CURABLE THERMALLY CONDUCTIVE COMPOSITION CONTAINING DIAMOND PARTICLES - Patent application

A curable thermally conductive composition with 30-55 wt% diamond particles and specific additives achieves both high thermal conductivity and extrusion rate, addressing the dual challenges of existing materials in small electronic devices.

JP2024540473AActive Publication Date: 2024-10-31DOW GLOBAL TECHNOLOGIES LLC +1

Patent Information

Application Number
JP2024529313
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-10-31
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing thermally conductive interface materials face challenges in achieving both high thermal conductivity and easy extrudability, particularly in small electronic devices, as increasing filler content for conductivity reduces extrusion rate.

Method used

A curable thermally conductive composition comprising 30-55 wt% diamond particles with Dv50 of 60-150 micrometers, combined with specific ratios of vinyl dimethyl terminated polydimethylsiloxanes, silylhydride-functional polysiloxane crosslinking agents, and other fillers, to maintain an extrusion rate above 60 g/min and thermal conductivity of 94-97 W/mK.

Benefits of technology

The composition achieves a balance of high thermal conductivity and extrusion rate, enabling efficient heat transfer in small electronic devices while maintaining material integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540473000001
    Figure 2024540473000001
  • Figure 2024540473000002
    Figure 2024540473000002
  • Figure 2024540473000003
    Figure 2024540473000003
Patent Text Reader

Abstract

The curable thermally conductive composition comprises: (a) one or more vinyl dimethyl terminated polydimethylsiloxanes; (b) a silylhydride functional polysiloxane having at least two silylhydride groups per molecule; (c) a filler treating agent; and (d) 94-97 wt. % of a thermally conductive filler comprising diamond particles having a Dv50 in the range of 60-150 micrometers.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable thermally conductive composition containing a thermally conductive filler comprising diamond particles having a Dv50 particle size in the range of 60 to 150 micrometers. [Background technology]

[0002] The trend of miniaturization and powering of electronic devices in industry has increased the demand for thermally conductive compositions useful for dissipating heat generated by such devices. For example, the telecommunications industry is undergoing a generational shift to 5G networks, which requires small highly integrated electrical devices and doubles the required power (from 600 watts to 1200 watts). If the heat generated by the high power in small devices is not efficiently dissipated, the devices will be damaged. Thermally conductive interface materials are often used in electronic devices to thermally couple heat-generating components with heat-dissipating components.

[0003] The challenge of a thermally conductive interface material is to provide a combination of both high thermal conductivity properties and being easily extrudable to allow for precise application of the thermally conductive material onto small components. Specifically, the thermally conductive interface material should have an extrusion rate of greater than 60 grams / minute and an extrusion rate of at least 8 watts / meter when measured using the Extrusion Rate Test defined herein below. * It is desirable to provide a thermally conductive interface material that cures to a material with a thermal conductivity of 1 Kelvin. Thermal conductivity can be increased by increasing the amount of thermally conductive filler, but this also reduces the extrusion rate of the composition. Thus, meeting these two performance parameters is particularly difficult. Summary of the Invention

[0004] The present invention is directed to a method for producing a gyro fiber having an extrusion rate of greater than 60 grams per minute (g / min) and an extrusion speed of at least 8 watts / meter when measured using the Extrusion Rate Test defined herein below. * Kelvin (W / m *To provide a thermally conductive interface material that cures to a material having a thermal conductivity of 0.1 K.

[0005] Surprisingly, it has been found that such compositions can be prepared from a curable polysiloxane composition containing 94 to 97 weight percent (wt%) of a thermally conductive filler including 30 to 55 weight percent (wt%) diamond particles having a Dv50 in the range of 60 to 150 micrometers, where wt% is based on the weight of the curable polysiloxane composition.

