Electrochemical Equipment
A magnesium-doped carbon-silicon-oxygen material with a carbon nanotube coating addresses the volume change issues in silicon-based electrodes, enhancing the efficiency and stability of electrochemical devices.
Patent Information
- Application Number
- JP2024523468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-01-21
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-01-21
AI Technical Summary
Existing negative electrode active materials, particularly silicon-based materials, suffer from significant volume changes during lithium intercalation and desorption, leading to deteriorated cycle characteristics and poor initial Coulombic efficiency in electrochemical devices like lithium ion batteries.
A magnesium-doped carbon-silicon-oxygen material with a carbon nanotube coating layer is used to form a conductive network, improving electrical conductivity and structural stability, thereby enhancing the initial Coulombic efficiency and cycle characteristics.
The solution results in improved initial Coulombic efficiency, reduced volume expansion, and extended cycle life of electrochemical devices by forming a uniform lithium metal deposit and maintaining structural integrity during cycling.
Smart Images

Figure 2024540913000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of energy storage, and in particular to negative electrode active materials and electrochemical devices containing same, particularly lithium ion batteries. [Background technology]
[0002] With the development of technology and the increasing demand for mobile devices, the demand for electrochemical devices (e.g., lithium-ion batteries) has increased significantly. In order to provide electrochemical devices with high energy density, high discharge characteristics and high cycle characteristics, one of the main research directions in the electrochemical energy storage field is the study and improvement of electrode materials in electrochemical devices.
[0003] Currently, most commercial electrochemical devices use graphite as the negative electrode active material of the electrode, but the gram capacity of graphite is low. Silicon-based materials have a higher theoretical gram capacity as a negative electrode active material than graphite, and are the main negative electrode active materials for developing electrochemical devices with high volumetric energy density in the future. However, in practical applications, such high energy density negative electrode active materials have a huge volume change effect during the lithium absorption and release process, which causes a decrease in the cycle characteristics of the electrochemical device and a poor initial coulombic efficiency. There are still various defects in the improvement proposals for silicon-based materials.
[0004] In view of these circumstances, there is a need to continue research and improvement into negative electrode materials and negative electrode active materials in order to improve the battery capacity, cycle characteristics, and rate characteristics of electrochemical devices. Summary of the Invention
[0005] SUMMARY OF THE DISCLOSURE To solve, at least in part, at least one of the problems existing in the related art, embodiments of the present invention provide a negative electrode active material having a substrate-free adhesive film and an electrochemical device including the same.
[0006] According to one aspect of the present invention, some embodiments of the present invention provide a negative electrode active material, which includes a magnesium-doped carbon silicon oxygen material. By using carbon nanotubes to coat the particles of the magnesium-doped carbon silicon oxygen material, the magnesium-doped carbon silicon oxygen material further includes a carbon nanotube coating layer, and the carbon nanotube coating layer is provided on the particle surface of the crystalline oxide of the magnesium-doped carbon silicon oxygen material. The negative electrode active material according to the present invention can improve the initial Coulomb efficiency of the carbon silicon oxygen material and enhance the rate performance of the carbon silicon oxygen material by using the magnesium-doped carbon silicon oxygen material. In addition, by providing a carbon nanotube coating layer on the particle surface of the crystalline oxide of the magnesium-doped carbon silicon oxygen material, a network conductive structure can be formed, and the electrical conductivity of the negative electrode active material can be improved.
[0007] According to another aspect of the present invention, some embodiments of the present invention provide an electrochemical device, which includes a negative electrode. The negative electrode includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes a magnesium-doped carbon silicon oxygen material, and the magnesium-doped carbon silicon oxygen material includes a carbon nanotube coating layer. The carbon nanotube coating layer is provided on the surface of the crystalline oxide of the magnesium-doped carbon silicon oxygen material. The electrochemical device according to the present invention can improve the initial Coulomb efficiency of the electrochemical device, improve the structural stability during the cycling process of the electrochemical device, and further improve the cycle retention rate and cycle performance of the electrochemical device by using the magnesium-doped carbon silicon oxygen material having a carbon nanotube coating layer.
[0008] According to some embodiments of the present invention, the general formula of the crystalline oxide of the magnesium-doped carbon silicon oxygen material is Mg z SiC x O y where x, y, and z satisfy 0 < x < 0.3, 0.4 < y < 1.0, and 0.1 < z < 0.2.
[0009] According to some embodiments of the present invention, in the magnesium doped carbon silicon oxygen material, the molar silicon content is 40%-70%, the molar carbon content is 3.5%-24%, and the molar magnesium content is 7.0%-7.5%.
[0010] According to some embodiments of the present invention, in the magnesium-doped carbon silicon oxygen material, the molar ratio of magnesium to silicon is 0.1-0.2, and the molar ratio of magnesium to carbon is 0.2-10.0.
[0011] According to some embodiments of the present invention, the I in the Raman spectrum of the magnesium doped carbon silicon oxygen material D / I G The value is 0.023 to 0.32.
[0012] According to some embodiments of the present invention, the I in the Raman spectrum of magnesium doped carbon silicon oxygen material versus the molar carbon content is D / I G The value of the ratio of values is 0.095 to 6.78.
[0013] According to some embodiments of the present invention, the carbon nanotube coating layer has a thickness of 0.5 nm to 5.0 μm.
[0014] According to some embodiments of the present invention, the carbon nanotube coating layer includes carbon nanotube clusters, which extend from a surface of the carbon nanotube coating layer, and the length of the carbon nanotube clusters is 0.1 μm to 1.0 μm.
[0015] According to some embodiments of the present invention, the negative electrode active material layer further includes a binder, the binder including synthetic rubber, the binder including one or more selected from the group consisting of polyacrylic acid ester, polyimide, polyamide, polyamideimide, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethylcellulose, potassium carboxymethylcellulose, sodium hydroxymethylcellulose, and potassium hydroxymethylcellulose.
[0016] According to some embodiments of the present invention, the weight percentage of the binder is 2% to 6% based on the total weight of the negative electrode active material layer.
[0017] According to some embodiments of the present invention, an electrolyte for an electrochemical device includes an organic solvent and a lithium salt, the organic solvent includes one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate, vinylene carbonate, propyl propionate, and ethyl propionate, and the lithium salt includes lithium hexafluorophosphate. The lithium fluoride-containing oxides include one or more selected from the group consisting of lithium fluoride (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (Li(N(SO2F)2)), lithium bis(oxalato)borate (LiB(C2O4)2), and lithium difluoro(oxalato)borate (LiBF2(C2O4)).
