Adhesive

An adhesive with defined stress and relaxation properties addresses the challenges of repeated deformation in flexible devices, ensuring effective recovery, cuttability, and reliability for foldable and rollable devices.

JP2024541564AInactive Publication Date: 2024-11-08LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024531595
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-06
Filing Date
2023-01-05
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional adhesives for flexible devices, such as foldable or rollable devices, face challenges in effectively coping with repeated deformation due to their low elastic modulus, leading to deteriorated recovery properties, cuttability, and reliability.

Method used

The development of an adhesive with specific physical properties, including low maximum stress (S MAX ) and stress relaxation (S 1200 ) within defined ranges, along with a predetermined ratio (S MAX /S 1200 ) and stress variation (ΔS X1, ΔS X2, ΔS X3, ΔS XL1, ΔS XL50 ) during repeated deformation, ensuring excellent recovery, cuttability, and reliability.

Benefits of technology

The adhesive effectively manages stress during repeated deformation, maintaining excellent recovery properties, cuttability, and reliability, suitable for flexible devices like foldable and rollable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541564000001_ABST
    Figure 2024541564000001_ABST
Patent Text Reader

Abstract

The present application may provide an adhesive suitable for flexible devices and a device including the same. In one example, the present application may provide an adhesive that is applied to flexible devices and effectively responds to repeated deformation and recovery, does not induce defects before and after deformation, and has excellent recovery properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0002056, filed on January 6, 2022, and all contents disclosed in the documents of that patent application are incorporated herein by reference.

[0002] The present application relates to a pressure sensitive adhesive and its uses. [Background technology]

[0003] As a type of flexible device, there are known so-called foldable or rollable devices, etc. Such devices are folded and then unfolded or rolled and then unfolded multiple times.

[0004] Therefore, the adhesive applied to the foldable device must be able to effectively respond to the stress applied during the repeated deformation. Conventionally, in order to obtain such an adhesive, attention has been paid mainly to the elastic modulus of the adhesive, particularly the elastic modulus at low temperatures. It is generally known that the lower the elastic modulus at low temperatures, the more effectively the adhesive can respond to the stress applied by the repeated deformation.

[0005] However, when a pressure sensitive adhesive is designed with only a focus on a low elastic modulus, recovery, reliability, cuttability, and the like tend to decrease.

[0006] As described above, since a foldable or rollable device is folded and then unfolded or rolled and then unfolded multiple times, it is required that the device has the property of returning to its original state after being deformed. However, an adhesive that is simply low in elastic modulus reduces the recovery property.

[0007] Furthermore, during the process of manufacturing a device, the adhesive is cut into a desired shape, but an adhesive with too low an elastic modulus reduces cuttability, and a low elastic modulus is also disadvantageous in terms of the reliability of the adhesive. Summary of the Invention [Problem to be solved by the invention]

[0008] The present application relates to an adhesive. The present application aims to provide an adhesive having excellent recovery, cuttability and reliability while having conformability and stress characteristics that can effectively respond to repeated deformation. The present application also aims to provide uses of the adhesive. In one example, the adhesive can be effectively applied to construct a flexible device such as a foldable device or a rollable device. [Means for solving the problem]

[0009] In the present specification, the physical properties are measured at room temperature unless otherwise specified, in cases where the measurement temperature affects the physical property.

[0010] The term "room temperature" as used herein means a temperature in a state in which the temperature is not particularly increased or decreased, and may mean any temperature within a range of about 10° C. to 30° C., for example, about 15° C. or higher, 18° C. or higher, 20° C. or higher, or about 23° C. or higher, and about 27° C. or lower. Unless otherwise specified, the unit of temperature referred to in this specification is ° C.

[0011] Of the physical properties referred to in this specification, the physical properties are those measured at normal pressure, unless otherwise specified in cases where the measurement pressure affects the physical properties.

[0012] In this specification, the term "normal pressure" refers to pressure in a state where there is no particular increase or decrease in pressure, and generally refers to a pressure of approximately 700 mmHg to 800 mmHg, which is the atmospheric pressure level.

[0013] In the present specification, unless otherwise specified, the physical properties are measured at the natural humidity at room temperature and pressure as described above, in cases where the humidity at which the properties are measured affects the physical properties.

[0014] The present application relates to pressure sensitive adhesives.

[0015] The pressure-sensitive adhesive of the present application exhibits the properties described below, and such properties are useful in devices in which repeated deformation and recovery occur, for example, flexible devices such as foldable devices and rollable devices.

[0016] In one example, the adhesive may exhibit low stress in an environment in which a deformation is instantaneously applied and then maintained for a certain period of time, and may also exhibit the property of relieving the applied stress within a relatively short period of time.

[0017] For example, the adhesive is applied with a shear force at -20°C so that 100% strain is applied within 0.05 seconds, and the maximum stress (S MAX ) may be within a predetermined range.

[0018] The maximum stress S MAX The method for measuring S is described in the Examples of this specification (Stress-Relaxation Measurement Item in the Examples). MAX and S, which will be described later. 1200 may be measured using a measuring device such as an ARES G2 (Advanced Rheometric Expansion System G2) (TA), and the adhesive is applied in a circular shape with a thickness of about 800 μm and a diameter of about 8 mm. MAX The upper limit of the maximum stress S may be about 1 MPa, 0.9 MPa, 0.8 MPa, 0.7 MPa, 0.6 MPa, 0.5 MPa, or 0.4 MPa. MAX There is no particular limit to the lower limit of the maximum stress S MAXThe lower limit of the maximum stress S may be about 0.01 MPa, 0.05 MPa, 0.1 MPa, 0.15 MPa, 0.2 MPa, 0.25 MPa, 0.3 MPa, or 0.35 MPa. MAX may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0019] The adhesive was subjected to a process of maintaining the 100% strain for 1200 seconds, and the stress (S 1200 The stress may also be evaluated by the evaluation method in the Stress-Relaxation measurement item in the Examples of the present specification.

[0020] The stress S 1200 The upper limit of the maximum stress S may be about 12,000 Pa, 11,000 Pa, 10,000 Pa, 9,500 Pa, 9,000 Pa, 8,500 Pa, 8,000 Pa, or 7,500 Pa, and the lower limit may be about 1,000 Pa, 2,000 Pa, 3,000 Pa, 4,000 Pa, 5,000 Pa, 6,000 Pa, 7,000 Pa, or 8,000 Pa. 1200 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0021] An adhesive exhibiting the above-mentioned properties can effectively withstand stress applied to the adhesive in an environment where a momentary deformation is maintained for a certain period of time, and such an adhesive can also exhibit excellent cuttability, workability, recovery, and reliability.

[0022] The adhesive further comprises the maximum stress S MAX and the stress S 1200 Percentage of S MAX / S1200 For example, the ratio S may be within a predetermined range. MAX / S 1200 The lower limit of the ratio S may be about 30, 32, 34, 36, 38, 40, 42, 44, 46, or 48, and the upper limit of the ratio S may be about 60, 58, 56, 54, 52, 50, 48, 46, or 44. MAX / S 1200 may be less than or equal to any of the aforementioned upper limits, or may be greater than or equal to or exceed any of the aforementioned lower limits, or may be less than or equal to any of the aforementioned upper limits but greater than or equal to or exceed any of the aforementioned lower limits.

[0023] The adhesive can effectively withstand stresses applied to the adhesive in an environment where deformations are repeatedly applied instantaneously, and such adhesives can also exhibit excellent cuttability, workability, recovery, and reliability.

[0024] The adhesive has a ΔS represented by the following formula 1: X1 may be within a predetermined range.

[0025] [Formula 1] △S X1 =0.02×(S MAX1 -S MAX50 )

[0026] In formula 1, S MAX1 and S MAX50 is the maximum stress observed at each specific point in the process of applying a shear force to the adhesive according to the sine wave equation.

[0027] That is, in Equation 1, S MAX1 is the maximum stress (unit: Pa) observed within 0 to 2 seconds in the process of applying a shear force to the adhesive for 100 seconds according to the following formula 2, and S MAX50is the maximum stress (unit: Pa) observed within 99 to 100 seconds in the process of applying a shear force according to the following formula 2 to the adhesive for 100 seconds.

[0028] [Formula 2] Sin wave equation=4×sin(1.575×t)

[0029] In Equation 2, t is time (unit: seconds).

[0030] Unless otherwise specified, maximum stress or stress in this specification is in units of Pa.

[0031] The process of applying shear force according to the formula 2 and the method of measurement are described in the Examples section of the present specification (stress measurement section for Sin strain). The application of the shear force is performed at -20°C.

[0032] The shear force may be applied using a measuring device such as ARES G2 (Advanced Rheometric Expansion System G2) (TA). At this time, the adhesive is applied in a circular shape with a thickness of about 800 μm and a diameter of about 8 mm.

[0033] When a shear force is applied to the adhesive according to Equation 2, a certain level of strain is applied to the adhesive for a predetermined time, and then a certain level of strain is applied in the opposite direction. For example, when a shear force is applied according to Equation 2, a shear force is applied for 1 second to apply about 400% strain to the adhesive for 1 second, and then a shear force is applied in the opposite direction for 1 second to apply 0% strain to the adhesive for 1 second. This application of a shear force for 2 seconds is defined as one cycle. In the above, the opposite direction means that a shear force is applied in the opposite direction to the direction of the shear force applied to apply the 400% strain for 1 second.

[0034] Therefore, S in the above formula 1 MAX1 is the maximum stress observed during one cycle, and S MAX50 is the maximum stress observed when the application of the shear force by the above-mentioned shear force application cycle is repeated 50 times, i.e., within the 50th cycle.

[0035] When a shear force is applied in the above manner, a strain similar to a sine curve (sine strain) is applied to the adhesive. Under the strain applied in this manner, ΔS in Equation 1 X1 may be within a predetermined range.

[0036] For example, ΔS in Eq. X1 The upper limit of ΔS may be about 3500 Pa / cycle, 3400 Pa / cycle, 3300 Pa / cycle, 3200 Pa / cycle, 3100 Pa / cycle, 3000 Pa / cycle, 2900 Pa / cycle, 2800 Pa / cycle, 2700 Pa / cycle, 2600 Pa / cycle, 2500 Pa / cycle, 2400 Pa / cycle, or 2300 Pa / cycle, and the lower limit may be about 1000 Pa / cycle, 1200 Pa / cycle, 1400 Pa / cycle, 1600 Pa / cycle, 1800 Pa / cycle, 2000 Pa / cycle, or 2200 Pa / cycle. X1 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0037] S in Eq. MAX50The upper limit of the S may be about 250,000 Pa, 245,000 Pa, 240,000 Pa, 235,000 Pa, 230,000 Pa, 225,000 Pa, 220,000 Pa, 215,000 Pa, 210,000 Pa, 205,000 Pa, 200,000 Pa, 195,000 Pa, 190,000 Pa, or 185,000 Pa, and the lower limit may be about 100,000 Pa, 110,000 Pa, 120,000 Pa, 130,000 Pa, 140,000 Pa, 150,000 Pa, 160,000 Pa, 170,000 Pa, or 180,000 Pa. MAX50 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0038] The adhesive can effectively withstand stresses applied to the adhesive in an environment where deformations are repeatedly applied instantaneously, and such adhesives can also exhibit excellent cuttability, workability, recovery, and reliability.

