Cerium-Gadolinium Complex Oxide

The cerium-gadolinium complex oxide addresses the need for high-temperature sintering in SOFCs by achieving high relative densities at 950°C without sintering agents, ensuring robust electrolytes and preventing component deterioration, thus enhancing energy efficiency and durability.

JP2024541273APending Publication Date: 2024-11-08RHODIA OPERATIONS SAS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024526477
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-08
Filing Date
2022-11-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing solid oxide fuel cell (SOFC) electrolytes require high-temperature sintering processes to achieve high relative densities, which can lead to energy inefficiency and potential deterioration of cell components, and there is a need for electrolytes that can withstand harsh conditions at high temperatures without additional sintering agents.

Method used

A cerium-gadolinium complex oxide with a gadolinium proportion between 22.0 mol% and 45.0 mol% is used, allowing for high relative densities to be achieved at temperatures as low as 950°C without the addition of sintering agents, ensuring robustness and gas-tightness.

Benefits of technology

The cerium-gadolinium complex oxide achieves high relative densities at lower temperatures, maintaining electrolyte integrity and preventing component deterioration, while avoiding the introduction of additional elements that could alter the fuel cell's physicochemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541273000005
    Figure 2024541273000005
  • Figure 2024541273000006
    Figure 2024541273000006
  • Figure 2024541273000007
    Figure 2024541273000007
Patent Text Reader

Abstract

The present invention relates to a complex oxide based on cerium and gadolinium, having a proportion of Gd between 22 and 45 mol %, which proportion corresponds to a molar ratio Gd / (Ce+Gd) expressed in %, which complex oxide exhibits an improved relative density.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cerium-gadolinium complex oxide, a process for its preparation and its use. The present invention also relates to a SOFC or SOEC containing the complex oxide of the present invention. [Background technology]

[0002] A solid oxide fuel cell (or SOFC) is an electrochemical conversion device that produces electricity directly from the oxidation of a fuel. It is an electrochemical device for generating electrical energy by electrochemical oxidation of a fuel gas (usually hydrogen-based). The device is ceramic-based and uses an oxygen-ion conducting metal oxide-derived ceramic as the electrolyte. All SOFCs need to operate at high temperatures, since the ceramic oxygen-ion conductors known in the art (most typically doped zirconium oxide or doped cerium oxide) only exhibit technically relevant ionic conductivity at temperatures above 500° C. (for cerium oxide-based electrolytes) or 600° C. (for zirconium oxide-based ceramics).

[0003] The electrolyte is an essential part of the cell and in SOFCs has the following main functions: - the ability to pass electrical current in the form of mobile oxygen ions between the cathode (positive air electrode) and the anode (negative fuel electrode); - the function of blocking the passage of current between the electrodes in the form of electrons, which causes an internal short circuit in the cell; - To prevent mixing of the fuel with air, i.e. to have no interconnected pores, the electrolyte must be at least 94% of theoretical density, so that the electrolyte layer is gas-impermeable and substantially free of defects.

[0004] As disclosed in US 2016 / 233534, recent developments in the field of SOFCs have led to the development of oxygen ion conducting electrolytes of the formula Ce, which have inherently higher oxygen ion conductivity than zirconia-based materials. 0.9 Gd 0.1 O1.95 A cerium-gadolinium complex of

[0005] European Patent No. 1484282B1 discloses a cerium-gadolinium complex oxide that can obtain a high relative density at a high processing temperature, but does not disclose the same complex oxide as the present invention.

[0006] US Patent No. 6,709,628 discloses a process for producing sintered oxide ceramics based on cerium, a first doping element selected from the group consisting of Lu, Yb, Tm, Er, Y, Ho, Dy, Gd, Eu, Sm and Nd, and a second doping element selected from the group consisting of Cu, Co, Fe, Ni and Mn, which includes a sintering step at temperatures between 750°C and 1200°C to reach at least about 98% of the theoretically possible density. In the absence of the second dopant, the density is only 90% at 1450°C. Ce 0.8 Gd 0.2 Co z O 2-a Or Ce 0.8 Gd 0.2 CuzO 2-a Specific compositions such as the following are disclosed.

[0007] US Patent Application Publication No. 2016 / 0233535 discloses a method for the preparation of Ce 0.9 Gd 0.1 O 1.95 Or Ce 0.9 Sm 0.1 O 1.95 discloses a process for forming an electrolyte for a metal-supported solid oxide fuel cell (SOFC), comprising combining a doped ceria electrolyte such as CoO with a sintering aid. As seen in Figure 9, the relative density of the doped ceria electrolyte without a sintering aid (e.g., Co3O4 or CuO) is lower than 94% after firing at 1100°C, meaning that it will be even lower at lower temperatures.

[0008] US Patent No. 7,947,212 B2 discloses the densification of ceria-based electrolytes by using divalent or trivalent cations. Without any cations, the relative density is below 94% (Figure 2).

[0009] JP 2000-007435 A discloses a ceria-based complex oxide that can be used for the preparation of SOFCs. This complex oxide is prepared by a process different from that of the present invention. Moreover, high density is obtained, but at temperatures higher than 1500° C.

[0010] Duran et al., "Sintering and microstructural development of ceria-gadolinia dispersed powders", J. Mat. Sci. 1994, 29(7), discloses a complex oxide ceria-gadolinia having a lower percentage of Gd than in claim 1 and exhibiting a relative density at temperatures above 1300°C. Summary of the Invention [Problem to be solved by the invention]

[0011] The electrolyte densification process requires sintering at high temperatures. It is also advantageous to reach a high relative density to ensure the preparation of a gas-tight and robust electrolyte to avoid contact with fuel and oxidizing gases (see Journal of The Electrochemical Society 2002, 149(7), A797-A803).

[0012] Naturally, it is more advantageous to reach a high relative density at the lowest possible temperature in order to save energy, and it is also desirable to sinter at the lowest possible temperature in order to avoid degradation, such as oxidation, or sintering of other components used in the preparation of the SOFC.

[0013] Finally, the electrolyte must also be able to withstand the harsh conditions encountered as it comes into contact with the gases at high temperatures. [Means for solving the problem]

[0014] It has been found that the complex oxide of the invention can reach high relative densities at high temperatures, such as 950° C., without the addition or incorporation of any sintering agent, making it possible to avoid the introduction of further elements that may affect the final physicochemical properties of the inorganic layers of the fuel cell containing the complex oxide.

[0015] Therefore, the present invention aims to prepare a ceria-based electrolyte suitable for the manufacture of SOFCs, which can be sintered at high temperatures, such as 950° C., with high relative density without the addition of any sintering agent.

[0016] The present invention relates to a complex oxide based on cerium and gadolinium, in which the proportion of gadolinium is in the range greater than 22.0 mol % and up to 45.0 mol %, said proportion corresponding to the molar ratio Gd / (Ce+Gd) expressed in %.

[0017] The complex oxide of the present invention is disclosed in claims 1 to 43. The present invention also relates to a composition C disclosed in claims 44 to 48.