[0018] Additional aspects and advantages of embodiments of the present invention are set forth in part in the description that follows, and in part are illustrated by, or may be learned by, the practice of the embodiments of the present application. [Brief description of the drawings]
[0019] In the following, in order to describe the embodiments of the present application, the drawings necessary for describing the embodiments of the present application or the prior art will be briefly described. Obviously, the drawings described below are only some of the embodiments in the present application. Those skilled in the art can still obtain drawings of other embodiments based on the structures illustrated in these drawings without creative labor.
[0020] [Figure 1] FIG. 1 is a schematic diagram of the particle structure of negative electrode active materials according to some embodiments of the present invention. [Diagram 2] FIG. 2 is the XRD diffraction spectrum of the magnesium-doped carbon silicon oxygen material of Example 1 of the present invention. [Diagram 3] FIG. 3 is a 5000x microscope image of the negative electrode active material of Example 1 of the present invention taken by a scanning electron microscope. [Figure 4] FIG. 4 is a graph showing cycle capacity curves of the electrochemical devices of Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The embodiments of the present invention are described in detail below, which should not be construed as limitations on the present application.
[0022] As used herein, the following terms have the meanings indicated below, unless otherwise specified.
[0023] As used herein, the terms "approximately", "approximately", "substantially", and "about" are intended to indicate and describe small variations. When used in conjunction with an instance or circumstance, the term can refer to instances where the instance or circumstance occurred exactly and instances where the instance or circumstance occurred very approximately. By way of example, when used in conjunction with a numerical value, the term can refer to a variation range of ±10% or less of the numerical value, for example, ±5% or less, ±4% or less, ±3% or less, ±2% or less, ±1% or less, ±0.5% or less, ±0.1% or less, or ±0.05% or less. By way of example, two numerical values are considered to be "approximately" the same if the difference between them is ±10% or less of the average value of the values (e.g., ±5% or less, ±4% or less, ±3% or less, ±2% or less, ±1% or less, ±0.5% or less, ±0.1% or less, or ±0.05% or less).
[0024] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "one or more selected from the group consisting of," "at least one or more of," or other similar terms can refer to any combination of the listed items. For example, if items A and B are listed, the phrase "one or more of A and B" means A only, B only, or A and B. In another example, if items A, B, and C are listed, the phrase "one or more of A, B, and C" means A only, B only, C only, A and B (removing C), A and C (removing B), B and C (removing A), or all of A, B, and C. Item A may include one element or multiple elements. Item B may include one element or multiple elements. Item C may include one element or multiple elements.
[0025] Also, for convenience of description, "first," "second," "third," etc. may be used herein to distinguish between different components in a figure or series of figures. "First," "second," "third," etc. are not intended to describe corresponding components unless specifically specified or limited.
[0026] In the field of electrochemical energy storage, attempts have been made to replace the graphite in the conventional anode active material with a high energy density anode active material in order to obtain the optimal energy density. However, when applying such anode active materials with high energy density, further processing is required due to different material properties. For example, silicon-based materials have a high theoretical gram capacity of 4200 mAh / g, and therefore will become the mainstream anode active material for the development of future electrochemical devices with high volumetric energy density (e.g., lithium-ion batteries). Such high energy density anode active materials bring about a huge volume change effect (e.g., more than about 300%) during the lithium absorption / release process. If the anode expands significantly, the interface between the anode and the separator will be deformed and separated, and the cycle characteristics of the lithium-ion battery will be further deteriorated. At the same time, the lithium ion pathway during the lithium absorption / release process of silicon-based materials is unstable, which makes it easy to cause non-uniform lithium metal precipitation and the dead lithium phenomenon. This leads to a poor initial coulombic efficiency of an electrochemical device using a silicon-based material as the negative electrode active material. The initial charge / discharge coulombic efficiency can directly reflect the electrochemical performance of the electrochemical device.
[0027] Chinese patent CN108767241A discloses an anode material, which uses magnesium-doped silicon oxide formed by doping magnesium into silicon-oxygen material, and can improve the rate characteristic and initial coulombic efficiency of lithium-ion batteries. However, during the charge-discharge cycle, the magnesium-doped silicon oxide has insufficient electrical conductivity and a high volume expansion rate during the lithium absorption-release process, so that the magnesium-doped silicon oxide as the anode active material still cannot effectively form uniform lithium metal deposition, which results in a decrease in the cycle efficiency of magnesium-doped silicon oxide and a shortened service life.
[0028] In view of the above problems, according to one aspect of the present invention, as shown in Fig. 1, some embodiments of the present invention provide an anode active material, which includes a composite material, i.e., magnesium-doped carbon silicon oxygen material, formed by carbon doping and magnesium doping silicon oxide through a high-temperature manufacturing process. The surface of the crystalline oxide 101 of the magnesium-doped carbon silicon oxygen material further includes a carbon nanotube coating layer 102. The carbon nanotube coating layer 102 is provided on the particle surface of the crystalline oxide 101 of the magnesium-doped carbon silicon oxygen material through a carbon nanotube coating process.
[0029] By doping silicon-oxygen materials with magnesium, magnesium silicon oxides can be formed, and the initial Coulombic efficiency of electrochemical devices can be improved. At the same time, by doping carbon, carbon-containing magnesium silicon oxides can be further formed in the composite magnesium-doped carbon silicon-oxygen materials. The carbon-containing magnesium silicon oxides have a low volume expansion rate and excellent cycle structure stability during the lithium insertion and extraction process. The magnesium-doped carbon silicon-oxygen materials can effectively form uniform lithium metal precipitation during the cycling process, improve the cycle characteristics of electrochemical devices, and extend their service life. In addition, the present invention can further improve the conductivity of the anode active material by coating the particle surface of the magnesium-doped carbon silicon-oxygen material with carbon nanotubes.
