A method for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline
By employing a β-zeolite catalyst with W, Mo, Ni, and Co in a hydrogen atmosphere and controlling reaction temperatures, the method enhances 2-methylpyridine production efficiency and selectivity, overcoming conventional limitations.
Patent Information
- Application Number
- JP2024524605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-31
- Filing Date
- 2022-10-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-10-19
AI Technical Summary
Conventional methods for producing 2-methylpyridine from aniline suffer from low conversion rates and selectivity, making large-scale production difficult.
A method utilizing a β-zeolite catalyst supported with active metal components like W, Mo, Ni, and Co, in a hydrogen-containing atmosphere, with controlled reaction temperatures between 100°C to 240°C, allows for selective production of 2-methylpyridine and diphenylamine.
This approach achieves high conversion rates and selectivity for 2-methylpyridine, enabling efficient production using existing diphenylamine process equipment and avoiding the need for high ammonia gas concentrations.
Smart Images

Figure 2024541230000001_ABST
Abstract
Description
Detailed Description of the Invention
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of Chinese Patent Application No. 202111278790.6, filed on October 31, 2021, the contents of which are incorporated herein by reference.
[0002] [Technical field] The present invention relates to the field of fine chemicals, and specifically to a method for synthesizing 2-methylpyridine from aniline, and a method for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline.
[0003] [Background technology] 2-Methylpyridine, with the molecular formula C6H7N, is also known as α-methylpyridine and α-picoline. It is a kind of pyridine base. It is a colorless oily liquid with a strong unpleasant odor at room temperature. Its freezing point is -38.9℃, its boiling point is 129.5℃, it is highly toxic, and it is soluble in acetone, ethanol, ether and water. 2-Methylpyridine is an important chemical intermediate and an important raw material for fine chemicals. It can be used to produce long-acting sulfonamides, pesticide intermediates, and feed intermediates, as well as to synthesize special resin vinylpyridine and 2-vinylpyridine intermediates. The domestic consumption of 2-methylpyridine in China is increasing by about 25% every year, so the potential of the domestic market for 2-methylpyridine in China is very large.
[0004] The production of pyridine base in the industrial field mainly includes coal tar separation method and chemical synthesis method. The coal tar separation method not only has the disadvantages of serious pollution, small variety of products, high cost, low quality, high energy consumption, etc., but also has low product yield and is difficult to improve. The chemical synthesis method usually uses the ammonium-aldehyde condensation method, which synthesizes pyridine base by reacting aldehyde, ketone, and ammonia as raw materials. However, the products of the ammonium-aldehyde condensation method include 3-methylpyridine, 2-methylpyridine, 4-methylpyridine, etc., and there are problems such as difficulty in separating the products afterwards.
[0005] CN105384683A discloses a method for separating 2-methylpyridine and 4-methylpyridine, which are by-products in the synthesis of diphenylamine from aniline. The steps are as follows: Aniline is used as raw material, and is passed through a fixed-bed reactor filled with a molecular sieve catalyst. The temperature and pressure of the reactor are controlled, and the raw material is converted into diphenylamine, ammonia, and by-products such as 2-methylpyridine, 4-methylpyridine, water, acridine, and 4-aminobiphenyl through a condensation reaction. These mixed reaction liquids are rectified in multiple stages to obtain a low-boiling mixed fraction, which is dehydrated, the mixture after dehydration is dried, and the mixed liquid after drying is rectified to obtain 2-methylpyridine and 4-methylpyridine according to the difference in boiling point. This method is essentially a method for separating 2-methylpyridine and 4-methylpyridine, which are by-products in the conventional synthesis of diphenylamine from aniline. Therefore, in this method, 2-methylpyridine is by-produced during the reaction process, resulting in a low yield and making it impossible to mass-produce.