[0018] The present invention also relates to a process for preparing a complex oxide as disclosed in claims 51-52, to the use of a complex oxide or composition C as disclosed in any one of claims 49 or 50. The present invention also relates to a SOFC as disclosed in claim 53 or 54. The present invention also relates to a SOEC as disclosed in claim 55.

[0019] These targets are described in more detail below. [Brief description of the drawings]

[0020] [Figure 1] 1 is a size distribution obtained by laser diffraction for the complex oxides disclosed in the examples. [Diagram 2] 1 is a size distribution obtained by laser diffraction for the complex oxides disclosed in the examples. [Diagram 3] 1 is a porogram obtained by Hg porosimetry of a complex oxide disclosed in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] It is noted that in the remainder of the specification, unless otherwise stated, the ranges of values ​​given include upper and / or lower values.

[0022] The complex oxide of the invention is based on cerium oxide and gadolinium oxide and is characterized by a proportion of Gd ranging from greater than 22.0 mol % to less than or equal to 45.0 mol % of gadolinium, which proportion corresponds to the molar ratio Gd / (Ce+Gd) expressed in %.

[0023] The percentage of Ce corresponds to the complement of 100%, and therefore the percentage of Ce is 55.0 mol % to 78.0 mol %.

[0024] The proportion of Gd may more particularly be between 30.0 mol % and 45.0 mol %, in which case the proportion of Ce is between 55.0 mol % and 70.0 mol %.

[0025] The proportion of Gd may more particularly be between 35.0 mol % and 45.0 mol %, in which case the proportion of Ce is between 55.0 mol % and 65.0 mol %.

[0026] The proportion of Gd may more particularly be between 37.0 mol % and 43.0 mol %, in which case the proportion of Ce is between 57.0 mol % and 63.0 mol %.

[0027] The proportion of Gd may more particularly be between 38.0 mol % and 42.0 mol %, in which case the proportion of Ce is between 58.0 mol % and 62.0 mol %.

[0028] The proportion of Gd may more particularly be between 39.0 mol % and 41.0 mol %, in which case the proportion of Ce is between 59.0 mol % and 61.0 mol %.

[0029] The proportion of Gd may more particularly be between 39.5 mol % and 40.5 mol %, in which case the proportion of Ce is between 59.5 mol % and 60.5 mol %.

[0030] The proportion of Gd may more particularly be between 28.0 mol % and 32.0 mol %, in which case the proportion of Ce is between 68.0 mol % and 72.0 mol %.

[0031] The proportion of Gd may more particularly be between 29.0 mol % and 31.0 mol %, in which case the proportion of Ce is between 69.0 mol % and 71.0 mol %.

[0032] The proportion of Gd may more particularly be between 29.5 mol% and 30.5 mol%, in which case the proportion of Ce is between 69.5 mol% and 70.5 mol%.

[0033] The invention also relates to a complex oxide consisting of the two oxides CeO2 and Gd2O3, in particular according to the proportions indicated above.

[0034] According to one embodiment, the X-ray diffractogram (CuKα1, λ=1.5406 Å) of the complex oxide shows a solid solution pattern. According to another embodiment, the X-ray diffractogram (CuKα1, λ=1.5406 Å) of the complex oxide shows a peak P at 2θ between 27.0 and 30.0°. This peak P is of the highest intensity on the diffractogram.

[0035] The presence of Gd2O3 can also be detected on an X-ray diffractogram by referencing ICDD pattern 03-065-3181. The peaks on the diffractogram indicating the presence of Gd2O3 are generally barely visible on the diffractogram.

[0036] The complex oxide of the present invention contains the above elements (Ce, Gd) in the above ratios, but it may further contain impurities. The impurities may come from the raw materials or starting materials used in the process of preparing the complex oxide. The total ratio of impurities is less than 0.20% by weight, preferably less than 0.10% by weight, and more preferably less than 0.05% by weight, based on the complex oxide. Everything disclosed in this specification applies to the complex oxide consisting of CeO2 and Gd2O3 in the above ratios and impurities whose total ratio is less than 0.20% by weight, preferably less than 0.10% by weight, and more preferably less than 0.05% by weight.

[0037] The complexes of the present invention exhibit the following specific physicochemical properties:

[0038] 1) Relative density RD The complex oxide has a relative density RD of at least 94.0% after calcination at 1000°C for 5 hours in air. 1000℃ / 5h RD 1000℃ / 5h Preferably, RD is at least 95.0%. 1000℃ / 5h is usually at most 98.0% or at most 96.0%. 1000℃ / 5h may be 94.0% to 98.0%, more particularly 94.0% to 96.0%.

[0039] The complex oxide has a relative density RD of at least 80.0% after calcination at 950°C for 5 hours in air. 950℃ / 5h RD 950℃ / 5h is preferably at least 88.0%. 950℃ / 5h is usually at most 94.0% or at most 90.0%. 950℃ / 5h may be 80.0% to 90.0%, more particularly 88.0% to 90.0%.

[0040] The complex oxide has a relative density RD of at least 96.0%, preferably at least 97.0%, after calcination at 1100° C. for 5 hours in air. 1100℃ / 5h RD 1100℃ / 5his usually at most 99.0% or at most 98.0%. 1100℃ / 5h may be 96.0% to 99.0%, more particularly 96.0% to 98.0%.

[0041] The complex oxide has a relative density RD of at least 99.0% after calcination at 1200°C for 5 hours in air. 1200℃ / 5h RD 1200℃ / 5h is preferably at least 99.5%.

[0042] The complex oxide may, for example, exhibit the following: - RD of at least 94.0% after calcination at 1000°C for 5 hours 1000℃ / 5h , and - After calcination at 950°C for 5 hours, RD of at least 80.0% 950℃ / 5h .

[0043] The relative density of the complex oxide is determined on a sample without any other materials added, such as sintering aids.

[0044] The relative density RD is well known to those skilled in the ceramic art and corresponds to the density of a complex oxide relative to its absolute density, expressed in %, (RD in %=density / absolute density×100).

[0045] In the context of the present invention, the density of the complex oxide is measured on a compressed sample of the complex oxide after calcining the compressed sample in air at the temperature of the test (950°C, 1000°C, 1100°C or 1200°C) for 5 hours. The compressed sample is obtained by applying pressure to the complex oxide in powder form introduced into a molding die. Advantageously, the die has a parallelepiped shape, since this shape makes it possible to easily measure the volume after calcination in air.

[0046] More specifically, the compressed sample may be prepared by the following method: i) a powder of a composite oxide is weighed and introduced into a molding die; ii) the powder is compressed under pressure; iii) the compressed sample obtained at the end of step ii) is removed from the mould; iv) The pressed samples are then fired in air at the target temperature for 5 hours; v) the density of the fired pressed samples is measured; vi) The relative density is then calculated.

[0047] Density is measured according to any laboratory technique known to those skilled in the art.

