Olefin-based polymer with excellent processability and method for producing same
A mixed metallocene catalyst system produces an olefin polymer with a unimodal broad molecular weight distribution and shoulder, addressing the poor processability of metallocene-based polymers by minimizing melt fracture and shark skin, thereby improving high-speed processing capabilities.
Patent Information
- Application Number
- JP2024529893
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-23
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyolefins produced using metallocene catalysts exhibit narrow molecular weight distribution, leading to excellent mechanical strength but poor processability, making them unsuitable for high-speed processing applications such as LAN cables, and existing bimodal distributions either have too wide or insufficient molecular weight differences.
A mixed metallocene catalyst system is used to produce an olefin polymer with a unimodal broad molecular weight distribution and a shoulder, achieving improved processability by minimizing melt fracture and shark skin phenomena at high shear rates.
The olefin polymer demonstrates excellent high-speed processability with reduced melt fracture and shark skin occurrence, enhancing its suitability for high-speed processing applications.
Smart Images

Figure 2024541729000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an olefin-based polymer having excellent processability, and a method for producing the same, and more particularly to an olefin-based polymer having a unimodal broad molecular weight distribution having a shoulder, which is polymerized in the presence of a mixed metallocene catalyst, and has excellent processability, and a method for producing the same. [Background technology]
[0002] Polyolefin polymers are widely used in daily life as materials for shopping bags, vinyl greenhouses, fishing nets, cigarette wrappers, noodle bags, yogurt bottles, battery cases, automobile bumpers, interior materials, shoe soles, washing machines, and the like.
[0003] Traditionally, polyolefin polymers such as polyethylene, polypropylene, and ethylene-α-olefin copolymers and their copolymers have been produced using heterogeneous catalysts such as Ziegler-Natta catalysts consisting of titanium compounds and alkylaluminum compounds.
[0004] In recent years, research has been conducted into the production of polyolefins using metallocene catalysts, which are homogeneous catalysts with extremely high catalytic activity. Metallocene catalysts are compounds in which ligands such as cyclopentadienyl, indenyl, and cycloheptadienyl are coordinated to transition metals or transition metal halides, and have a sandwich structure as their basic form. In this case, they have various molecular structures depending on the form of the ligand and the type of central metal.
[0005] In the case of Ziegler-Natta catalysts, which are heterogeneous catalysts, the metal components that act as active sites are dispersed on an inert solid surface, and the properties of the active sites are not uniform. In contrast, metallocene catalysts are a single compound with a fixed structure, and therefore all active sites have the same polymerization properties. They are therefore known as single-site catalysts.
[0006] Such metallocene catalysts are easy to copolymerize and can adjust the three-dimensional structure of the polymer depending on the symmetry of the catalyst. The polymers produced thereby have the advantages of a narrow molecular weight distribution and a uniform distribution of the comonomer. However, polymers produced using metallocene catalysts have a narrow molecular weight distribution, and therefore have a problem of poor processability, although they have excellent mechanical strength.
[0007] On the other hand, polyolefins obtained using chromium-based or Ziegler-Natta catalysts have been mainly used for the production of LAN (local area network) cables. In order to increase the production volume of LAN cables, they must be processed at high speeds, and melt fracture or shark skin phenomenon may occur during high-speed processing. Furthermore, polyolefins produced using metallocene catalysts are known to be unsuitable for the production of LAN cables due to their poor processability.
[0008] In order to improve the processability of polyolefins produced by metallocene catalysts, there have been attempts to produce supported catalysts by mixing different metallocene catalysts. For example, U.S. Patent No. 4,935,474, U.S. Patent No. 6,828,394, U.S. Patent No. 6,894,128, Korean Patent No. 1437509, and U.S. Patent No. 6,841,631 disclose methods for producing polyolefins with bimodal molecular weight distribution by mixing catalysts with different reactivity to comonomers.
[0009] However, the molecular weight difference between the resins produced by the two catalysts was so great that the molecular weight distribution was too broad, or the molecular weight difference was so small that there was little difference compared to a single metallocene catalyst. Also, the more pronounced the bimodal molecular weight distribution of the polyolefin, the better the processability, but the worse the processability may be compared to polyolefins with a unimodal distribution. Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide an olefin polymer which is polymerized in the presence of a hybrid metallocene catalyst, has a single-peaked broad molecular weight distribution having a shoulder and is excellent in high-speed processability, and a method for producing the same. [Means for solving the problem]
[0011] According to one embodiment of the present invention for achieving the above object, the density is 0.930 to 0.970 g / cm 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) of the polymer is 30 to 200, the molecular weight distribution is unimodal with a shoulder when measured by gel permeation chromatography (GPC), and melt fracture or shark skin phenomenon occurs when measured by a capillary rheometer. -1 Thus, an olefin polymer is provided.
