Manufacturing method of superabsorbent resin
By employing a method that includes hydrothermal treatment to adsorb moisture on the dried superabsorbent resin, the generation of fine powder during pulverization is minimized, enhancing yield and safety in the production process.
Patent Information
- Application Number
- JP2024509454
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-21
- Filing Date
- 2023-06-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The production of superabsorbent resin is hindered by the generation of excessive fine powder during the pulverization step due to surface destruction of the dried body, leading to reduced yield and potential health hazards.
A method involving a water-soluble ethylenically unsaturated monomer, internal crosslinking agent, and polymerization initiator is used to form a hydrogel polymer, followed by drying, hydrothermal treatment to adsorb moisture, and subsequent pulverization, reducing surface destruction and fine powder generation.
The method effectively reduces fine powder generation, increases the yield of superabsorbent resin, and minimizes health risks by preventing surface destruction during pulverization.
Smart Images

Figure 2024541167000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0136874, filed on October 21, 2022, and all contents disclosed in the documents of said Korean patent application are incorporated by reference into this specification.
[0002] The present invention relates to a method for producing a superabsorbent resin, and more particularly to a method for producing a superabsorbent resin in which the amount of fine particles generated is reduced by a water addition treatment. [Background technology]
[0003] Super absorbent polymer (SAP) is a synthetic polymeric substance that has the ability to absorb about 500 to 1,000 times its own weight in water, and different developers give it different names, such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). Such super absorbent polymers have started to be put to practical use as sanitary products, and are currently widely used as soil water retention agents for horticulture, water stoppers for civil engineering and construction, seedling sheets, freshness maintaining agents in the food distribution field, and materials for steaming, and are mainly used in the field of sanitary materials such as diapers and sanitary napkins.
[0004] Meanwhile, among the series of steps for producing a superabsorbent polymer, there has been a problem in that the amount of fine powder generated increases due to surface destruction of the dried body during the pulverization step. If the fine powder is generated during the pulverization process, the yield of the superabsorbent polymer that is the final product may decrease, and the fine powder may be inhaled into the respiratory tract of the worker performing the pulverization step, causing health problems.
[0005] Therefore, there is a need for a method that can reduce the amount of fine powder generated when grinding is performed in the grinding step. Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a method for producing a superabsorbent resin capable of reducing the amount of fine powder generated in the grinding step in order to solve the problems mentioned in the background of the invention above. [Means for solving the problem]
[0007] According to one embodiment of the present invention for solving the above problems, there is provided a method for producing a superabsorbent polymer, the method including: supplying a composition including a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and polymerizing the composition to obtain a hydrous gel polymer; drying the hydrous gel polymer to obtain a dried substance; hydrating the dried substance to adsorb moisture into the dried substance; and pulverizing the hydrated dried substance to obtain a superabsorbent polymer. Effect of the Invention
[0008] According to the method for producing a superabsorbent polymer of the present invention, the dried body after drying can be subjected to a hydration treatment to adsorb moisture onto the dried body. The hydration treatment can increase the moisture content on the surface of the dried body, thereby preventing the surface of the dried body from being destroyed during pulverization. This can reduce the amount of fine powder generated due to the destruction of the surface of the dried body during the pulverization step. Furthermore, the reduction in the amount of fine powder generated can increase the yield of the superabsorbent polymer that is made into a final product. [Brief description of the drawings]
[0009] [Figure 1] 1 is a flow chart illustrating a method for producing a superabsorbent polymer according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The terms and words used in the description of the present invention and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0011] In order to facilitate understanding of the present invention, the present invention will now be described in more detail with reference to FIG.
[0012] A method for producing a superabsorbent polymer according to an embodiment of the present invention may include the steps of: supplying a composition including a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor, and polymerizing the composition to obtain a hydrous gel polymer; drying the hydrous gel polymer to obtain a dried body a; hydrating the dried body a to adsorb moisture into the dried body a; and pulverizing the hydrated dried body b to obtain a superabsorbent polymer.