[0006] In a first aspect, the present invention provides a curable thermally conductive composition comprising: (a) a vinyl functional silicone polymer, the vinyl functional silicone polymer being one or a combination of vinyl dimethyl terminated polydimethylsiloxanes, having a viscosity of 30 to 2000 millipascals as measured by ASTM D445-21 using a glass capillary Cannon-Fenske viscometer at 25° C. and at a concentration ranging from 1 to 4.0 weight percent; *(b) at least one silylhydride functional polysiloxane crosslinker having at least two silylhydride groups per molecule and present at a concentration such that the molar ratio of silylhydride groups to vinyl groups in the composition is in the range of 0.5 to 1.0; (c) a filler treating agent at a concentration in the range of 0.1 to 2.0 weight percent, the filler treating agent comprising any one of a plurality of trialkoxysilyl compounds or any combination thereof; and (d) a thermally conductive filler at a concentration in the range of 94 to 97 weight percent, (ii) a thermally conductive filler having a Dv50 in the range of greater than 1 to 10 micrometers at a concentration in the range of 25 to 35 weight percent; (iii) a thermally conductive filler having a Dv50 in the range of 0.1 to 1 micrometers at a concentration in the range of 10 to 20 weight percent; and (iv) optionally a thermally conductive filler having a Dv50 in the range of 20 to 60 micrometers at a concentration in the range of 0 to 20 weight percent.

[0007] In a second aspect, the invention is a process for using the curable thermally conductive composition of the first aspect, comprising applying the curable thermally conductive composition between and in contact with two components and then heating the curable composition to cure it while in place between the components.

[0008] In a third aspect, the invention is an article comprising the curable thermally conductive composition of the first aspect between and in contact with two components of the article, the curable thermally conductive composition being either in a cured or uncured form.

[0009] The compositions of the invention are useful as thermally conductive interface materials for efficiently transferring heat between two components. The processes of the invention are useful for applying the compositions of the invention. The articles of the invention are useful as devices that benefit from efficient heat transfer between components. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Test methods refer to the test method most recent to the priority date of this document unless a date is given with the test method number. References to test methods contain both a reference to the testing institute and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International Methods, EN refers to European Norm, DIN refers to Deutsches Institut fur Normung, ISO refers to the International Organization for Standards, and UL refers to the Underwriters Laboratory.

[0011] Products identified by trade names refer to compositions available under those trade names as of the priority date of this document.

[0012] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges are inclusive of the endpoints unless otherwise indicated.

[0013] Particle size (used interchangeably as "average particle size" and "Dv50") is determined as the volume weighted median of the particle size distribution (Dv50) using a Malvern Instruments Mastersizer™ (a trademark of Malvern Instruments Limited) 3000 laser diffraction particle size analyzer.

[0014] Viscosity is measured using a glass capillary Cannon-Fenske viscometer at 25°C according to ASTM D445-21 unless otherwise stated.

[0015] The thermal conductivity of the cured composition samples is measured using a Hot Disk TPS 2500S instrument meeting ISO22007-2 on the cured samples. The sensor is a model 5465 (3.189 mm Kapton sensor). The cured samples for thermal conductivity evaluation are prepared by curing samples having dimensions of 25 mm x 25 mm square x 8 mm thick at 120 degrees Celsius (°C) for 60 minutes.

[0016] The following extrusion rate test using a Nordson EFD dispenser is used to measure the extrusion rate (ER) of the composition. The sample material is packaged in a 30 milliliter syringe with a 2.54 millimeter opening (EFD Syringe manufactured by Nordson Company). The sample is dispensed from the opening by applying 0.62 megapascals of pressure to the plunger of the syringe. The mass of the sample in grams that is expelled from the 2.54 millimeter opening in one minute is recorded to obtain the extrusion rate value in grams per minute (g / min).

[0017] In one aspect, the present invention is a curable thermally conductive composition. In that respect, the present invention is a "curable composition." The curable composition is capable of undergoing a crosslinking reaction ("cure reaction"). In this composition, the crosslinking reaction is a hydrosilylation reaction between a vinyl-functional silicone polymer component and a silyl-hydride (Si-H)-functional polysiloxane crosslinker.

[0018] Vinyl-functional silicone polymers have a resistance of 30 to 2000 millipascals. * seconds (mPa * The vinyl-functional silicone polymer may comprise or consist of one or any combination of vinyldimethyl-terminated polydimethylsiloxanes having a viscosity in the range of 30 mPa.s. If the vinyl-functional silicone polymer is a combination of vinyldimethyl-terminated polydimethylsiloxanes, the viscosity is that of the combination of vinyldimethyl-terminated polydimethylsiloxanes. The viscosity of the vinyl-functional silicone polymer may be in the range of 30 mPa.s. *s or more, 40 mPa * s or more, 50mPa * s or more, 60mPa * s or more, 70mPa * s or more, 75mPa * s or more, 78mPa * s or more, 80mPa * s or more, 100mPa * s or more, 125mPa * s or more, 150mPa * s or more, 175mPa * s or more, even 200mPa * s or more, and at the same time 2000 mPa * s or less, 1500mPa * s or less, 1000mPa * s or less, 500mPa * s or less, preferably 400mPa * s or less, 300mPa * s or less, 200mPa * s or less, 150mPa * s or less, 100mPa * s or less, 90mPa * s or less, or even 80mPa * s or less.