[0012]
number
[0013] In the above formula, TIFF2024541729000003.tif10170 is the apparent shear rate (sec -1 ), and V is the volumetric flow rate (mm 3 / sec) and R is the radius of the circular hole capillary (mm).
[0014] According to one embodiment of the present invention, there is provided an olefin-based polymer produced by polymerization of ethylene and at least one α-olefin in the presence of a hybrid metallocene catalyst, the polymer having a density of 0.930 to 0.970 g / cm. 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) of the polymer is 30 to 200, the molecular weight distribution is unimodal when measured by gel permeation chromatography (GPC), and melt fracture or shark skin phenomenon occurs when measured by a capillary rheometer. -1 Thus, an olefin polymer is provided.
[0015] According to one embodiment of the present invention, there is provided an olefin-based polymer produced by polymerization of ethylene and at least one α-olefin in the presence of a hybrid metallocene catalyst, the polymer having a density of 0.930 to 0.970 g / cm. 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16The melt flow ratio (MFR) of the polymer is 30 to 200, the molecular weight distribution is unimodal when measured by gel permeation chromatography (GPC), and melt fracture or shark skin phenomenon occurs when measured by a capillary rheometer. -1 Thus, an olefin polymer is provided.
[0016] In a specific example of the present invention, the density of the olefin polymer is 0.930 to 0.965 g / cm 3 , preferably 0.935 to 0.960 g / cm 3 and the melt index (I 2.16 ) is 0.5 to 4.5 g / 10 min, preferably 0.5 to 4.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 ) is 30 to 150, preferably 40 to 135, and the shear rate at which melt fracture or sharkskin phenomenon occurs when measured with a capillary rheometer is 700 sec -1 More than 750sec, preferably -1 It may be more than that.
[0017] In a specific example of the present invention, the olefin polymer is produced by polymerizing ethylene and at least one α-olefin in the presence of a hybrid metallocene catalyst, which may include: (a) at least one first transition metal compound selected from a transition metal compound represented by the following chemical formula 1 and a transition metal compound represented by the following chemical formula 2; (b) at least one second transition metal compound selected from a transition metal compound represented by the following chemical formula 3; (c) at least one third transition metal compound selected from a transition metal compound represented by the following chemical formula 4, a transition metal compound represented by the following chemical formula 5a, and a transition metal compound represented by the following chemical formula 5b; and (d) a co-catalyst compound.
[0018] [ka]
[0019] In the above chemical formula, l1 and m1 each independently represent an integer of 0 to 5. l2, l3, m2, and n1 each independently represent an integer of 0 to 4; m3 and o1 each independently represent an integer of 0 to 2; p is the oxidation state of M, +3, +4, or +5; q is the formal charge of the YZL ligand, which can be 0, -1, -2, or -3; M is independently titanium (Ti), zirconium (Zr), or hafnium (Hf); M' is titanium, zirconium, or hafnium, in the formal oxidation states +2, +3, or +4, respectively; X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide, or C 6-20 is an aryl amide, Each X' is independently alkyl; Each Q is independently carbon (C), silicon (Si), germanium (Ge), or tin (Sn); Q' is an anionic leaving group, and each Q' is independently hydrogen, substituted or unsubstituted C 1-40 Hydrocarbon radicals, substituted or unsubstituted C 1-40 a heterohydrocarbon group, a heteroatom, or a halogen; L is an element of group 15 or 16, preferably nitrogen; Y is a group 15 element, preferably nitrogen or phosphorus, more preferably nitrogen; Z is a group 15 element, preferably nitrogen or phosphorus, more preferably nitrogen; Z' is independently -O-, -S-, -N(C 1-40 Hydrocarbon group)-, or -P(C 1-40 a hydrocarbon group)-, R1~R4, R7, R8, R 11 , and R 12 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, each of which is independently a substituted or unsubstituted, saturated or unsaturated C 4-20 may or may not form a ring, R5, R6, R9, R 10 , R 13 , and R 14 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, where R5 and R6, R9 and R 10 , R 13 and R 14 are each independently linked to each other and are substituted or unsubstituted, saturated or unsaturated C 2-20 may or may not form a ring, R 15 and R 16 are each independently 1-20 a hydrocarbon group or a heteroatom-containing group, where the heteroatom is silicon, germanium, tin, lead, or phosphorus, or R 15 and R 16 may be linked to each other, R 17 is absent or hydrogen, C 1-20 is an alkyl, halogen, or heteroatom-containing group; R 18 and R 19 are each independently an alkyl group, an aryl group, a substituted aryl group, a cyclic alkyl group, a substituted cyclic alkyl group, or a polycyclic ring system; R 20 and R 21 are each independently absent, a hydrogen, an alkyl group, a halogen, a heteroatom, a hydrocarbon group, or a heteroatom-containing group; R x and R y each independently represents a substituted or unsubstituted C 1-40 Hydrocarbon radicals, substituted or unsubstituted C 1-40 a heterohydrocarbon group, a halogen, or hydrogen; R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R28c , R 29c , R 26d , R 27d , R 28d , and R 29d each independently represents a substituted or unsubstituted C 1-40 Hydrocarbon radicals, substituted or unsubstituted C 1-40 Heterohydrocarbon group, -Si(R e )3, -OSi(R e )3, -Ge(R e )3, -P(R e )2, -N(R e )2, -OR e , -SR e , -NO2, -CN, -CF3, -OCF3, -S(O)R e , -S(O)2R e , -N=C(R e )2, -OC(O)R e , -C(O)OR e , -N(R)C(O)R e , -C(O)N(R e )2, halogen, and hydrogen, where R e each independently represents a substituted or unsubstituted C 1-30 Hydrocarbon group or substituted or unsubstituted C 1-30 Heterohydrocarbon group, where R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d Two or more of may or may not form one or more ring structures.