[0013] First, the method for producing a superabsorbent resin according to one embodiment of the present invention can include a step of supplying a composition containing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and polymerizing the composition to obtain a hydrogel polymer. As described above, the composition can contain the water-soluble ethylenically unsaturated monomer, the internal crosslinking agent, and the polymerization initiator, and can further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, as necessary.
[0014] Here, the water-soluble ethylenically unsaturated monomer may be (meth)acrylic acid or a salt thereof. For example, when acrylic acid in which at least a part of acrylic acid is neutralized and an alkali metal salt thereof, which is a sodium salt thereof, are used as the water-soluble ethylenically unsaturated monomer, a highly water-absorbent resin having improved water absorption properties can be obtained.
[0015] In addition, the water-soluble ethylenically unsaturated monomer may be an anionic monomer such as maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamido-2-methylpropanesulfonic acid, or a salt thereof; a nonionic hydrophilic monomer such as (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and an amino group-containing unsaturated monomer such as (N,N)-dimethylaminoethyl (meth)acrylate, or (N,N)-dimethylaminopropyl (meth)acrylamide, or a quaternary product thereof. The salt of the anionic monomer may be a metal salt, a divalent metal salt, an ammonium salt, or an organic amine salt.
[0016] The water-soluble ethylenically unsaturated monomer may include at least a partially neutralized acidic group. The water-soluble ethylenically unsaturated monomer including at least a partially neutralized acidic group may be prepared by neutralizing the acidic group of the water-soluble ethylenically unsaturated monomer using a neutralizing agent. Here, the neutralizing agent may be a basic substance such as sodium hydroxide (or caustic soda), potassium hydroxide, or ammonium hydroxide that can neutralize the acidic group.
[0017] Meanwhile, the internal crosslinking agent can crosslink and polymerize the unsaturated bonds of the water-soluble ethylenically unsaturated monomer.
[0018] The internal crosslinking agent may be a (meth)acrylate-based compound that undergoes a crosslinking reaction by a free-radical polymerization (FRP) reaction. Specifically, the internal crosslinking agent may be one or more compounds selected from the group consisting of ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. More specifically, the internal crosslinking agent may be one or more of ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, and polyethylene glycol di(meth)acrylate.
[0019] Meanwhile, in the composition, the polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator by UV irradiation depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by UV irradiation, and a certain amount of heat is generated as the polymerization reaction, which is an exothermic reaction, proceeds, so a thermal polymerization initiator may also be included.
[0020] The photopolymerization initiator may be a compound capable of forming a radical by light such as ultraviolet light. The photopolymerization initiator may be at least one selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acyl phosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate.
[0021] The thermal polymerization initiator may be one or more selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid.Specific examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8).
[0022] Specifically, polymerization methods are broadly classified into thermal polymerization and photopolymerization depending on the polymerization energy source. Thermal polymerization can be carried out in a polymerization reactor having a stirring shaft such as a kneader, and photopolymerization can be carried out in a polymerization reactor equipped with a movable conveyor belt.
[0023] The hydrogel polymer of the present invention can be prepared by a polymerization reaction carried out by supplying a composition containing a water-soluble ethylenically unsaturated monomer, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor, and in the composition, the internal crosslinking agent can be 0.01 to 5 parts by weight relative to 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.2 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less relative to 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the internal crosslinking agent is too low, crosslinking may not be sufficient, making it difficult to achieve strength above an appropriate level, and if the content of the upper internal crosslinking agent is too high, the internal crosslinking density may be high, making it difficult to achieve the desired water retention ability.
[0024] The composition of the present invention may be prepared in the form of a solution dissolved in a solvent. Here, the solvent that can dissolve the above-mentioned raw materials may be used. For example, the solvent may be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.
[0025] Next, the hydrogel polymer formed by the polymerization reaction of the composition may be dried, crushed and classified. Here, in order to increase the efficiency of drying the hydrogel polymer, a coarse crushing step may be further performed. The crusher used in the coarse crushing step may be any one selected from the group of crushers consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper and a disc cutter.