[0048] For step v), in particular the following methods can be used: v1) The fired pressed sample is weighed (weight in g); v2) The volume of the compressed sample was measured (cm 3 (volume in units), the compressed sample is in the shape of a parallelepiped, and the volume of the parallelepiped is Volume = length (cm) x width (cm) x height (cm) The length, width and height of the parallelepiped can be conveniently measured in micrometers.

[0049] In step ii), the pressure applied to obtain the compressed sample is preferably at least 95 MPa or even at least 98 MPa.

[0050] The test conditions given in the examples may conveniently be used.

[0051] The absolute density (or theoretical density) is obtained by first calculating the lattice constant of the complex oxide structure from the XRD pattern, and then calculating the absolute density according to the following formula: Absolute density (g / cm 3 )=SA / (a×b×c×N) SA represents the molar mass of all atoms in a unit cell, a, b, and c represent the lattice constants, and N represents the Avogadro constant.

[0052] The absolute densities used in the calculations are given in the table below.

[0053] [Table 1]

[0054] 2) Porosity and pore diameter Dp (Hg porosity) The process of the invention makes it possible to obtain complex oxides with a particular distribution of pore sizes. The complex oxides may exhibit a peak in the range of pores with diameters of up to 200 nm, corresponding to a pore diameter Dp with a maximum value between 30 and 100 nm. Dp may also be between 30 and 70 nm. The pore diameters are obtained by mercury porosimetry.

[0055] Said peak typically exhibits a half-width of the peak of less than 80 nm, more particularly less than 70 nm, even more particularly less than 60 nm, even more particularly less than 50 nm, even more particularly less than 40 nm, even more particularly less than 30 nm, even more particularly less than 20 nm.

[0056] The pore volume (Vp <200nm ) is generally less than 0.40 mL / g, more particularly less than 0.35 mL / g, and even more particularly less than 0.30 mL / g. <200nm is generally at least 0.10 mL / g.

[0057] Typically, the porogram shows a single peak in the range of pores with diameters below 200 nm.

[0058] 3) BET specific surface area Complex oxides are usually 5-40m 2 The BET specific surface area is 10 to 35 m / g. 2 / g, or 20-30m 2 / g, or 25-30m 2 / g. The BET specific surface area is well known to those skilled in the art. It is measured by nitrogen adsorption using the well-known Brunauer-Emmett-Teller method. The BET method is described, inter alia, in the journal "The Journal of the American Chemical Society, 60, 309 (1938)". The recommendations of the standard ASTM D3663-03 can be followed.

[0059] 4) Particle size (by laser diffraction) Complex oxides may also exhibit size specific properties in terms of size (in volume) distribution, as determined by laser diffraction analysis. The technique of laser diffraction is well known to those skilled in the art. It allows the particle size distribution to be determined by measuring the angular change in intensity of the light scattered as a laser beam passes through a sample of dispersed particles. Large particles scatter light at small angles to the laser beam, and small particles scatter light at higher angles.

[0060] D50 may be from 0.1 to 15.0 μm. D50 may be more particularly from 0.2 to 15 μm, or even from 1.0 to 15.0 μm or from 5.0 to 15.0 μm.

[0061] D16 may be from 0.1 to 4.0 μm. D16 may be, more particularly, from 0.1 to 1.0 μm.

[0062] D84 may be 10.0 to 50.0 μm. D84 may be more particularly 15.0 to 50.0 μm.

[0063] The parameters D16, D84 and D50 are obtained from the volume distribution determined by laser diffraction. D16 is the diameter determined from the distribution obtained by laser diffraction where 16% of the particles have a diameter less than D16. D84 is the diameter determined from the distribution obtained by laser diffraction where 84% of the particles have a diameter less than D84. D50 is the diameter determined from the distribution obtained by laser diffraction where 50% of the particles have a diameter less than D50. D50 is also referred to as the median of the distribution.

[0064] The distribution may exhibit at least two populations. More specifically, the distribution may exhibit at least two populations P1 and P2 having the following characteristics: a population P1 centered on a diameter D1 of less than 3.0 μm, and / or - A population P2 centered on a diameter D2 greater than 8.0 μm.

[0065] In particular in the region of diameters less than 100 μm, the distribution may show two populations P1 and P2 with the following characteristics: a population P1 centered on a diameter D1 of less than 3.0 μm, and / or - A population P2 centered on a diameter D2 greater than 8.0 μm.

[0066] The expression "population centred on diameter D" means that on the distribution curve a peak is observed whose maximum is located at D.

[0067] According to one embodiment, the distribution includes a shoulder around the peak of population P1. Thus, in such an embodiment, the distribution exhibits three peaks: the peaks of populations P1 and P2 and a shoulder peak.

[0068] D1 may in particular be between 0.1 and 3.0 μm, more in particular between 0.1 and 1.0 μm.

[0069] D2 may in particular be from 8.0 to 100.0 μm, more in particular from 10.0 to 100.0 μm, even more in particular from 10.0 to 70.0 μm, and more in particular from 10.0 to 50.0 μm.

[0070] The two populations P1 and P2 may be such that the ratio H2 / H1 of the heights H1 and H2 of the two peaks of P1 and P2, respectively, is: - higher than 0.1, more particularly higher than 0.3, more particularly higher than 1.0, even more particularly higher than 1.5, or - lower than 7.0, more particularly lower than 5.5, even more particularly lower than 1.0, even more particularly lower than 0.8, even more particularly lower than 0.5.

[0071] The ratio H2 / H1 is usually between 0.1 and 7.0, more particularly between 0.1 and 5.5, even more particularly between 0.1 and 1.0. H2 / H1 can also be between 0.1 and 0.8, or between 0.1 and 0.5, or between 0.4 and 0.5.

[0072] The ratio H2 / H1 depends on the process conditions, in particular the concentration of solution S and the conditions of step e). The more concentrated the solution S, the lower the ratio. The higher the duration and / or intensity of the grinding step e), the lower the ratio.

[0073] The complex oxide is usually in the form of a powder.

[0074] Process for preparing complex oxides The process for preparing the complex oxide of the present invention comprises the following steps: a) Cerium nitrate (Ce III ) and an aqueous solution S containing gadolinium nitrate is added to a basic aqueous solution of ammonium bicarbonate (NH4HCO3), thereby forming a precipitate; b) heating the aqueous slurry containing the precipitate obtained at the end of step a) at a temperature between 50° C. and 95° C.; c) the solid obtained at the end of step b) is recovered and washed with water; d) calcining the solid recovered from step c) in air at a temperature between 600° C. and 1000° C.; e) The calcined solid is ground.

[0075] Step a) In step a), two aqueous solutions are prepared: a basic solution of NH4HCO3 and a solution of cerium nitrate (Ce) with the desired ratio of Gd. IIIThe aqueous solution S containing cerium nitrate and gadolinium nitrate is used. The concentration of cerium nitrate in the aqueous solution S is usually 0.15 to 0.50 mol / L. The aqueous solution S contains Ce III , Gd III , NO 3- , H + The concentrations of cerium nitrate in solution S disclosed in Example 1 or Example 2 may be advantageously used.