[0039] The pressure-sensitive adhesive further has a ΔS X2 may be within a predetermined range. A pressure-sensitive adhesive that satisfies the above conditions can more effectively satisfy the physical properties required for flexible devices.

[0040] [Formula 3] △S X2 =0.1×(S MAX1 -S MAX10 )

[0041] In Equation 3, S MAX1 In Equation 1, S MAX1 is the same as:

[0042] In Equation 3, S MAX10 is S in Eq. MAX1 and S. MAX50This is the maximum stress (unit: Pa) observed within 19 to 20 seconds in the process of applying a shear force according to Equation 2 to the adhesive for 100 seconds in the same manner as in determining the maximum stress.

[0043] Such a S MAX10 is the maximum stress observed within the 10th cycle when the shear force application cycle described in Equation 1 is repeated 10 times.

[0044] In Equation 3, △S X2 The upper limit of ΔS may be about 15,000 Pa / cycle, 14,000 Pa / cycle, 13,000 Pa / cycle, 12,000 Pa / cycle, 11,000 Pa / cycle, 10,000 Pa / cycle, or 9,500 Pa / cycle, and the lower limit may be about 5,000 Pa / cycle, 6,000 Pa / cycle, 7,000 Pa / cycle, 8,000 Pa / cycle, 8,500 Pa / cycle, or 9,000 Pa / cycle. X2 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0045] In Equation 3, S MAX10 The upper limit of the S may be about 300,000 Pa, 280,000 Pa, 260,000 Pa, 240,000 Pa, 220,000 Pa, or 210,000 Pa, or may be about 90,000 Pa, 100,000 Pa, 150,000 Pa, or 200,000 Pa. MAX10 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0046] The pressure-sensitive adhesive further has a ΔS X3 may be within a predetermined range. A pressure-sensitive adhesive that satisfies the above conditions can more effectively satisfy the physical properties required for flexible devices.

[0047] [Formula 4] △S X3 =0.025×(S MAX10 -S MAX50 )

[0048] In Equation 4, S MAX10 In Equation 3, S MAX10 is the same as S MAX50 In Equation 1, S MAX50 is the same as:

[0049] The above △S X3 The upper limit of ΔS may be about 700 Pa / cycle, 650 Pa / cycle, or 600 Pa / cycle, and the lower limit of ΔS may be about 100 Pa / cycle, 200 Pa / cycle, 300 Pa / cycle, 400 Pa / cycle, or 550 Pa / cycle. X3 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0050] In formula 1, S MAX1 The upper limit of ΔS may be about 350,000 Pa, 340,000 Pa, 330,000 Pa, 320,000 Pa, 310,000 Pa, or 300,000 Pa, and the lower limit may be about 100,000 Pa, 150,000 Pa, 200,000 Pa, or 250,000 Pa. MAX1 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0051] The pressure-sensitive adhesive further has a ΔS represented by the following formula 5: XL1 may be within a predetermined range. A pressure-sensitive adhesive that satisfies the above conditions can more effectively satisfy the physical properties required for flexible devices.

[0052] [Formula 5] △S XL1 =(S MAX1 -S LAST1 )

[0053] In Equation 5, S MAX1 is S in Eq. MAX1 is the same as:

[0054] In Equation 5, S LAST1 is the stress observed after the adhesive is subjected to a single shear force cycle.

[0055] That is, in Equation 5, S LAST1 is S in Eq. MAX1 and S. MAX50 This is the stress (unit: Pa) observed at 2 seconds in the process of applying a shear force to an adhesive for 100 seconds according to Equation 2 in the same manner as for determining the stress (unit: Pa), i.e., the stress (unit: Pa) observed after 2 seconds have elapsed in the 100-second application process.

[0056] In Equation 5, △S XL1 The upper limit of ΔS may be about 600,000 Pa, 550,000 Pa, 500,000 Pa, or 450,000 Pa, and the lower limit may be about 100,000 Pa, 150,000 Pa, 200,000 Pa, 250,000 Pa, 300,000 Pa, 350,000 Pa, or 400,000 Pa. XL1 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0057] The adhesive has a ΔS represented by the following formula 6: XL50 may be within a predetermined range. A pressure-sensitive adhesive that satisfies the above conditions can more effectively satisfy the physical properties required for flexible devices.

[0058] [Formula 6] △S XL50 =(SMAX50 -S LAST50 )

[0059] In Equation 6, S MAX50 is S in Eq. MAX50 is the same as:

[0060] In Equation 6, S LAST50 is the stress observed after the pressure sensitive adhesive is subjected to 50 shear force cycles.

[0061] That is, in Equation 6, S LAST50 is S in Eq. MAX1 and S. MAX50 The stress (unit: Pa) observed at 100 seconds in the process of applying a shear force according to Equation 2 to the adhesive for 100 seconds in the same manner as in determining the stress (unit: Pa), i.e., the stress (unit: Pa) observed after 100 seconds have elapsed in the 100-second application process.

[0062] In Equation 6, △S XL50 The upper limit of ΔS may be about 500,000 Pa, 480,000 Pa, 460,000 Pa, 440,000 Pa, 420,000 Pa, 400,000 Pa, 380,000 Pa, or 360,000 Pa, and the lower limit may be about 100,000 Pa, 150,000 Pa, 200,000 Pa, 250,000 Pa, 300,000 Pa, or 350,000 Pa. XL50 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0063] The adhesive has a formula 7 below: ΔS XL10 may be within a predetermined range. A pressure-sensitive adhesive that satisfies the above conditions can more effectively satisfy the physical properties required for flexible devices.

[0064] [Formula 7] △S XL10 =(SMAX10 -S LAST10 )

[0065] In Equation 7, S MAX10 is S in Eq. MAX10 is the same as:

[0066] In Equation 7, S LAST10 is the stress observed after the pressure sensitive adhesive is subjected to ten shear stress cycles.

[0067] That is, in Equation 7, S LAST10 is S in Eq. MAX1 and S. MAX50 This is the stress (unit: Pa) observed at 20 seconds in the process of applying a shear force to an adhesive for 100 seconds according to Equation 2 in the same manner as for determining the stress (unit: Pa), i.e., the stress (unit: Pa) observed after 20 seconds have elapsed in the 100-second application process.

[0068] In Equation 7, △S XL10 The upper limit of ΔS may be about 500,000 Pa, 480,000 Pa, 460,000 Pa, 440,000 Pa, 420,000 Pa, 400,000 Pa, or 380,000 Pa, and the lower limit may be about 100,000 Pa, 150,0000 Pa, 200,000 Pa, 250,000 Pa, 300,000 Pa, or 350,000 Pa. XL10 may be less than or equal to any of the upper limits set forth above, or may be less than or equal to any of the upper limits set forth above but greater than or equal to any of the lower limits set forth above.

[0069] The adhesive may have at least one of the aforementioned characteristics, and in one example, may have a combination of two or more of the aforementioned characteristics, and suitably may have all of the aforementioned characteristics.

[0070] Generally, whether an adhesive is suitable for flexible devices such as foldable devices is confirmed by checking the elastic modulus of the adhesive. For example, it is known that adhesives applied to flexible devices are generally advantageous for having a low elastic modulus at low temperatures because they are repeatedly subjected to deformation, and it is common to check whether an adhesive is suitable for flexible devices by checking the elastic modulus of the adhesive, particularly whether the elastic modulus is low at low temperatures.

[0071] However, when focusing only on the low-temperature elastic modulus of the adhesive, problems often arise when the adhesive is applied to an actual flexible device in an environment where the device is subjected to repeated instantaneous deformations, such as being unable to effectively follow the deformations, or, even if it does follow the deformations, not being able to recover sufficiently when the deformation disappears. In some cases, the stress applied to the adhesive under the repeated deformations can adversely affect the performance of the device.

[0072] However, if the adhesive is designed to exhibit one or more of the above-mentioned properties, it can be made to exhibit performance suitable for an actual flexible device when applied to the device.

[0073] The adhesive may further maintain or improve the performance or prevent degradation of the performance of other components when applied to the device.

[0074] For example, the pressure-sensitive adhesive may exhibit a property in which the absolute value of ΔR1 in the following formula 8 falls within a predetermined range.

[0075] [Formula 8] △R1=100×(R5-Ri) / Ri

[0076] In Equation 8, R5 is the resistance of the ITO layer of the ITO film after the process of folding and unfolding a laminate including an ITO (Indium Tin Oxide) film, the adhesive, and a PET (poly(ethyleneterephthalate)) film in that order once every two seconds is repeated 50,000 times, and Ri is the resistance of the ITO layer of the ITO film before the process of folding and unfolding is repeated 50,000 times.

[0077] The adhesive may be applied to a device including an electrode, allowing the properties of the electrode to be stably maintained even when exposed to repeated deformation.

[0078] The upper limit of the absolute value of ΔR1 in formula 8 may be about 200%, 195%, 190%, 185%, 180%, 175%, 170%, 165%, 160%, 155%, 150%, 145%, 140%, 135%, 130%, 125%, 120%, 115%, 110%, 105% or 100%, and the lower limit may be about 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 110%, 120%, 130%, 140% or 150%. The absolute value of ΔR1 may be less than or equal to any of the upper limits described above, or may be less than or equal to any of the upper limits described above but greater than or equal to any of the lower limits described above.

[0079] A method of forming a laminate for determining ΔR1 will be described with reference to Fig. 1. The laminate may be manufactured to have a laminated structure of ITO film / adhesive layer / PET film by laminating an ITO (Indium Tin Oxide) film and a PET (poly(ethylene terephthalate)) film with the adhesive interposed therebetween, as shown in Fig. 1. The laminate may be cut to have horizontal and vertical lengths of about 15 cm and about 2.5 cm, respectively, and applied to the folding.

[0080] The ITO film may be a crystalline ITO (indium tin oxide) layer having a thickness of about 1 μm formed on the surface of a PET (poly(ethylene terephthalate)) film (base film) having a thickness of about 50 μm, and a film having a thickness of about 50 μm may be used as the PET film. The thickness of the adhesive layer applied to the laminate may be adjusted to about 25 μm, and the ITO film is laminated so that the base film is in contact with the adhesive during lamination.

[0081] As shown in Figure 1, a silver paste is printed on the ITO layer of the cut laminate with a width of about 1 cm. Two silver pastes are printed at about 4 cm apart on either side of the center of the ITO layer (the dotted line in the lower diagram of Figure 1), and the printed paste is dried at about 150°C for about 1 hour.

[0082] The folding may be performed using the laminate as a specimen. In this case, the laminate is loaded into a dynamic chamber, and the specimen is folded once at the center (dotted part in the lower diagram of FIG. 1) and unfolded, which constitutes one cycle, and the cycle is repeated. The folding is performed at a curvature of about 2.5R, and the temperature is fixed at -20°C. One cycle of folding and unfolding is performed for 2 seconds, and the folding is performed so that the silver paste of the ITO film is at the top.

[0083] The silver paste is used to determine the initial resistance Ri of the ITO layer before folding, and the resistance R5 of the ITO layer after 50,000 foldings is determined, which can be substituted into Equation 1 to determine ΔR1.

[0084] The adhesive may further maintain the properties of the ITO layer even after further repetitions of the folding.

[0085] For example, the pressure-sensitive adhesive may exhibit a characteristic in which ΔR2 in the following formula 9 or its absolute value falls within a predetermined range.