[0020] In a specific example of the present invention, the transition metal compound of Chemical Formula 1 may be at least one of transition metal compounds represented by the following Chemical Formulas 1-1 to 1-8, and the transition metal compound of Chemical Formula 2 may be a transition metal compound represented by the following Chemical Formula 2-1.
[0021] [ka] In the above formula, Me is methyl.
[0022] In a specific example of the present invention, the transition metal compound of the formula 3 may be at least one of the transition metal compounds represented by the following formulas 3-1 to 3-10. [ka] TIFF2024541729000007.tif77170In the above chemical formula, Me is methyl, n-Bu is n-butyl, t-Bu is t-butyl, Ph is phenyl, and p-Tol is p-tolyl.
[0023] In a specific example of the present invention, the transition metal compound of chemical formula 4 may be at least one of the transition metal compounds represented by the following chemical formulae 4-1 to 4-2, the transition metal compound of chemical formula 5a may be at least one of the transition metal compounds represented by the following chemical formulae 5-1 to 5-4, and the compound of chemical formula 5b may be at least one of the transition metal compounds represented by the following chemical formulae 5-5 and 5-6. [ka] TIFF2024541729000009.tif5170In the above chemical formula, Me is methyl, t-Bu is t-butyl, and Ph is phenyl.
[0024] In an embodiment of the present invention, the co-catalyst compound may include at least one selected from the group consisting of a compound represented by the following chemical formula 6, a compound represented by the following chemical formula 7, and a compound represented by the following chemical formula 8. [ka] (Chemical formula 6) TIFF2024541729000011.tif18170 (chemical formula 7) [LH] + [Z(A)4] - or [L] + [Z(A)4] - (Chemical formula 8)
[0025] In the above Chemical Formula 6, n is an integer of 2 or more, and R a is a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, In the above formula 7, D is aluminum (Al) or boron (B), and R b , R c , and R d each independently represents a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen-substituted hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, In the above formula 8, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.
[0026] In a preferred embodiment of the present invention, the compound represented by Chemical Formula 6 is at least one selected from the group consisting of methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, and butylaluminoxane.
[0027] In a preferred embodiment of the present invention, the compound represented by Chemical Formula 7 is at least one selected from the group consisting of trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylchloroaluminum, triisopropylaluminum, tri-s-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, and tributylboron.
[0028] In a preferred embodiment of the present invention, the compound represented by Chemical Formula 8 is selected from the group consisting of triethylammonium tetraphenylboron, tributylammonium tetraphenylboron, trimethylammonium tetraphenylboron, tripropylammonium tetraphenylboron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron, tributylammonium tetrapentafluorophenylboron, N,N-diethylanilinium tetraphenylboron, N,N-diethylanilinium tetrapentafluorophenylboron, diethylammonium tetrapentafluorophenylboron, triphenylphosphonium tetraphenylboron, trimethylphosphonium tetraphenylboron, triethylammonium tetraphenylaluminum, tributylammonium tetraphenylaluminum, trimethylammonium tetraphenylaluminum, tripropylammonium tetraphenylboron, and at least one selected from the group consisting of N,N-diethylanilinium tetraphenylaluminum, trimethylammonium tetra(p-tolyl)aluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetrapentafluorophenylaluminum, N,N-diethylanilinium tetraphenylaluminum, N,N-diethylanilinium tetrapentafluorophenylaluminum, diethylammonium tetrapentatetraphenylaluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl)boron, triphenylcarbonium tetra(p-trifluoromethylphenyl)boron, and triphenylcarbonium tetrapentafluorophenylboron.
