises at least 50% by weight of thermoplastic polymer, based on the total weight of the powder.
[0053] According to certain embodiments, the powder comprises at least 50% by weight, or at least 75% by weight, or at least 80% by weight, or at least 85% by weight, or at least 90% by weight, or at least 92.5% by weight, or at least 95% by weight, or at least 97.5% by weight, or at least 98% by weight, or at least 98.5% by weight, or at least 99% by weight, or at least 99.5% by weight of thermoplastic polymer, based on the total weight of the powdered thermoplastic polymer powder of the invention.
[0054] According to certain embodiments, the thermoplastic polymer powder may comprise only a single thermoplastic polymer, for example polyester, polyolefin, polyamide, polyester, PEBA or PAEK. According to certain embodiments, the powder according to the invention comprises a plurality of polymers differing in at least one property. These properties can be in particular molar mass, crystallinity, but also thermal properties or particle size.
[0055] According to a particular embodiment, the thermoplastic polymer powder has a viscosity of 0.65 to 1.50, preferably 0.85 to 1.40, and even more preferably 1.00 to 1.30. These viscosity ranges are particularly advantageous, as they provide a good compromise between good cohesive properties during sintering (sufficiently low viscosity) and good mechanical properties of the sintered body (sufficiently high viscosity).
[0056] Furthermore, the thermoplastic polymer powder may contain, in addition to one or more thermoplastic polymers, one or more conventional additives and fillers.
[0057] The additives generally represent less than 5% by weight based on the total weight of the composition. Preferably, the additives represent less than 1% by weight of the total powder weight. The additives can include flow aids, stabilizers (light, especially UV and heat), optical brighteners, dyes, pigments, energy absorber additives (including UV absorbers).
[0058] Among the flow aids, mention may be made, for example, of hydrophilic or hydrophobic silica. Advantageously, the flow aid represents between 0.01 and 0.4% by weight relative to the total weight of the composition. In another embodiment, the powder composition does not contain a flow aid.
[0059] The thermoplastic polymer powder may also contain one or more fillers, generally representing less than 50% by weight, preferably less than 40% by weight, relative to the total weight of the final powder. Among the fillers, mention may be made of reinforcing fillers, in particular mineral fillers such as carbon black, talc, carbon or other nanotubes, and fibres, in particular glass fibres or carbon fibres (crushed or not crushed), or also glass (hollow or not hollow) in another form, for example flakes or spheres.
[0060] B. Method for producing thermoplastic polymer powder The thermoplastic polymer powder is obtained in particular by comminuting the thermoplastic polymer in the form of extruded granules or flakes, according to conventional techniques.
[0061] Grinding can be carried out using equipment known for this purpose, for example a mill with counter-rotating pins (pin mill), a mill with hammers (hammer mill) or a whirl mill.
[0062] If the powder contains multiple polymers and / or specific additives and / or specific reinforcing fillers, some or all of them can be incorporated by mixing in the molten state, for example by extrusion (compounding) and granulation followed by grinding of the granules. Alternatively, other polymers and / or specific additives and / or specific reinforcing fillers can be added by dry blending ("dry blend"). Preferably, flow aids are added by dry blending.
[0063] According to one embodiment, particularly for polyamides, the method for producing the powder composition comprises the following steps: (i) a prepolymerization step of one or more monomers of a thermoplastic polymer followed by a granulation step; (ii) grinding to a powder; (iii) if necessary, thereafter sieving the resulting prepolymer powder; (iv) A step of subjecting the obtained prepolymer powder to solid-phase polycondensation to obtain a polymer powder. Includes.
[0064] Additives and / or reinforcing fillers may then be added to the prepolymer by melt mixing (compounding) or dry mixing between steps (i) and (ii) or by dry mixing thereafter.
[0065] C. Use of Powder The above-mentioned polymer powder compositions are particularly useful for application in 3D printing processes by sintering. Preferably, the compositions of the invention are used in selective laser sintering (SLS, in English Selective Laser Sintering) processes, sintering processes of the MJF (Multi Jet Fusion) type or sintering processes of the HSS (High Speed Sintering) type.
[0066] The SLS method is widely known: in this connection reference may be made in particular to US Pat. No. 6,136,948 and WO 96 / 06881.