[0006] CA1190928A discloses a method for producing α-picoline from aniline, in which an aniline starting material is passed through an acidic zeolite catalyst at 200-650°C in the presence of an inert gas such as nitrogen or helium to produce an α-picoline-containing product. The reaction pressure is from normal pressure to 25000kPa, usually 200kPa, and the space velocity of aniline is preferably 0.2-5WHSV. The acidic zeolite is preferably of the hydrogen type, contains β-zeolite, and has a silica / alumina ratio of 10-100, and may reach 150. Among these, in Example 1, using pure HZSM-5, the aniline conversion was 13.1% and the selectivity to α-picoline was 51.6 under the conditions of 510°C, pressure 2860kPa, ammonia of 1.5 mol% of aniline, and nitrogen space velocity of 100GHSV.
[0007] "The zeolite-catalysed isomerization of aniline to a-picoline[J]. Applied catalysis A: General 172(1998)285-294" discloses a method for producing α-picoline by aniline rearrangement reaction. This method uses a molecular sieve as a catalyst, preferably Ga-MFI molecular sieve (superior to ZSM-5), and is carried out under the conditions of 673K, total pressure of 75 bar, and ammonia partial pressure of 5-60 bar, preferably 20-25 bar. In this process, the selectivity of α-picoline reaches 85% or more, but the conversion rate is only 3.7%.
[0008] Summary of the Invention [Problem to be solved by the invention] The technical problem to be solved by the present invention is to solve the drawbacks of the prior art, such as low conversion rate of aniline and low selectivity of 2-methylpyridine in the method for producing 2-methylpyridine by aniline rearrangement reaction, and to provide a method for selectively producing aniline and 2-methylpyridine based on the conventional apparatus for producing diphenylamine from aniline. The method of the present invention can easily and efficiently switch between the products of aniline and 2-methylpyridine by controlling the temperature, has mild reaction conditions, a high yield of 2-methylpyridine, and good reaction selectivity, and is expected to be industrialized.
[0009] The inventors of the present invention have discovered that the isomerization rearrangement reaction of aniline to produce 2-methylpyridine and the condensation reaction of aniline to produce diphenylamine are doubly affected by two factors: catalyst and reaction temperature. When the beta zeolite catalyst of the present invention carrying at least one active metal component selected from W, Mo, Ni, and Co is used, the reaction path of aniline can be switched between 2-methylpyridine and diphenylamine due to the change in the catalytic active center. In addition, the reaction temperature is low, which is more favorable for the synthesis of 2-methylpyridine. Based on this finding, the present invention proposes a method for producing 2-methylpyridine and a method for selectively and continuously producing aniline and 2-methylpyridine.
[0010] [Means for solving the problems] In a first aspect of the present invention, there is provided a method for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline, comprising a step of catalytically reacting aniline with a catalyst under a hydrogen-containing atmosphere at a temperature of 100 to 400°C, wherein the catalyst is a β zeolite carrying a metal component, the metal component containing at least one active metal component selected from W, Mo, Ni, and Co, and the temperature of the catalytic reaction is controlled to 100°C to 240°C in order to obtain a product mainly consisting of 2-methylpyridine, and the temperature of the catalytic reaction is controlled to 260°C to 400°C in order to obtain a product mainly consisting of diphenylamine.
[0011] In a second aspect of the present invention, there is provided a method for synthesizing 2-methylpyridine from aniline, comprising the step of catalytically reacting aniline with a catalyst under isomerization rearrangement reaction conditions in a hydrogen-containing atmosphere, the catalyst being a β zeolite carrying a metal component, the metal component including at least one active metal component selected from W, Mo, Ni, and Co, and the temperature of the catalytic reaction being 100°C to 240°C.
[0012] [Effects of the Invention] The method of the present invention for producing 2-methylpyridine has a high conversion rate of aniline and a high selectivity for the target product 2-methylpyridine. The reason for this is that the reaction mechanism is greatly changed by selecting a β zeolite catalyst containing at least one active metal selected from W, Mo, Ni, and Co under a hydrogen-containing atmosphere, and thermodynamic factors are one of the factors that affect the selectivity of 2-methylpyridine. At high temperatures, the main reaction is the condensation of two aniline molecules to form one diphenylamine molecule, but when the temperature is lowered, the main reaction is the isomerization rearrangement of aniline molecules to produce 2-methylpyridine. Therefore, the method of the present invention can achieve the purpose of producing 2-methylpyridine using aniline as a raw material, and can selectively produce diphenylamine and 2-methylpyridine using existing diphenylamine process equipment.