[0029] In an embodiment of the present invention, the hybrid metallocene catalyst may further comprise a support supporting the hybrid transition metal compound, the cocatalyst compound, or both. In an embodiment of the present invention, the support may comprise at least one selected from the group consisting of silica, alumina, and magnesia.
[0030] Here, the total amount of the mixed transition metal compounds supported on the support is 0.001 to 1 mmole based on 1 g of the support, and the total amount of the promoter compounds supported on the support is 2 to 15 mmole based on 1 g of the support.
[0031] According to one embodiment of the present invention, the method includes a step of polymerizing ethylene and at least one α-olefin in the presence of a mixed metallocene catalyst comprising: (a) at least one first transition metal compound selected from the transition metal compound represented by Chemical Formula 1 and the transition metal compound represented by Chemical Formula 2; (b) at least one second transition metal compound selected from the transition metal compound represented by Chemical Formula 3; (c) at least one third transition metal compound selected from the transition metal compound represented by Chemical Formula 4, the transition metal compound represented by Chemical Formula 5a, and the transition metal compound represented by Chemical Formula 5b; and (d) a co-catalyst compound, to obtain an olefin polymer, wherein the density of the olefin polymer is 0.930 to 0.970 g / cm. 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) of the polymer is 30 to 200, the molecular weight distribution is unimodal with a shoulder when measured by gel permeation chromatography, and melt fracture or shark skin phenomenon occurs when measured by a capillary rheometer.-1 Thus, there is provided a method for producing an olefin polymer.
[0032] In an embodiment of the present invention, the α-olefin may be at least one selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, and 1-hexadecene. Preferably, the α-olefin may be 1-hexene.
[0033] In an embodiment of the present invention, the polymerization of ethylene and at least one α-olefin may be carried out by gas phase polymerization, specifically, the polymerization of ethylene and at least one α-olefin may be carried out in a gas phase fluidized bed reactor. Effect of the Invention
[0034] According to an embodiment of the present invention, an olefin polymer produced by using a hybrid metallocene catalyst has a broad, unimodal molecular weight distribution having a shoulder, and is excellent in high-speed processability. [Brief description of the drawings]
[0035] [Figure 1] 1 is a GPC-FTIR graph for explaining a unimodal molecular weight distribution. [Diagram 2] 1 is a GPC graph of an olefin polymer according to an embodiment of the present invention. [Diagram 3] 1 is a GPC graph of an olefin polymer according to an embodiment of the present invention. [Figure 4] 1 is a GPC graph of an olefin polymer according to an embodiment of the present invention. [Diagram 5] 1 is a GPC graph of an olefin polymer according to an embodiment of the present invention. [Figure 6] 1 is a GPC graph of an olefin polymer of a comparative example of the present invention. [Figure 7] 1 is a GPC graph of an olefin polymer of a comparative example of the present invention. [Figure 8]1 is a photograph showing the observation of the presence or absence of melt fracture or sharkskin depending on the shear rate of an olefin polymer according to an embodiment of the present invention. [Figure 9] 1 is a photograph showing the observation of the presence or absence of melt fracture or sharkskin depending on the shear rate of an olefin polymer of a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The present invention will now be described in more detail. [Olefin polymer] According to one embodiment of the present invention, the density is 0.930 to 0.970 g / cm 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) of the olefin polymer is 30 to 200.
[0037] The olefin polymer according to the embodiment of the present invention has a density of 0.930 to 0.970 g / cm 3 The density of the olefin polymer is preferably 0.930 to 0.965 g / cm 3 , more preferably 0.935 to 0.960 g / cm 3 , particularly preferably 0.940 to 0.950 g / cm 3 may be also possible.
[0038] The olefin polymer according to the embodiment of the present invention has a melt index (I 2.16 The melt index of the olefin polymer measured at 190° C. under a load of 2.16 kg may be preferably 0.5 to 4.5 g / 10 min, more preferably 0.5 to 4.0 g / 10 min, and particularly preferably 0.5 to 2.0 g / 10 min.
[0039] The olefin polymer according to the embodiment of the present invention has a melt index (I 21.6 ) and the melt index (I 2.16 ) is from 30 to 200. The MFR of the olefin polymer may be from 30 to 150, more preferably from 40 to 135, and particularly preferably from 50 to 120.
[0040] The olefin polymer according to the embodiment of the present invention has a unimodal molecular weight distribution as measured by gel permeation chromatography (GPC).