[0086] [Formula 9] △R2=100×(R10-Ri) / Ri

[0087] In Equation 9, R10 is the resistance of the ITO layer of the ITO film after the process of folding and unfolding a laminate including an ITO (indium tin oxide) film, the adhesive, and a PET (poly(ethylene terephthalate)) film in that order once every two seconds is repeated 100,000 times, and Ri is the resistance of the ITO layer of the ITO film before the process of folding and unfolding is repeated 100,000 times.

[0088] The folding process for determining ΔR2 in Equation 9 is the same as that for determining ΔR1 in Equation 8.

[0089] The upper limit of ΔR2 or its absolute value in Equation 9 is 290%, 285%, 280%, 275%, 270%, 265%, 260%, 255%, 250%, 245%, 240%, 235%, 230%, 225%, 220%, 215%, 210%, 205%, 200%, 195%, 190%, 185%, 180%, 175%, 170%, 165%, 160%, 155%, 150%, 145%, The ΔR2 or its absolute value may be less than or equal to any one of the upper limits described above, or may be less than or equal to any one of the upper limits described above but not less than or equal to any one of the lower limits described above.

[0090] The adhesive may exhibit an excellent recovery rate in addition to the above-mentioned properties. For example, the adhesive may have a lower limit of the recovery rate of about 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82% or 83%, and an upper limit of about 100%, 98%, 96%, 94%, 92%, 90%, 88%, 86%, 84% or 82%. The recovery rate may be equal to or greater than any of the lower limits, or may be equal to or less than any of the upper limits, but equal to or greater than any of the lower limits.

[0091] The recovery rate is the result measured by the recovery rate measurement method in the Examples of this specification.

[0092] The adhesive can exhibit an appropriate modulus of elasticity at low temperatures.

[0093] For example, the upper limit of the elastic modulus of the pressure-sensitive adhesive at -20°C may be about 1 MPa, 0.9 MPa, 0.8 MPa, 0.7 MPa, 0.6 MPa, 0.5 MPa, 0.4 MPa, 0.3 MPa or 0.2 MPa, and the lower limit may be about 0.01 MPa, 0.03 MPa, 0.05 MPa, 0.07 MPa, 0.09 MPa, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa or 0.5 MPa. The elastic modulus may be equal to or less than any of the above upper limits, or may be equal to or less than any of the above upper limits but equal to or greater than any of the above lower limits.

[0094] In addition, the pressure-sensitive adhesive may have a maximum stress in a linear section of a strain-stress curve for confirming the elastic modulus within a predetermined range. For example, the upper limit of the maximum stress may be about 30,000 Pa, 25,000 Pa, 20,000 Pa, 15,000 Pa, 10,000 Pa, or 9,000 Pa, and the lower limit may be about 1,000 Pa, 3,000 Pa, 5,000 Pa, 7,000 Pa, 8,000 Pa, 8,500 Pa, 10,000 Pa, 15,000 Pa, 20,000 Pa, 22,000 Pa, or 24,000 Pa. The maximum stress may be less than or equal to any of the above upper limits, or may be less than or equal to any of the above upper limits but greater than or equal to any of the above lower limits.

[0095] The method for measuring the elastic modulus and maximum stress is described in the Examples of this specification (measurement items of elastic modulus and maximum stress).

[0096] The elastic modulus is Young's modulus, which is obtained by measuring the stress applied to the adhesive while applying a shear force to generate a certain strain, and then graphing the change in stress due to the strain (strain-stress curve, a graph in which the X-axis is strain (%) and the Y-axis is stress (Pa)). The Young's modulus is usually measured in a section where the change in stress with respect to strain is substantially linear in the strain-stress curve. Since the Young's modulus indicates the rate of change in stress due to the applied strain, adhesives having the same Young's modulus may behave differently with respect to stress, and therefore a maximum stress within the linear section may be introduced to reflect this. That is, an adhesive that simultaneously exhibits the Young's modulus and maximum stress can effectively meet the required physical properties of a flexible device.

[0097] In one example, the linear section may be the section from 0.7% to 4% strain in a strain-stress curve shown via an instrument set to generate a constant strain from 0% strain to 400% strain for 1 second, and therefore the maximum stress may be the stress at 4% strain in the strain-stress curve.

[0098] The adhesive can exhibit excellent cuttability, workability, recovery and reliability along with elastic properties suitable for foldable devices. That is, the adhesive can be applied to a foldable device and can effectively follow repeated deformation while exhibiting appropriate recovery, cuttability and reliability.

[0099] In one example, the adhesive exhibiting the above-mentioned properties may be the following adhesive:

[0100] The adhesive may include an adhesive polymer.

[0101] The adhesive polymer may be a polymer known in the art to be capable of forming an adhesive. The adhesiveness, as is well known, refers to the property of being able to adhere and peel by applying pressure at room temperature without using water, solvent, heat, etc.

[0102] In one example, the adhesive polymer may be an acrylic copolymer.

[0103] As used herein, the term copolymer refers to the result of a polymerization reaction of a monomer mixture containing two or more monomers.

[0104] In this specification, the term "monomer unit" refers to the state of a monomer after the polymerization reaction.

[0105] The term "acrylic copolymer" as used herein refers to a copolymer containing acrylic monomer units as a main component. In this case, the main component refers to the case where the proportion of the acrylic monomer units in the acrylic copolymer is 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more. There is no particular upper limit to the content of the acrylic monomer units in the acrylic copolymer. For example, the acrylic copolymer may contain 100% by weight or less or less than 100% by weight of the acrylic monomer units.

[0106] As used herein, the term acrylic monomer means acrylic acid, methacrylic acid, an acrylic acid ester, or a methacrylic acid ester.

[0107] As used herein, the term (meth)acrylic means acrylic or methacrylic.

[0108] In the pressure-sensitive adhesive of the present application, when the adhesive polymer is crosslinkable, the polymer may be in a crosslinked state within the pressure-sensitive adhesive. Such a pressure-sensitive adhesive may be formed, for example, by crosslinking a pressure-sensitive adhesive composition containing the adhesive polymer.

[0109] The adhesive may contain the adhesive polymer as a main component. For example, the proportion of the adhesive polymer in the adhesive composition may be about 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, 95% by weight or more, 97% by weight or more, or 99% by weight or more. There is no particular upper limit to the content of the adhesive polymer in the adhesive. For example, the adhesive polymer may be contained in the adhesive at 100% by weight or less or less than 100% by weight.

[0110] In the present application, a specific acrylic copolymer may be applied as the adhesive polymer to form the specific adhesive.

[0111] For example, the acrylic copolymer may be an acrylic copolymer exhibiting crystallinity. In the present application, the acrylic copolymer exhibiting crystallinity means that the melting point (Tm, melting point) is confirmed by the DSC (Differential Scanning Calorimeter) measurement method described in the examples of the present specification. In the present specification, the melting point and the melting temperature have the same meaning.

[0112] Acrylic copolymers are generally non-crystalline. In the present application, crystallinity is imparted to the acrylic copolymer through control of the monomer units of the copolymer.

[0113] In the present application, the acrylic copolymer may be a copolymer having both a glass transition temperature (Tg) and a melting point, thereby effectively forming a desired adhesive. In the above, having both a glass transition temperature and a melting point means that the glass transition temperature and the melting point are confirmed simultaneously in the DSC (Differential Scanning Calorimeter) measurement method.

[0114] The melting point and glass transition temperature may be adjusted to ensure desired properties.

[0115] For example, the upper limit of the glass transition temperature of the acrylic copolymer may be about −30° C., −35° C., −40° C., −45° C., −50° C., −55° C. or −60° C., and the lower limit may be about −100° C., −90° C., −80° C., −70° C. or −65° C. The glass transition temperature may be equal to or lower than any of the above upper limits, or may be equal to or lower than any of the above upper limits but equal to or higher than any of the above lower limits.

[0116] The upper limit of the melting point of the acrylic copolymer may be about -10° C., -15° C., -20° C., -25° C., -30° C., -35° C. or -40° C., and the lower limit may be about -80° C., -75° C., -70° C., -65° C., -60° C., -55° C., -50° C. or -45° C. The melting point may be equal to or less than any of the above upper limits, or may be equal to or less than any of the above upper limits but equal to or greater than any of the above lower limits.

[0117] The difference between the melting point (Tm) and the glass transition temperature (Tg) of the acrylic copolymer may be within a predetermined range. The difference is the melting point (Tm) minus the glass transition temperature (Tg) (Tm-Tg). The lower limit of the difference may be about 5°C, 10°C, or 15°C, and the upper limit may be about 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, or 20°C. The difference between the melting point (Tm) and the glass transition temperature (Tg) may be less than or equal to any of the upper limits described above, or may be greater than or equal to any of the lower limits described above, or may be less than or equal to any of the upper limits described above but greater than or equal to any of the lower limits described above.

[0118] By using an acrylic copolymer exhibiting such properties, desired properties can be efficiently secured.

[0119] To ensure appropriate properties, the weight average molecular weight of the acrylic copolymer may be adjusted. The weight average molecular weight and the molecular weight distribution described below are measured by gel permeation chromatography (GPC) as described herein.

[0120] The lower limit of the weight average molecular weight of the acrylic copolymer may be about 1 million, 1.1 million, 1.2 million, 1.3 million, 1.4 million, or 1.5 million, and the upper limit may be about 5 million, 4 million, 3 million, 2.5 million, 2 million, 1.9 million, 1.8 million, 1.7 million, 1.6 million, or 1.55 million. The weight average molecular weight may be less than or equal to any of the above upper limits, or greater than or equal to any of the above lower limits, or less than or equal to any of the above upper limits but greater than or equal to any of the above lower limits.

[0121] The acrylic copolymer may have a molecular weight distribution within a predetermined range. In addition, the acrylic copolymer is preferably crosslinked with a suitable crosslinking agent according to the molecular weight distribution and then included in the adhesive. The molecular weight distribution is a value (Mw / Mn) obtained by dividing the weight average molecular weight (Mw) by the number average molecular weight (Mn). In general, it is recognized that the smaller the molecular weight distribution, the smaller the proportion of components with relatively low molecular weights and components with relatively high molecular weights based on the average molecular weight in the copolymer, the more uniform the composition of the copolymer, and the more stable the flow properties such as elastic modulus. However, the properties suitable for flexible devices include mutually contradictory properties such as conformability and recovery to deformation, conformability, cuttability, and reliability, and therefore, in order to stably ensure such properties, it may be necessary to adjust the molecular weight distribution according to the type of crosslinking agent applied.

[0122] In one example, when the acrylic copolymer is crosslinked with a thermal crosslinking agent described later, the lower limit of the molecular weight distribution may be about 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9 or 5.0, and the upper limit may be about 10, 9.5, 9, 8.5, 8, 7.5, 7, 6.5, 6 or 5.5. The molecular weight distribution may be less than or equal to any of the upper limits described above, or greater than or equal to any of the lower limits described above, or less than or equal to any of the upper limits described above but greater than or equal to any of the lower limits described above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a thermal crosslinking agent described later. It is appropriate that such a type of acrylic copolymer is crosslinked only by the thermal crosslinking agent. For example, the acrylic copolymer is crosslinked only by the thermal crosslinking agent, or when the thermal crosslinking agent and the radical crosslinking agent are simultaneously applied to crosslink the acrylic copolymer, it is appropriate that the ratio (B / A) of the weight (A) of the thermal crosslinking agent to the weight (B) of the radical crosslinking agent used is equal to or less than a certain level. For example, the upper limit of the weight ratio B / A may be about 0.5, 0.4, 0.3, 0.2, 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003, 0.0002 or 0.0001, and the lower limit may be about 0. The ratio B / A may be equal to or less than any of the upper limits described above, or may be equal to or less than any of the upper limits and equal to or more than any of the lower limits described above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a radical crosslinking agent described below.