[0026] Meanwhile, referring to the flow chart of Fig. 1, the method for producing a superabsorbent resin of the present invention can include a step of drying the hydrogel polymer that has been coarsely pulverized as described above or that has not been subjected to the coarse pulverization step to obtain a dried body A. The drying method of the drying step can be specifically performed by a method of hot air supply, infrared radiation, ultrashort wave radiation, or ultraviolet radiation, and the dried body A can be obtained by performing the drying step by the drying method.
[0027] Here, the moisture content of the dried body a may be 2 to 9% by weight. More specifically, it may be 3 to 7% by weight or 4 to 6% by weight. Here, the moisture content of the dried body a may mean the moisture content of the dried body a that has been subjected to a drying step but has not been subjected to a subsequent hydration treatment. If the moisture content of the dried body is less than 2% by weight, the dried body may be in an overdried state, and the content of fine powder in the dried body may increase excessively. If the moisture content of the dried body is more than 9% by weight, the dried body is considered to be in an undried state, and when the dried body is subjected to a hydration treatment and introduced into the next pulverization step, pulverization may not proceed.
[0028] The method for producing a superabsorbent resin according to one embodiment of the present invention may include a step of hydrating the dried body a to adsorb moisture to the dried body a. Specifically, a certain amount of moisture is adsorbed on the surface of the dried body a by the hydration treatment, thereby obtaining a hydrated dried body b.
[0029] The hydration treatment can be carried out under conditions of 15° C. to 70° C., specifically, 20° C. to 40° C. This allows an appropriate amount of moisture to be maintained on the surface of the dried body a, enabling smooth hydration treatment. Specifically, when the hydration treatment is carried out by spray hydration, the hydration treatment temperature can be the temperature of the droplets.
[0030] The hydration treatment is carried out under the above conditions, and as a means for creating this atmosphere, for example, a method of directly spraying water can be used. By such hydration treatment, water can be adsorbed on the surface of the dried body a. The water adsorbed on the surface of the dried body b thus hydrated can be diffused and absorbed inside over time.
[0031] The amount of moisture adsorbed in the dry material a by the hydration treatment may be 1% by weight or more, 2% by weight or more, or 3% by weight or more, and 10% by weight or less, 7% by weight or less, or 5% by weight or less, based on 100% by weight of the dry material a. The amount of moisture adsorption may refer to the amount of moisture adsorbed in the dry material a by the hydration treatment. When the moisture is adsorbed in the dry material a within the above range, the moisture content of the hydration-treated dry material b can reach a desired level in the present invention. Here, the amount of moisture adsorption may be measured according to the International Organization for Standardization (ISO) 171904-4:2001 method.
[0032] Meanwhile, the moisture content of the hydrated dried body b may be 5 wt% or more, 6 wt% or more, or 9 wt% or more, and 15 wt% or less, 13 wt% or less, or 11 wt% or less. Here, the moisture content of the hydrated dried body b may mean the moisture content of the hydrated dried body b that has been subjected to the hydration treatment but has not been subjected to the subsequent pulverization step. When the moisture content of the hydrated dried body b is within the above range, the amount of fine powder generated in the pulverization step described below may be reduced to, for example, a level of less than 20%. Therefore, the moisture content of the hydrated dried body b may be controlled within the above range by adjusting the amount of moisture adsorbed by the dried body a during the hydration treatment.
[0033] If the moisture content of the hydrated dry body b is less than 5 wt%, it may be difficult to reduce the generation of fine powder during pulverization as intended in the present invention. If the moisture content of the hydrated dry body b is more than 15 wt%, the moisture content of the hydrated dry body b may be too high, making it impossible to pulverize in the pulverization step. Here, the moisture content can be measured by a moisture meter (AND MX_50).
[0034] According to an embodiment of the present invention, the method may include a step of pulverizing the hydrated dried body b to obtain a superabsorbent polymer. The pulverization step may be performed once, but may be performed one or more times. When a conventional dry body that has not been hydrated is pulverized, the surface of the dry body is destroyed, resulting in excessive generation of fine powder. Usually, the fine powder has a particle size (D50) of less than 150 μm, which may be inappropriate for commercialization as a superabsorbent polymer. Here, the particle size (D50) may refer to the particle size at the 50% point of the cumulative particle number distribution according to the particle size. Therefore, the more the amount of fine powder generated in the pulverization step increases, the lower the yield of the superabsorbent polymer may be. However, in the present invention, by performing a hydration treatment before the pulverization step, moisture is adsorbed on the surface of the dried body a, and the surface destruction of the hydrated dried body b by the moisture can be suppressed. As a result, the amount of fine powder generated during pulverization can be reduced, and the yield of the superabsorbent polymer can be increased.