[0041] Specifically, referring to FIG. 1 showing a typical GPC graph of a polymer, if the points (a and c) where the tangent slope changes from a positive value to a negative value in the GPC graph of this polymer are defined as "peaks" and the point (b) where the tangent slope changes from a negative value to a positive value is defined as a "valley," the olefin-based polymer according to the embodiment of the present invention exhibits a unimodal molecular weight distribution having one peak.
[0042] As shown in Figures 2 to 5, the olefin polymer according to the embodiment of the present invention has a shoulder on the GPC graph. The shoulder may refer to a section on the GPC graph where, as the molecular weight increases, the absolute value of the positive slope on the low molecular weight component side (left side of the peak) becomes larger and then decreases again, but does not change to a negative value, or a section where the absolute value of the negative slope on the high molecular weight component side (right side of the peak) becomes smaller and then increases again, but does not change to a positive value. Unless the value of the tangent to the graph at this point changes from positive to negative or from negative to positive, it is not classified as a peak.
[0043] When the olefin-based polymer according to the embodiment of the present invention is subjected to GPC measurement, the value of the fraction (vertical axis) relative to the molecular weight (horizontal axis) is quantified, and the presence and number of peaks on the GPC graph can be confirmed by checking the change in the value.
[0044] The olefin polymer according to the embodiment of the present invention exhibits melt fracture and shark skin phenomena when measured by a capillary rheometer. The shear rate is defined by the following mathematical formula 1. -1 The shear rate at which melt fracture or shark skin occurs is preferably 700 sec -1 More than 750 seconds, preferably -1 That's all, 1,050sec -1 or more, or 1,100sec -1 It may be more than that.
number
[0045] Melt fracture or sharkskin refers to a phenomenon in which irregular unevenness or a sharkskin-like shape occurs on the surface of a polymer during extrusion, or the surface loses luster. The higher the shear rate at which such melt fracture or sharkskin occurs, the better the processability of the polymer.
[0046] The olefin polymer according to the embodiment of the present invention is produced by polymerization of ethylene and at least one α-olefin. In a specific example of the present invention, an olefin polymer is produced by polymerizing ethylene and at least one α-olefin in the presence of a mixed metallocene catalyst comprising: (a) at least one first transition metal compound selected from a transition metal compound represented by the following chemical formula 1 and a transition metal compound represented by the following chemical formula 2; (b) at least one second transition metal compound selected from a transition metal compound represented by the following chemical formula 3; (c) at least one third transition metal compound selected from a transition metal compound represented by the following chemical formula 4, a transition metal compound represented by the following chemical formula 5a, and a transition metal compound represented by the following chemical formula 5b; and (d) a co-catalyst compound.
[0047] [ka]
[0048] In the above chemical formula, l1 and m1 each independently represent an integer of 0 to 5. Preferably, l1 is 1, and m1 each independently represents an integer of 1 to 5.
[0049] l2, l3, m2, and n1 each independently represent an integer of 0 to 4. Preferably, l2, l3, and m2 each represent 1, and n1 each represent 0.
[0050] m3 and o1 each independently represent an integer of 0 to 2. Preferably, each m3 is 1, and each o1 is 0. P is the oxidation state of M, +3, +4, or +5. q is the formal charge of the YZL ligand and can be 0, -1, -2, or -3.
[0051] M is a transition metal of Group 4 of the periodic table of elements. Specifically, M may be titanium (Ti), zirconium (Zr), or hafnium (Hf), and more specifically, may be zirconium or hafnium.
[0052] M' is titanium, zirconium, or hafnium, each in a formal oxidation state of +2, +3, or +4. Specifically, M' may be zirconium or hafnium.
[0053] X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide, or C 6-20 Specifically, each X is independently a halogen or C 1-20 It may be an alkyl, more specifically, chlorine (Cl) or methyl. Each X' is independently alkyl. Specifically, each X' may be independently methyl.
[0054] Each Q is independently carbon (C), silicon (Si), germanium (Ge), or tin (Sn). Specifically, each Q may be independently carbon (C) or silicon (Si).
[0055] Q' is an anionic leaving group, and each Q' is independently hydrogen, substituted or unsubstituted C 1-40 Hydrocarbon radicals, substituted or unsubstituted C 1-40 Q' is a heterohydrocarbon group, a heteroatom, or a halogen. Specifically, Q' may be a linear or branched alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an aryl group, an alkylaryl group, an arylalkyl group, an acyl group, an aroyl group, an alkoxy group, an aryloxy group, an alkylthio group, a dialkylamino group, an alkoxycarbonyl group, an aryloxycarbonyl group, a carbamoyl group, an alkyl- or dialkyl-carbamoyl group, an acyloxy group, an acylamino group, an aroylamino group, a linear, branched, or cyclic alkylene group, or a combination thereof.