[0030] The magnesium-doped carbon silicon-oxygen material is a composite material comprising a crystalline oxide composed of magnesium, carbon, silicon and oxygen, and carbon nanotubes coated on its surface. In some embodiments, the crystalline oxide of the magnesium-doped carbon silicon-oxygen material can be represented by the general formula Mg z SiC x O y . In some embodiments, the stoichiometry of the general formula Mg z SiC x O y of the crystalline oxide of the magnesium-doped carbon silicon-oxygen material is 0 < x < 0.3, 0.4 < y < 1.0, and 0.1 < z < 0.2. In some embodiments, 0.15 < x < 0.28, 0.6 < y < 0.8, and 0.1 < z < 0.2. In some embodiments, 0.2 < x < 0.25, 0.7 < y < 0.78, and 0.1 < z < 0.2.
[0031] Each component and its crystal structure composition in the magnesium doped carbon silicon oxygen material have a certain effect on the cycle characteristics, gram capacity and structural stability of the magnesium doped carbon silicon oxygen material in an electrochemical device. In some embodiments, the molar content of elemental silicon Si in the magnesium doped carbon silicon oxygen material is 40% to 70%. If the content of elemental silicon is too low, the gram capacity of the negative electrode active material will be low, and if the content of elemental silicon is too high, the volume expansion rate of the negative electrode active material will be high. In some embodiments, the molar content of elemental silicon Si in the magnesium doped carbon silicon oxygen material is 60%.
[0032] In some embodiments, the molar content of magnesium element Mg in the magnesium doped carbon silicon oxygen material is 7.00%-7.5%. When the magnesium element is in the above content range, it can effectively form carbon-containing magnesium silicon oxide, and avoid the magnesium element and oxygen from forming highly active magnesium oxide or magnesium metal, thereby improving the initial coulombic efficiency of the magnesium doped carbon silicon oxygen material as the negative electrode active material, and reducing the safety risk during the electrochemical cycle reaction of the magnesium doped carbon silicon oxygen material.
[0033] In some embodiments, the molar content of carbon element C in the magnesium doped carbon silicon oxygen material is 3.5%-24%. The carbon element source in the magnesium doped carbon silicon oxygen material includes carbon doped in a crystalline oxide and carbon nanotubes coated with a crystalline oxide. If the carbon doping amount is too low, the structural stability of the negative electrode active material is reduced and the volume expansion rate is increased, and if the carbon doping amount is too high, the gram capacity of the negative electrode active material is reduced. In some embodiments, the molar content of carbon element C in the magnesium doped carbon silicon oxygen material is 4.5%-10%. In some embodiments, the molar content of carbon element C in the magnesium doped carbon silicon oxygen material is about 6%.
[0034] It should be understood that the content of each elemental component in the magnesium-doped carbon silicon oxygen material of the present invention can be detected by any suitable detection method in the art, but is not limited thereto. In some embodiments, the magnesium content and silicon content in the magnesium-doped carbon silicon oxygen material can be measured by X-ray diffraction analysis. In some embodiments, the carbon content of the magnesium-doped carbon silicon oxygen material can be measured by the following carbon content test. Under oxygen-enriched conditions, the sample is heated at high temperature by a high-frequency furnace to combust, and carbon and sulfur are oxidized to carbon dioxide and sulfur dioxide, respectively. After the gas is treated, it enters the corresponding absorption cell, absorbs the corresponding infrared radiation, and is converted into a corresponding signal by the detector. The signal is sampled by a computer, linearly corrected, and then converted into a value proportional to the concentration of carbon dioxide and sulfur dioxide. The values of the entire analysis process are then accumulated, and after the analysis is completed, the accumulated value is divided by the weight value by the computer, multiplied by a correction factor, and the blank is subtracted to obtain the carbon and sulfur contents in the sample. A high frequency infrared sulfur carbon analyzer (Shanghai Dekai Instrument Co., Ltd. HCS-140) is used for sample testing.
[0035] FIG. 2 is an XRD diffraction spectrum of the magnesium-doped carbon silicon oxygen material of Example 1 of the present invention. As shown in FIG. 2, in one embodiment, the magnesium-doped carbon silicon oxygen material is subjected to X-ray diffraction analysis, and the XRD diffraction spectrum shows that the magnesium-doped carbon silicon oxygen material contains one or more characteristic peaks selected from Si, SiO2, MgSiO3, and Mg2SiO4. In some embodiments, the magnesium-doped carbon silicon oxygen material has a molar ratio of magnesium to silicon of 0.1-0.2 and a molar ratio of magnesium to carbon of 0.2-10.0. Thereby, the cycle characteristics and the initial coulombic efficiency of the magnesium-doped carbon silicon oxygen material in an electrochemical device are improved. In some embodiments, the magnesium-doped carbon silicon oxygen material has a molar ratio of magnesium to silicon of about 0.12.
[0036] Figure 3 is a 5000x scanning electron microscope image of the magnesium-doped carbon silicon oxygen material of Example 1 of the present invention. As can be seen from Figure 3, the carbon nanotube coating layer on the surface of the crystalline oxide particles of the magnesium-doped carbon silicon oxygen material can form a network conductive structure, which can make the distribution of lithium metal deposition during cycling more uniform, improve the volume expansion distribution of the magnesium-doped carbon silicon oxygen material, and make the negative electrode active material have better structural stability during cycling.
[0037] In some embodiments, the thickness of the carbon nanotube coating layer can affect the electrical conductivity and energy density of the magnesium doped carbon silicon oxygen material in an electrochemical device. If the carbon nanotube coating layer is too thick, the gram capacity of the magnesium doped carbon silicon oxygen material decreases, and if the carbon nanotube coating layer is too thin, the electrical conductivity decreases and the structural stability of the magnesium doped carbon silicon oxygen material cannot be improved. In some embodiments, the thickness of the carbon nanotube coating layer is about 0.5 nm, 1.0 nm, 5 nm, 10 nm, 50 nm, 100 nm, 250 nm, 500 nm, 1.0 μm, or 5.0 μm, or a range of any two of the above values. In some embodiments, the thickness of the carbon nanotube coating layer is 0.5 nm to 5.0 μm. In some embodiments, the thickness of the carbon nanotube coating layer is 2.0 nm to 150 nm.
[0038] In some embodiments, the carbon nanotube coating comprises carbon nanotube clusters. The carbon nanotube clusters extend outward from the surface of the particles of the magnesium doped carbon silicon oxygen material and contact the carbon nanotube coating on the surface of other particles to form an effective conductive network and improve the electrical conductivity of the magnesium doped carbon silicon oxygen material. In some embodiments, the extension length of the carbon nanotube clusters is between 0.1 μm and 1.0 μm. In some embodiments, the thickness of the carbon nanotube clusters is about 0.5 μm.