[0076] Solution S is obtained by mixing two aqueous solutions of cerium nitrate and gadolinium nitrate and diluting the resulting co-nitrate solution with water. The volume of water used for dilution can be 5 to 10 times the volume of the co-nitrate solution. The ratio of the volume of water / volume of the co-nitrate solution can be as disclosed in Example 1 or 2.

[0077] Each of the two solutions (Ce nitrate and Gd nitrate) used to prepare the co-nitrate solution may exhibit a residual acidity, which may be conveniently measured by acid / base titration using methyl orange as indicator. The aqueous cerium nitrate solution preferably exhibits a residual acidity of less than 0.1 mol / L, even less than 0.07 mol / L. The aqueous cerium nitrate solution used in the examples may be conveniently used. The aqueous gadolinium nitrate solution preferably exhibits a residual acidity of less than 1.0 mol / L. The aqueous cerium nitrate solution used in the examples may be conveniently used.

[0078] The basic aqueous solution of NH4HCO3 is prepared by dissolving solid NH4HCO3 in water. The concentration of the basic aqueous solution of NH4HCO3 is preferably 30-100 g / L. The concentrations disclosed in Example 1 or Example 2 can be conveniently used.

[0079] Cerium nitrate (Ce III) and gadolinium nitrate are added to a basic aqueous solution of ammonium hydrogen carbonate (NH4HCO3), whereby a precipitate is formed (this is usually disclosed as "reverse precipitation"). The addition flow rate of the aqueous solution S to be added to the basic aqueous solution is usually 50 to 200 L / h. Typically, the addition is carried out for 20 to 120 minutes, more particularly 20 to 60 minutes. The flow rates and / or times used in the other examples may be used conveniently.

[0080] The temperature at which step a) is carried out is expediently between 10°C and 30°C.

[0081] The amount of hydrogen carbonate used in step a) is such that the molar ratio r=NH4HCO3 / (Ce+Gd) is between 3.00 and 3.50, more particularly between 3.10 and 3.45. The molar ratio r can conveniently be any of the molar ratios used in Example 1 or 2.

[0082] Bicarbonate is only used in step a).

[0083] Step b) In step b), the aqueous slurry containing the precipitate obtained at the end of step a) is heated at a temperature between 50° C. and 95° C., more particularly between 70° C. and 95° C. The temperature disclosed in example 1 or 2 (80° C.) may conveniently be used. The treatment time may be between 1 hour and 4 hours. The time disclosed in example 1 or 2 (3 hours) may conveniently be used.

[0084] The aqueous slurry heated during step b) can be obtained according to two embodiments. According to a first (preferred) embodiment, the aqueous slurry is obtained directly at the end of step a). This means that steps a) and b) can be conveniently carried out in the same vessel.

[0085] According to a second embodiment, the aqueous slurry of step b) is obtained by diluting the aqueous slurry obtained at the end of step a) with water.

[0086] Step c) In step c), the solid obtained at the end of step b) is collected and washed with water, for example deionized water. The solid can be collected by any technique available for separating solids from aqueous media. Any type of filtration can be used. Washing is usually carried out until the conductivity of the filtrate is less than 5 mS / cm.

[0087] Step d) In step d), the cake recovered from step c) is calcined in air at a temperature between 600°C and 1000°C. The calcination temperature is preferably between 750°C and 850°C. The time of step d) can be between 1 hour and 25 hours, more particularly between 1 hour and 20 hours. Under certain conditions, the calcination temperature is 795°C and the calcination time is 8 hours. The conditions of step d) of example 1 can be applied. The calcination step aims to obtain the conversion of cerium and gadolinium to oxides and to increase the crystallinity of the composition.

[0088] Step e) The calcined solid obtained at the end of step d) is ground. A hammer mill may be used. The calcined solid may be ground in a mortar.

[0089] The preparation of the complex oxide according to the invention can be carried out according to the experimental procedures given in Examples 1 and 2 (especially in the range of proportions given in claim 1).

[0090] Use of Complex Oxides The complex oxide of the present invention can be used to prepare a SOFC. In a SOFC, electricity is generated by the reaction of a fuel with an oxygen source. The oxygen source (typically air) contacts the cathode and forms oxygen ions upon reduction by electrons at the cathode. When the SOFC operates with a hydrocarbon fuel and electrons, the oxygen ions encounter the fuel at the anode and form water and carbon dioxide.

[0091] The SOFC comprises two porous electrodes (A) and (C) separated by at least one electrolyte layer (L). In the preparation of any one or more of these three components, i.e. the anode, the cathode or at least one layer, the complex oxide of the present invention can be used as the oxygen ion conducting material. Each of these three components of the SOFC will now be described in detail. Thus, the present invention also relates to a SOFC comprising one porous anode (A) and one porous cathode (C) separated by at least one layer (L), where at least one of the components (A), (C) or (L) is prepared from or comprises the complex oxide of the present invention.

[0092] The function of layer (L) is to act as a barrier to prevent direct contact between the fuel and the oxygen source. Another function of the barrier is to allow the diffusion of oxygen ions through the layer.

[0093] In the context of the present invention, at least one of components (A), (C) or (L) is prepared from or comprises a complex oxide of the invention.

[0094] Anode (A) The present invention also relates to an anode comprising or prepared from the complex oxide of the present invention and optionally at least one other inorganic material. The oxidation of fuel occurs in the anode. The inorganic material other than the complex oxide used in the anode can be selected from the group consisting of zirconia doped with at least one element selected from the group of Y, Sc, Ce and combinations of two or more of these three elements; mixed oxides of cerium and gadolinium; metals such as nickel; lanthanum titanate; and lanthanum chromite.

[0095] Examples of lanthanum titanate include those of the formula La 0.2 Sr 0.25 Ca 0.45 It is TiO3.

[0096] Cathode (C) The present invention also relates to a cathode comprising or prepared from the complex oxide of the present invention and optionally at least one other inorganic material. Reduction of oxygen occurs at the cathode. The inorganic material other than the complex oxide used in the cathode can be selected from the group consisting of zirconia doped with at least one element selected from the group consisting of Y, Sc, Ce and combinations of two or more of these three elements; mixed oxides of cerium and gadolinium; mixed oxides of cerium and samarium; perovskites containing La, Sr, Co and Fe; and perovskites containing La, Sr, Mn.

[0097] La, Sr, Co and Fe containing perovskites are generally represented by the general formula La x Sr 1-x Co y Fe 1-y O 3{プラス又はマイナス}δ where x and y are numbers between 0.5 and 0.9 and between 0.1 and 0.9, respectively. For example, х=0.8, y=0.8 or x=0.6 and у=0.2. Examples of such perovskites are disclosed in “Synthesis and Study of LSCF Perovskites for IT SOFC Cathode Application”, ECS Transactions, 2009, 25(2) (DOI:10.1149 / 1.3205796).