[0123] In one example, when the acrylic copolymer is crosslinked with a radical crosslinking agent described later, the lower limit of the molecular weight distribution may be about 0.5, 1, 1.5 or 2, and the upper limit may be about 3, 2.8, 2.6 or 2.4. The molecular weight distribution may be below or below any of the upper limits described above, or above or above any of the lower limits described above, or below or below any of the upper limits described above but above or above any of the lower limits described above. An acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a radical crosslinking agent described later. An acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a thermal crosslinking agent described later. An acrylic copolymer of such a type is suitable for crosslinking only with the radical crosslinking agent. For example, when the acrylic copolymer is crosslinked only by the radical crosslinking agent, or when the thermal crosslinking agent and the radical crosslinking agent are simultaneously applied to crosslink the acrylic copolymer, it is appropriate that the ratio (C / D) of the weight of the thermal crosslinking agent (C) to the weight of the radical crosslinking agent (D) used is equal to or less than a certain level. For example, the upper limit of the weight ratio C / D may be about 0.5, 0.4, 0.3, 0.2, 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003, 0.0002 or 0.0001, and the lower limit may be about 0. The ratio C / D may be less than or equal to any of the upper limits described above, or may be less than or equal to any of the upper limits and greater than or equal to any of the lower limits described above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a radical crosslinking agent described below.

[0124] The method for adjusting the molecular weight distribution of the acrylic copolymer is known per se. For example, the molecular weight distribution can be controlled by one or more methods selected from the following: use of a molecular weight regulator, adjustment of the ratio of an initiator, and / or adjustment of the polymerization time.

[0125] Such an acrylic copolymer may contain at least an alkyl (meth)acrylate unit, a unit of the following formula 1, and a polar functional group-containing unit.

[0126] Moreover, the term "unit" means a monomer unit.

[0127] [ka]

[0128] In Chemical formula 1, R1 represents a hydrogen atom or an alkyl group, and R2 represents an alkyl group having 11 to 13 carbon atoms.

[0129] Acrylic copolymers containing the above monomer units are effective in forming the desired adhesive.

[0130] The acrylic copolymer may be formed from the above-mentioned crystalline copolymer with a predetermined ratio of the unit of Chemical Formula 1 and / or the polar functional group-containing unit, or may be formed from a copolymer having similar properties. In addition, by forming such a crystalline copolymer with the above-mentioned molecular weight distribution, a pressure-sensitive adhesive that effectively satisfies the desired characteristics can be obtained.

[0131] For example, when the units of Chemical 1 are present in a predetermined ratio, and when the units of Chemical 1 interact with polar functional groups present in a predetermined ratio, such a copolymer may exhibit crystallinity or at least a property similar to crystallinity. When a copolymer having crystallinity or a property similar to crystallinity is applied, a pressure-sensitive adhesive having the above-mentioned properties can be effectively formed. Therefore, a pressure-sensitive adhesive having the above-mentioned elastic modulus properties can be effectively formed through a pressure-sensitive adhesive to which such a copolymer is applied.

[0132] As the alkyl(meth)acrylate unit contained in the copolymer, for example, a unit derived from an alkyl(meth)acrylate having an alkyl group having 1 to 10 carbon atoms may be used. In other examples, the alkyl group may be an alkyl group having 2 to 20 carbon atoms, 3 to 10 carbon atoms, 4 to 10 carbon atoms, 4 to 10 carbon atoms, 4 to 9 carbon atoms, or 4 to 8 carbon atoms. The alkyl group may be linear or branched, and may be substituted or unsubstituted. In one example, the unit may be formed using an alkyl(meth)acrylate having a linear or branched, unsubstituted alkyl group as the alkyl group.

[0133] Examples of the alkyl (meth)acrylate include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, isononyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate.

[0134] The acrylic copolymer may contain the alkyl (meth)acrylate unit at a predetermined ratio. For example, the lower limit of the content of the unit in the copolymer may be about 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or 40 wt%, and the upper limit may be about 60 wt%, 55 wt%, 50 wt%, 45 wt%, or 40 wt%. A desired adhesive may be effectively formed within such a range. The ratio may be less than or equal to any of the upper limits, or may be greater than or equal to any of the lower limits, or may be less than or equal to any of the upper limits, but greater than or equal to any of the lower limits.

[0135] The polar functional group-containing unit is a unit formed by a monomer having a polar functional group. Such a monomer usually contains both a polymerizable group (e.g., a carbon-carbon double bond) and a polar functional group.

[0136] Examples of the monomer having a polar functional group include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and a nitrogen-containing monomer. In the present application, it is particularly advantageous to apply a hydroxyl group-containing monomer, but the present invention is not limited thereto.

[0137] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxypolyethylene glycol (meth)acrylate, or 2-hydroxypolypropylene glycol (meth)acrylate, and examples of carboxyl group-containing monomers include (meth)acrylic acid, 2-(meth)acryloyloxyacetic acid, 3-(meth)acryloyloxypropyl acid, 4-(meth)acryloyloxybutyric acid, acrylic acid dimer, itaconic acid, maleic acid, and maleic anhydride, and examples of nitrogen-containing monomers include, but are not limited to, (meth)acrylamide, N-vinylpyrrolidone, or N-vinylcaprolactam. One or more of the above may be used in combination.

[0138] In one example, the polar functional group-containing unit may be a hydroxy-containing monomer unit, specifically a hydroxyalkyl(meth)acrylate unit, in which the carbon number of the alkyl in the hydroxyalkyl moiety is 1 to 20, 1 to 16, 1 to 12, 1 to 8, 1 to 4, or 2 to 4. The alkyl in the hydroxyalkyl moiety may be linear or branched.

[0139] The lower limit of the weight of the polar functional group-containing unit relative to 100 parts by weight of the alkyl (meth)acrylate unit may be about 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, or 50 parts by weight, and the upper limit of the polar functional group-containing unit may be about 200 parts by weight, 195 parts by weight, 190 parts by weight, 185 parts by weight, 180 parts by weight, 175 parts by weight, 170 parts by weight, 165 parts by weight, 160 parts by weight, 175 parts by weight, 17 ... It may be about 0 parts by weight, 155 parts by weight, 150 parts by weight, 145 parts by weight, 140 parts by weight, 135 parts by weight, 130 parts by weight, 125 parts by weight, 120 parts by weight, 115 parts by weight, 110 parts by weight, 105 parts by weight, 100 parts by weight, 95 parts by weight, 90 parts by weight, 85 parts by weight, 80 parts by weight, 75 parts by weight, 70 parts by weight, 65 parts by weight, 60 parts by weight, 55 parts by weight, 50 parts by weight, 45 parts by weight, 40 parts by weight, or 38 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or greater than or equal to any of the lower limits mentioned above, or less than or equal to any of the upper limits mentioned above, but greater than or equal to any of the lower limits mentioned above. Under such a ratio, the durability, adhesion, and peel strength of the adhesive may be stably maintained.

[0140] The unit of Chemical Formula 1 is a unit containing a long-chain alkyl group, and when such a unit is contained in a copolymer in a certain proportion or more, it can interact with a polar functional group depending on the case and impart crystallinity or crystal-like properties to the copolymer.

[0141] In the unit of Chemical Formula 1, R1 may be hydrogen or an alkyl group having 1 to 4 carbon atoms, specifically, hydrogen, a methyl group, or an ethyl group.

[0142] In Chemical formula 1, R2 is an alkyl group having 11 to 13 carbon atoms, and such an alkyl group may be linear or branched, and may be substituted or unsubstituted. In one example, R2 may be a linear, unsubstituted alkyl group. For example, lauryl (meth)acrylate and / or tetradecyl (meth)acrylate may be used to form the unit of Chemical formula 1.

[0143] The lower limit of the weight part of the unit of Chemical Formula 1 relative to 100 parts by weight of the alkyl (meth)acrylate unit is 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, 105 parts by weight, 110 parts by weight, 115 parts by weight, 120 parts by weight, 125 parts by weight, 130 parts by weight, 135 parts by weight, 140 parts by weight, 145 parts by weight, 150 parts by weight, 155 parts by weight, 160 parts by weight, 175 parts by weight, 180 parts by weight, 185 parts by weight, 190 parts by weight, 195 parts by weight, 200 parts by weight, 205 parts by weight, 210 parts by weight, 215 parts by weight, 220 parts by weight, 225 parts by weight, 230 parts by weight, 235 parts by weight, 240 parts by weight, 245 parts by weight, 250 parts by weight, 260 parts by weight, 270 parts by weight, 280 parts by weight, 290 parts by weight, 300 parts by weight, 310 parts by weight, 320 parts by weight, 330 parts by weight, 340 parts by weight, 350 parts by weight, 360 parts by weight, 370 parts by weight, 380 parts by weight, 390 parts by weight, 400 parts by weight, 410 parts by weight, 420 parts by weight, 430 parts by weight, 440 parts by weight, 450 parts by weight, 460 parts by weight, 470 parts by weight, 480 parts by weight, 490 parts by weight, 500 parts by weight, 510 parts by weight, 520 parts by weight, 5 It may be about 40 parts by weight, 245 parts by weight, 250 parts by weight, 255 parts by weight, 260 parts by weight, 275 parts by weight, 280 parts by weight, 285 parts by weight, 290 parts by weight, 295 parts by weight, or 300 parts by weight, and the upper limit is 600 parts by weight, 595 parts by weight, 590 parts by weight, 585 parts by weight, 580 parts by weight, 575 parts by weight, 570 parts by weight, 565 parts by weight, 560 parts by weight, 555 parts by weight, 550 parts by weight, 545 parts by weight, 540 parts by weight, 535 parts by weight, 530 parts by weight, 525 parts by weight, 520 parts by weight, 515 parts by weight, 510 parts by weight, 505 parts by weight, 500 parts by weight, 495 parts by weight, 490 parts by weight, and the upper limit is about ... Parts by weight, 485 parts by weight, 480 parts by weight, 475 parts by weight, 470 parts by weight, 465 parts by weight, 460 parts by weight, 455 parts by weight, 450 parts by weight, 445 parts by weight, 440 parts by weight, 435 parts by weight, 430 parts by weight, 425 parts by weight, 420 parts by weight, 415 parts by weight, 410 parts by weight, 405 parts by weight, 400 parts by weight Parts by weight, 395 parts by weight, 390 parts by weight, 385 parts by weight, 380 parts by weight, 375 parts by weight, 370 parts by weight, 365 parts by weight, 360 parts by weight, 355 parts by weight, 350 parts by weight, 345 parts by weight, 340 parts by weight, 335 parts by weight, 330 parts by weight, 325 parts by weight, 320 parts by weight, 315 parts by weight, 31 0 parts by weight, 305 parts by weight, 300 parts by weight, 295 parts by weight, 290 parts by weight, 285 parts by weight, 280 parts by weight, 275 parts by weight, 270 parts by weight, 265 parts by weight, 260 parts by weight, 255 parts by weight, 250 parts by weight, 245 parts by weight, 240 parts by weight, 235 parts by weight, 230 parts by weight, 225 parts by weight, 2 20 parts by weight, 215 parts by weight, 210 parts by weight, 205 parts by weight, 200 parts by weight, 195 parts by weight, 190 parts by weight, 185 parts by weight, 180 parts by weight, 175 parts by weight, 170 parts by weight, 165 parts by weight, 160 parts by weight, 155 parts by weight, 150 parts by weight, 145 parts by weight, 140 parts by weight, 135 parts by weight,The ratio may be about 130 parts by weight, 125 parts by weight, 120 parts by weight, 115 parts by weight, 110 parts by weight, 105 parts by weight, or 100 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or greater than or equal to any of the lower limits mentioned above, or less than or equal to any of the upper limits mentioned above but greater than or equal to any of the lower limits mentioned above.