[0019] Each vinyldimethyl terminated polydimethylsiloxane can have the average chemical structure (I): Vi(CH3)2SiO-((CH3)2SiO) d -Si(CH3)2Vi (I) wherein the subscript d is the average number of ((CH3)2SiO) groups per molecule and has a value of 25 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, 100 or more, 120 or more, 140 or more, 160 or more, 180 or more, 200 or more, 220 or more, 240 or more, 260 or more, 280 or more, 300 or more, 320 or more, or even 340 or more, and at the same time 350 or less, 340 or less, 320 or less, 300 or less, 280 or less, 260 or less, 240 or less, 240 or less, 220 or less, 200 or less, 180 or less, 160 or less, 140 or less, 120 or less, 100 or less, 80 or less, 60 or less, or even 40 or less. For example, vinyl-functional silicone polymers may have a viscosity of 78 mPa, such as that sold by Gelest under the product name SMS-V21. * The polydimethylsiloxane may be a vinyl dimethyl terminated polydimethylsiloxane having a viscosity of 1.25 wt. s ​​and containing 1.25 weight percent (wt %) vinyl groups based on the molecular weight.

[0020] The concentration of the vinyl functional silicone polymer is 1 wt% or more, and can be 2.0 wt% or more, 2.5 wt% or more, 2.7 wt% or more, or even 3.0 wt% or more, relative to the weight of the curable thermally conductive composition, and at the same time can be 4.0 wt% or less, 3.5 wt% or less, or even 3.3 wt% or less.

[0021] The curable thermally conductive composition further comprises at least one silylhydride (SiH)-functional polysiloxane crosslinker. The SiH-functional crosslinker contains at least two SiH groups per molecule. The SiH groups can be pendant, terminal, or a combination of both pendant and terminal. A "terminal" group is on a terminal siloxane group of the molecule. A "terminal" siloxane group is bonded to only one other siloxane group. A "pendant" group is on an internal siloxane group of the molecule (a siloxane group bonded to at least two other siloxane groups). A "siloxane group" is a group that contains SiO that is bonded to another Si through an oxygen of the SiO.

[0022] The SiH functional polysiloxane crosslinker can have the average chemical structure (II): R (3-h) H h SiO-(HRSiO) a -(R2SiO) b -SiH h’ R (3-h’) (II) During the ceremony, R is independently selected from alkyl and aryl groups having 1 to 6 carbon atoms in each occurrence. The R group can have 1 or more carbons, 2 or more carbons, 3 or more carbons, 4 or more carbons, or even 5 or more carbons, while having 6 or less carbons, 5 or less carbons, 4 or less carbons, 3 or less carbons, or even 2 or less carbons. Desirably, the R group is independently selected in each occurrence from methyl and phenyl groups.

[0023] H is a hydrogen atom.

[0024] The subscripts h and h' refer to the average number of terminal hydrogen atoms at either end, each independently selected from a value ranging from 0 to 3 in each instance, with the proviso that the combination of a, h, and h' is at least 2. Preferably, h and h' are independently in each instance 0 or more, 1 or more, or even 2 or more, and simultaneously 3 or less, 2 or less, or even 1 or less. More preferably, h and h' have the same value. Most preferably, h and h' are both 0.

[0025] The subscript a is the average number of (HRSiO) groups per molecule. If h and h' are both 0, then a is 2 or more. If h and h' are not both 0, then subscript a can be 0, provided that the combination of a, h, and h' is 2 or more. Preferably, subscript a is 1 or more, and may be 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, or even 9 or more, while typically being 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less.