[0039] In this specification, the thickness of the carbon nanotube coating layer and the extension length of the carbon nanotube cluster are not particularly limited and can be detected by any suitable detection method in the art. In some embodiments, the thickness of the carbon nanotube coating layer and the extension length of the carbon nanotube cluster are evaluated by a scanning electron microscope (SEM) or a transmission electron microscope (TEM). In some embodiments, the evaluation by the scanning electron microscope is recorded using a Philips XL-30 type field emission scanning electron microscope, and is performed under the conditions of 10 kV and 10 mA.
[0040] In some embodiments, the magnesium doped carbon silicon oxygen material particles have a particle size (Dv50) of 2.5 μm to 10.0 μm. In some embodiments, the magnesium doped carbon silicon oxygen material particles have a particle size (Dv50) of 2.7 μm to 5.3 μm, improving the coating distribution of the magnesium doped carbon silicon oxygen material in the negative electrode active material layer. In some embodiments, the particle size distribution of the magnesium doped carbon silicon oxygen material particles satisfies the relationship: 0.3≦Dn10 / Dv50≦0.6.
[0041] In this specification, the term "particle size" includes, unless otherwise specified, a characteristic particle property of a sample obtained by a particle size test, such as Dn10 or Dv50. Here, Dn10 indicates a particle size at which the particle number accumulation is 10% from the small particle size side in the particle size-based particle distribution of the material. Dv50 indicates a particle size at which the volume accumulation is 50% from the small particle size side in the volume-based particle distribution of the material. In some examples, the particle size test method used a Mastersizer2000 laser particle size distribution tester to analyze the particle size of the particles of the sample. The sample was dispersed in 100 mL of dispersant (deionized water) to set the light blocking degree to 8 to 12%. Then, the sample was subjected to ultrasonic treatment for 5 minutes at an ultrasonic intensity of 40 KHz and 180 w. After ultrasonic treatment, the sample was subjected to laser particle size distribution analysis to obtain particle size distribution data.
[0042] In some embodiments, the magnesium doped carbon silicon oxygen material particles have a specific surface area of 1 m 2 / g~50m 2 In some embodiments, the specific surface area of the magnesium doped carbon silicon oxygen material particles is 5 m 2 / g~20m 2 / g maintains the reaction rate between the magnesium-doped carbon silicon oxygen material and the electrolyte.
[0043] In some embodiments, the coverage and structural stability of the carbon nanotube coating layer in the magnesium-doped carbon silicon oxygen material can be evaluated by Raman spectroscopy. -1 and 1580cm -1 The D and G peaks in the vicinity are characteristic peaks in the Raman spectrum of carbon atom crystals. In some embodiments, the ratio value of the characteristic peak D peak to the characteristic peak G peak in the Raman spectrum of the magnesium-doped carbon silicon oxygen material, i.e., I D / I GThe I value can be used to evaluate the network conductive structure due to the carbon nanotube coating layer in the magnesium-doped carbon silicon oxygen material particles. D / I G A low value indicates that the network conductive structure of the carbon nanotube coating is relatively complete. In some embodiments, the I D / I G In some embodiments, the I value in the Raman spectrum of the magnesium doped carbon silicon oxygen material is 0.32 or less. D / I G By setting the value to 0.023 to 0.32, the network conductive structure of the carbon nanotube coating layer is improved.
[0044] In some embodiments, the I in the Raman spectrum of the magnesium doped carbon silicon oxygen material versus the molar carbon content is D / I G The ratio of the I value to the carbon molar content in the Raman spectrum of the magnesium-doped carbon silicon oxygen material can be used to evaluate the degree of coverage of the carbon nanotube coating layer on the magnesium-doped carbon silicon oxygen material. D / I G If the ratio of the values is too low, the gram capacity of the magnesium doped carbon silicon oxygen material will be low. D / I G If the ratio of the values is too high, the carbon nanotube coating layer on the magnesium doped carbon silicon oxygen material will be poorly coated. In some embodiments, the I in the Raman spectrum of the magnesium doped carbon silicon oxygen material versus the molar carbon content is D / I G The ratio of values is 0.095 to 6.78.
[0045] According to another aspect of the present invention, some embodiments of the present invention provide a method for preparing said magnesium doped carbon silicon oxygen material, the specific process is as follows:
[0046] (1) A carbon nanotube raw material is mixed with ethanol to prepare an ethanol dispersion having a predetermined carbon nanotube concentration. In some embodiments, the weight percentage concentration of the carbon nanotubes in the ethanol dispersion is 1.5% to 10.0%. In some embodiments, the weight percentage concentration of the carbon nanotubes in the ethanol dispersion is 1.6% to 6.6%.
[0047] (2) The precursor of the magnesium-doped carbon silicon oxygen material is mixed with the ethanol dispersion and stirred uniformly. The mixture of the precursor of the magnesium-doped carbon silicon oxygen material and the ethanol dispersion is evaporated to dryness, and the dry powder is collected.
[0048] (3) High temperature treatment of the collected dry powder under argon atmosphere to obtain magnesium doped carbon silicon oxygen material. In some embodiments, the temperature of the high temperature treatment is 400°C to 800°C. In some embodiments, the temperature of the high temperature treatment is about 600°C. In some embodiments, the time of the high temperature treatment is 1h to 5h. In some embodiments, the time of the high temperature treatment is about 3h.
[0049] The present invention can use ethanol dispersion to coat the precursor of magnesium-doped carbon silicon oxygen material with carbon nanotubes to form magnesium-doped carbon silicon oxygen material with carbon nanotube coating layer. The magnesium-doped carbon silicon oxygen material with carbon nanotube coating layer of the present invention can not only improve the electrical conductivity compared with the simple carbon-coated or carbon-doped negative electrode active material, but also reduce the impact of the carbon material on the electrical performance and gram capacity of the magnesium-doped carbon silicon oxygen material, improve the lithium deposition absorption and release mechanism of the magnesium-doped carbon silicon oxygen material, and further improve the electrical performance and cycle characteristics of the magnesium-doped carbon silicon oxygen material in electrochemical devices. In some embodiments, the temperature and reaction time of high-temperature treatment can be adjusted to further improve the electrical conductivity and coating structure of the carbon nanotube coating layer in the magnesium-doped carbon silicon oxygen material, so that the magnesium-doped carbon silicon oxygen material can exhibit excellent cycle characteristics and initial coulombic efficiency as a negative electrode active material.