[0035] Meanwhile, the pulverizer used in the pulverizing step may be, specifically, a ball mill, a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, or a jog mill.
[0036] According to one embodiment of the present invention, the step of obtaining a superabsorbent resin by pulverizing the hydrated dried body b may be performed immediately after the hydration of the dried body a or within 24 hours after the hydration. The term "immediately after the hydration" may mean the end of the hydration or the minimum time required for the pulverization step after the hydration. In this way, the moisture content of the surface of the hydrated dried body b may be higher immediately after the hydration, and thus, when the pulverization step is performed immediately after the hydration, the surface destruction of the hydrated dried body b can be prevented and the desired result can be obtained. Therefore, even if the amount of moisture adsorption during the hydration is relatively small, for example, 1% by weight to 3% by weight, when the pulverization step is performed immediately after the hydration, the moisture is not diffused from the surface of the hydrated dried body b to the inside, so that the amount of fine powder generated during pulverization may be reduced.
[0037] Meanwhile, after the hydration treatment, the moisture present on the surface of the hydration-treated dried body b may diffuse into the interior as time passes. However, if the amount of moisture adsorbed on the dried body a during the hydration treatment is relatively high, for example, 4% by weight to 10% by weight, the amount of moisture remaining on the surface of the hydration-treated dried body b may be maintained high even if the hydration-treated dried body b is stabilized for a predetermined time. Therefore, when a grinding step is performed after the stabilization process, surface destruction of the hydration-treated dried body b may be prevented, and the amount of fine powder generation may be reduced. Here, the stabilization may mean, for example, aging the hydration-treated dried body b for a predetermined time in a humid atmosphere in a sealed container.
[0038] Meanwhile, after the pulverization step, a separate process of classification according to an appropriate particle size may be performed in order to control the physical properties of the superabsorbent polymer to be manufactured as a final product. Furthermore, the classification may be performed after each pulverization.
[0039] Here, the appropriate particle size (D50) may be a particle size of 150 μm to 850 μm, and particles having such a particle size may be classified as normal particles. Meanwhile, as described above, particles having a particle size of less than 150 μm may be classified as fine powder. Such particle size may be measured according to the EDANA WSP 220.3 method, a standard of the European Disposables and Nonwovens Association (EDANA).
[0040] Through such a series of grinding steps, normal particles, i.e., highly water-absorbent polymer, can be produced.
[0041] Next, if necessary, the method may further include a step of surface-crosslinking the produced superabsorbent resin in the presence of a surface crosslinking agent to produce a superabsorbent resin having a surface crosslinked layer formed on at least a part of the surface. Here, the surface crosslinked layer may be produced from a surface crosslinking agent, the surface crosslinking agent may include a polyfunctional epoxy compound, and the polyfunctional epoxy compound may be a glycidyl ether compound of a polyhydric alcohol.
[0042] Specifically, the surface cross-linking agent may include one or more polyfunctional epoxy compounds selected from the group consisting of ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, glycerin polyglycidyl ether, and sorbitol polyglycidyl ether.
[0043] The surface cross-linking agent can be mixed with the superabsorbent resin in a solution state, specifically, in a surface cross-linking solution state dissolved in a solvent. The surface cross-linking solution can contain water and methanol in addition to the surface cross-linking agent. In general, the surface cross-linking solution is applied to the surface of the superabsorbent resin. Thus, the surface cross-linking reaction is carried out on the surface of the superabsorbent resin, which improves the cross-linking property on the surface of the particle without substantially affecting the inside of the particle. Thus, the surface cross-linked superabsorbent resin has a higher degree of cross-linking near the surface than in the inside. The surface cross-linking reaction and drying can be carried out simultaneously by heating the superabsorbent resin to which the surface cross-linking agent has been added.