[0013] In the prior art, a large amount of ammonia gas is usually introduced in the synthesis of pyridine base compounds. The presence of ammonia gas occupies the acidic sites of the catalyst, reducing the catalytic activity. In addition, the high temperature and pressure also limit the industrial application of this method. On the other hand, the method according to the present invention does not require the introduction of a large amount of ammonia gas, and only requires the introduction of a small amount of hydrogen gas, and the reaction conditions are mild, the reaction raw material is only aniline, and high-purity 2-methylpyridine and high-purity diphenylamine can be obtained by the subsequent distillation operation.
[0014] BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is a relationship diagram showing the change in product distribution with temperature in the process for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline according to the present invention.
[0015] [Mode for carrying out the invention] The endpoints of the ranges and any values disclosed herein should be understood to be not limited to the exact ranges or values, but to include values close to these ranges or values. In the case of numerical ranges, the values between the endpoints of each range, between the endpoints of each range and the individual point values, and between the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0016] The method for synthesizing 2-methylpyridine from aniline according to the present invention includes a step of contacting aniline with a catalyst under isomerization rearrangement reaction conditions in a hydrogen-containing atmosphere, the catalyst being β zeolite carrying a metal component, the metal component including at least one active metal component selected from W, Mo, Ni, and Co, and the temperature of the contact reaction being 100°C to 240°C.
[0017] In the present invention, a higher aniline conversion rate was obtained and the selectivity for 2-methylpyridine was unexpectedly improved by controlling the reaction temperature in a hydrogen-containing atmosphere to be lower than the temperature required for the normal synthesis reaction of diphenylamine from aniline using β zeolite carrying at least one active metal component selected from W, Mo, Ni, and Co. In addition, diphenylamine and 2-methylpyridine can be selectively produced by adjusting the reaction temperature using the same apparatus and the same catalyst.
[0018] According to a preferred embodiment of the present invention, the content of the active metal component is 0.5 to 5 wt %, preferably 0.5 to 3 wt %, calculated as the metal element based on the total amount of the catalyst.
[0019] Preferably, the metal component further contains at least one auxiliary metal component selected from Li, Na, K, Mg, and Ca, and the content of the auxiliary metal component is 0 to 6.5 wt%, preferably 0.5 to 5.5 wt%, calculated in terms of the oxidation state based on the total amount of the catalyst.
[0020] The addition of the auxiliary metal component improves the acid distribution on the catalyst surface and the pore structure of the catalyst, thereby further improving the aniline conversion and the selectivity to the target product.
[0021] Although the mechanism is not yet clear, the present inventors have found that the above-mentioned effect of producing aniline or 2-methylpyridine as the main product by adjusting the temperature can be obtained only by supporting the above-mentioned metal components using β zeolite under a hydrogen-containing atmosphere, and that the above-mentioned effect cannot be obtained with other molecular sieves such as ZSM-5.
[0022] Preferably, the silica / alumina molar ratio of the β zeolite is 25-300, preferably 60-220.
[0023] Preferably, the catalyst has a specific surface area of 400 to 700 m 2 / g, preferably 450 to 650 m 2 / g, the pore volume is 0.25 to 0.6 mL / g, preferably 0.4 to 0.55 mL / g, the average pore diameter is 1.5 to 5 nm, preferably 2 to 4 nm, and the particle diameter is preferably less than 9 nm.
[0024] The catalyst may contain an alumina binder to obtain a shaped catalyst body.
[0025] According to a preferred embodiment of the present invention, the catalyst may contain, based on the total amount of the catalyst, 50-85 wt% of zeolite, 0.5-5 wt% of active metal components calculated as metal elements, 0-6.5 wt% of auxiliary metal components calculated as oxidation states, and 10-45 wt% of alumina binder. Preferably, the catalyst contains 60-85 wt% of zeolite, 0.5-3 wt% of active metal components calculated as metal elements, 0.5-5.5 wt% of auxiliary metal components calculated as oxidation states, and 15-34.5 wt% of alumina binder.