[0050] According to another aspect of the present invention, some embodiments of the present invention provide an electrochemical device, the electrochemical device includes a negative electrode, the negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the magnesium-doped carbon silicon oxygen material in the above embodiment. The electrochemical device uses the magnesium-doped carbon silicon oxygen material with a carbon nanotube coating layer to improve the initial coulombic efficiency of the electrochemical device, improve the structural stability during the cycle process of the electrochemical device, and further improve the cycle retention rate and cycle characteristics of the electrochemical device. In some embodiments, the weight percentage of the magnesium-doped carbon silicon oxygen material is 20% or more with respect to the total weight of the negative electrode active material. In some embodiments, the weight percentage of the magnesium-doped carbon silicon oxygen material is 60% or more. In some embodiments, the negative electrode active material is formed from the magnesium-doped carbon silicon oxygen material in the above embodiment.
[0051] In some embodiments, the negative electrode active material further includes graphite, and the graphite includes one or more selected from the group consisting of natural graphite, artificial graphite, and mesocarbon microbeads. This can improve the electrical conductivity and cycle characteristics of the negative electrode active material. The negative electrode active material can include other common negative electrode active materials in the field that can absorb and release lithium (Li) as long as they are not contrary to the spirit of the present invention. Other common negative electrode active materials include, but are not limited to, one or more selected from carbon materials, metal compounds, oxides, sulfides, lithium nitrides such as LiN3, lithium metal, metal elements and semimetal elements alloyed with lithium, polymer materials, and combinations thereof.
[0052] In some embodiments, the powder electrical conductivity of the negative electrode active material can be controlled by adjusting the content of magnesium-doped carbon silicon oxygen material, thereby improving the cycle characteristics of the negative electrode active material layer. In some embodiments, the powder electrical conductivity of the negative electrode active material is 2.0 S / cm to 30 S / cm. In some embodiments, the powder electrical conductivity of the negative electrode active material is 5.0 S / cm to 10 S / cm. In this specification, the powder electrical conductivity of the negative electrode active material is not particularly limited and can be detected using any suitable detection method in the art. In some embodiments, the method for detecting the powder electrical conductivity of the negative electrode active material is as follows. A resistivity tester (Suzhou Jingge Electronic Co.,LTD, ST-2255A) was used to take 5g of powder sample, and press it with an electronic press at a constant pressure of 5000kg±2kg for 15-25s. The sample was placed between the electrodes of the tester, and the powder electronic conductivity was calculated by the formula δ=h / (S*R) / 1000, where h is the height of the sample (cm), R is the resistance (KΩ), and S is the area after pressing the powder sample into a sheet, i.e., 3.14cm. 2 It is.
[0053] In some embodiments, the resistance range of the negative electrode active material layer is 0.2Ω to 1Ω.
[0054] In some embodiments, the negative electrode active material layer further includes a binder, which can improve the structural stability of the negative electrode active material layer. In some embodiments, the binder includes a synthetic rubber, and the binder includes one or more selected from the group consisting of polyacrylic acid ester, polyimide, polyamide, polyamideimide, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose, and potassium hydroxymethyl cellulose. In some embodiments, the weight percentage of the binder is 2% to 6% with respect to the total weight of the negative electrode active material layer. In another embodiment, the weight percentage of the binder is, for example, about 2%, about 3%, about 4%, about 5%, or about 6% with respect to the total weight of the negative electrode active material, or a range consisting of any two of these values.
[0055] In some embodiments, the negative electrode active material layer further includes a conductive agent to improve the conductivity of the negative electrode active material layer. The conductive agent includes one or more selected from the group consisting of carbon nanotubes, conductive carbon black, acetylene black, graphene, and ketjen black. Those skilled in the art can select a conventional conductive agent according to actual needs, but are not limited thereto. In some embodiments, the weight percentage of the conductive agent is 1% to 10% with respect to the total weight of the negative electrode active material layer. In another embodiment, the weight percentage of the conductive agent is, for example, about 1%, about 2%, about 3%, about 5%, or about 10% with respect to the total weight of the negative electrode active material, or a range consisting of any two of these values.
[0056] In some embodiments, the negative electrode further comprises a negative current collector, which may be a copper foil or a nickel foil, but other negative current collectors commonly used in the art may be used, but are not limited to these.
[0057] In some embodiments, the electrochemical device further includes a positive electrode and a separator, and the positive electrode, the separator, and the negative electrode in the above embodiments can be wound or stacked to form an electrode assembly. The electrode assembly in the present invention can be any suitable electrode assembly in the art without being limited thereto, as long as it is within the scope of the present invention. In some embodiments, the electrode assembly is a wound structure. In some embodiments, the electrode assembly can be a stacked structure or a multi-tab structure. In some embodiments, the electrochemical device is a lithium ion battery.
[0058] In some embodiments, the positive electrode includes a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector may be an aluminum foil or a nickel foil, but other positive electrode current collectors commonly used in the art may be used, but are not limited thereto. In some embodiments, the positive electrode active material layer includes a positive electrode active material capable of absorbing and releasing lithium (Li) (hereinafter, may be referred to as a "positive electrode active material capable of absorbing / releasing lithium Li"). Examples of positive electrode active materials capable of absorbing / releasing lithium (Li) include one or more selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxygen phosphate, lithium iron phosphate, lithium titanate, and lithium-rich manganese-based materials.
[0059] In some embodiments, the positive electrode active material layer may further include at least one of a binder and a conductive agent. The binder may include one or more selected from the group consisting of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylic acid ester, polyacrylic acid, polyacrylate, sodium carboxymethylcellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene. The conductive agent may include one or more selected from the group consisting of carbon nanotubes, conductive carbon black, acetylene black, graphene, and ketjen black. It should be noted that those skilled in the art may select ordinary binders and conductive agents according to actual needs, but are not limited thereto.
[0060] In some embodiments, the separator includes at least one selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, polyimide, and aramid, but is not limited thereto. For example, the polyethylene includes at least one component selected from high density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene. Among them, polyethylene and polypropylene play a good role in preventing short circuit, and can also improve the stability of the battery by the off effect. It should be noted that those skilled in the art can select ordinary separators in the field according to the actual needs, but are not limited thereto.