[0044] The present invention will be described in more detail with reference to the following examples. However, the following examples are merely for the purpose of illustrating the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of the present invention, and the scope of the present invention is not limited thereto.
[0045] Working Example Example 1 In a 3 L glass container equipped with a stirrer and a thermometer, 100 g of acrylic acid, 0.16 g of polyethylene glycol diacrylate (PEGDA) as an internal crosslinking agent, 0.008 g of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide as a photopolymerization initiator, 0.12 g of sodium persulfate as a thermal polymerization initiator, and 123.5 g of caustic soda (NaOH) solution as a neutralizing agent were mixed at room temperature to a solid content of 45.0 wt %, to prepare a composition.
[0046] Next, the composition was supplied at a rate of 500 to 2000 mL / min onto a conveyor belt having a width of 10 cm and a length of 2 m, which was moving at a speed of 10 cm / min. 2 The mixture was irradiated with ultraviolet light having an intensity of 1000 nm for 60 seconds to carry out a polymerization reaction, thereby obtaining a hydrogel polymer.
[0047] Next, the hydrogel polymer was roughly pulverized using a chopper. The pulverized hydrogel polymer was then dried for 30 minutes with hot air at 185°C using an air-flow oven. As a result, 100 g of a dried product with a moisture content of 5% by weight was obtained.
[0048] The dried body was evenly spread on a SUS tray of 320 mm x 200 mm x 50 mm, and 3.2 g of water was sprayed to add moisture. As a result, the amount of moisture adsorbed on the dried body was 3 wt% based on 100 wt% of the dried body, and the amount of moisture adsorption was measured according to the International Organization for Standardization (ISO) 17190-4:2001 method. The moisture content of the dried body hydrated by spraying moisture in this manner was 8 wt%. Next, the hydrated dried body was placed in a sealed container and mixed by stirring. Then, a stabilization process was carried out in the sealed container for 24 hours.
[0049] After stabilization in such a sealed container, the hydrated dried body was pulverized in a roll mill to obtain a pulverized material. The pulverized material was placed in a mesh set consisting of ASTM meshes #6, #10, #20, #25, #30, #40, #50, #70, #80, and #100, and the mesh set was attached to a sieve shaker. The sieve shaker was operated for 10 minutes at an amplitude of 1.5 mm to classify the pulverized material. As a result, a highly water-absorbent resin having a particle size of 150 μm to 850 μm was obtained.
[0050] Example 2 A superabsorbent resin was produced in the same manner as in Example 1, except that 5.8 g of water (water adsorption amount is 5 wt% relative to 100 wt% of the dried body) was sprayed onto the dried body to add water, so that the water content of the hydrated dried body became 10 wt%.
[0051] Example 3 A superabsorbent resin was produced in the same manner as in Example 1, except that 11 g of water (water adsorption amount is 10 wt% relative to 100 wt% of the dried body) was sprayed onto the dried body to add water, so that the water content of the hydrated dried body became 15 wt%.
[0052] Example 4 In Example 1, 1.1 g of water (water adsorption amount is 1 wt% for 100 wt% of dried material) was sprayed onto the dried material to add water, so that the water content of the hydrated dried material became 6 wt%, and the stabilization process of the hydrated dried material was omitted, and the material was pulverized immediately after the hydration treatment. A superabsorbent resin was produced in the same manner as in Example 1.
[0053] Example 5 In Example 1, 1.1 g of water (water adsorption amount is 1 wt% for 100 wt% of dried body) was sprayed onto the dried body to obtain a water content of 6 wt%. A stabilization process of the hydrated dried body was carried out for 1 hour. The same method as in Example 1 was used to produce a superabsorbent resin.
[0054] Example 6 In Example 1, 3.2 g of water (water adsorption amount is 3 wt% relative to 100 wt% of the dried material) was sprayed onto the dried material having a moisture content of 2 wt%, so that the moisture content of the hydrated dried material became 5 wt%, and the stabilization process of the hydrated dried material was omitted, and the material was pulverized immediately after the hydration treatment. Except for this, a superabsorbent resin was produced in the same manner as in Example 1.