[0056] L, as an element of Group 15 or 16, is preferably nitrogen. Y, as a Group 15 element, is preferably nitrogen or phosphorus, more preferably nitrogen.
[0057] Z, as a Group 15 element, is preferably nitrogen or phosphorus, more preferably nitrogen. Z' is independently -O-, -S-, -N(C 1-40 Hydrocarbon group)-, or -P(C 1-40 Specifically, each Z' may be independently -O-.
[0058] R1~R4, R7, R8, R 11 , and R 12 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, each of which is independently a substituted or unsubstituted, saturated or unsaturated C 4-20 A ring may or may not be formed. Specifically, R1 to R4, R7, R8, R 11 , and R 12 each independently represents a substituted or unsubstituted C 1-20 Alkyl, or substituted or unsubstituted C 6-20 It may be aryl.
[0059] R5, R6, R9, R 10 , R 13 , and R 14 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, where R5 and R6, R9 and R 10 , R 13 and R 14 each independently represents a substituted or unsubstituted saturated or unsaturated C 2-20 A ring may or may not be formed. Specifically, R5, R6, R9, R 10 , R 13 , and R 14 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, or substituted or unsubstituted C 6-20 It may be aryl.
[0060] R 15 and R 16 are each independently 1-20 a hydrocarbon group or a heteroatom-containing group, where the heteroatom is silicon, germanium, tin, lead, or phosphorus, or R 15 and R 16 may be linked to each other. 15 and R 16 are each independently 1-6 It may also be a hydrocarbon group.
[0061] R 17 is absent or hydrogen, C 1-20 R is an alkyl, halogen, or heteroatom-containing group. 17 may be hydrogen or methyl.
[0062] R 18 and R 19 are each independently an alkyl group, an aryl group, a substituted aryl group, a cyclic alkyl group, a substituted cyclic alkyl group, or a polycyclic ring system. 18 and R 19 may each independently be a substituted aryl group.
[0063] R 20 and R 21 may each independently be absent, a hydrogen, an alkyl group, a halogen, a heteroatom, a hydrocarbon group, or a heteroatom-containing group.
[0064] R x and R y each independently represents a substituted or unsubstituted C 1-40 Hydrocarbon radicals, substituted or unsubstituted C 1-40 R is a heterohydrocarbon group, a halogen, or a hydrogen. x and R y may each independently be methyl or hydrogen.
[0065] R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d each independently represents a substituted or unsubstituted C 1-40Hydrocarbon radicals, substituted or unsubstituted C 1-40 Heterohydrocarbon group, -Si(R e )3, -OSi(R e )3, -Ge(R e )3, -P(R e )2, -N(R e )2, -OR e , -SR e , -NO2, -CN, -CF3, -OCF3, -S(O)R e , -S(O)2R e , -N=C(R e )2, -OC(O)R e , -C(O)OR e , -N(R)C(O)R e , -C(O)N(R e )2, halogen, and hydrogen, where R e each independently represents a substituted or unsubstituted C 1-30 Hydrocarbon group or substituted or unsubstituted C 1-30 Heterohydrocarbon group, where R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d Two or more of may or may not form one or more ring structures.
[0066] In the hybrid metallocene catalyst for olefin polymerization according to the embodiment of the present invention, the content of the first transition metal compound, the second transition metal compound, and the third transition metal compound may be determined according to the activity of each catalyst. Preferably, based on the total amount of the transition metal compounds in the hybrid metallocene catalyst for olefin polymerization, the first transition metal compound, the second transition metal compound, and the third transition metal compound may each be contained in an amount of 10 wt% or more.
[0067] In a specific example of the present invention, the transition metal compound of Chemical Formula 1 may be at least one of transition metal compounds represented by the following Chemical Formulas 1-1 to 1-8, and the transition metal compound of Chemical Formula 2 may be a transition metal compound represented by the following Chemical Formula 2-1. [ka] In the above formula, Me is methyl.
[0068] In a specific example of the present invention, the transition metal compound of the formula 3 may be at least one of the transition metal compounds represented by the following formulas 3-1 to 3-10. [ka] TIFF2024541729000017.tif53170In the above chemical formula, Me is methyl, n-Bu is n-butyl, t-Bu is t-butyl, Ph is phenyl, and p-Tol is p-tolyl.