[0067] In this type of method, a thin layer of powder is deposited on a horizontal plate held in an enclosure heated to a temperature called the build temperature. In most cases, heating to the build temperature is carried out using IR radiation lamps, for example halogen lamps, with a maximum emission of wavelengths generally between 750 nm and 1250 nm. The build temperature refers to the temperature to which the powder bed of the constituent layers of the three-dimensional article being built is heated during the layer-by-layer sintering process of the powder. Subsequently, electromagnetic radiation, for example in the form of a laser, supplies the energy necessary to sinter the powder particles at various points of the powder layer according to the shape corresponding to the object, for example using a computer that stores the shape of the object, restoring this shape in slices. The horizontal plate is then lowered by a height corresponding to the thickness of one layer of powder, and a new layer of powder is spread, heated and sintered in the same way. This procedure is repeated until the object is manufactured.
[0068] The layer of powder deposited on the horizontal plate may have a thickness before sintering of, for example, 20-200 μm, preferably 50-150 μm. After sintering, the layer of agglomerated material may have a slightly smaller thickness, for example, 10-150 μm, preferably 30-100 μm.
[0069] In MJF and HSS methods, an entire layer of build material is exposed to radiation, but only the portions covered by the flux melt into one layer of the 3D part. The flux is a compound that can absorb radiation and convert it to thermal energy, for example black ink. It is selectively applied to selected areas of the build material. The flux is able to penetrate the layer of build material and transfer the absorbed energy to adjacent build material, thereby melting or sintering the build material. By melting, bonding, and then hardening each layer of build material, the object is formed.
[0070] In the specific case of MJF, refinement is also added to the edges of the melted area to allow for greater resolution of the part.
[0071] Advantageously, the use of the polymer powder composition of the present invention in these processes does not require any special modifications and, as mentioned above, results in parts with less roughness and higher resolution.
[0072] The polymer powder composition according to the invention is recyclable and reusable in multiple successive structures, either alone or mixed with other recycled or non-recycled powders.
[0073] Below, by way of example, the use of the above described thermoplastic polymer powder composition in a method for building up three-dimensional objects layer-by-layer by sintering induced by electromagnetic radiation in an apparatus 1 shown diagrammatically in FIG. 1 is described.
[0074] The electromagnetic radiation may for example be infrared, ultraviolet or preferably laser radiation. In particular, in the device 1 shown diagrammatically in Figure 1, the electromagnetic radiation may comprise a combination of infrared radiation 100 and laser radiation 200.
[0075] The sintering process is a layer-by-layer manufacturing method for building a three-dimensional object 80 .
[0076] The apparatus 1 comprises a sintering housing 10 in which is placed a feed tray 40 containing thermoplastic polymer powder and a movable horizontal plate 30. The horizontal plate 30 may also serve to support the three-dimensional object 80 being built. However, objects made from thermoplastic polymer powders generally do not require additional support and can usually be self-supported by the unsintered powder of the previous layer.
[0077] According to this method, thermoplastic polymer powder is removed from a supply tray 40 and deposited onto a horizontal plate 30 to form a thin layer 50 of powder that comprises the three-dimensional object 80 being built. The powder layer 50 is heated by infrared radiation 100 to reach a substantially uniform temperature equal to a predetermined minimum build temperature Tc.
[0078] The energy required to sinter the thermoplastic polymer powder particles at various points of the powder layer 50 is then provided by laser radiation 200 from a laser 20 moving in a plane (xy) following a shape corresponding to the shape of the object. The melted powder resolidifies to form a sintered part 55, while the remaining part of the layer 50 remains in the form of unsintered powder 56. One pass of a single laser radiation 200 is generally sufficient to ensure sintering of the powder. However, in certain embodiments, multiple passes over the same location and / or multiple electromagnetic radiation reaching the same location may be considered to ensure sintering of the powder.
[0079] The horizontal plate 30 is then lowered along axis (z) a distance corresponding to the thickness of the powder layer, and a new layer is deposited. The laser 20 provides the energy necessary to sinter the powder particles along a shape corresponding to this new slice of the object, and so on. This procedure is repeated until the object 80 is produced.