[0144] The ratio of the monomer units may be adjusted so that the acrylic copolymer simultaneously exhibits the above-mentioned glass transition temperature and melting point.

[0145] That is, the acrylic copolymer containing the above-mentioned three types of monomer units in a certain ratio is likely to have crystallinity or exhibit properties similar to crystallinity, but the composition of the acrylic copolymer may be further adjusted so that it simultaneously has the above-mentioned melting point and glass transition temperature.

[0146] For example, in order for the acrylic copolymer to exhibit the above-mentioned crystallinity, the units of Chemical formula 1 among the above-mentioned units must be contained in an amount of at least 80 parts by weight relative to 100 parts by weight of the alkyl (meth)acrylate units. In another example, the ratio of the units of Chemical formula 1 in the crystalline acrylic copolymer is about 85 parts by weight or more, 95 parts by weight or more, or 100 parts by weight or more relative to 100 parts by weight of the alkyl (meth)acrylate units, or 500 parts by weight or less, 495 parts by weight or less, 490 parts by weight or less, 485 parts by weight or less, 480 parts by weight or less, 475 parts by weight or less, 470 parts by weight or less, 465 parts by weight or less, 460 parts by weight or less, 455 parts by weight or less, 450 parts by weight or less, 445 ... 0 parts by weight or less, 435 parts by weight or less, 430 parts by weight or less, 425 parts by weight or less, 420 parts by weight or less, 415 parts by weight or less, 410 parts by weight or less, 405 parts by weight or less, 400 parts by weight or less, 395 parts by weight or less, 390 parts by weight or less, 385 parts by weight or less , 380 parts by weight or less, 375 parts by weight or less, 370 parts by weight or less, 365 parts by weight or less, 360 parts by weight or less, 355 parts by weight or less, 350 parts by weight or less, 345 parts by weight or less, 340 parts by weight or less, 335 parts by weight or less, 330 parts by weight or less, 325 parts by weight 320 parts by weight or less, 315 parts by weight or less, 310 parts by weight or less, 305 parts by weight or less, 300 parts by weight or less, 295 parts by weight or less, 290 parts by weight or less, 285 parts by weight or less, 280 parts by weight or less, 275 parts by weight or less, 270 parts by weight or less, 26 5 parts by weight or less, 260 parts by weight or less, 255 parts by weight or less, 250 parts by weight or less, 245 parts by weight or less, 240 parts by weight or less, 235 parts by weight or less, 230 parts by weight or less, 225 parts by weight or less, 220 parts by weight or less, 215 parts by weight or less, 210 parts by weight or less , 205 parts by weight or less, 200 parts by weight or less, 195 parts by weight or less, 190 parts by weight or less, 185 parts by weight or less, 180 parts by weight or less, 175 parts by weight or less, 170 parts by weight or less, 165 parts by weight or less, 160 parts by weight or less, 155 parts by weight or less, 150 parts by weight or less, 145 parts by weight or less, 140 parts by weight or less, 135 parts by weight or less, 130 parts by weight or less, 125 parts by weight or less, 120 parts by weight or less, 115 parts by weight or less, 110 parts by weight or less, 105 parts by weight or less, or 100 parts by weight or less.

[0147] In the crystalline acrylic copolymer, the ratio (A / B) of the weight (A) of the unit of Chemical formula 1 to the weight (B) of the polar functional group-containing unit may be 1.5 or more. In other examples, the ratio (A / B) may be 1.7 or more, 1.9 or more, 2.1 or more, 2.3 or more, or 2.5 or more, and may be about 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, or 3 or less. In addition, in the crystalline acrylic copolymer, the polar functional group-containing unit may be a hydroxy group-containing unit. In one example, a hydroxyalkyl (meth)acrylate having a hydroxyalkyl group having 3 to 6 carbon atoms, 3 to 5 carbon atoms, 3 to 4 carbon atoms, or about 4 carbon atoms can appropriately form the crystalline acrylic copolymer. The reason is not clear, but it is considered that the interaction between the alkyl group (R2) of the unit of Chemical formula 1 and the hydroxyalkyl group contributes to the development of crystallinity of the acrylic copolymer.

[0148] The crystalline acrylic copolymer may contain the alkyl (meth)acrylate units in a ratio within the range of about 15 to 55% by weight. In other examples, the ratio of the alkyl (meth)acrylate units may be 20% by weight or more, 25% by weight or more, 30% by weight or more, 35% by weight or more, or 40% by weight or more, and may be about 50% by weight or less, or 45% by weight or less. Within such a range, a desired pressure-sensitive adhesive layer can be effectively formed.

[0149] It is believed that the interaction or regularity of the monomer units contained in the above ratio imparts crystallinity to the acrylic copolymer, and the melting point is confirmed.

[0150] The acrylic copolymer may contain other monomer units in addition to the above-mentioned monomer units, so long as the purpose is not impaired.

[0151] For example, the acrylic copolymer may further contain a monomer unit of the following formula 2. The monomer unit of the following formula 2 is an optional monomer unit and may not be included in the acrylic copolymer.

[0152] [ka]

[0153] In Chemical Formula 2, R1 represents hydrogen or an alkyl group, and R3 represents an aromatic ketone group or a (meth)acryloyl group.

[0154] The unit of Chemical Formula 2 is a unit containing an aromatic ketone group or a (meth)acryloyl group in the side chain.

[0155] In the pressure-sensitive adhesive, the aromatic ketone group or (meth)acryloyl group may exist as is, or may exist after undergoing a hydrogen elimination reaction or a radical reaction, which will be described later.

[0156] In the unit of formula 2, the aromatic ketone group refers to an aromatic ketone group or a substituent containing such an aromatic ketone group that induces hydrogen abstraction from a polymer chain when exposed to electromagnetic waves.

[0157] When exposed to electromagnetic waves, the aromatic ketone groups can remove hydrogen atoms from other polymer chains or from other portions of the polymer chain. Such removal can lead to the formation of radicals that can form cross-links between polymer chains or within the same polymer chain. Categories of such aromatic ketone groups include, for example, aromatic ketone groups such as derivatives of benzophenone, acetophenone, or anthroquinone.

[0158] Examples of monomers that derive the unit of formula 2 having an aromatic ketone group include, but are not limited to, 4-benzoylphenyl (meth)acrylate, 4-(meth)acryloyloxyethoxybenzophenone, 4-(meth)acryloyloxy-4'-methoxybenzophenone, 4-(meth)acryloyloxyethoxy-4'-methoxybenzophenone, 4-(meth)acryloyloxy-4'-bromobenzophenone, and / or 4-acryloyloxyethoxy-4'-bromobenzophenone.

[0159] In the unit of Chemical Formula 2, the (meth)acryloyl group means a (meth)acryloyl group or a substituent containing the same that induces free radical polymerization when exposed to electromagnetic waves in the presence of a suitable radical initiator. Such a (meth)acryloyl group can act similarly to the aromatic ketone group when exposed to electromagnetic waves.

[0160] The unit of formula 2 in which R3 is a (meth)acryloyl group may be formed, for example, by preparing a precursor copolymer and then further reacting with an unsaturated reagent compound to introduce a (meth)acryloyl group. Typically, the introduction of the (meth)acryloyl group involves (1) a reaction between a nucleophilic group on the precursor copolymer and an electrophilic group on the unsaturated reagent compound (i.e., the unsaturated reagent compound contains both an electrophilic group and a (meth)acryloyl group), or (2) a reaction between an electrophilic group on the precursor copolymer and a nucleophilic group on the unsaturated reagent compound (i.e., the unsaturated reagent compound contains both a nucleophilic group and a (meth)acryloyl group). These reactions between nucleophilic groups and electrophilic groups are typically ring-opening reactions, addition reactions, or condensation reactions.

[0161] In this case, the precursor copolymer has hydroxy, carboxylic acid (-COOH), or anhydride (-O-(CO)-O-) groups. If the precursor copolymer has hydroxy groups, the unsaturated reagent compound has carboxylic acid (-COOH), isocyanate (-NCO), epoxy (i.e., oxiranyl), or anhydride groups in addition to the (meth)acryloyl groups. If the precursor copolymer has carboxyl groups, the unsaturated reagent compound has hydroxy, amino, epoxy, isocyanate, aziridinyl, azetidinyl, or oxazolinyl groups in addition to the (meth)acryloyl groups. If the precursor (meth)acrylate copolymer has anhydride groups, the unsaturated reagent compound has hydroxy or amine groups in addition to the (meth)acryloyl groups.

[0162] In one example, the precursor copolymer has a carboxyl group and the unsaturated reagent compound may have an epoxy group. Exemplary unsaturated reagent compounds include, for example, glycidyl (meth)acrylate and 4-hydroxybutyl acrylate glycidyl ether. In another example, the precursor copolymer has an anhydride group that reacts with an unsaturated reagent compound such as a hydroxy-substituted alkyl (meth)acrylate, for example, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, etc. In yet another example, the precursor copolymer has a hydroxy group and the unsaturated reagent compound has an isocyanate group and a (meth)acryloyl group. Such unsaturated reagent compounds include, but are not limited to, isocyanato alkyl (meth)acrylate, for example, isocyanato ethyl (meth)acrylate.

[0163] In one example, the (meth)acryloyl group has the formula CH2=CHR 1 It is represented by -(CO)-QL-, where L is a linking group and Q is oxy (-O-) or -NH-. The L includes alkylene, arylene, or a combination thereof, and further includes -O-, -O-(CO)-, -NH-(CO)-, -NH-, or a combination thereof depending on the precursor copolymer and the specific unsaturated reagent compound reacting to form a (meth)acryloyl group. In some specific examples, the (meth)acryloyl group is represented by the chemical formula -(CO)-OR of the precursor copolymer. 5 Hydroxy-containing groups represented by -OH and the chemical formula H2C=CHR 1 -(CO)-OR 6 -H2C=CHR formed by reaction with an unsaturated reagent compound which is an isocyanato alkyl (meth)acrylate represented by -NCO 1- (CO)-OR 6 -NH-(CO)-OR 5 -O-(CO)-. 5 and R 6are each independently an alkylene group, for example, an alkylene group having 1 to 10 carbon atoms, 1 to 6 carbon atoms, or 1 to 4 carbon atoms. 1 is methyl or hydrogen.

[0164] In the unit of Chemical Formula 2, R1 may be hydrogen or an alkyl group having 1 to 4 carbon atoms, specifically, hydrogen, a methyl group, or an ethyl group.