[0069] In a specific example of the present invention, the transition metal compound of chemical formula 4 may be at least one of the transition metal compounds represented by the following chemical formulae 4-1 to 4-2, the transition metal compound of chemical formula 5a may be at least one of the transition metal compounds represented by the following chemical formulae 5-1 to 5-4, and the compound of chemical formula 5b may be at least one of the transition metal compounds represented by the following chemical formulae 5-5 and 5-6. [ka] In the above formula, Me is methyl, t-Bu is t-butyl, and Ph is phenyl.
[0070] In an embodiment of the present invention, the co-catalyst compound may include at least one selected from the group consisting of a compound represented by the following chemical formula 6, a compound represented by the following chemical formula 7, and a compound represented by the following chemical formula 8.
[0071] [ka] (Chemical formula 6) In the above Chemical Formula 6, n is an integer of 2 or more, and R a may be a halogen atom, a hydrocarbon having 1 to 20 carbon atoms, or a hydrocarbon having 1 to 20 carbon atoms substituted with a halogen atom. a may be methyl, ethyl, n-butyl, or isobutyl.
[0072] [ka] (Chemical formula 7) In the above formula 7, D is aluminum (Al) or boron (B), and R b , R c , and R d are each independently a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, or an alkoxy group having 1 to 20 carbon atoms. Specifically, when D is aluminum (Al), R b , R c , and R d may each independently be methyl or isobutyl, and when D is boron (B), R b , R c , and R d may each be pentafluorophenyl.
[0073] [ka] In the above formula 8, L is a neutral or cationic Lewis base, [LH] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms. + may be a dimethylanilinium cation, [Z(A)4] - is [B(C6F5)4]- [L] + is [(C6H5)3C] + may be also possible.
[0074] Examples of the compound represented by Formula 6 include methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, etc., and methylaluminoxane is preferred, but is not limited thereto.
[0075] Examples of the compound represented by Chemical Formula 7 include trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylchloroaluminum, triisopropylaluminum, tri-s-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, and tributylboron. Of these, trimethylaluminum, triethylaluminum, and triisobutylaluminum are preferred, but the examples are not limited thereto.
[0076] Examples of the compound represented by Chemical Formula 8 include triethylammonium tetraphenylboron, tributylammonium tetraphenylboron, trimethylammonium tetraphenylboron, tripropylammonium tetraphenylboron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron, tributylammonium tetrapentafluorophenylboron, N,N-diethylanilinium tetraphenylboron, N,N-diethylanilinium tetrapentafluorophenylboron, diethylammonium tetrapentafluorophenylboron, triphenylphosphonium tetraphenylboron, trimethylphosphonium tetraphenylboron, triethylammonium tetraphenylaluminum, tributylammonium tetraphenylaluminum, trimethylammonium tetraphenylaluminum, tripropylammonium tetra Phenylaluminum, trimethylammonium tetra(p-tolyl)aluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetrapentafluorophenylaluminum, N,N-diethylanilinium tetraphenylaluminum, N,N-diethylanilinium tetrapentafluorophenylaluminum, diethylammonium tetrapentatetraphenylaluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl)boron, triphenylcarbonium tetra(p-trifluoromethylphenyl)boron, triphenylcarbonium tetrapentafluorophenylboron, and the like.
[0077] In an embodiment of the present invention, the hybrid metallocene catalyst for olefin polymerization may further comprise a support supporting the hybrid transition metal compound, the cocatalyst compound, or both.
[0078] Here, the carrier may include a substance containing a hydroxyl group on the surface, and preferably a substance having a highly reactive hydroxyl group and a siloxane group, which has been dried to remove moisture from the surface, may be used. For example, the carrier may include at least one selected from the group consisting of silica, alumina, and magnesia. Specifically, silica, silica-alumina, and silica-magnesia, etc., dried at high temperature may be used as the carrier, and these may usually contain oxide, carbonate, sulfate, and nitrate components such as Na2O, K2CO3, BaSO4, and Mg(NO3)2. These may also include carbon, zeolite, magnesium chloride, etc. However, the carrier is not particularly limited to these.
[0079] The carrier may have an average particle size of 10 to 250 μm, preferably 10 to 150 μm, and more preferably 20 to 100 μm.
[0080] The volume of the micropores in the carrier may be 0.1 to 10 ml / g, preferably 0.5 to 5 ml / g, and more preferably 1.0 to 3.0 ml / g.
[0081] The specific surface area of the support is 1 to 1,000 m 2 / g, preferably 100 to 800m 2 / g, more preferably 200 to 600m 2 / g.
[0082] In a preferred embodiment, when the support is silica, the drying temperature may be 200 to 900° C. The drying temperature may be preferably 300 to 800° C., more preferably 400 to 700° C. If the drying temperature is less than 200° C., there will be too much moisture, and the moisture on the surface will react with the first promoter compound, and if the drying temperature exceeds 900° C., the structure of the support may collapse.