[0026] The subscript b is the average number of (R2SiO) groups per molecule. In general, the subscript b is 5 or more, 10 or more, 20 or more, 25 or more, 30 or more, 40 or more, 50 or more, and may be 75 or more, 100 or more, 125 or more, 150 or more, 175 or more, or even 190 or more, while typically being 200 or less, 175 or less, 150 or less, 125 or less, 100 or less, 75 or less, 50 or less, 40 or less, 30 or less, or even 25 or less, or even 20 or less.

[0027] The SiH-functional polysiloxane crosslinker has a crosslinking strength of (i) 14 mPascals * (ii) a trimethyl-terminated dimethyl-co-hydrogen methylpolysiloxane having a viscosity of 0.25 to 1.0 mPa.s and containing 0.36 weight percent hydrogen in the silyl hydride groups; and (iii) a viscosity of 0.25 to 1.0 mPa.s. * The polymer may be one or a combination of both polymers selected from the group consisting of hydride terminated polydimethylsiloxanes having a viscosity in the range of 0.5 seconds and containing 0.16 weight percent hydrogen in the silyl hydride groups.

[0028] The concentration of the SiH functional polysiloxane crosslinker is sufficient to provide a molar ratio of SiH groups to vinyl groups (SiH / Vi ratio) of 0.5 or more, and may be 0.6 or more, 0.7 or more, 0.8 or more, or even 0.9 or more, and at the same time 1.0 or less, and may be 0.9 or less, 0.8 or less, 0.7 or less, or even 0.6 or less. The SiH / Vi ratio determines the degree of crosslinking that occurs when the curable thermally conductive composition cures. If the SiH / Vinyl ratio is too low, the composition will not cure sufficiently and will not provide sufficient vertical stability. If the SiH / Vinyl ratio is too high, the composition will cure too hard and become brittle, prone to surface cracking.

[0029] The curable thermally conductive composition includes a filler treating agent that is a trialkoxysilyl compound, which is a compound having a -Si(OR)3 group, where each R, at each occurrence, is independently as described herein above for R.

[0030] The filler treating agent is desirably one or any combination of components selected from the group consisting of alkyltrialkoxysilanes and mono-trialkoxysiloxy terminated diorganopolysiloxanes.

[0031] Suitable alkyltrialkoxysilanes include those having the formula R a (R b O)Si, where R a and R b Each of R independently has in each instance 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, or even 11 or more carbon atoms, while typically having 20 or less, 18 or less, 16 or less, 14 or less, 12 or less carbon atoms, and may have 10 or less carbon atoms. b is preferably methyl so as to form a methoxyl group bonded to the silicon atom. A particularly preferred alkyltrialkoxysilane is n-decyltrimethoxysilane.

[0032] Suitable monotrialkoxysiloxy-terminated diorganopolysiloxanes include those having the average chemical formula R c 3SiO[R] d 2[SiO] g Si(OR e ) 3, wherein each R c , R d and R eis independently selected from hydrocarbyls having, in each occurrence, 1 or more carbon atoms, and can have 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, or even 8 or more carbon atoms, while typically having 10 or less, 8 or less, 6 or less, 4 or less, or even 2 or less carbon atoms, and the subscript g typically has a value of 20 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, 100 or more, or even 110 or more, while typically having a value of 200 or less, 150 or less, 125 or less, 120 or less, or even 110 or less. Particularly desirable monotrialkoxysiloxy-terminated diorganopolysiloxanes have the average chemical formula (CH3)3SiO[(CH3)2[SiO] 30 Has Si(OCH3)3.

[0033] The concentration of the filler treating agent, in weight % relative to the weight of the curable composition, can be 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.4 wt% or more, 0.5 wt% or more, 0.6 wt% or more, 0.7 wt% or more, 0.8 wt% or more, 0.9 wt% or more, 1.0 wt% or more, 1.2 wt% or more, 1.3 wt% or more, or even 1.4 wt% or more, while typically being 2.0 wt% or less, 1.8 wt% or less, 1.6 wt% or less, 1.4 wt% or less, 1.3 wt% or less, or even 1.2 wt% or less.

[0034] For example, the curable composition may be a mixture of n-decyltrimethoxysilane and (CH3)3SiO[(CH3)2SiO] 30 Si(OCH3)3. Preferably, the curable composition comprises 0.2 weight percent n-decyltrimethoxysilane and 0.10 to 0.12 weight percent of a silane having the average chemical structure (CH3)3SiO[(CH3)2SiO]. 30 and monotrimethoxysiloxy and trimethylsiloxy terminated polydimethylsiloxanes having Si(OCH3)3.