[0165] When the unit of Chemical Formula 2 is contained, it may be contained in the acrylic copolymer in a ratio of about 0.001 to 5 parts by weight per 100 parts by weight of the alkyl (meth)acrylate unit.

[0166] In a suitable example, the acrylic copolymer may not contain the unit of Chemical formula 2 or may contain a relatively small amount of the unit, and under such a composition, an adhesive with desired physical properties may be more effectively formed. That is, the unit of Chemical formula 2 is a unit that can form a crosslinked structure in the adhesive by additional energy such as electromagnetic waves, but if such a unit exists at a certain level or more, the crosslinked structure of the designed adhesive may be changed and the flow properties may be impaired, so in order to ensure the desired properties, it may be more advantageous not to contain the unit.

[0167] Therefore, in one example, the upper limit of the ratio of the unit of Chemical 2 based on the total weight of the acrylic copolymer may be about 0.1 wt%, 0.09 wt%, 0.08 wt%, 0.07 wt%, 0.06 wt%, 0.05 wt%, 0.04 wt%, 0.03 wt%, 0.02 wt%, 0.01 wt%, 0.009 wt%, 0.008 wt%, 0.007 wt%, 0.006 wt%, 0.005 wt%, 0.004 wt%, 0.003 wt%, 0.002 wt%, or 0.001 wt%, and the lower limit may be about 0 wt%. The ratio may be less than or equal to any of the upper limits mentioned above, or may be greater than or equal to any of the lower limits mentioned above, but less than or equal to any of the upper limits mentioned above.

[0168] In another example, the upper limit of the ratio of the units of Chemical formula 2 to 100 parts by weight of the alkyl (meth)acrylate units may be about 0.2 parts by weight, 0.15 parts by weight, 0.1 parts by weight, 0.05 parts by weight, 0.01 parts by weight, 0.005 parts by weight, 0.004 parts by weight, 0.003 parts by weight, 0.002 parts by weight, 0.001 parts by weight, 0.00095 parts by weight, or 0.0009 parts by weight, and the lower limit may be about 0 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or may be greater than or equal to any of the lower limits mentioned above, but less than or equal to any of the upper limits mentioned above.

[0169] The pressure-sensitive adhesive layer may further include a crosslinking agent, which may react with the acrylic copolymer to form a crosslinked structure.

[0170] The type of crosslinking agent is not particularly limited, and may be a general crosslinking agent such as an isocyanate-based compound, an epoxy-based compound, an aziridine-based compound, or a metal chelate-based compound. Such a type of crosslinking agent is a so-called thermal crosslinking agent that realizes a crosslinked structure by application of heat, and is different from the radical crosslinking agent described below. Such a crosslinking agent may be selected according to the molecular weight distribution of the acrylic copolymer according to the above. Specific examples of the isocyanate-based compound include one or more selected from the group consisting of tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, and any of the above-mentioned polyols (e.g., trimethylolpropane). Specific examples of the epoxy-based compound include ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, and the like. Specific examples of the aziridine-based compound include, but are not limited to, one or more selected from the group consisting of N,N'-toluene-2,4-bis(1-aziridinecarboxamide), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), triethylenemelamine, bisisopropyl 1-(2-methylaziridine) and tri-1-aziridinylphosphine oxide. Specific examples of the metal chelate-based compound include, but are not limited to, compounds in which a polyvalent metal such as aluminum, iron, zinc, tin, titanium, antimony, magnesium and / or vanadium is coordinated with acetylacetone or ethyl acetoacetate.

[0171] In the pressure-sensitive adhesive layer, the lower limit of the weight of the thermal crosslinking agent relative to 100 parts by weight of the acrylic copolymer may be about 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.05 parts by weight, 0.06 parts by weight, or 0.07 parts by weight, and the upper limit may be about 20 parts by weight, 15 parts by weight, 10 parts by weight, 5 parts by weight, 4 parts by weight, 3 parts by weight, 2 parts by weight, 1 part by weight, 0.8 parts by weight, 0.6 parts by weight, 0.4 parts by weight, 0.2 parts by weight, 0.15 parts by weight, 0.1 parts by weight, or 0.09 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or greater than or equal to any of the lower limits mentioned above, or greater than or equal to any of the lower limits mentioned above but less than or equal to any of the upper limits mentioned above.

[0172] When the content of the crosslinking agent is selected so as to crosslink the acrylic copolymer at an appropriate level within the above content range, a desired adhesive can be effectively formed.

[0173] The adhesive may contain, as the crosslinking agent, a so-called radical crosslinking agent, which is a type of crosslinking agent different from the thermal crosslinking agent. Such a crosslinking agent realizes a crosslinked structure by a radical reaction. Such a crosslinking agent may also be selected according to the molecular weight distribution of the acrylic copolymer. In order to efficiently achieve desired properties, it may be more advantageous to apply such a radical crosslinking agent. Examples of such radical crosslinking agents include so-called polyfunctional acrylates, such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid, etc. acid) neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone modified dicyclopentenyl di(meth)acrylate, ethylene oxide modified di(meth)acrylate, di(meth)acryloxyethyl isocyanurate, allyl cyclohexyl di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, ethylene oxide modified hexahydrophthalic acid di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, neopentyl glycol modified trimethylpropane di(meth)acrylate, adamantane di(meth)acrylate or 9,Bifunctional acrylates such as 9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, trifunctional urethane (meth)acrylate, or tris(meth)acryloxyethyl isocyanurate, diglycerides, Examples of the acrylate include, but are not limited to, tetrafunctional acrylates such as phosphorus tetra(meth)acrylate or pentaerythritol tetra(meth)acrylate, pentafunctional acrylates such as propionic acid modified dipentaerythritol penta(meth)acrylate, and hexafunctional acrylates such as dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, or urethane(meth)acrylate (e.g., a reaction product of an isocyanate monomer and trimethylolpropane tri(meth)acrylate).

[0174] The radical crosslinking agent may be present in the pressure-sensitive adhesive layer in an appropriate ratio depending on the purpose. For example, the lower limit of the weight ratio of the radical crosslinking agent relative to 100 parts by weight of the acrylic copolymer may be about 0.001 parts by weight, 0.005 parts by weight, 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, or 0.05 parts by weight, and the upper limit of the weight ratio of the radical crosslinking agent relative to 100 parts by weight of the acrylic copolymer may be about 10 parts by weight, 9.5 parts by weight, 9 parts by weight, 8.5 parts by weight, 8 parts by weight, 7.5 parts by weight, The ratio may be about 7 parts by weight, 6.5 parts by weight, 6 parts by weight, 5.5 parts by weight, 5 parts by weight, 4.5 parts by weight, 4 parts by weight, 3.5 parts by weight, 3 parts by weight, 2.5 parts by weight, 2 parts by weight, 1.5 parts by weight, 1 part by weight, 0.9 parts by weight, 0.8 parts by weight, 0.7 parts by weight, 0.6 parts by weight, 0.5 parts by weight, 0.4 parts by weight, 0.3 parts by weight, 0.2 parts by weight, 0.1 parts by weight, 0.09 parts by weight, 0.08 parts by weight, 0.07 parts by weight, 0.06 parts by weight, or 0.05 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or greater than or equal to any of the lower limits mentioned above, or greater than or equal to any of the lower limits mentioned above but less than or equal to any of the upper limits mentioned above.

[0175] In addition to the above components, the pressure-sensitive adhesive may contain appropriate additive components as necessary, and may further contain components such as a radical initiator, an ultraviolet absorber, a light stabilizer, a plasticizer and / or a crosslinking catalyst.

[0176] However, the adhesive may not contain a citrate ester-based compound, for example, a citrate ester-based compound whose terminal is substituted with hydrogen or an alkyl group, or if it does contain one, the content may be limited to a certain level or less. Although the reason for this is unclear, the citrate ester-based compound tends to adjust the crosslinking structure of the adhesive to a different level than the desired level, making it difficult to ensure the desired physical properties.

[0177] In one example, the upper limit of the weight ratio of the citrate ester-based compound relative to 100 parts by weight of the acrylic copolymer may be about 5 parts by weight, 4.5 parts by weight, 4 parts by weight, 3.5 parts by weight, 3 parts by weight, 2.5 parts by weight, 2 parts by weight, 1.5 parts by weight, 1 part by weight, or 0.5 parts by weight, and the lower limit may be about 0 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, or 3 parts by weight. The ratio may be less than or equal to any of the upper limits mentioned above, or may be greater than or equal to any of the lower limits mentioned above, but less than or equal to any of the upper limits mentioned above.

[0178] The pressure-sensitive adhesive may be formed by crosslinking a pressure-sensitive adhesive composition containing the components. The method of forming the pressure-sensitive adhesive layer by crosslinking is not particularly limited, and the pressure-sensitive adhesive may be formed by applying an appropriate crosslinking method in consideration of the type of the pressure-sensitive adhesive polymer and / or crosslinking agent. For example, if the polymer and / or crosslinking agent is of a type that is crosslinked by application of heat, a crosslinked product may be formed by applying appropriate heat, if the polymer and / or crosslinking agent is of a type that is crosslinked by irradiation of electromagnetic waves, a crosslinked product may be formed by irradiating appropriate electromagnetic waves, or other crosslinking methods may also be applied.

[0179] Such adhesives can exhibit the properties described above.

[0180] The pressure-sensitive adhesive of the present application may be in the form of a layer. In this case, the thickness of the pressure-sensitive adhesive layer is not particularly limited, and may have a normal thickness of a pressure-sensitive adhesive layer in consideration of the intended use. The thickness of the pressure-sensitive adhesive layer is usually set within the range of 5 μm to 100 μm, but is not limited thereto.

[0181] The present application further relates to a pressure-sensitive adhesive film or optical laminate comprising a base film and a pressure-sensitive adhesive formed on one or both sides of the base film. In the case of an optical laminate, the base film may be an optical film. The pressure-sensitive adhesive may be included in a layer form.

[0182] The pressure-sensitive adhesive of the present application may be formed on one or both sides of the base film to form a pressure-sensitive adhesive film, or may be formed on one or both sides of the base film, which is an optical film, to form an optical laminate.

[0183] The type of the base film is not particularly limited. As the base film, a base film that can be generally used for forming a pressure-sensitive adhesive film may be used.

[0184] For example, the substrate film may include, but is not limited to, a PET (poly(ethylene terephthalate)) film, a PTFE (poly(tetrafluoroethylene)) film, a PP (polypropylene) film, a PE (polyethylene) film, a polyimide film, a polyamide film, a COP (cyclic olefin polymer) film, a polybutene film, a polybutadiene film, a vinyl chloride copolymer film, a polyurethane film, an ethylene-vinyl acetate film, an ethylene-propylene copolymer film, an ethylene-ethyl acrylate copolymer film, an ethylene-methyl acrylate copolymer film, and / or a polyimide film.

[0185] The thickness of the base film is not particularly limited, and may be any appropriate thickness within a range suitable for the purpose.

[0186] When an optical film is used as the substrate film, the type of the optical film is not particularly limited. In one example, the optical film may be a polarizing film, a polarizing plate, or a retardation film. In this case, the optical film may have a thickness in an appropriate range depending on the purpose.

[0187] The pressure-sensitive adhesive film or optical laminate may further include a release film or a protective film for protecting the pressure-sensitive adhesive layer before use, as necessary.