[0098] La, Sr, Mn-containing perovskites have the general formula La 1-x Sr x It is represented as MnO3, where x is a number between 0 and 1.0.

[0099] Electrolyte layer (L) The present invention also relates to a layer comprising or prepared from the complex oxide of the present invention and, optionally, at least one other inorganic material, which may be selected from the group consisting of zirconia or mixed oxides of cerium and gadolinium doped with at least one element selected from the group of Y, Sc, Ce and combinations of two or more of these three elements.

[0100] The preparation of SOFCs may use the complex oxides of the invention disclosed in full detail above, which may also include the complex oxides of the invention modified by the addition of sintering aids (see below) and / or by mechanical treatments such as a grinding step.

[0101] Examples of SOFCs are given below. SOFC example Ex1 is based on the following configuration: - Anode (A), a layer (L) comprising or prepared from a complex oxide of the invention and optionally further comprising at least one other inorganic material, - Cathode (C).

[0102] The SOFC of Ex1 may also include an additional layer (L1) between (L) and (C), the function of which is to prevent short circuits. This additional layer (L1) typically includes zirconia doped with at least one element selected from the group Y, Sc, Ce and combinations of two or more of these three elements. If the SOFC of Ex1 includes an additional layer (L1), it may include an additional layer (L2) between (L1) and (C) that includes or is prepared from a complex oxide of the invention and / or a mixed oxide of cerium and gadolinium different from the complex oxide of the invention. This additional layer (L2) serves to prevent the diffusion of elements from the cathode (C) into the additional layer (L1), such as strontium.

[0103] In Ex1, the anode (A) and / or the cathode (C) may comprise a complex oxide of the invention and / or a mixed oxide of cerium and gadolinium different from the complex oxide of the invention.

[0104] Another embodiment Ex2 of the SOFC is based on the following construction: - Anode (A), - Layer (L), an additional layer (L2) comprising or prepared from a complex oxide of the invention and optionally further comprising at least one other inorganic material, - Cathode (C).

[0105] Layer (L) typically comprises zirconia doped with at least one element selected from the group Y, Sc, Ce and combinations of two or more of these three elements.

[0106] In Ex2, the anode (A) and / or the cathode (C) may comprise or be prepared from a mixed oxide of cerium and gadolinium different from the inventive complex and / or the inventive complex oxide.

[0107] The complex oxide of the present invention may be used for the preparation of a cell disclosed in one of the following documents, by replacing the cerium-gadolinium disclosed therein with the complex oxide of the present invention: WO 02 / 35628; WO 03 / 075382; WO 2004 / 089848; WO 2005 / 078843; WO 2006 / 079800; WO 2006 / 106334; WO 2007 / 085863; WO 2007 / 110587; WO 2008 / 001119; WO 2008 / 003976; WO 2008 / WO 2008 / 053213;WO 2008 / 104760;WO 2008 / 132493;US2013 / 0052562;WO 2021 / 151692;WO 2016 / 124929;WO 2015 / 033104 No. 2017 / 153751; WO 2021 / 096828; U.S. Pat. No. 8,435,694 B2; U.S. Pat. No. 10,749,188 B2; U.S. Patent Application Publication No. 2008 / 254336; DE 102013007637; U.S. Patent Application Publication No. 2013 / 0095408. The complex oxide of the present invention is disclosed in the doctoral thesis of Clement Nicollet ("Nouvelles electrodes a oxygene pour SOFC a base de nickelates Ln2NiO 4+δ (Ln=La, Pr) prepares par infiltration”).

[0108] The SOFC and the layers of the SOFC are prepared by known methods: - casting methods (e.g. tape or slip casting) for thicknesses from 100 μm to mm scale (typically <800 μm and <300 μm) for the support layer (electrolyte or anode); - printing methods (e.g. screen, inkjet printing), spraying, lamination, spin coating for thin layers (typically <50 μm), - in addition to printing methods, sputtering methods (e.g. magnetron or gas flow), physical vapor deposition, atomic layer deposition, pulsed laser deposition for ultra-thin layers L1 and L2 (typically <5 μm), For tubular cells, dip coating or injection molding can be used.

[0109] Those skilled in the art may find relevant preparative teachings in the above mentioned articles.

[0110] The method disclosed in one of the documents disclosed above may also be used.

[0111] The composite oxides of the present invention can also be used to prepare solid oxide electrolyzer cells (SOECs). SOECs allow the production of green hydrogen by high-temperature electrolysis (typically 700-800 ° C). Examples of SOECs are described in the paper by Pysik et al., referenced by Renewable and Sustainable Energy Reviews, Vol. 149, October 2021, 111322 ("Alternative and innovative solid oxide electrolysis cell materials: A short review") or https: / / doi.org / 10.1002 / fuce.201900245 ("Long-Term Behavior of a Solid Oxide Electrolyzer (SOEC) Stack").

[0112] The structure of SOEC is very similar to that of SOFC. Therefore, SOEC: - Anode (A * ), a layer (L) comprising or prepared from a complex oxide of the invention and / or a mixed oxide of cerium and gadolinium different from the complex oxide of the invention, and optionally further comprising at least one other inorganic material, - Cathode (C * ) may include.

[0113] However, the anode (A * ) and cathode (C * The accuracy provided above for the anode (C) and cathode (A) must be taken from the accuracy of the cathode (C) and anode (A), respectively, since the SOEC works in a reverse mode compared to the SOFC. For clarity, what has been disclosed above for the SOFC is taken with the following accuracy: anode (A) ⇒ cathode (C * ) and cathode (C) ⇒ anode (A * ) is also valid for SOEC. For example, one example of an SOEC would be constructed as follows: - Cathode (C * ), - Layer (L), - an additional layer (L1) comprising a complex oxide of the invention and optionally further comprising at least one other inorganic material, - Anode (A * ).

[0114] The complex oxide of the present invention can be used in the preparation of a cell disclosed in one of the following documents by replacing the cerium-gadolinium disclosed therein with the complex oxide of the present invention: Korean Patent No. 102305294B1; Chinese Patent No. 113445061; European Patent No. 3793012.

[0115] Composition C containing the complex oxide of the present invention In the context of the present invention, the complex oxide already exhibits a high relative density at a "low" temperature of around 950° C. However, sintering aids may be added to the complex oxide in order to further improve its sinterability. The present invention therefore also relates to a composition C comprising the complex oxide of the present invention and further comprising at least one sintering aid.

[0116] The sintering aid may be, for example, element E, selected from the group of Zn, transition metal elements, rare earth elements or alkali metals. E is in particular selected from the group of transition elements. E may be, for example, selected from the group consisting of Li, Zn, Cu, Co, Fe, Mn, Ni and combinations thereof. Element E may be added in the form of a salt, such as an acetate or nitrate. Element E may be present in the composition in the form of an oxide.

[0117] The proportion of the sintering aid in the composition C may be 0.1-5.0% by weight. It may be higher than 0.5% by weight. It may be lower than 3.0% by weight.