[0055] Example 7 A superabsorbent resin was produced in the same manner as in Example 1, except that 18 g of water (water adsorption amount is 15 wt% relative to 100 wt% of the dried body) was sprayed onto the dried body to add water, and the water content of the hydrated dried body became 20 wt%.
[0056] Example 8 A superabsorbent resin was produced in the same manner as in Example 1, except that 26 g of water (water adsorption amount is 20 wt% relative to 100 wt% of the dried body) was sprayed onto the dried body to add water, and the water content of the hydrated dried body became 25 wt%.
[0057] Comparative Example Comparative Example 1 A highly water-absorbent resin was produced in the same manner as in Example 1, except that the dried product was not hydrated and was immediately pulverized.
[0058] Comparative Example 2 A highly water-absorbent resin was produced in the same manner as in Example 1, except that the dried product having a moisture content of 2% by weight was not subjected to a moisture treatment but was immediately pulverized.
[0059] Comparative Example 3 A highly water-absorbent resin was produced in the same manner as in Example 1, except that the dried product having a moisture content of 10% by weight was not subjected to a moisture treatment but was immediately pulverized.
[0060] Experimental Example The superabsorbent resins produced in the above Examples and Comparative Examples were measured by the following methods, and the results are shown in Table 1 below.
[0061] 1) Moisture content The moisture content may refer to the moisture content of the hydrated dried body after hydration and before pulverization when the hydration treatment is performed (Example), and may refer to the moisture content of the dried body after drying and before pulverization when the hydration treatment is not performed (Comparative Example). Specifically, the moisture content is measured from the change in weight caused by heating the hydrated dried body or dried body with a halogen lamp (400W) in a moisture meter (AND MX_50) to evaporate the moisture. Specifically, the moisture content was measured according to the following procedure.
[0062] (i) Set the measurement conditions of the moisture meter (heating temperature: 180°C, heating time: 40 minutes). (ii) With no sample present on the sample pan, adjust the weight to zero (0). (iii) A sample of 5 g (error: 0.02%) is taken from the hydrated dried body or dried body and loaded evenly onto the sample pan. (iv) After the measurement is completed, check the moisture content.
[0063] 2) Amount of fine powder generated The amount of fine powder generated may refer to the amount of fine powder having a particle size of less than 150 μm contained in the pulverized product pulverized in the pulverization step. Specifically, the amount of fine powder generated was measured by the following method.
[0064] First, 100 g of the pulverized material obtained in the examples and comparative examples was sampled as a sample and put into a mesh set consisting of ASTM meshes #6, #10, #20, #25, #30, #40, #50, #70 and #100. The mesh set was attached to a sieve shaker and operated for 10 minutes at an amplitude of 1.5 mm to classify the pulverized material according to particle size for each mesh. Then, the mesh ratio corresponding to each mesh was calculated according to the following mathematical formula 1.
[0065]
number
[0066] Next, the ratio of meshes of the pulverized material that fell under #100 (particle size less than 150 μm) was added up to measure the amount of fine powder generated.
[0067] 3) Particle size The particle size was measured by measuring the particle size of the pulverized material, and was calculated according to the following mathematical formula 2, in the same manner as in the method for measuring the "amount of fine powder generated" described above, by classifying the pulverized material (100 g) using a mesh set.
[0068]
number
[0069] Here, the meshes (#40-100) are the meshes #40-#100 included in the above mesh set, and the mesh ratio is the mesh ratio according to the above mathematical formula 1. That is, the grain size is the result of arithmetically calculating the average grain size based on the mesh ratio of meshes #40-#100.
[0070] [Table 1]
[0071] Referring to Table 1, in the case of the Example in which the hydration treatment was performed after the dried body was made to adsorb moisture, it was confirmed that the amount of fine powder generated due to surface destruction occurring in the pulverization step was reduced because moisture was adsorbed on the surface of the dried body by the hydration treatment. In addition, it was confirmed that the amount of fine powder generated was smaller in Examples 1 to 5 in which the hydration treatment was performed on a dried body with the same moisture content as that of Comparative Example 1 in which the hydration treatment step was not performed on a dried body having a moisture content of 5% by weight.