[0188] The present application further relates to a flexible device comprising the adhesive, adhesive film or optical laminate. The adhesive may be included in a layer. There is no particular limitation on the application form of the adhesive, adhesive film or optical laminate in the device. For example, the adhesive may be used in the device as a so-called OCA (Optically Clear Adhesive) or OCR (Optically Clear Resin), and therefore the application form of the adhesive, adhesive film or optical laminate may be the same as the application form of a normal OCA or OCR.

[0189] In this case, in one example, the flexible device may include a display panel and the adhesive, adhesive film, or optical laminate present on one or both sides of the display panel, where the display panel may be configured to be folded or rolled about one or more folding or rolling axes.

[0190] Other elements constituting the flexible device as described above are not particularly limited, and known components of a flexible device may be adopted without any limitations. Effect of the Invention

[0191] The present application may provide an adhesive suitable for flexible devices and a device including the same. In one example, the present application may provide an adhesive that is applied to flexible devices and effectively responds to repeated deformation and recovery, does not induce defects before and after deformation, and has excellent recovery, cuttability, workability, and reliability. The present application may further provide an adhesive film or optical film including the adhesive, and a flexible device such as a foldable device or a rollable device. [Brief description of the drawings]

[0192] [Figure 1] FIG. 13 is a diagram showing a process in which a folding test is performed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0193] The present application will be described in detail below through examples and comparative examples, but the scope of the present application is not limited to the following examples.

[0194] 1. Measurement of elastic modulus and maximum stress The elastic modulus of the adhesive layer was evaluated using an ARES G2 (Advanced Rheometric Expansion System G2) (TA). A specimen was prepared by cutting an adhesive layer sample with a thickness of about 800 μm into a circle with a diameter of about 8 mm. The adhesive layer sample was prepared by stacking 32 adhesive layers with a thickness of about 25 μm. A parallel plate fixture (diameter: about 8 mm) was used to evaluate the elastic modulus of the specimen at the measurement temperature. Specifically, the stress on the adhesive was measured while applying a shear force so that a certain strain was generated in the specimen, and the maximum stress (STS) in the section where the change in stress due to strain shows linearity (linear section, 0.7% to 4% strain section) was calculated. MAX ) and minimum stress (STS MIN The maximum stress (STS MAX ) and minimum stress (STS MIN ) can be substituted into the following formula A to obtain the elastic modulus (Young's Modulus). The change in strain was performed by setting the device so that a constant strain from 0% to 400% was generated for 1 second.

[0195] [Formula A] Young's Modulus (unit: Pa) = 100 × (STS MAX -STS MIN ) / (STN MAX -STN MIN )

[0196] In formula A, STS MAX is the maximum stress (unit: Pa) applied to the adhesive within the linear section, STSMIN is the minimum stress (unit: Pa) applied to the adhesive within the linear section, and STN MAX is the strain (unit: %) at which the maximum stress is confirmed, and STN MIN is the strain (unit: %) at which the minimum stress is confirmed.

[0197] 2. Measurement of Stress-Relaxation The stress-relaxation of the adhesive was evaluated using an ARES G2 (Advanced Rheometric Expansion System G2) (TA). A specimen was prepared by cutting an adhesive layer sample with a thickness of about 800 μm into a circle with a diameter of about 8 mm. The adhesive layer sample was prepared by stacking 32 adhesive layers with a thickness of about 25 μm to achieve the thickness. A parallel plate fixture (diameter: about 8 mm) was used to evaluate the stress-relaxation. The device was set so that 100% strain was generated within 0.05 seconds, and shear force was applied. The specimen was loaded into the equipment, and the equipment was driven so that 100% strain was applied according to the settings. The equipment was driven, and the maximum stress S was measured while checking the stress applied to the specimen while maintaining the state of 100% strain. MAX The stress S at the time when the 100% strain was maintained for 1200 seconds was calculated. 1200 The strain was applied for 1200 seconds or more from the time the equipment was driven, and the temperature was fixed at -20° C. The 1200 seconds was the time calculated from the time the strain was applied.

[0198] 3. Measurement of Recovery Rate The recovery rate of the pressure-sensitive adhesive was calculated by maintaining a strain of 100% for 1200 seconds in the same manner as in the above-mentioned stress-relaxation measurement, and using the following formula B.

[0199] [Formula B] Recovery rate (%)=100×(S 1s -S1200s ) / S 1s

[0200] In formula B, S 1s is the stress applied to the adhesive 1 second after the shear force is applied during the process of maintaining the 100% strain for 1200 seconds, and S 1200s is the stress applied to the adhesive 1200 seconds after application of shear force during the process of maintaining the 100% strain for 1200 seconds.

[0201] 4. Measurement of stress against sin strain The stress of the adhesive against the sine strain was evaluated using an ARES G2 (Advanced Rheometric Expansion System G2) (TA). A sample of the adhesive layer with a thickness of about 800 μm was cut into a circle with a diameter of about 8 mm to prepare a test piece. The adhesive layer sample was prepared by stacking 32 adhesive layers with a thickness of about 25 μm to obtain the thickness. A parallel plate fixture (diameter: about 8 mm) was used to evaluate the stress against the sine strain. The device was set so that the test piece was strained according to the sine wave equation of the following formula C according to time, and the strain according to the following formula C was applied to the adhesive sample for 2 seconds, which was defined as one cycle. This was repeated 50 times (100 seconds) to evaluate the initial stress, maximum stress, and final stress of the test piece.

[0202] [Formula C] Sin wave equation=4×sin(1.575×t)

[0203] In formula C, t is time (unit: seconds).

[0204] When strain is generated in the above-described manner, strain of approximately 400% is generated in the sample within 1 second, and the shear force is applied in the reverse direction so that strain of 0% within 1 second is generated again. The initial stress is the stress confirmed from the adhesive specimen at the time when each individual cycle starts (i.e., the time when the shear force is applied), the maximum stress is the maximum stress confirmed within each individual cycle, and the final stress is the stress confirmed in the adhesive specimen at the time when each individual cycle ends.

[0205] 5. Evaluation of Melting Point and Glass Transition Temperature The melting point and glass transition temperature were measured by a measurement method using a DSC (Differential Scanning Calorimeter) device. As the device, a DSC2500 device (TA Instruments) was used. Approximately 10 mg of the sample (copolymer) was filled into a dedicated pan, and the endothermic and exothermic amounts were confirmed according to the temperature under N2 atmosphere with a heating rate of 10 °C / min and a cooling rate of -10 °C / min, and the melting point and glass transition temperature were measured. The measurement temperature range was -120 °C to 200 °C. The conditions were first cooled from room temperature (about 30 °C) to -120 °C at a rate of about -10 °C / min, and then heated to 200 °C at a heating rate of 10 °C / min (primary heating). Thereafter, it was cooled to -120 °C again at a rate of about -10 °C / min, and then heated to 200 °C again at a heating rate of 10 °C / min (secondary heating). The melting point and glass transition temperature were evaluated during the secondary heating.

[0206] 6. Evaluation of Weight-Average Molecular Weight The weight-average molecular weight (Mw) and molecular weight distribution were measured using GPC (Gel Permeation Chromatograph), and the measurement conditions are as follows. When preparing the calibration curve for the measurement of the weight-average molecular weight, the measurement results were converted using standard polystyrene (manufactured by Aglient system). The molecular weight distribution was the value (Mw / Mn) obtained by dividing the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) obtained by the above method.

[0207] <GPC Measurement Conditions> Measuring machine: Aglient GPC (Aglient 1200 series, US) Column: PL Mixed B 2 pieces connected Column temperature: 40℃ Eluent: THF (Tetrahydrofuran) Flow rate: 1.0μL / min Concentration: ~1mg / mL (100μl injection)

[0208] 7. Dynamic folding test The folding test was carried out by manufacturing the specimen shown in FIG. 1. An ITO (indium tin oxide) film and a PET (poly(ethylene terephthalate)) film (SG00) were laminated with an adhesive (F-OCA) to manufacture a sample with a laminated structure of ITO film / adhesive layer / PET film, which was then cut to a horizontal length of about 15 cm and a vertical length of about 2.5 cm. The ITO film used was a PET (poly(ethylene terephthalate)) film (base film) with a thickness of about 50 μm on which a crystalline ITO (indium tin oxide) layer with a thickness of about 1 μm was formed, and the PET film used was a film with a thickness of about 50 μm, and the adhesive layer was about 25 μm thick. In addition, the base film of the ITO film was made to contact the adhesive during lamination. As shown in FIG. 1, a silver paste was printed with a width of about 1 cm on the ITO layer of the cut laminate. Two silver pastes were printed at a distance of about 4 cm on either side of the center of the ITO layer (dotted line in the lower diagram of FIG. 1). After printing, the printed paste was dried at about 150° C. for about 1 hour. A dynamic folding test was performed using the laminate as a specimen. The specimen was loaded into a dynamic chamber. Then, the specimen was folded once at the center (dotted line in the lower diagram of FIG. 1) and unfolded, which constituted one cycle, and the cycle was repeated. The folding was performed with a curvature of about 2.5R, and the temperature was fixed at -20° C., and the folding and unfolding were performed once per cycle for 2 seconds. The folding was performed so that the silver paste of the ITO film was at the top. After the folding test, the adhesive samples were evaluated according to the following criteria.

[0209] <Evaluation criteria> O: When the resistance change rate of the ITO film is 300% or less △: When the resistance change rate of the ITO film is over 300% and is 500% or less ×: When the resistance change rate of the ITO film exceeds 500%

[0210] Production Example 1. Production of Copolymer (A) 2-Ethylhexyl acrylate (2-EHA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) were added to the ethyl acetate solvent in a reactor in a weight ratio of 40:40:20 (2-EHA:LA:HBA), and about 500 ppm of a radical initiator (2,2'-Azobis(4-methoxy-2,4-dimethylvaleronitrile)) was added. The mixture was polymerized at about 50°C for about 8 hours to produce a polymer (copolymer (A)).

[0211] Production Example 2. Production of Copolymer (B) 2-Ethylhexyl acrylate (2-EHA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) were mixed in a weight ratio of 45:40:15 (2-EHA:LA:HBA) in a 50 mL vial and purged with N2. A photoradical initiator (Irgacure 184) was added to the mixture in an amount of about 500 ppm and irradiated with light from a metal halide lamp to produce copolymer (B) (irradiation conditions: UV A standard, light intensity: 0.8 J / cm2). 2 (Irradiation time: about 20 seconds) The copolymer (B) was in the form of a partially polymerized prepolymer.

[0212] Production Example 3. Production of Copolymer (C) 2-Ethylhexyl acrylate (2-EHA) and acrylic acid (AA) were added to the ethyl acetate solvent in a reactor in a weight ratio of 98:2 (2-EHA:AA), and approximately 500 ppm of a radical initiator (2,2'-Azobis(4-methoxy-2,4-dimethylvaleronitrile)) was added. The mixture was polymerized at approximately 50°C for approximately 8 hours to produce a polymer (copolymer (C)).

[0213] Production Example 4. Production of Copolymer (D) 2-Ethylhexyl acrylate (2-EHA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) were added to the ethyl acetate solvent in a reactor in a weight ratio of 60:20:20 (2-EHA:LA:HBA), and about 500 ppm of a radical initiator (2,2'-Azobis(4-methoxy-2,4-dimethylvaleronitrile)) was added. The mixture was polymerized at about 50°C for about 8 hours to produce a polymer (copolymer (D)).