[0035] The curable thermally conductive composition further comprises a thermally conductive filler, the concentration of which, based on the weight of the curable composition, is 94% by weight or more, 94.5% by weight or more, 95% by weight or more, or even 95.5% by weight or more, and at the same time is typically 97% by weight or less, 96% by weight or less, 95.5% by weight or less, or even 95% by weight or less.

[0036] The thermally conductive fillers may include and consist of a combination of at least three, and sometimes four, different thermally conductive fillers.

[0037] The first thermally conductive filler is diamond particles having a Dv50 of 60 micrometers or more, and may have a Dv50 of 70 micrometers or more, 80 micrometers or more, 90 micrometers or more, 100 micrometers or more, 110 micrometers or more, 120 micrometers or more, 130 micrometers or more, or even 140 micrometers or more, while having a Dv50 of 150 micrometers or less, and may have a Dv50 of 140 micrometers or less, 130 micrometers or less, 120 micrometers or less, 110 micrometers or less, 100 micrometers or less, 90 micrometers or less, 80 micrometers or less, or even 70 micrometers or less. The concentration of the first thermally conductive filler, in weight percent relative to the weight of the curable thermally conductive composition, may be 30 wt% or more, 34 wt% or more, 35 wt% or more, 40 wt% or more, or even 50 wt% or more, and at the same time 55 wt% or less, 50 wt% or less, 45 wt% or less, 40 wt% or less, or even 35 wt% or less.

[0038] The second thermally conductive filler may have a Dv50 of 1 micrometer or more, 2 micrometers or more, 3 micrometers or more, 4 micrometers or more, or even 5 micrometers or more, and may have a Dv50 of 10 micrometers or less, and may have a Dv50 of 9 micrometers or less, 8 micrometers or less, 7 micrometers or less, 6 micrometers or less, or even 5 micrometers or less. The concentration of the second thermally conductive filler, in weight percent relative to the weight of the curable thermally conductive composition, may be 25 wt% or more, 26 wt% or more, 28 wt% or more, 30 wt% or more, 32 wt% or more, or even 34 wt% or more, and may be 35 wt% or less, 33 wt% or less, 31 wt% or less, 29 wt% or less, or even 27 wt% or less.

[0039] The third thermally conductive filler has a Dv50 of 0.1 or more, and may have a Dv50 of 0.3 or more, 0.5 or more, 0.7 or more, or even 0.9 or more, and may have a Dv50 of 1 or less, and may have a Dv50 of 0.8 or less, 0.6 or less, 0.4 or less, or even 0.2 or less. The concentration of the third thermally conductive filler, in weight percent relative to the weight of the curable thermally conductive composition, may be 10 wt% or more, 12 wt% or more, 14 wt% or more, 16 wt% or more, or even 18 wt% or more, and may be 20 wt% or less, 19 wt% or less, 17 wt% or less, 15 wt% or less, 13 wt% or less, or even 11 wt% or less.

[0040] The fourth thermally conductive filler may have a Dv50 of 20 micrometers or more, 25 micrometers or more, 30 micrometers or more, 35 micrometers or more, 40 micrometers or more, 45 micrometers or more, or even 50 micrometers or more, and at the same time, have a Dv50 of 60 micrometers or less, 55 micrometers or less, 50 micrometers or less, or even 45 micrometers or less. The concentration of the fourth thermally conductive filler, in weight percent relative to the weight of the curable thermally conductive composition, may be 0 wt% or more, 2 wt% or more, 4 wt% or more, 6 wt% or more, 8 wt% or more, 10 wt% or more, 12 wt% or more, 14 wt% or more, 16 wt% or more, or even 18 wt% or more, and at the same time, 20 wt% or less, 19 wt% or less, 17 wt% or less, 15 wt% or less, 13 wt% or less, or even 11 wt% or less.

[0041] The thermally conductive filler may include a filler in addition to these four thermally conductive fillers, or may not include a thermally conductive filler other than these four.