[0080] The temperature in the multi-layer sintering housing 10 beneath the layer being built may be lower than the build temperature. However, this temperature generally remains above or even much higher than the glass transition temperature of the powder. It is particularly advantageous to maintain the temperature of the bottom of the housing at a temperature Tb, called the "tray bottom temperature", so that Tb is less than 40°C, preferably less than 25°C, and even more preferably less than 10°C, lower than Tc.
[0081] Once the object 80 is completed, it is removed from the horizontal plate 30 and the green powder 56 can be sieved and then at least partially returned to the feed tray 40 for use as recycled powder.
[0082] D. Parts that can be manufactured The use of the composition according to the invention therefore allows the production of high quality three-dimensional articles with a very satisfactory surface appearance, in particular low roughness and precise and well-defined dimensions and contours.
[0083] The thermoplastic polymer powder composition allows for the production of parts by 3D printing with sintering, with the resulting parts having at least similar properties, if not superior properties, especially mechanical properties, compared to conventional thermoplastic polymer powders.
[0084] The following examples further illustrate the invention. EXAMPLES
[0085] Example 1 Polyamide powder composition 11 was prepared according to the following method.
[0086] First, polyamide 11 (prepolymer) was synthesized from 1.2 kg of 11-aminoundecanoic acid in the presence of 0.5 kg of water, 5 g of hypophosphorous acid (50% strength, expressed as % by weight in the aqueous solution) and 9.8 g of phosphoric acid (75% strength, expressed as % by weight in the aqueous solution). As soon as the temperature reached 160 °C or the pressure exceeded 8.5 bar, the mixture was heated to a temperature of 190 °C for 2 hours with stirring. The water in which 11-aminoundecanoic acid was initially contained during the synthesis was removed by evaporation at constant pressure (P = 10 bar). After removing an amount of water of 430 g, the prepolymer was extracted from the pressurized reactor through a die. It was then cooled using two steel rollers with circulating cold water, solidified cooled and crushed into flakes.
[0087] The prepolymer thus obtained was mixed with 3.3 g of carbon black in a suitable container. The mixture was introduced into a twin-screw extruder, melt-mixed thoroughly, and then extruded. The mixture was then cooled using two steel rollers while circulating cold water, solidified, cooled, and crushed into flakes.
[0088] The lamination prepolymer recovered in the form of flakes was then ground in a hammer mill equipped with an internal selector until a powder with a volume median diameter Dv50 of 64 μm was obtained. The powder thus obtained was then subjected to solid-state polycondensation in a dryer under vacuum at 140-155°C to increase the intrinsic viscosity of the polyamide to 1.15.
[0089] The resulting coloured polyamide powder 11 was then sieved through an ultrasonically blocked vibrating sieve RUSSEL type FINEX 22 using an 80 μm square screen.
[0090] The resulting powder compositions were then characterized for particle size and density as shown below, and the results are summarized in Tables 1 and 2 below.
[0091] Powder characterization particle size The powder particle size was characterized by measuring the particle size distribution with a Coulter Counter-Multisizer 3 (Beckman Coulter) instrument applying the ISO13319-1:2021 standard. From the particle size distribution, the mean diameter and the diameters corresponding to the 1st, 5th and 9th deciles of the particle size distribution were determined, after which the span was calculated according to the following formula: [Number 6] TIFF2024540414000007.tif10170
[0092] ratio d Apparent density of powder d p was measured applying the ISO787-11:1981 standard using a 250 mL precision glass test tube with 2-2 mL graduations and at least 50 mL of ungraded top. The powder was slowly introduced into the test tube tilted at 45°. The volume of powder was 220-250 mL. This volume of powder was then weighed to calculate the bulk density and divided by the bulk density of water to estimate the density.
[0093] Density of the material d m was measured after the powder was melted in a hot press (T>Tf+40°C, 2 ton pressure). The density of the resulting film and thus the material density was measured by vertical thrust in water (21°C) according to the ISO1183-1 standard using a Sartorius AC 210P hydrostatic balance with density kit YDK01.