[0026] The catalyst is preferably in the form of strip-shaped or spherical particles. In the case of strip-shaped particles, the cross-sectional shape may be cylindrical, cloverleaf, four-leaf cloverleaf, etc., and the cross-sectional width of the strip-shaped particles is 0.5 to 3.0 mm, preferably 1.0 to 2.0 mm. In the case of spherical particles, the particle diameter is 0.5 to 5.0 mm, preferably 1.0 to 3.0 mm.
[0027] The above catalysts can be prepared using methods known to those skilled in the art or can be purchased commercially. For example, the catalyst of the present invention can be prepared by the following method: (1) Hβ zeolite is contacted with an aqueous solution of nitrates of the auxiliary metal components by equal volume impregnation. (2) The mixture obtained in step (1) is filtered, washed, and dried. (3) The modified Hβ zeolite obtained in step (2), alumina binder, and processing aids (e.g., extrusion aid, peptizer) are thoroughly kneaded, then molded, dried, and roasted. (4) NaBH4 is added to the aqueous nitric acid solution of the support and active metal components obtained in step (3), and the mixture is refluxed, filtered, and vacuum dried to produce the catalyst.
[0028] In step (1), the contact temperature is 80-100°C and the contact time is 3-6 hours, and in step (2), drying is performed at 60-120°C for 6-12 hours. In step (3), drying is performed at 60-120°C for 6-12 hours, followed by roasting at 450-550°C for 4-16 hours. In step (4), reflux reduction is performed at 80-100°C for 6-8 hours, followed by vacuum drying at 80-100°C for 6-12 hours.
[0029] In the present invention, by using the above catalyst, a high yield of 2-methylpyridine can be obtained at a low temperature in a hydrogen-containing atmosphere, not in a conventional ammonia gas atmosphere. Therefore, the contact reaction is preferably carried out without introducing ammonia gas. The hydrogen-containing atmosphere refers to an atmosphere in which the hydrogen concentration is 10 to 100% by volume.
[0030] Furthermore, the temperature of the contact reaction may be 100 to 240°C, specifically, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 199°C, 200°C, 210°C, 220°C, 230°C, 240°C, and any value within the range consisting of any two of these point values. A preferred reaction temperature is 130 to 180°C, specifically, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, and any value within the range consisting of any two of these point values.
[0031] The method of the present invention can be carried out in a continuous or intermittent manner, but is preferably carried out continuously. Intermittent operation refers to a typical kettle type operation in which the raw material aniline and catalyst are added to a reaction kettle and the reaction is carried out under appropriate conditions to obtain the target product. Continuous operation is usually an operation in which the raw material aniline is reacted through a fixed bed reactor containing a catalyst.
[0032] The inventors of the present invention found that the optimal reaction temperature and pressure for the continuous and intermittent systems are slightly different. When the intermittent system is adopted, the temperature of the contact reaction is preferably 130 to 180°C, the pressure is preferably 2 to 4 MPa, and the reaction time is preferably 4 to 8 h. The amount of catalyst used is preferably 1 to 4 wt% of the amount of aniline used as the raw material. When the continuous system is adopted, the temperature of the contact reaction is preferably 160 to 240°C, the pressure is preferably 1.5 to 3 MPa, and the liquid weight hourly space velocity of aniline is preferably 0.5 to 3 h. -1 , more preferably 1 to 1.5 h -1 It is.
[0033] In the continuous operation, the raw material aniline is preferably reacted by passing it through a catalyst layer of a fixed bed reactor containing a catalyst in a downward feeding manner.
[0034] The inventors of the present invention also found that the isomerization rearrangement reaction of aniline to produce 2-methylpyridine and the condensation reaction of aniline to produce diphenylamine are doubly influenced by two factors: catalyst and reaction temperature. By using a metal-supported β zeolite catalyst in the present invention, the reaction path of aniline can be switched between 2-methylpyridine and diphenylamine due to the change of the catalytic active center. In addition, a low reaction temperature is more favorable for the synthesis of 2-methylpyridine, and a high temperature is more favorable for the production of diphenylamine.