[0118] Composition C may be prepared by a method comprising the steps of: (i) contacting the complex oxide of the present invention with a salt of element E or a precursor of the oxide of element E; (ii) removing the solution; (iii) drying the solid; and (iv) optionally calcining in air. Step (i) may be carried out in a liquid medium such as water or alcohol. The salt of element (E) may be, for example, a nitrate or acetate. The precursor of the oxide of element (E) may be, for example, an acetylacetonate.

[0119] Composition C may be in powder form. For composition C, all the properties disclosed in 1) to 4) are still applicable.

[0120] Composition C can be used to prepare an SOFC or SOEC. Even if the composite oxide of the present invention is replaced with composition C containing the composite oxide of the present invention and a sintering aid, all of the contents disclosed above regarding the SOFC or SOEC are valid. EXAMPLES

[0121] Those skilled in the art will be able to practice the invention disclosed above and in the claims using and in consideration of the examples set forth below.

[0122] In the following examples, cerium(III) nitrate and gadolinium nitrate are used, both of which are obtained by direct attack of the corresponding oxides with nitric acid. The aqueous cerium nitrate solution used to prepare the co-nitric acid solution exhibits a residual acidity of 0.05 mol / L. The aqueous gadolinium nitrate solution used to prepare the co-nitric acid solution exhibits a residual acidity of 0.60 mol / L. The residual acidity was measured by acid-base titration.

[0123] The basic solution used was prepared before each example by dissolving NH4HCO3 (Nissan Chemical) in water. In the following examples 1 to 3, a 200 liter reactor equipped with a stirrer was used.

[0124] Measurement of D16, D50 and D84 The particle size distribution was determined using a laser diffraction analyzer (HORIBA, LA-920). The particles were dispersed in water containing 0.2 wt% hexametaphosphate. A refractive index of 1.20 was used.

[0125] BET specific surface area The BET specific surface area was measured using a Macsorb HM model-1220 from MOUNTECH Co., Ltd. after desorption of the adsorbed species at 210° C. for 30 min.

[0126] Hg porosity Porosity was obtained using an Autopore IV 9500 automated mercury porosimeter following the manufacturer's guidelines after pretreatment for 30 minutes at 210° C. The sample size was approximately 0.2 g, the mercury contact angle was 130°, and the mercury surface tension was 485 dyn / cm.

[0127] X-ray diffraction An Ultima IV X-ray diffractometer equipped with a copper source (CuKα1, λ=1.5406 Å) was used.

[0128] Density and relative density measurements The following methods are and can be used in connection with the present invention.

[0129] [Table 2]

[0130] The specific conditions of use were as follows: - in step i), dimensions of the cuboid: 23 x 7 mm; - Amount of powder to use: approx. 1g, In step ii), the powder is compressed under uniaxial pressure to obtain a compressed sample.

[0131] The strength applied during pressing is 15.8 kN, which corresponds to a pressure of 98 MPa.

[0132] Example 1: Preparation of 40% Gd-complex oxide containing 0.18 mol / L cerium nitrate and 0.12 mol / L gadolinium nitrate (total concentration 0.3 mol / L) Step a): An aqueous solution of cerium(III) nitrate (approximately 3 mol / L) and an aqueous solution of gadolinium nitrate (approximately 2 mol / L) were added to the CeO2:GdO 1.5 = 60:40 (molar ratio) to prepare a co-nitrate solution. This co-nitrate solution (equivalent to 2.6 kg of the complex oxide) was diluted with deionized water to prepare starting solution S (cerium nitrate 0.18 mol / L and gadolinium nitrate 0.12 mol / L, total concentration 0.3 mol / L).

[0133] The starting solution S was added at a constant flow rate to 80.0 L of an aqueous ammonium hydrogen carbonate solution (48.8 g / L) over 30 minutes under stirring at 25° C. to obtain a precipitate containing cerium and gadolinium. The pH of the slurry was 5.9.

[0134] Step b): The slurry obtained at the end of step a) is heat treated at 80° C. for 3 hours in a reactor equipped with air flushing above the liquid level. The slurry is cooled to room temperature. The pH of the slurry is 7.3.

[0135] Step c): The cake obtained at the end of step b) was filtered and washed several times with deionized water until the conductivity of the filtrate was less than 5 mS / cm.

[0136] Step d): The solid obtained at the end of step c) was heated in a furnace under air at a rate of 1.6° C. / min until it reached 800° C. and was kept at 800° C. for 8 hours. It was then allowed to cool naturally in the oven.

[0137] Step e): The calcined solid is pulverized with a hammer mill to obtain a powder with a diameter of D<50 μm, thereby obtaining a powdered complex oxide Ce. 0.6 Gd 0.4 O 2-δ obtained.

[0138] Example 2: Preparation of 40% Gd-composite oxide containing 0.24 mol / L cerium nitrate and 0.16 mol / L gadolinium nitrate (total concentration 0.4 mol / L) Step a): An aqueous solution of cerium(III) nitrate (approximately 3 mol / L) and an aqueous solution of gadolinium nitrate (approximately 2 mol / L) were added to the CeO2:GdO 1.5 = 60:40 (molar ratio) to prepare a mixed solution. This mixed solution (equivalent to 5.2 kg of the composite oxide) was diluted with deionized water to prepare starting solution S (cerium nitrate 0.24 mol / L and gadolinium nitrate 0.16 mol / L, total concentration 0.4 mol / L).

[0139] The starting solution S was added at a constant flow rate to 107.0 L of an aqueous ammonium bicarbonate solution (72.9 g / L) over 45 minutes under stirring at 25° C. to obtain a precipitate slurry containing cerium and gadolinium. The pH reached was 6.0.

[0140] Step b): The slurry obtained at the end of step a) is heat treated at 80° C. for 3 hours in a reactor equipped with air flushing above the liquid level. The slurry is cooled to room temperature. The pH reached is 7.4.

[0141] Step c): The slurry obtained at the end of step b) was filtered and washed several times with deionized water until the conductivity of the filtrate was below 5 mS / cm.

[0142] Step d): The cake obtained at the end of step c) was heated in a furnace under air at a rate of 1.6° C. / min until it reached 800° C. and was kept at 800° C. for 8 hours. It was then allowed to cool naturally in the oven.

[0143] Step e): The calcined solid is pulverized in a hammer mill to obtain a powder with a diameter of D<50 μm, thereby obtaining powdered Ce. 0.6 Gd 0.4 O 2-δ obtained.

[0144] Example 3: Preparation of a complex oxide containing 30% Gd A 30% Gd composite oxide was prepared in the same manner as in Example 1, with the molar ratio r set to 3.32. Co-nitrate solution: CeO2:GdO 1.5 =70:30 (molar ratio).