[0094] Apparent density of powder dp and the density of the material measured in powder form after melting, d m The ratio d of [Number 7] TIFF2024540414000008.tif13170[Table 1] TIFF2024540414000009.tif63170[Table 2] TIFF2024540414000010.tif68170
[0095] The obtained polymer powder was then used to produce test specimens 1BA XY (1BA test specimens according to the ISO 527-1BA standard, called “XY” because they are printed on the horizontal plane of the printer) by sintering, specifically 3D printing by SLS, by laser sintering on a P100 machine (sold by the company EOS) using the following set of parameters while adjusting the powder layer thickness to 100 μm: [Table 3] TIFF2024540414000011.tif50170
[0096] The specimens were visually evaluated in terms of printing resolution, and the results are summarized in Table 2 above.
[0097] Furthermore, the specimens were characterized by the roughness of the upper and lower surfaces using the arithmetic mean deviation Ra of the surface profile of the samples according to the ISO4287:1997 standard using a PERTHOMETER S8P instrument (the result corresponds to the average value of three values obtained at three different base lengths).
[0098] The specimens were then mechanically polished using a polisher equipped with 320 grit emery cloth, after which the surface roughness measurements of these specimens were repeated under the same conditions as above. The results are summarized in Table 2 below.
[0099] Example 2 The powdered PA11 prepared in Example C2 was sieved through an ultrasonically blocked vibrating sieve RUSSEL type FINEX 22 using a 80 μm square screen.
[0100] The particle size characteristics of the resulting polyamide 11 powder were measured as described in Example 1. The results are summarized above in Table 1. In addition, the density of the material was measured as described in Example 1 (see Table 2 above).
[0101] The resulting powder was used to prepare test specimens as shown in Example 1. These specimens were then characterized by their top and bottom surface roughness, and the results are summarized in Table 2 above.
[0102] Example 3 First, polyamide 12 (prepolymer) was synthesized from 1 kg of lauryllactam in the presence of 0.1 kg of water. As soon as the temperature reached 160 °C or the pressure exceeded 8.5 bar, the mixture was heated with stirring for 4 hours to a temperature of 260 °C. The water with which the lauryllactam was initially contained during the synthesis was removed by evaporation at constant pressure (P = 20 bar). After removing an amount of water of 30 g, the prepolymer was extracted from the pressurized reactor through a die. It was then cooled using two steel rollers with circulating cold water, solidified, cooled and crushed into flakes.
[0103] The prepolymer recovered in the form of flakes was then ground in a hammer mill equipped with an internal selector, using a second dynamic selector at the output to remove the finest particles, until a powder with a volume median diameter Dv50 of 82 μm was obtained. The powder thus obtained was then subjected to solid-state polycondensation in a dryer under vacuum at 140-155 °C to increase the intrinsic viscosity of the polyamide to 1.10.
[0104] The powder thus obtained was sieved through an ultrasonically blocked vibrating sieve RUSSEL type FINEX 22 using a 80 μm square screen.
[0105] The particle size characteristics of the resulting polyamide 12 powder were measured as described in Example 1. The results are summarized above in Table 1. In addition, the density of the material was measured as described in Example 1 (see Table 2 above).
[0106] The resulting powder was used to prepare test specimens as described in Example 1 using the following set of parameters: [Table 4] TIFF2024540414000012.tif50170
[0107] These specimens were then characterized by their top and bottom surface roughness, and the results are summarized in Table 2 above.
[0108] Example C1 Polyamide powder composition 11 was prepared according to the following method.
[0109] First, a low-viscosity polymer 11 (hereinafter referred to as "prepolymer") was synthesized from 1.2 kg of 11-aminoundecanoic acid in the presence of 0.5 kg of water, 5 g of hypophosphorous acid (50% titer) and 9.8 g of phosphoric acid (75% titer). As soon as the temperature reaches 160 ° C or the pressure exceeds 8.5 bar, the mixture is heated to a temperature of 190 ° C for 2 hours with stirring. The water, which initially contained 11-aminoundecanoic acid during the synthesis, is removed by evaporation at constant pressure (P = 10 bar). After removing an amount of water of 430 g, the prepolymer was extracted from the pressurized reactor through a die. It is then cooled using two steel rollers with circulating cold water, solidified, cooled and crushed into flakes.