[0042] The particles can have any shape, such as spherical, irregular, crushed, or plate-like. Desirably, the second thermally conductive filler is one or both of spherical aluminum oxide and irregular aluminum nitride. Desirably, the third thermally conductive filler is crushed zinc oxide. Desirably, the fourth thermally conductive filler is spherical aluminum nitride.

[0043] Desirably, each thermally conductive filler is independently selected from the group consisting of diamond particles, aluminum nitride particles, aluminum oxide particles, zinc oxide particles, and boron nitride particles.Preferably, the first thermally conductive filler is selected from 34 weight percent diamond particles having a Dv50 of 120 micrometers, or 30.5 weight percent diamond particles having a Dv50 of 120 micrometers and 20 weight percent diamond particles having a Dv50 of 20 micrometers, or 50.4 to 50.8 weight percent diamond particles having a Dv50 of 60 micrometers.

[0044] Desirably, the second thermally conductive filler is a combination of one or both of aluminum nitride and aluminum oxide. Preferably, the second thermally conductive filler is selected from 30 weight percent spherical aluminum oxide particles having a Dv50 in the range of 2-5 micrometers, or a combination of 19 weight percent spherical aluminum oxide particles having a Dv50 of 2 micrometers and 10 weight percent irregular aluminum nitride particles having a Dv50 of 1.5 micrometers.

[0045] Desirably, the third thermally conductive filler is zinc oxide. Preferably, the third thermally conductive filler is 15 weight percent irregular zinc oxide particles having a Dv50 of 0.2 micrometers.

[0046] Desirably, the fourth thermally conductive filler is aluminum nitride. Preferably, the fourth thermally conductive filler, when present, is 16.50 weight percent spherical aluminum nitride particles having a Dv50 in the range of 30 to 50 micrometers.

[0047] Typically, the curable thermally conductive composition further comprises a platinum-based hydrosilylation catalyst, which includes compounds and complexes such as platinum(0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane (Karstedt's catalyst), HPtCl, di-μ.-carbonyldi-.π.-cyclopentadienyldinickel, platinum-carbonyl complexes, platinum-divinyltetramethyldisiloxane complexes, platinum cyclovinylmethylsiloxane complexes, platinum acetylacetonate (acac), platinum black, platinum compounds such as chloroplatinic acid, chloroplatinic acid hexahydrate, reaction products of chloroplatinic acid with monohydric alcohols, platinum bis(ethylacetoacetate), platinum bis(acetylacetonate), platinum dichloride, and complexes of platinum compounds with olefins or low molecular weight organopolysiloxanes, or platinum compounds microencapsulated in a matrix or core-shell structure. The hydrosilylation catalyst may be part of a solution containing complexes of platinum with low molecular weight organopolysiloxanes, including 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. These complexes may be microencapsulated in a resin matrix. The catalyst may be 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. Typically, the platinum-based hydrosilylation catalyst is present in a concentration sufficient to provide a platinum concentration, based on the weight of the curable thermally conductive composition, of 0.03 wt.% or more, 0.04 wt.% or more, 0.05 wt.% or more, or even 0.06 wt.% or more, while typically 0.4 wt.% or less, or 0.3 wt.% or less, 0.2 wt.% or less, 0.1 wt.% or less, 0.09 wt.% or less, 0.08 wt.% or less, 0.07 wt.% or less, 0.06 wt.% or less, 0.05 wt.% or less, or even 0.04 wt.% or less.

[0048] The curable thermally conductive composition may further include a cure inhibitor. The cure inhibitor may serve to stabilize the curable thermally conductive composition from premature curing and provide storage stability to the composition. Examples of suitable cure inhibitors include acetylenic compounds such as 2-methyl-3-butyn-2-ol, 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, 3-phenyl-1-butyn-3-ol, 1-ethynyl-1-cyclohexanol, 1,1-dimethyl-2-propynyl)oxy)trimethylsilane, and methyl(tris(1,1-dimethyl-2-propynyloxy))silane; 3-methyl-3-penten-1-yne, and and 3,5-dimethyl-3-hexen-1-yne; triazoles such as benzotriazole; hydrazine-based compounds; phosphine-based compounds; mercaptan-based compounds; and cycloalkenyl siloxanes including methylvinyl cyclosiloxanes such as 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane and 1,3,5,7-tetramethyl-1,3,5,7-tetrahexenylcyclotetrasiloxane.