[0145] Comparative Example 1: Preparation of a complex oxide containing 40% Gd-cerium nitrate 0.18 mol / L and gadolinium nitrate 0.12 mol / L (total concentration 0.3 mol / L) by adapting the method disclosed in Example 1 of EP 1 484 282 B1. The recipe disclosed in Example 1 of EP 1 484 282 B1 concerns a complex oxide containing only 10% Gd, therefore this recipe was followed but with a modification regarding the composition of the complex oxide (40% Gd instead of 10% Gd).

[0146] Aqueous solutions of cerium nitrate (3 mol / L) and gadolinium nitrate (2 mol / L) were used to prepare CeO2:GdO 1.5 A mixed solution was prepared by mixing them at a molar ratio of 60:40. This solution (equivalent to 20 g of the complex oxide) was diluted with deionized water to prepare a 0.3 mol / L starting solution.

[0147] 0.4 L of the prepared 75 g / L ammonium bicarbonate aqueous solution was added to the starting solution under stirring at 25°C to prepare a precipitate. 20 mL of a 100 g / L ammonium bicarbonate aqueous solution was further added to this slurry. The pH of the slurry was 6.5. This slurry was heated at 100°C for 3 hours under atmospheric pressure in a flask equipped with a reflux condenser. Thereafter, filtration and washing were repeated 10 times using deionized water, and the conductivity of the filtrate was 0.27 mS / cm. The obtained precipitate was calcined in air at 700°C for 5 hours, then crushed in a mortar to obtain 20 g of powdered Ce. 0.6 Gd 0.4 O 2-δ obtained.

[0148] The composition of the obtained powder was confirmed using an ICP emission spectrophotometer (Hitachi High-Tech Corporation, inductively coupled plasma emission spectrophotometer, PS-3500DD).

[0149] The composite oxides of Examples 1 and 2 exhibit different properties from the composite oxide of the Comparative Example.

[0150] In particular, it can be seen that the relative densities of the composite oxides of Examples 1 and 2 are higher at 950° C. and 1000° C. As can be seen in Table I, other properties are also different.

[0151] [Table 3]

Claims

1. A complex oxide based on cerium and gadolinium, the proportion of gadolinium being in the range greater than 22.0 mol % and not greater than 45.0 mol %, said proportion corresponding to the molar ratio Gd / (Ce+Gd) expressed in %.

2. CeO 2 and Gd 2 O 3 % and ≦45.0 mol %, said proportion corresponding to a molar ratio Gd / (Ce+Gd) expressed in %.

3. The ratio of Gd is 30.0 to 45.0 mol %, or 35.0 to 45.0 mol %, or 37.0 to 43.0 mol %, or 38.0 to 42.0 mol %, or 39.0 to 41.0 mol %, or 39.5 to 40.5 mol %, or 28.0 to 32.0 mol %, or 29.0 to 31.0 mol %, or 29.5 to 30.5 mol% 3. The complex oxide according to claim 1 or 2, wherein

4. 4. The complex oxide according to claim 1, wherein an X-ray diffraction diffractogram (CuKα1, λ=1.5406 angstroms) of the complex oxide shows a solid solution pattern.

5. The complex oxide according to any one of claims 1 to 4, wherein the X-ray diffractogram (CuKα1, λ = 1.5406 angstroms) of the complex oxide shows a peak P at 2θ of 27.0 to 30.0°.

6. 6. The complex oxide of claim 5, wherein peak P is of highest intensity on the diffractogram.

7. After sintering the pressed sample at 1000° C. for 5 hours in air, the relative density RD is at least 94.0%, preferably at least 95.0%. 1000℃/5h The complex oxide according to any one of claims 1 to 6, wherein

8. After sintering the compressed samples at 1000°C for 5 hours in air, the relative density RD was up to 98.0%. 1000℃/5h The complex oxide according to any one of claims 1 to 7, wherein

9. After sintering the compressed samples at 1000°C for 5 hours in air, the relative density RD was up to 96.0%. 1000℃/5h The complex oxide according to any one of claims 1 to 8, wherein

10. R.D. 1000℃/5h The complex oxide according to any one of claims 7 to 9, wherein the content of the oxide is 94.0% to 98.0%.

11. After sintering the pressed sample in air at 950° C. for 5 hours, the relative density RD is at least 80.0%, preferably at least 88.0%. 950℃/5h The complex oxide according to any one of claims 1 to 10, wherein

12. After sintering the compressed samples at 950° C. for 5 hours in air, the relative density RD was up to 94.0%. 950℃/5h The complex oxide according to any one of claims 1 to 11, wherein

13. After sintering the compressed samples in air at 950° C. for 5 hours, the relative density RD of up to 90.0% was observed. 950℃/5h The complex oxide according to any one of claims 1 to 12, wherein

14. After sintering the pressed sample in air at 1100° C. for 5 hours, the relative density RD is at least 96.0%, preferably at least 97.0%. 1100℃/5h The complex oxide according to any one of claims 1 to 13, wherein

15. After sintering the compressed samples at 1100°C for 5 hours in air, the relative density RD was up to 99.0%. 1100℃/5h The complex oxide according to any one of claims 1 to 14, wherein

16. After sintering the pressed samples at 1100°C for 5 hours in air, the relative density RD was up to 98.0%. 1100℃/5h The complex oxide according to any one of claims 1 to 15, wherein

17. After sintering the pressed sample at 1200° C. for 5 hours in air, the relative density RD is at least 99.0%, preferably at least 99.5%. 1200℃/5h The complex oxide according to any one of claims 1 to 16, wherein

18. The relative density is given by the formula: RD=density in % / absolute density×100, where the density is measured on the pressed sample of the composite oxide after firing the pressed sample in air at the temperature of the test (950° C., 1000° C., 1100° C. or 1200° C.) for 5 hours, and the absolute density is given in the following table: [Table 1] The complex oxide according to any one of claims 7 to 17,

19. The compressed sample is i) the powder of said composite oxide is weighed and introduced into a molding die; ii) the powder is compressed under pressure; iii) the compressed sample obtained at the end of step ii) is removed from the mould; iv) the pressed samples are then calcined in air at the target temperature for 5 hours; v) the density of the fired pressed sample is measured; vi) then, the relative density is calculated. The complex oxide according to any one of claims 7 to 18, which is prepared by

20. Step v) is v1) the calcined compressed sample is weighed (weight in g); v2) The volume of the compressed sample is measured (cm 3 the volume in units of mass), the compressed sample being in the shape of a parallelepiped, and the volume of the parallelepiped being Volume = length (cm) x width (cm) x height (cm) The method is given by The complex oxide according to claim 19, wherein the reaction is carried out using

21. A complex oxide according to any one of claims 7 to 20, wherein the compressed sample is obtained by applying a pressure of at least 95 MPa, preferably at least 98 MPa.

22. The complex oxide according to any one of claims 7 to 21, wherein the compressed sample is obtained by applying a strength of 15.8 kN.

23. A complex oxide according to any one of claims 19 to 22, wherein the forming tool has the shape of a parallelepiped, in particular with dimensions 23 x 7 mm.