[0110] The prepolymer recovered in the form of flakes was then ground in a hammer mill equipped with an internal selector until a powder with a volume median diameter Dv50 of 74 μm was obtained. The powder thus obtained was then subjected to solid-state polycondensation in a dryer under vacuum at 140-155 ° C to increase the viscosity of the polyamide to 1.18.
[0111] The resulting powder was used to prepare test specimens as shown in Example 1. These specimens were then characterized by their top and bottom surface roughness, and the results are summarized in Table 2 above.
[0112] Example C2 The prepolymer PA11 recovered in the form of flakes in Example C1 was ground with the same grinding parameters as in C1, using a second dynamic selector at the output to remove the finest particles, until a powder with a volume median diameter Dv50 of 91 μm was obtained. The powder thus obtained was then subjected to solid-state polycondensation in a dryer under vacuum at 140-155 ° C, increasing the viscosity of the polyamide to 1.16. Powder PA11 was obtained with the particle size characteristics shown in Table 1 above.
[0113] The resulting powder was used to prepare test specimens as shown in Example 1. These specimens were then characterized by their top and bottom surface roughness, and the results are summarized in Table 2 above.
[0114] Example C3 The powder PA11 prepared in Example C1 was sieved on an ultrasonically blocked vibrating sieve RUSSEL type FINEX 22 using a 80 μm square screen. Powder PA11 was obtained having the particle size characteristics shown in Table 1 above.
[0115] The resulting powder was used to prepare test specimens as shown in Example 1. These specimens were then characterized by their top and bottom surface roughness, and the results are summarized in Table 2 above.
[0116] Example C4 Granules of polyamide 12 (Rilsamid® AECNO TL sold by Arkema) were extruded using a die obtaining fibers with a diameter of 60 μm, which were cooled and could be atomized over a length of 70 μm. The intrinsic viscosity of the polyamide powder thus obtained was 1.09.
[0117] The particle size characteristics of the resulting polyamide 12 powder were measured as described in Example 1. The results are summarized above in Table 1. In addition, the density of the material was measured as described in Example 1 (see Table 2 above).
[0118] The resulting powder was used to produce test specimens as shown in Example 3. These specimens were then characterized by their top and bottom surface roughness, with the results summarized in Table 2 above.
[0119] Example C5 According to Example 1 of Chinese Patent No. 104356643B, polyamide 12.12 powder was obtained. First, dodecanedioic acid was solubilized in ethanol at 60°C, and an ethanol solution of dodecanediamine was gradually introduced while monitoring the pH. When pH=7, the solution contained a stoichiometric amount of nylon 12.12 salt, which precipitated. After filtering and drying, the salt was collected, put into an autoclave, and polymerized at a temperature of 250°C to obtain PA12.12 with an intrinsic viscosity of 1.15. It was then extracted from the reactor through a die, cooled, and granulated. These granules were then dissolved in ethanol at a temperature of 140°C and a pressure of 8 bar, and directly precipitated in the form of a powder by cooling. The powder was collected after dehydration and drying. The intrinsic viscosity of the polyamide powder thus obtained was 1.12.
[0120] The particle size characteristics of the resulting polyamide 12.12 powder were measured as described in Example 1. The results are summarized above in Table 1. In addition, the density of the material was measured as described in Example 1 (see Table 2 above).
[0121] The resulting powder was used to produce test specimens as shown in Example 3. These specimens were then characterized by their top and bottom surface roughness, with the results summarized in Table 2 above.
[0122] Example 4 Powder PA12.12 prepared according to Example C5 (Example 1 of China Patent No. 104356643B) was sieved through an ultrasonically anti-clogging vibrating sieve RUSSEL type FINEX 22 using an 80 μm square screen and then defined.
[0123] The particle size characteristics of the resulting polyamide 12.12 powder were measured as described in Example 1. The results are summarized above in Table 1. In addition, the density of the material was measured as described in Example 1 (see Table 2 above).
[0124] The resulting powder was used to produce test specimens as shown in Example 3. These specimens were then characterized by their top and bottom surface roughness, with the results summarized in Table 2 above.