[0061] In some embodiments, the electrochemical device further comprises an electrolyte, the electrolyte comprising a lithium salt and an organic solvent.
[0062] In some embodiments, the lithium salt comprises one or more selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (Li(N(SO2F)2)), lithium bis(oxalato)borate (LiB(C2O4)2), and lithium difluoro(oxalato)borate (LiBF2(C2O4)). For example, lithium hexafluorophosphate (LiPF6) is selected as the lithium salt because of its high ionic conductivity and improved cycle characteristics.
[0063] In some embodiments, the organic solvent comprises one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate, vinylene carbonate, propyl propionate, and ethyl propionate. The lithium salt comprises one or more selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (Li(N(SO2F)2)), lithium bis(oxalato)borate (LiB(C2O4)2), and lithium difluoro(oxalato)borate (LiBF2(C2O4)).
[0064] In some embodiments, the electrolyte further comprises an additive, which may be any suitable additive in the art without being limited thereto, as long as it is not contrary to the spirit of the present invention.
[0065] In addition, the manufacturing methods of the positive electrode, separator, negative electrode and electrolyte in the examples of the present invention may be selected from any suitable conventional methods in the art according to specific needs, as long as they are not contrary to the spirit of the present invention, but are not limited thereto. In one embodiment of the manufacturing method of the electrochemical device, the manufacturing method of the lithium ion battery includes the following steps. The negative electrode, separator and positive electrode in the examples are wound, folded or stacked in order to form an electrode assembly, and then the electrode assembly is placed in a case such as an aluminum plastic film, and an electrolyte is injected. The lithium ion battery with the electrode assembly attached is subjected to subsequent processes such as vacuum sealing, standing, formation, shaping, etc. to obtain a lithium ion battery.
[0066] Although the above description is given by taking a lithium ion battery as an example, those skilled in the art can imagine that the adhesive film of the negative electrode active material of the present invention can be applied to other suitable electrochemical devices based on the present invention. Such electrochemical devices include any device that generates an electrochemical reaction, and specific examples thereof include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0067] Some embodiments of the present invention further provide an electronic device, the electronic device including an electrochemical device according to an embodiment of the present invention.
[0068] The electronic device of the embodiment of the present invention is not particularly limited and may be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a portable facsimile, a portable copy machine, a portable printer, a stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini CD, a walkie-talkie, an electronic notebook, a calculator, a memory card, a portable tape recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a bicycle assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flashlight, a camera, a large household storage battery, and a lithium ion capacitor.
[0069] Specific Examples The following provides some specific examples and comparative examples, and describes the test methods and results of the Raman test, cycle test, rate characteristic test, and expansion rate test for the electrochemical device (lithium ion battery), to better explain the technical solution of the present invention.
[0070] 1. Test method 1.1 Raman testing: A Raman spectrometer (Jobin Yvon LabRAM HR) was used, the wavelength of the light source was 532 nm, and the test range was 0 cm -1 ~4000cm -1 The test was performed on a negative electrode active material measuring 100 μm × 100 μm, and the -1 and 1580cm -1 The peak intensity around the peak was recorded. 100 values were taken for each group, and the average value of the ratio of the characteristic peak values of the D peak and the G peak, i.e., I D / I G The value was calculated.
[0071] 1.2 Rate characteristic test: The lithium ion battery formed in the following examples and comparative examples was left in a thermostat at 45°C ± 2°C for 2 hours, charged to 4.45V at a constant current of 0.5C, then charged to 0.025C at a constant voltage of 4.45V, left for 5 minutes, and discharged to 3.0V at a constant current of 0.2C. This is the initial capacity, and the discharge capacity of the first cycle of the lithium ion battery was recorded. Then, it was charged to 4.45V at a constant current of 0.5C, and discharged to 3.0V at a constant current of 2C, and the discharge capacity was recorded. The gram capacity of the negative electrode active material was calculated from the initial capacity, and the ratio of the discharge capacity of 2C to the initial capacity was calculated as the initial efficiency of the negative electrode active material.
[0072] 1.3 Cycle characteristic test: The lithium ion batteries formed in the following examples and comparative examples were left in a thermostat at 25°C ± 2°C for 2 hours, charged to 4.45V at a constant current of 0.5C, charged to 0.025C at a constant voltage of 4.45V, left for 5 minutes, and then discharged to 3.0V at a constant current of 0.3C. This is one charge-discharge cycle process, and the discharge capacity of the first cycle of the lithium ion battery was recorded. Thereafter, the charge-discharge cycle process was repeated according to the above method, and the ratio of the discharge capacity to the first discharge capacity was recorded to obtain a capacity change curve graph.
[0073] Four lithium-ion batteries were taken from each group, and the average capacity retention rate of the lithium-ion batteries was calculated. The cycle capacity retention rate of the lithium-ion battery = discharge capacity (mAh) at the 400th cycle / discharge capacity (mAh) after the first cycle × 100%.
[0074] 1.4 Cyclic thickness expansion test: The thickness of the lithium-ion battery was measured using a 600g flat plate thickness gauge (ELASTOCON, EV01).
[0075] The lithium ion batteries formed in the following examples and comparative examples were left in a thermostat at 25°C ± 2°C for 2 hours, charged to 4.45V at a constant current of 0.7C, then charged to 0.05C at a constant voltage of 4.45V and left for 15 minutes, the thickness of the fully charged lithium ion battery was recorded, and then discharged to 3.0V at a constant current of 0.5C. This is one charge-discharge cycle process, and the thickness of the lithium ion battery in the first cycle of the lithium ion battery was recorded. After that, the charge-discharge cycle process was repeated 400 times according to the above method, and the thickness of the lithium ion battery after 400 cycles was recorded.
[0076] Four lithium-ion batteries were taken from each group, and the average cycling thickness expansion rate of the lithium-ion batteries was calculated: cycling thickness expansion rate of lithium-ion batteries = (lithium-ion battery thickness at the 400th cycle / lithium-ion battery thickness at the first cycle - 1) x 100%.