[0035] Therefore, the present invention also provides a method for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline, the method comprising the step of catalytically reacting aniline with a catalyst at a temperature of 100 to 400°C in a hydrogen-containing atmosphere, the catalyst being a zeolite carrying a metal component, the metal component including at least one active metal component selected from W, Mo, Ni, and Co, the temperature of the catalytic reaction being controlled to 100 to 240°C in order to obtain a product mainly consisting of 2-methylpyridine, and the temperature of the catalytic reaction being controlled to 260 to 400°C in order to obtain a product mainly consisting of diphenylamine.
[0036] In order to obtain a product mainly consisting of 2-methylpyridine, the contact reaction is preferably carried out at a temperature of 160 to 240° C. and a pressure of 1.5 to 3 MPa, and the liquid weight hourly space velocity of the aniline is preferably 0.5 to 3 h -1 In the case of obtaining a product mainly consisting of diphenylamine, the contact reaction is carried out at a temperature of 280 to 360° C. and a pressure of 1.5 to 3 MPa, and preferably at a liquid weight hourly space velocity of 0.3 to 1.5 h -1 It is.
[0037] In the present invention, a product mainly consisting of 2-methylpyridine means that the selectivity for 2-methylpyridine is 40% or more, and a product mainly consisting of diphenylamine means that the selectivity for diphenylamine is 40% or more.
[0038] The catalyst is described above and will not be described in detail here.
[0039] The conditions for synthesizing diphenylamine from aniline in the present invention are that the temperature of the contact reaction is preferably 280 to 360° C., the pressure is preferably 1.5 to 3 MPa, and the liquid weight hourly space velocity of aniline is preferably 0.3 to 1.5 h -1 , preferably 0.5 to 1 h -1 This includes being.
[0040] In the examples and comparative examples, the calculation methods for the conversion of aniline, the selectivity and yield of 2-methylpyridine, and the selectivity and yield of diphenylamine are as follows.
[0041] Conversion rate of aniline = (number of moles of aniline in raw material before reaction - number of moles of aniline in product) / number of moles of aniline in raw material before reaction × 100% Yield of 2-methylpyridine = moles of 2-methylpyridine in the product / theoretical moles of 2-methylpyridine when all the aniline in the raw material before the reaction is converted Selectivity of 2-methylpyridine = (moles of 2-methylpyridine in the product) / (moles of aniline in the raw material before reaction - moles of aniline in the product) x 100% Diphenylamine yield = moles of diphenylamine in the product / theoretical moles of diphenylamine when all the aniline in the raw material before reaction is converted Selectivity of diphenylamine = 2 x (moles of diphenylamine in the product) / (moles of aniline in the raw material before reaction - moles of aniline in the product) x 100% The contents of aniline, diphenylamine and 2-methylpyridine are measured by gas chromatography.
[0042] The alumina binder used is commercially available γ-alumina, and the zeolite used is commercially available Hβ zeolite, which has a specific surface area of 620 m 2 / g, particle size is less than 9 nm.
[0043] The catalysts used in the examples and comparative examples are manufactured by supporting auxiliary metal components and active metal components by a saturation impregnation method. The specific method is as follows: (1) Hβ zeolite is contacted with an aqueous nitrate solution of the auxiliary metal components by equal volume impregnation. (2) The mixture obtained in step (1) is filtered, washed, and dried. (3) The modified Hβ zeolite obtained in step (2), an alumina binder (e.g., pseudoboehmite), and a processing aid (e.g., extrusion aid, peptizer) are thoroughly kneaded, then molded, dried, and roasted. (4) NaBH4 is added to the aqueous nitric acid solution of the support and active metal components obtained in step (3), and the mixture is refluxed and reduced, filtered, and vacuum dried to produce a spherical catalyst with a particle size of 3 mm. The contact temperature in step (1) is 90°C and the contact time is 4h, step (2) is drying at 80°C for 10h, step (3) is drying at 80°C for 10h and roasting at 550°C for 10h, and step (4) is reflux reduction at 100°C for 8h, followed by vacuum drying at 100°C for 10h.