[0049] The concentration of the cure inhibitor, in weight percent based on the weight of the curable thermally conductive composition, can be 0 wt% or more, 0.001 wt% or more, 0.002 wt% or more, or even 0.003 wt% or more, while typically is 0.5 wt% or less, or even 0.3 wt% or less, 0.1 wt% or less, 0.05 wt% or less, 0.01 wt% or less, or even 0.005 wt% or less, 0.004 wt% or less, or even 0.003 wt% or less.

[0050] The invention also includes a process for using a curable thermally conductive composition that includes applying the curable thermally conductive composition between and in contact with two components and then heating the curable composition to cure it while in place between the components.

[0051] The present invention further includes an article comprising a curable thermally conductive composition and at least two components, the curable thermally conductive composition being between and in contact with the two components. The curable thermally conductive composition may be in either a cured or uncured form. EXAMPLES

[0052] Table 1 shows the materials used in the following Examples (Examples) and Comparative Examples (Comparative Examples).

[0053] [Table 1]

[0054] Each sample is characterized for extrusion rate using the Extrusion Rate Test and for thermal conductivity using the method described herein above. Extrusion rates above 60 g / min and at least 8 W / m * The aim is to obtain the thermal conductivity of 100 K. Table 2 shows the results of the characteristic evaluation of each sample composition.

[0055] [Table 2]

[0056] Samples without diamond fillers with Dv50 in the range of 60-150 micrometers have an ER of more than 60 g / min and a RMS of at least 8 W / m2, even if the sample contains diamond fillers (only diamond fillers smaller than 60-150 micrometers). * Thermal conductivity (TC) of 100 K cannot be achieved.

Claims

1. A curable thermally conductive composition, the weight percentages being based on the weight of the curable thermally conductive composition and comprising: a. a vinyl functional silicone polymer which is one or a combination of vinyl dimethyl terminated polydimethylsiloxanes having a viscosity of 30 to 2000 millipascals as measured by ASTM D445-21 using a glass capillary Cannon-Fenske type viscometer at 25° C. and at concentrations ranging from 1 to 4.0 weight percent; * a vinyl functional silicone polymer having a viscosity in the range of 1000 to 2000 s; b. at least one silyl hydride functional polysiloxane crosslinker having at least two silyl hydride groups per molecule and present in a concentration such that the molar ratio of silyl hydride groups to vinyl groups in the composition ranges from 0.5 to 1.0; c. a filler treating agent at a concentration ranging from 0.1 to 2.0 weight percent, the filler treating agent being any one or any combination of compounds selected from trialkoxysilyl compounds; d. a thermally conductive filler at a concentration ranging from 94 to 97 weight percent; i. diamond particles having a Dv50 in the range of 60 to 150 micrometers in a concentration in the range of 30 to 55 weight percent; ii. a thermally conductive filler having a Dv50 in the range of greater than 1 to 10 micrometers, at a concentration in the range of 25 to 35 weight percent; iii. a thermally conductive filler having a Dv50 in the range of 0.1 to 1 micrometers, at a concentration in the range of 10 to 20 weight percent; iv. optionally, a thermally conductive filler having a Dv50 in the range of 20 to 60 micrometers at a concentration in the range of 0 to 20 weight percent; It is a curable thermally conductive composition.

2. The curable thermally conductive composition comprises: e. The curable thermally conductive composition of claim 1, further comprising a platinum-based hydrosilylation catalyst at a concentration ranging from 0.03 to 0.4 weight percent, where weight percent refers to the weight of platinum relative to the weight of the curable thermally conductive composition.

3. The curable thermally conductive composition comprises: f. The curable thermally conductive composition of claim 1 or 2, further comprising a cure inhibitor at a concentration in the range of 0.001 to 0.005 weight percent, where weight percent is based on the weight of the curable thermally conductive composition.

4. The vinyl functional silicone polymer has an average chemical structure (I): Vi(CH 3 , 2 t0.834597 3 , 2 SiO) d t0.5k 3 , 2 Vi (I) [Wherein, d is ((CH 3 ) 2 The curable thermally conductive composition according to any one of claims 1 to 3, wherein R is the average number of (SiO) groups, and has a value of 25 or more and at the same time 350 or less.