[0077] 2. Manufacturing method 2.1 Manufacturing of the positive electrode The positive electrode active material lithium cobalt oxide (LiCoO2), conductive carbon black (SuperP), and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 0.75, which was then uniformly stirred. The slurry was uniformly applied to an aluminum foil positive electrode current collector and dried at 90°C. Then, a positive electrode was obtained after cold pressing, cutting, and slitting processes.
[0078] 2.2 Preparation of electrolyte In an environment with a water content of less than 150 ppm (dry argon atmosphere), a solution prepared by mixing a lithium salt, LiPF6, and an organic solvent (ethylene carbonate (EC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): vinylene carbonate (VC) = 20:30:20:28:2, mass ratio) in a mass ratio of 8:92 was used as the electrolyte for the lithium-ion battery.
[0079] 2.3 Manufacturing of the negative electrode A copper foil was used as the negative electrode current collector, and the negative electrode active material provided in the following examples or comparative examples and graphite were mixed in an equal mass ratio (1:1) to obtain a mixed powder with a designed mixed gram capacity of 850 mAh / g. The mixed powder, acetylene black, and polyacrylic acid (PAA) were thoroughly mixed in a deionized water solvent system in a weight ratio of 95:1.2:3.8 until homogeneous to form a negative electrode active material slurry. Then, one layer of the negative electrode active material slurry was uniformly applied to the surface of the copper foil and dried at 90°C. Then, after performing cold pressing, cutting, and slitting processes, the negative electrode was manufactured by drying in a vacuum at 85°C for 4 hours.
[0080] 2.4 Lithium-ion battery manufacturing A 15 μm thick polyethylene film was used as the separator, and the positive electrode, separator, and negative electrode were stacked in this order so that the separator was interposed between the positive electrode and the negative electrode to play a role of isolation. The stacked electrode assembly was heated at 80° C. to remove moisture, and a dried electrode assembly was obtained. The dried electrode assembly was placed in an outer casing, and the prepared electrolyte was injected, sealed, and subjected to processes such as formation, degassing, and side cutting, to obtain a lithium-ion battery.
[0081] 2.5 Preparation of negative electrode active material Example 1 (1) Carbon nanotube raw material was mixed with ethanol to prepare an ethanol dispersion having a carbon nanotube concentration of 3.3 wt %.
[0082] (2) A precursor of a magnesium-doped carbon silicon oxygen material is mixed and stirred uniformly with the ethanol dispersion, and the precursor is mixed with the magnesium-doped carbon silicon oxygen material having the general formula: Mg 0.14 Silicon Carbide 0.25 O 0.77The magnesium raw material (magnesium powder), carbon raw material (acetylene gas), and silicon oxygen raw material were mixed in a stoichiometric ratio of 2:1:10 by weight. The mixture of the precursor of the magnesium-doped carbon silicon oxygen material and the ethanol dispersion was evaporated to dryness, and the dry powder was collected.
[0083] (3) The collected dried powder was subjected to high-temperature treatment under argon atmosphere to obtain magnesium-doped carbon silicon oxygen material, where the high-temperature treatment temperature was about 600°C and the time was 3h.
[0084] Examples 2 and 3 In step (1), the manufacturing method is almost the same as that in Example 1, except that the carbon nanotube concentration in the ethanol dispersion is different. For details, see the table of examples below.
[0085] Examples 4 to 7 In step (3), except for the temperature of the high-temperature treatment, the manufacturing method is almost the same as that of Example 1. For details, see the table of Examples below.
[0086] Examples 8 and 9 In step (3), except for the time of the high-temperature treatment, the manufacturing method is almost the same as that of Example 3. For details, see the table of examples below.
[0087] Comparative Example 1 The precursor of the magnesium-doped carbon silicon oxygen material was treated at high temperature under an argon atmosphere to obtain a magnesium-doped carbon silicon oxygen material. The precursor has the general formula of the magnesium-doped carbon silicon oxygen material: Mg 0.14 Silicon Carbide 0.18 O 0.8 The magnesium raw material (magnesium powder), carbon raw material (acetylene gas), and silicon-oxygen raw material were mixed in a stoichiometric ratio of 2:1:10 by weight, and the high-temperature treatment was performed at a temperature of approximately 600°C for 3 hours.
[0088] 3. Comparison results 3.1 Comparison of negative electrode active material compositions The lithium ion batteries of Examples 1 to 9 and Comparative Example 1 are distinguished from each other by the composition of the negative electrode active material (after the carbon nanotube coating layer is disposed) and its precursor (without the carbon nanotube coating layer disposed) used therein. The composition of the precursor of the negative electrode active material and the results of the component test and Raman test for the magnesium-doped carbon silicon oxygen material are shown in Table 1 below.
[0089] [Table 1]
[0090] N / A indicates no corresponding value.
[0091] As can be seen from Table 1, the present invention can effectively form a carbon nanotube coating layer on the surface of the crystalline oxide of the negative electrode active material particles by a manufacturing process using an ethanol dispersion. As a result, the manufactured negative electrode active material powder has a higher carbon content than the negative electrode active material before manufacturing. As can be seen from Examples 1 to 3, the thickness of the carbon nanotube coating layer can be controlled by adjusting the carbon nanotube concentration in the ethanol dispersion. And, as can be seen from the results of the Raman test, the thickness of the carbon nanotube coating layer affects the stability and conductivity of its carbon structure.
[0092] As can be seen from Examples 1 and 4 to 9, the coating structure of the carbon nanotube coating layer can be affected by the temperature and time of the high-temperature treatment. As can be seen from the results of the Raman test, when the temperature of the high-temperature treatment decreases, the carbonization degree of the carbon nanotube coating layer decreases, and the disorder degree and defects of the carbon structure of the carbon nanotube coating layer increase. When the temperature of the high-temperature treatment increases, the carbonization degree of the carbon nanotube coating layer increases, and the disorder degree and defects of the carbon structure of the carbon nanotube coating layer decrease.
[0093] 3.2 Comparison of electrochemical device performance The results of the rate test, cycle characteristic test, and cycle thickness expansion rate test for the lithium ion batteries of Examples 1 to 9 and Comparative Example 1 are shown in Table 2 below.