[0044] The catalyst properties are shown in Table 1.
[0045] [Table 1]
[0046] Examples 1 to 8 The reaction was carried out in a kettle reactor under hydrogen atmosphere, the catalyst amount was 1g, and the aniline amount was 50g. The reaction conditions are shown in Table 2 below.
[0047] Comparative Examples 1-2 The conversion reaction of aniline was carried out according to the method of Example 1, except that the reaction conditions were changed as shown in Table 2 below.
[0048] Comparative Example 3 Aniline conversion reaction was carried out by the method of Example 1, except that β zeolite (without metal component support) was used as the catalyst and the remaining reaction conditions were changed to those shown in Table 2 below.
[0049] Comparative Example 4 2-Methylpyridine was produced from aniline by the method described in Example 1 of CA1190928A, that is, using pure HZSM-5, the temperature was 510°C, the pressure was 2.9 MPa, and the molar ratio of raw aniline to ammonia was 1:8, and the weight hourly space velocity was 1.0 h -1 Aniline was converted to 2-methylpyridine under the conditions.
[0050] [Table 2]
[0051] Examples 9 to 16 A fixed-bed reactor was selected, and the raw material aniline was fed downward through the catalyst layer. Under hydrogen atmosphere, the reaction was first carried out under conditions suitable for the production of 2-methylpyridine for 48 hours, and then the reaction was continued for 48 hours under conditions suitable for the production of diphenylamine at a heating rate of 30°C / hour. The product distribution was measured and shown in Table 3 below.
[0052] [Table 3]
[0053] Example 17 Using the method of Example 9, diphenylamine and 2-methylpyridine were produced from the raw material aniline, and the effect of temperature on the product distribution was investigated. After each sampling, the temperature was increased to the next temperature at a rate of 30°C / hour. The product distribution changed with temperature, and the change relationship diagram is shown in Figure 1.
[0054] From the results in Table 2 and FIG. 1, it can be seen that the method for producing 2-methylpyridine according to the present invention can obtain a higher aniline conversion and a higher 2-methylpyridine selectivity at a lower reaction temperature.
[0055] From the results of Table 3 and FIG. 1, the method for selectively and continuously producing diphenylamine and 2-methylpyridine according to the present invention can easily obtain different target products, diphenylamine and 2-methylpyridine, in the same apparatus by adjusting process parameters such as reaction temperature and pressure. [Brief description of the drawings]
[0056] [Figure 1] FIG. 2 is a relationship diagram showing the change in product distribution with temperature in the process for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline according to the present invention.
Claims
1. A method for selectively and continuously producing 2-methylpyridine and diphenylamine from aniline, comprising the step of catalytically reacting aniline with a catalyst under a hydrogen-containing atmosphere at a temperature of 100 to 400° C., the catalyst is a β zeolite carrying a metal component, the metal component containing at least one active metal component selected from W, Mo, Ni, and Co; and the temperature of the contact reaction is controlled to 100 to 240°C to obtain a product mainly containing 2-methylpyridine, and the temperature of the contact reaction is controlled to 260 to 400°C to obtain a product mainly containing diphenylamine.
2. The method according to claim 1, wherein the content of the active metal component is 0.5 to 5 wt %, preferably 0.5 to 3 wt %, calculated as metal element based on the total amount of the catalyst.
3. The method according to claim 1 or 2, wherein the metal component further comprises at least one auxiliary metal component selected from Li, Na, K, Mg, and Ca, and the content of the auxiliary metal component is 0 to 6.5 wt %, preferably 0.5 to 5.5 wt %, calculated in terms of an oxidation state based on the total amount of the catalyst.
4. The catalyst further contains an alumina binder, and the catalyst contains, based on the total amount of the catalyst, 50 to 85 wt % of β zeolite, 0.5 to 5 wt % of an active metal component calculated as a metal element, 0 to 6.5 wt % of an auxiliary metal component calculated as an oxidation state, and 10 to 45 wt % of the alumina binder.