[0072] However, in Examples 7 and 8, a large amount of water was adsorbed onto the dried material during the hydration treatment, resulting in a moisture content that far exceeded the moisture content range of the hydration-treated dried material to be obtained in the present invention, and it was confirmed that pulverization was impossible in the pulverization step.
[0073] On the other hand, Comparative Example 1 is a superabsorbent resin obtained by pulverizing a dried body with a moisture content of 5% by weight that was not subjected to a hydration treatment step, and it was confirmed that the amount of fine powder generated was significantly increased compared to Examples 1 to 5. In Examples 1 to 5, a dried body with the same moisture content as Comparative Example 1 was hydrated and pulverized, but in Comparative Example 1, no hydration treatment was performed, and it was confirmed that the pulverization step was performed, destroying the surface of the dried body and increasing the amount of fine powder generated.
[0074] In addition, Comparative Example 2 is a superabsorbent resin obtained by pulverizing a dried body with a moisture content of 2% by weight that was not subjected to a moisture treatment step, and it was confirmed that the amount of fine powder generated was increased compared to Example 6 in which a dried body with the same moisture content was subjected to moisture treatment. As described above, it was confirmed that the amount of fine powder generated can be improved for dried bodies with the same moisture content depending on whether or not a moisture treatment step is performed.
[0075] On the other hand, in Comparative Example 3, a hydration treatment step was not performed, and a dried body with a moisture content of 10% by weight was pulverized, but it was confirmed that pulverization was impossible. In this way, when the moisture content of the dried body is high, the hydrogel polymer may be in a wet state in the drying step, and when it is introduced into the pulverization step in this wet state, pulverization may be impossible as in Comparative Example 3.
Claims
1. A method for producing a hydrous gel polymer by feeding a composition including a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator into a polymerization reactor and carrying out a polymerization reaction therein; drying the hydrogel polymer to obtain a dry body; A step of hydrating the dried body to adsorb moisture onto the dried body; and pulverizing the hydrated dried body to obtain a superabsorbent resin.
2. Before drying the hydrogel polymer, The method for producing a highly water-absorbent resin according to claim 1, further comprising a step of coarsely pulverizing the hydrous gel polymer.
3. The step of pulverizing the hydrated dried body to obtain a superabsorbent resin includes: The method for producing a highly water-absorbent polymer according to claim 1 or 2, wherein the treatment is carried out immediately after the hydration treatment of the dried body or within 24 hours after the hydration treatment.
4. 2. The method for producing a highly water-absorbent resin according to claim 1, wherein the amount of water adsorbed by the dried body through the hydration treatment is 1% by weight to 10% by weight based on 100% by weight of the dried body.
5. The method for producing a highly water-absorbent resin according to claim 1 , wherein the hydration treatment is carried out by spraying water onto the dried body.
6. The method for producing a highly water-absorbent resin according to claim 1, wherein the hydration treatment is carried out under conditions of 15°C to 70°C.
7. The method for producing a highly water-absorbent polymer according to claim 1, wherein the moisture content of the dried body after the hydration treatment is 5% by weight to 15% by weight.
8. After the step of pulverizing the hydrated dried body to obtain a superabsorbent resin, surface cross-linking is performed in the presence of a surface cross-linking agent; The method for producing a highly water-absorbent resin according to claim 1, further comprising the step of forming a surface cross-linked layer on at least a portion of the surface.
9. 2. The method for producing a highly water-absorbent resin according to claim 1, wherein the internal crosslinking agent is one or more of ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, and polyethylene glycol di(meth)acrylate.
10. The method for producing a highly water-absorbent resin according to claim 1, wherein the water-soluble ethylenically unsaturated monomer is (meth)acrylic acid or a salt thereof.
Citation Information
Patent Citations
Method for producing particulate water-absorbing resin
JP2004051967A
Crushing-resistant superabsorbent resin and method for producing the same
JP2017505848A
Method for producing water-absorbing resin particle
JP2022088111A
Manufacturing method of superabsorbent resin
JP2022520790A
Method for preparing super absorbent polymer
KR1020180003815A