[0094] [Table 2]
[0095] Referring to Table 2, the magnesium-doped carbon silicon oxygen material according to the embodiment of the present invention has excellent initial coulombic efficiency and cycle characteristics. The present invention further dopes carbon into magnesium-doped silicon oxide, thereby improving the cycle effect of the negative electrode active material, reducing the cycle thickness expansion rate after a high number of cycles, and lengthening the cycle life. Further comparing the embodiment and Comparative Example 1, FIG. 4 is a comparison diagram between the cycle capacity curve 201 of Example 1 of the present invention and the cycle capacity curve 202 of the electrochemical device of Comparative Example 1. As shown in FIG. 4, Example 1 of the present invention includes a magnesium-doped carbon silicon oxygen material with a carbon nanotube coating layer, and by providing a specific carbon nanotube coating layer, the cycle capacity retention rate of the negative electrode active material can be improved and the cycle thickness expansion rate can be greatly reduced, so that the electrochemical device can have excellent initial coulombic efficiency and cycle characteristics.
[0096] As can be seen from Examples 1 to 3, when the carbon nanotube coating layer is thin, the coating layer is not dense and cannot effectively form a continuous and uniform conductive network, resulting in a decrease in the cycle retention rate of the material.When the carbon nanotube coating layer is thick, the accumulation of by-products increases, and the consumption of electrolyte and active lithium increases, resulting in a decrease in the cycle retention rate of the material and a decrease in the initial conductive efficiency of the material.
[0097] As can be seen from Examples 4 to 9, when the sintering temperature is decreased, the carbonization degree of the magnesium-doped carbon silicon oxygen material is decreased, which increases the defects of the coating layer, and the I D / I GAs the sintering temperature increases, the carbonization degree of the magnesium-doped carbon silicon oxygen material increases, which reduces the defects of the coating layer and reduces the I D / I G The value of the SiO2 content decreases and the electronic conduction performance of the conductive network improves. However, as the temperature increases, the silicate phase in the carbon-doped silicon material increases, which reduces the initial efficiency. The increase in the silicate phase also reduces the structural stability of the material, which reduces the cycle retention.
[0098] Throughout the specification, references to "in embodiments," "some embodiments," "one embodiment," "another example," "example," "particular example," or "some examples" mean that at least one embodiment or example of the invention includes a particular feature, structure, material, or characteristic described in that embodiment or example. Thus, references in various places in the specification to, for example, "in some embodiments," "in an embodiment," "in another example," "in one example," "in a particular example," or "example" do not necessarily refer to the same embodiment or example herein. Furthermore, particular features, structures, materials, or characteristics described herein may be incorporated in any suitable manner into one or more embodiments or examples.
[0099] Although exemplary embodiments have been shown and described, those skilled in the art should not construe the above-described embodiments as limitations on the present application, and may change, substitute, or modify the embodiments without departing from the spirit, principles, and scope of the present application.
Claims
1. a negative electrode including a negative electrode active material layer, the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a magnesium-doped silicon carbide material; An electrochemical device having a carbon nanotube coating disposed on a surface of the crystalline oxide of the magnesium doped carbon silicon oxygen material.
2. The general formula of the crystalline oxide of the magnesium doped carbon silicon oxygen material is Mg z SiC x O y 2. The electrochemical device of claim 1, wherein x, y, and z satisfy 0<x<0.3, 0.4<y<1.0, and 0.1<z<0.
2.
3. 2. The electrochemical device of claim 1, wherein in the magnesium doped carbon silicon oxygen material, the molar silicon content is between 40% and 70%, the molar carbon content is between 3.5% and 24%, and the molar magnesium content is between 7.0% and 7.5%.
4. 2. The electrochemical device of claim 1, wherein the magnesium doped carbon silicon oxygen material has a molar ratio of magnesium to silicon of 0.1 to 0.2 and a molar ratio of magnesium to carbon of 0.2 to 10.
0.
5. I in the Raman spectrum of the magnesium-doped carbon silicon oxygen material D / I G The electrochemical device of claim 1, wherein the value is between 0.023 and 0.
32.
6. I in the Raman spectrum of the magnesium doped carbon silicon oxygen material versus the molar carbon content D / I G 6. The electrochemical device according to claim 3, wherein the ratio of the values is from 0.095 to 6.
78.
7. The carbon nanotube coating layer is (1) the thickness of the carbon nanotube coating layer is 0.5 nm to 5.0 μm; (2) the carbon nanotube coating layer includes carbon nanotube clusters, the carbon nanotube clusters extend from a surface of the carbon nanotube coating layer, and the length of the carbon nanotube clusters is 0.1 μm to 1.0 μm; The electrochemical device according to claim 1 , wherein at least one of the following is satisfied:
8. The magnesium doped carbon silicon oxygen material is (1) the magnesium doped carbon silicon oxygen material has a particle size Dv50 of 2.5 μm to 10.0 μm; (2) the particle size distribution of the magnesium-doped carbide silicon oxygen material satisfies 0.3≦Dn10 / Dv50≦0.6; (3) The magnesium-doped carbon silicon oxygen material has a specific surface area of 1 m 2 / g to 50m 2 / g and The electrochemical device according to claim 1 , wherein at least one of the following is satisfied:
9. The negative electrode active material layer further includes a binder, The binder comprises a synthetic rubber, the binder comprises one or more selected from the group consisting of polyacrylic acid ester, polyimide, polyamide, polyamideimide, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethylcellulose, potassium carboxymethylcellulose, sodium hydroxymethylcellulose, and potassium hydroxymethylcellulose; 2. The electrochemical device of claim 1, wherein the weight percentage of the binder is 2% to 6% based on the total weight of the negative electrode active material layer.
10. The electrolyte of the electrochemical device comprises an organic solvent and a lithium salt; The organic solvent includes one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate, vinylene carbonate, propyl propionate, and ethyl propionate; The lithium salt is lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 ), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF 3 SO 2 ) 2 ), lithium bis(fluorosulfonyl)imide (Li(N(SO 2 F) 2 )), lithium bis(oxalato)borate (LiB(C 2 O 4 ) 2 ) and lithium difluoro(oxalato)borate (LiBF 2 (C 2 O 4 2. The electrochemical device of claim 1 , comprising one or more selected from the group consisting of:
Citation Information
Patent Citations
Uniformly modified silicon-based composite material as well as preparation method and application thereof
CN113437271A
Negative active material for nonaqueous electrolyte secondary battery, its manufacturing method, and nonaqueous electrolyte secondary battery
JP2003197191A
Anode active material, anode including said anode active material, secondary battery including said anode, and method for producing said anode active material
JP2020518962A