5. 5. The method according to claim 4, wherein the catalyst contains, based on the total amount of the catalyst, 60 to 85 wt % of β zeolite, 0.5 to 3 wt % of an active metal component calculated as a metal element, 0.5 to 5.5 wt % of an auxiliary metal component calculated as an oxidation state, and 15 to 34.5 wt % of an alumina binder.
6. The method according to any one of claims 1 to 5, wherein the pressure of the contact reaction is 1.5 to 4 MPa, and the contact reaction is carried out under a hydrogen atmosphere.
7. The method according to any one of claims 1 to 6, wherein the catalytic reaction is carried out without introducing ammonia gas.
8. In order to obtain a product mainly consisting of 2-methylpyridine, the contact reaction is carried out at a temperature of 160 to 240° C. and a pressure of 1.5 to 3 MPa, and preferably at a liquid weight hourly space velocity of 0.5 to 3 h -1 or In order to obtain a product mainly consisting of diphenylamine, the contact reaction is carried out at a temperature of 280 to 360° C. and a pressure of 1.5 to 3 MPa, and preferably at a liquid weight hourly space velocity of 0.3 to 1.5 h -1 The method according to any one of claims 1 to 7, wherein
9. The raw material aniline is reacted in a fixed bed reactor containing the catalyst, The method according to claim 8, wherein the raw aniline is preferably fed to the fixed bed reactor in a downward feeding manner and passes through a catalyst bed.
10. A method for the synthesis of 2-methylpyridine from aniline, comprising the steps of: A method comprising the steps of contacting aniline with a catalyst in a hydrogen-containing atmosphere under isomerization rearrangement reaction conditions, the catalyst being a β zeolite carrying a metal component, the metal component comprising at least one active metal component selected from W, Mo, Ni, and Co, and the contact reaction temperature being 100° C. to 240° C.
11. The method according to claim 10, wherein the content of the active metal is 0.5 to 5 wt %, preferably 0.5 to 3 wt %, calculated as metal element based on the total amount of the catalyst.
12. The method according to claim 10 or 11, wherein the metal component further comprises at least one auxiliary metal component selected from Li, Na, K, Mg, and Ca, and the auxiliary metal component content is 0 to 6.5 wt % in terms of oxidation state based on the total amount of the catalyst.
13. The catalyst further contains an alumina binder, and the catalyst contains, based on the total amount of the catalyst, 50 to 85 wt % of β zeolite, 0.5 to 5 wt % of an active metal component calculated as a metal element, 0 to 6.5 wt % of an auxiliary metal calculated as an oxidation state, and 10 to 45 wt % of the alumina binder.
14. The method according to claim 13, wherein the catalyst contains, based on the total amount of the catalyst, 60 to 85 wt % of β zeolite, 0.5 to 3 wt % of an active metal component calculated in a reduced state, 0.5 to 5.5 wt % of an auxiliary metal component calculated in an oxidized state, and 15 to 34.5 wt % of an alumina binder.
15. The method according to any one of claims 10 to 14, wherein the catalytic reaction is carried out without introducing ammonia gas.
16. The contact reaction is intermittently carried out, and the contact reaction is carried out at a temperature of 130 to 180° C., a pressure of 2 to 4 MPa, and a reaction time of 4 to 8 hours. Preferably, the amount of the catalyst used is 1 to 4 wt % of the amount of the raw aniline used; or The contact reaction is carried out continuously at a temperature of 160 to 240° C. and a pressure of 1.5 to 3 MPa. Preferably, the liquid weight hourly space velocity of the aniline is 0.5 to 3 h -1 and The method according to any one of claims 10 to 15, wherein the raw material aniline is reacted through a fixed bed reactor containing the catalyst, and preferably the raw material aniline enters the fixed bed reactor in a downward feeding manner and passes through a catalyst bed.
Citation Information
Patent Citations
2-Methyl-pyridine and 4-methylpyridine production method
CN105384683A
Manufacture of alpha-picoline
JP1983116465A
Manufacture of 2-amino-alkylpyridines
JP1985072864A
Production of diphenylamines
JP2000095736A
Method for producing diarylamines
JP2001172230A