[0214] The weight average molecular weight, glass transition temperature, melting point and molecular weight distribution of each of the copolymers prepared above are summarized in Table 1 below.

[0215] [Table 1]

[0216] Example 1. A pressure-sensitive adhesive composition was prepared by mixing about 0.07 parts by weight of an isocyanate crosslinking agent (xylylene diisocyanate) and 0.005 parts by weight of a catalyst with 100 parts by weight of the copolymer (A) of Preparation Example 1. The catalyst used was a catalyst that generally promotes the urethane reaction between a hydroxyl group and an isocyanate group. The prepared pressure-sensitive adhesive composition was applied onto the release surface of a release PET (poly(ethylene terephthalate)) film and maintained at 130°C for about 3 minutes to form a pressure-sensitive adhesive layer with a thickness of about 25 μm.

[0217] Example 2. An adhesive composition was prepared by mixing about 0.05 parts by weight of 1,6-hexanediol diacrylate and about 3 parts by weight of an initiator (Irgacure 651) with respect to 100 parts by weight of the copolymer (prepolymer) (B) of Preparation Example 2. The adhesive composition was applied onto the release surface of a release PET (poly(ethylene terephthalate)) film and irradiated with ultraviolet light to form an adhesive layer with a thickness of about 25 μm (ultraviolet light irradiation conditions: wavelength = about 365 nm (black light lamp), total light amount = about 1 J / cm).2 , exposure time: about 3 minutes).

[0218] Comparative Example 1 An adhesive composition was prepared by mixing about 0.035 parts by weight of a crosslinking agent (manufacturer: Samyoung Ink Paint Co., Ltd., product names: 0.03 parts by weight of BXX-5240 and 0.005 parts by weight of BXX-5627) with 100 parts by weight of the copolymer (polymer) (C) of Preparation Example 3. The prepared adhesive composition was applied onto the release surface of a release PET (poly(ethylene terephthalate)) film and maintained at 130°C for about 3 minutes to form an adhesive layer with a thickness of about 25 μm.

[0219] Comparative Example 2 A pressure-sensitive adhesive composition was prepared by mixing about 0.07 parts by weight of an isocyanate crosslinking agent (xylylene diisocyanate) and 0.005 parts by weight of a catalyst with 100 parts by weight of the copolymer (D) of Preparation Example 4. The catalyst used was a catalyst that generally promotes the urethane reaction between a hydroxyl group and an isocyanate group. The pressure-sensitive adhesive composition prepared above was applied onto the release surface of a release PET (poly(ethylene terephthalate)) film and maintained at 130°C for about 3 minutes to form a pressure-sensitive adhesive layer with a thickness of about 25 μm.

[0220] Comparative Example 3. An OCA adhesive (product name: CEF3502) from 3M was used as Comparative Example 3. The adhesive was formed to a thickness of about 25 μm on the release surface of a release PET (poly(ethylene terephthalate)) film, and used as Comparative Example 3.

[0221] The results of evaluating the elastic modulus of the pressure-sensitive adhesive layers of the Examples and Comparative Examples are summarized in Table 2 below. In Table 2 below, the elastic modulus (Young's Modulus) (unit: Pa) is a value obtained by the above formula A, and is calculated by STS MAX is the maximum stress (unit: Pa) applied to the adhesive within the linear section described in the measurement method above, and STS MIN is the minimum stress (unit: Pa) applied to the adhesive within the linear section, and STNMAX is the strain (unit: %) at which the maximum stress is confirmed, and STN MIN is the strain (unit: %) at which the minimum stress is confirmed. The results in Table 2 below were measured at about -20°C.

[0222] [Table 2]

[0223] The results of the stress-relaxation evaluation of the pressure-sensitive adhesive layers of the Examples and Comparative Examples are summarized in Table 3 below. In Table 3 below, MAX Stress is the maximum stress (S MAX ) and 1200s stress is the stress (S 1200 ) as S in the recovery rate evaluation formula B 1200s 1sStress is the stress applied to the adhesive when 1 second has elapsed since the device was started, and is the S in the recovery rate evaluation formula B. 1s It is.

[0224] [Table 3]

[0225] The results of measuring the stress against the Sin strain for the pressure-sensitive adhesive layers of the Examples and Comparative Examples are summarized in Table 4 below. In Table 4 below, 1 Cycle, 10 Cycle, and 50 Cycle refer to the results at the first cycle, the tenth cycle, and the fiftyth cycle, respectively. Additionally, Initial refers to the stress at the start of each cycle, MAX refers to the maximum stress measured in each cycle, and LAST refers to the stress at the end of each cycle.

[0226] Therefore, in Table 4 below, MAX in 1 cycle is S in Equations 1, 3 and 5. MAX1 MAX at 10 cycles is S in Equations 3, 4 and 7 MAX10 and MAX at 50 cycles is S in Equations 1, 4 and 6. MAX50 In addition, in Table 4 below, LAST in 1 cycle is S in Equation 5. LAST1 The LAST in 10 cycles is S in Equation 7. LAST10 The LAST at 50 cycles is S in Equation 6. LAST50 It is.

[0227] [Table 4]

[0228] The results of the dynamic folding test on the pressure-sensitive adhesive layers of the Examples and Comparative Examples are summarized in Table 5 below. In Table 5 below, 50,000 cycles and 100,000 cycles indicate the results of folding at a curvature of about 2.5R and then unfolding 50,000 times and 100,000 times, respectively, as described in the measurement method above. In addition, the values ​​shown in Table 5 below indicate the percentage increase in resistance when the initial resistance of the ITO film is taken as 100% (i.e., for example, a value of 400% means that the resistance has increased four times).

[0229] [Table 5]

Claims

1. The maximum stress S observed while maintaining a 100% strain applied within 0.05 seconds by a shear force applied at -20°C for 1200 seconds MAX is 1 MPa or less, and the stress S at the time when the 100% strain is maintained for 1200 seconds 1200 The adhesive has a modulus of 12,000 Pa or less.

2. ΔS in the following formula 1 X1 is 3,500 Pa / cycle or less, and S of the following formula 1 MAX50 The adhesive has a modulus of 250,000 Pa or less. [Formula 1] △S X1 = 0.02 × (S MAX1 -S MAX50 ) In formula 1, S MAX1 is the maximum stress (unit: Pa) observed within 0 to 2 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S MAX50 is the maximum stress (unit: Pa) observed within 99 to 100 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds. [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

3. Maximum stress S MAX Stress S 1200 Ratio to (S MAX / S 1200 2. The pressure-sensitive adhesive according to claim 1, wherein the molecular weight is 30 to 60.

4. ΔS in the following formula 3 X2 The pressure-sensitive adhesive according to claim 1 or 2, wherein the compressibility is 15,000 Pa / time or less. [Formula 3] △S X2 = 0.1 × (S MAX1 -S MAX10 ) In formula 3, S MAX1is the maximum stress (unit: Pa) observed within 0 to 2 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S MAX10 is the maximum stress (unit: Pa) observed within 19 to 20 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20° C. for 100 seconds. [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

5. ΔS in the following formula 4 X3 The pressure-sensitive adhesive according to claim 1 or 2, wherein the compressive strength is 700 Pa / time or less. [Formula 4] △S X3 = 0.025 × (S MAX10 -S MAX50 ) In formula 4, S MAX10 is the maximum stress (unit: Pa) observed within 19 to 20 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S MAX50 is the maximum stress (unit: Pa) observed within 99 to 100 seconds in the process of applying a shear force according to the following formula 2 to the pressure sensitive adhesive at -20°C for 100 seconds. [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

6. ΔS in the following formula 5 XL1 The pressure-sensitive adhesive according to claim 1 or 2, wherein the modulus of elasticity is 600,000 Pa or less. [Formula 5] △S XL1 = (S MAX1 -S LAST1 ) In formula 5, S MAX1is the maximum stress (unit: Pa) observed within 0 to 2 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S LAST1 is the maximum stress (unit: Pa) observed at 2 seconds during the process of applying a shear force according to the following formula 2 to the adhesive at −20° C. for 100 seconds. [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

7. ΔS in the following formula 6 XL50 The pressure-sensitive adhesive according to claim 1 or 2, wherein the modulus of elasticity is 500,000 Pa or less. [Formula 6] △S XL50 = (S MAX50 -S LAST50 ) In formula 6, S MAX50 is the maximum stress (unit: Pa) observed within 99 to 100 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S LAST50 is the maximum stress (unit: Pa) observed at 100 seconds during the process of applying a shear force according to the following formula 2 to the adhesive at −20° C. for 100 seconds. [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

8. ΔS in the following formula 7 XL10 The pressure-sensitive adhesive according to claim 1 or 2, wherein the modulus of elasticity is 500,000 Pa or less. [Formula 7] △S XL10 = (S MAX10 -S LAST10 ) In formula 7, S MAX10 is the maximum stress (unit: Pa) observed within 19 to 20 seconds in the process of applying a shear force according to the following formula 2 to the adhesive at -20°C for 100 seconds, and S LAST10is the maximum stress (unit: Pa) observed at 20 seconds during the process of applying a shear force to the adhesive at −20° C. for 100 seconds according to the following formula 2: [Formula 2] Sin wave equation=4×sin(1.575×t) In Equation 2, t is time (unit: seconds).

9. The adhesive according to claim 1 or 2, which has a recovery rate of 70% or more.

10. 3. The pressure-sensitive adhesive according to claim 1, wherein the elastic modulus at -20°C is 1 MPa or less, and the maximum stress in the linear section of a strain-stress curve for determining the elastic modulus is 30,000 Pa or less.

11. The adhesive of claim 1 or 2, comprising an adhesive polymer.

12. The adhesive of claim 11 , wherein the adhesive polymer is an acrylic copolymer exhibiting a glass transition temperature and a melting temperature.

13. The pressure-sensitive adhesive according to claim 12, wherein the glass transition temperature is −30° C. or lower and the melting temperature is −10° C. or lower.

14. The pressure-sensitive adhesive according to claim 12, wherein the difference between the melting temperature and the glass transition temperature (Tm-Tg) is 5°C or more.

15. The pressure-sensitive adhesive according to claim 12, wherein the acrylic copolymer has a molecular weight distribution of more than 3, and the acrylic copolymer is crosslinked with a thermal crosslinking agent.

16. The pressure-sensitive adhesive according to claim 12 , wherein the acrylic copolymer has a molecular weight distribution of 3 or less, and the acrylic copolymer is contained in a state crosslinked with a radical crosslinking agent.

17. The pressure-sensitive adhesive according to claim 12, wherein the acrylic copolymer comprises an alkyl (meth)acrylate unit, a unit of the following formula 1, and a polar functional group-containing unit. [Formula 1] In Chemical Formula 1, R 1 represents hydrogen or an alkyl group; R 2 represents an alkyl group having 11 to 13 carbon atoms.

18. An adhesive film comprising a base film and the adhesive according to claim 1 or 2 formed on one or both sides of the base film.

19. a display panel configured to be foldable or rollable about one or more folding or rolling axes; A flexible device comprising the adhesive of claim 1 or 2 present on one or both sides of the display panel.

Citation Information

Patent Citations

  • Adhesive agent layer for flexible image display device, laminate body for flexible image display device, and flexible image display device

    JP2019218513A

  • Adhesive layer

    WO2021118248A1