[0125] All the results make it clear that the powder with the claimed particle size allows a very clear improvement in the roughness of the parts obtained by 3D printing from this powder. In this context, not only the mean diameter but also the span, which indicates the width of the particle size distribution, is important. Thus, the roughness obtained with the powders of examples 1 to 3 is significantly lower than that obtained with the powder of example C3, which has similar mean diameters Dv10, Dv50 and Dv90 but a higher span.
[0126] The study also confirms that while high roughness is observed for the parts obtained from the powders of Examples C2 and C5, the span values of these powders are very low, indicating a favorable influence of the mean diameter value.
[0127] Furthermore, these examples reveal that the roughness is correlated with the investigated parameters according to the following equation: [Number 8] TIFF2024540414000013.tif13170
[0128] The powder composition according to the invention provides the best compromise.
[0129] List of cited references European Patent No. 1742986B1 European Patent No. 1413595B1 European Patent No. 2115043B1 European Patent No. 2627687B1 U.S. Patent No. 6,136,948 International Publication No. 96 / 06881 Brochure Chinese Patent No. 104356643B
Claims
1. A composition of thermoplastic polymer powder suitable for additive manufacturing by selective melting, the polymer powder comprising: A particle size characterized by: o a volume mean diameter Dv<55 μm, as measured, for example, by a Coulter Counter-Multisizer 3 (Beckman Coulter) particle counter, according to the ISO 13319-1:2021 standard, and a span of less than 1.20, the volume mean diameter used to calculate this span being measured in accordance with the ISO 13319-1:2021 standard, for example in a Coulter Counter - Multisizer 3 (Beckman Coulter) particle counter, The d ratio is 0.40 to 0.55, and the d ratio satisfies the following formula: [Equation 9] where d p is the apparent density of the powder measured according to the ISO 787-11:1981 standard, d m is the material density measured on the powder after melting according to the ISO 1183-1 standard; composition.
2. 2. The composition of claim 1, wherein the thermoplastic polymer comprises or consists of a thermoplastic polymer selected from the group consisting of polyesters, polyvinyl chloride, polyacetals, polyolefins such as polypropylene and polyethylene, polystyrene, polycarbonates, thermoplastic elastomers such as poly-(N-methylmethacrylate, PMMI), polymethylmethacrylate (PMMA), ionomers, polyamides, polyether block amides, PAEKs, and mixtures thereof.
3. 3. The composition of claim 2, wherein the thermoplastic polymer comprises or consists of semi-aromatic polyamides such as PA11, PA12, PA11 / 10T, PEBA or PAEKs such as PEKK, PEEK, PEEK-PEDEK and PEEK-PEmEK.
4. 4. The composition of claim 1 further comprising a flow aid.
5. 5. The composition of any one of claims 1 to 4, wherein the polymer powder has a span of less than 1.
00.
6. 6. The composition of claim 5, wherein the polymer powder has a span of less than 0.
90.
7. The composition according to any one of claims 1 to 6, wherein the polymer powder has a d ratio of 0.45 to 0.
55.
8. The composition of claim 7, wherein the polymer powder has a d ratio of 0.47 to 0.
51.
9. 9. The composition according to any one of claims 1 to 8, wherein the polymer powder has an intrinsic viscosity of 0.65 to 1.50, preferably 0.85 to 1.40, more preferably 1.00 to 1.30, when measured with an Ubbelohde viscometer according to the ISO 307:2019 standard, except when m-cresol is used as the solvent at a temperature of 20°C.
10. A method for producing a powder composition according to any one of claims 1 to 10, comprising the steps of: (i) a prepolymerization step of one or more monomers of a thermoplastic polymer followed by a granulation step; (ii) grinding to a powder; (iii) if necessary, thereafter sieving the resulting prepolymer powder; and (iv) A step of subjecting the obtained prepolymer powder to solid-phase polycondensation to obtain a polymer powder. A method comprising:
11. 11. Use of a composition according to any one of claims 1 to 9 or obtained by the method according to claim 10 for the manufacture of an article by additive manufacturing using selective melting.
12. 12. The use according to claim 11, wherein the additive manufacturing is selected from among selective laser sintering (SLS), multi-jet fusion (MJF) type sintering and high speed type sintering (HSS).
13. 11. An article obtained by additive manufacturing by selective melting of a composition according to any one of claims 1 to 9 or producible by the method according to claim 10.