5. said silylhydride-functional polysiloxane crosslinker having a viscosity of (i) 14 millipascals as determined by ASTM D445-21 using a glass capillary Cannon-Fenske viscometer at 25°C; * (ii) a trimethyl terminated dimethyl-co-hydrogen methylpolysiloxane having a viscosity of 7 to 10 millipascals and containing 0.36 weight percent hydrogen in the silyl hydride groups; * 5. The curable thermally conductive composition of claim 1, wherein the curable thermally conductive composition is a combination of one or both of a polymer selected from the group consisting of: a hydride terminated polydimethylsiloxane having a viscosity in the range of 0.5 to 100 s and containing 0.16 weight percent hydrogen in the silyl hydride groups; and

6. a. the thermally conductive filler having a Dv50 in the range of greater than 1 to 5 micrometers is one or more selected from the group consisting of aluminum nitride and aluminum oxide; b. the thermally conductive filler having a Dv50 in the range of 0.1 to 1 micrometer is zinc oxide; The curable thermally conductive composition of any one of claims 1 to 5, wherein an aluminum nitride thermally conductive filler is present having a Dv50 in the range of 40 to 60 micrometers.

7. The weight percentages are based on the weight of the curable thermally conductive composition: a. 75 to 80 millipascals at a concentration ranging from 2.7 to 3.3 percent by weight * a vinyl dimethyl terminated polydimethylsiloxane having a viscosity in the range of 1000 to 2000000 seconds; b. 14 millipascals * 0.04 weight percent trimethyl terminated dimethyl-co-hydrogen methylpolysiloxane having a viscosity of 7 to 10 millipascals; * 0.5 to 0.6 weight percent of a hydride-terminated polydimethylsiloxane having a viscosity in the range of 10 ... c. 0.2 weight percent n-decyltrimethoxysilane and 0.10 to 0.12 weight percent of a silane having the average chemical structure (CH 3 ) 3 SiO[(CH 3 ) 2 SiO 30 Si(OCH 3 ) 3 a filler treatment agent comprising a monotrimethoxysiloxy and trimethylsiloxy terminated polydimethylsiloxane having the formula: d. A thermally conductive filler, i. 34 wt.% diamond particles having a Dv50 of 120 micrometers, or 30.5 wt.% diamond particles having a Dv50 of 120 micrometers and 20 wt.% diamond particles having a Dv50 of 20 micrometers, or 50.4-50.8 wt.% diamond particles having a Dv50 of 60 micrometers; ii. 30 weight percent spherical aluminum oxide particles having a Dv50 in the range of 2 to 5 micrometers, or a combination of 19 weight percent spherical aluminum oxide particles having a Dv50 of 2 micrometers and 10 weight percent irregular aluminum nitride particles having a Dv50 of 1.5 micrometers; iii. 15% by weight of irregular zinc oxide particles having a Dv50 of 0.2 micrometers, and iv. optionally, a thermally conductive filler consisting of 16.50 weight percent spherical aluminum nitride particles having a Dv50 in the range of 30 to 50 micrometers; e. 0.06 weight percent of a platinum hydrosilylation catalyst; f. 0.002 weight percent methyl(tris(1,1'-dimethyl-2-propynyloxy))silane; 2. The curable thermally conductive composition of claim 1 comprising:

8. 8. A process for using a curable thermally conductive composition according to any one of claims 1 to 7, comprising applying the curable thermally conductive composition between and in contact with two components and then heating the curable composition to cure it while in place between the components.

9. The process of claim 8 , wherein applying the curable thermally conductive composition comprises extruding the curable thermally conductive composition.

10. 8. An article comprising the curable thermally conductive composition of any one of claims 1 to 7 between and in contact with two components of the article, said curable thermally conductive composition being either in a cured or uncured form.

Citation Information

Patent Citations

  • Thermally conductive polyorganosiloxane composition

    WO2018016564A1

  • Heat-conductive polyorganosiloxane composition

    WO2018221662A1

  • Highly thermally conductive flowable silicone composition

    WO2021109051A1

  • Resin composition, heat-radiating member, and electronic apparatus

    WO2021206064A1

Cited By

  • Vertically stable, room temperature storage, one-part, post-cure, thermally conductive silicone

    JP2024539437A

  • Vertically stable, room temperature storage, one-part, post-cure, thermally conductive silicone

    JP7653579B2