24. 24. A complex oxide according to claim 1, which in the range of pores with a diameter of up to 200 nm exhibits a peak with a maximum value corresponding to a pore diameter Dp determined by mercury porosimetry of 30 to 100 nm, more particularly 30 to 70 nm.

25. The peak having the maximum value at Dp is - less than 80 nm, or - less than 70 nm, or - less than 60 nm, or - less than 50 nm, or - less than 40 nm, or - less than 30 nm, or - Less than 20 nm 25. The complex oxide according to claim 24, wherein the peak has a half-width of:

26. 26. A complex oxide according to claim 24 or 25, in which the porogram obtained by Hg porosity shows a single peak in the range of pores with a diameter of 200 nm or less.

27. The pore volume (Vp) of said pores having a diameter of 200 nm or less, as determined by Hg porosimetry, is less than 0.40 mL / g, more particularly less than 0.35 mL / g, and even more particularly less than 0.30 mL / g. <200nm The complex oxide according to any one of claims 1 to 26, wherein

28. The pore volume (Vp) of the pores having a diameter of 200 nm or less, determined by Hg porosimetry, is greater than 0.10 mL / g. <200nm The complex oxide according to any one of claims 1 to 27, wherein

29. 5 to 40 m 2 The complex oxide according to any one of claims 1 to 28, having a BET specific surface area of ​​1 / g.

30. The BET specific surface area is 10 to 35 m 2 / g, or 25 to 30 m 2 / g, or 25 to 30 m 2 The complex oxide according to any one of claims 1 to 29, wherein the Mo content is 1 / g.

31. The particle size distribution in volume, obtained by laser diffraction, has the following characteristics: a population P1 centered on a diameter D1 of less than 3.0 μm, and / or - a population P2 centered on a diameter D2 greater than 8.0 μm and the expression "populations centered on a diameter D" means that on the distribution curve, a peak is observed whose maximum value is located at D.

32. In the region of diameters less than 100 μm, the distribution has the following characteristics: a population P1 centered on a diameter D1 of less than 3.0 μm, and / or - a population P2 centered on a diameter D2 greater than 8.0 μm 32. The complex oxide of claim 31, which exhibits two populations P1 and P2 having the following formula:

33. 33. The complex oxide of claim 31 or 32, wherein the distribution includes a shoulder region about the peak of population P1.

34. The complex oxide according to any one of claims 31 to 33, wherein D1 is 0.1 to 3.0 µm.

35. The complex oxide according to any one of claims 31 to 33, wherein D1 is 0.1 to 1.0 µm.

36. The complex oxide according to any one of claims 31 to 35, wherein D2 is 8.0 to 100.0 µm.

37. The complex oxide according to any one of claims 31 to 35, wherein D2 is 10.0 to 100.0 µm.

38. The complex oxide according to any one of claims 31 to 35, wherein D2 is 10.0 to 50.0 µm.

39. The ratio H2 / H1 of the heights H1 and H2 of the two peaks P1 and P2, respectively, is - higher than 0.1, or - higher than 0.3, or - higher than 1.0, or - higher than 1.

5.

40. The ratio H2 / H1 of the heights H1 and H2 of the two peaks of P1 and P2, respectively, is - lower than 7.0, or - lower than 5.5, or - lower than 1.0, or - lower than 0.8, or - lower than 0.

5.

41. The complex oxide according to any one of claims 1 to 40, wherein D50, corresponding to the median of the particle size volume distribution obtained by laser diffraction, is 0.1 to 15.0 µm.

42. The complex oxide according to any one of claims 1 to 41, wherein D16, the diameter at which 16% of the particles have a diameter less than D16, determined from the distribution in volume of the particle size obtained by laser diffraction, is 0.1 to 4.0 μm.

43. The complex oxide according to any one of claims 1 to 42, wherein D84, the diameter at which 84% of the particles have a diameter less than D84, determined from the distribution in volume of the particle size obtained by laser diffraction, is 10.0 to 50.0 μm.

44. A composition C comprising the complex oxide according to any one of claims 1 to 43 and a sintering aid.

45. 45. Composition C of claim 44, wherein the sintering aid is an element E selected from the group consisting of Li, Zn, Cu, Co, Fe, Mn, Ni, and combinations thereof.

46. 46. ​​Composition C according to claim 44 or 45, wherein the sintering aid is element E in the form of an oxide.

47. Composition C according to any one of claims 44 to 46, wherein the proportion of the sintering aid in the composition is 0.1 to 5.0% by weight.

48. Composition C according to any one of claims 44 to 47, exhibiting the properties according to any one of claims 7 to 42.

49. Use of a complex oxide according to any one of claims 1 to 43 for the preparation of an SOEC or SOFC.

50. Use of composition C according to any one of claims 44 to 48 for the preparation of an SOEC or SOFC.

51. A process for preparing a complex oxide according to any one of claims 1 to 43, comprising the steps of: a) Cerium nitrate (Ce III ) and gadolinium nitrate are added to the aqueous solution S of ammonium bicarbonate (NH 4 HCO 3 ) to a basic aqueous solution of 1,2-dichlorophenyl ether, thereby forming a precipitate; b) heating the aqueous slurry containing said precipitate obtained at the end of step a) at a temperature between 50° C. and 95° C.; c) recovering the precipitate at the end of step b) and washing with water; d) calcining the solid recovered from step c) in air at a temperature between 600° C. and 1000° C.; e) the calcined solid is ground. A process including.

52. Molar ratio r = NH 4 HCO 3 52. The process of claim 51, wherein / Ce+Gd is from 3.00 to 3.50, more particularly from 3.10 to 3.

45.

53. 49. A SOFC comprising one porous anode (A) and one porous cathode (C) separated by at least one layer (L), wherein at least one of said components (A), (C) or (L) is prepared from or comprises a complex oxide according to any one of claims 1 to 43, or is prepared from or comprises a composition C according to any one of claims 44 to 48.

54. - anode (A), a layer (L) comprising or prepared from a complex oxide of cerium and gadolinium and / or a complex oxide different from said complex oxide according to any one of claims 1 to 44, and optionally further comprising at least one other inorganic material, - cathode (C) 54. The SOFC of claim 53, comprising:

55. One porous anode (A) separated by at least one layer (L). * ) and one porous cathode (C * A SOEC comprising the component (A), * ), (C * 48. An SOEC, wherein at least one of (A) or (B) is prepared from or comprises a complex oxide according to any one of claims 1 to 44, or is prepared from or comprises composition C according to any one of claims 44 to 48.

Citation Information

Patent Citations

  • Method for manufacturing nanosphere particle ceria compound powder having easy sintering property

    JP2004107186A

  • Rare earth element-doped ceria sintered body and its producing method

    JP2008260673A

  • Methods for manufacturing ceria-based composite oxides

    JP2012025593A

  • A composition comprising an oxide of zirconium, cerium, and at least one other rare earth element, having a specific porosity, a method for preparing the same, and its use in catalytic activity.

    JP2013525255A

  • Electrode catalyst of oxygen electrode for solid oxide type steam electrolytic cell, and production method of the same