[0083] The concentration of hydroxyl groups in the dried silica may be 0.1 to 5 mmole / g, preferably 0.7 to 4 mmole / g, and more preferably 1.0 to 2 mmole / g. If the concentration of hydroxyl groups is less than 0.1 mmole / g, the amount of the co-catalyst supported will be low, and if it exceeds 5 mmole / g, the catalyst component may be inactivated.
[0084] The total amount of the mixed transition metal compound supported on the carrier may be 0.001 to 1 mmole based on 1 g of the carrier. When the ratio of the mixed transition metal compound to the carrier satisfies the above range, the supported catalyst exhibits appropriate activity, which is advantageous in terms of maintaining the activity of the catalyst and in terms of economic efficiency.
[0085] The total amount of the promoter compounds supported on the carrier may be 2 to 15 mmole per gram of carrier. When the ratio of the promoter compounds to the carrier is within the above range, it is advantageous in terms of maintaining the activity of the catalyst and economic efficiency.
[0086] The carrier may be one or more. For example, both the mixed transition metal compound and the co-catalyst compound may be supported on one carrier, or the mixed transition metal compound and the co-catalyst compound may be supported on two or more carriers. Also, only one of the mixed transition metal compound and the co-catalyst compound may be supported on the carrier.
[0087] In an embodiment of the present invention, the olefin-based polymer may be a homopolymer of an olefin-based monomer or a copolymer of an olefin-based monomer and a comonomer. Preferably, the olefin-based polymer is a copolymer of an olefin-based monomer and an olefin-based comonomer.
[0088] Here, the olefin monomer is C 2-20 α-olefin, C 1-20 Diolefin, C 3-20 Cycloolefin, and C 3-20 At least one selected from the group consisting of cyclodiolefins.
[0089] For example, the olefin monomer may be ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, or 1-hexadecene, and the olefin polymer may be a homopolymer containing only one of the olefin monomers exemplified above, or a copolymer containing two or more of them.
[0090] In an exemplary embodiment, the olefin polymer comprises ethylene and C 3-20 It may be a copolymer in which an α-olefin is copolymerized. Preferably, the olefin-based polymer is a linear low-density polyethylene in which the olefin-based monomer is ethylene and the olefin-based comonomer is 1-hexene.
[0091] In this case, the ethylene content is preferably 55 to 99.9% by weight, more preferably 90 to 99.9% by weight, and the α-olefin comonomer content is preferably 0.1 to 45% by weight, more preferably 0.1 to 10% by weight.
[0092] [Method of producing olefin polymer] According to one embodiment of the present invention, there is provided a method for producing an olefin polymer, comprising: polymerizing ethylene and at least one α-olefin in the presence of a mixed metallocene catalyst comprising: (a) at least one first transition metal compound selected from a transition metal compound represented by the following chemical formula 1 and a transition metal compound represented by the following chemical formula 2; (b) at least one second transition metal compound selected from a transition metal compound represented by the following chemical formula 3; (c) at least one third transition metal compound selected from a transition metal compound represented by the following chemical formula 4, a transition metal compound represented by the following chemical formula 5a, and a transition metal compound represented by the following chemical formula 5b; and (d) a co-catalyst compound.
[0093] [ka]
[0094] In the chemical formula, l1, l2, l3, m1, m2, m3, n1, o1, p, q, M, M', X, X', Q, Q', L, Y, Z, Z', R1~R 21 , R x , R y , R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d is the same as that explained in the above section [Olefin-based polymer].
[0095] As described above, the olefin polymer produced by the production method according to one embodiment of the present invention has a density of 0.930 to 0.970 g / cm 3 , preferably 0.935 to 0.965 g / cm 3 , more preferably 0.935 to 0.960 g / cm3 , particularly preferably 0.940 to 0.950 g / cm 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, preferably 0.5 to 4.5 g / 10 min, more preferably 0.5 to 4.0 g / 10 min, and particularly preferably 0.5 to 2.0 g / 10 min; and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) is 30 to 200, preferably 30 to 150, more preferably 40 to 135, and particularly preferably 50 to 120, and the molecular weight distribution is unimodal with a shoulder when measured by gel permeation chromatography, and melt fracture or sharkskin phenomenon appears when measured by a capillary rheometer. -1 More than 700sec, preferably -1 More than 750 seconds, preferably -1 That's all, 1,050sec -1 or more, or 1,100sec -1 That's all.
[0096]
number
[0097] In an exemplary embodiment of the present invention, the olefin-based polymer may be polymerized by polymerization reactions such as, but not limited to, free radical, cationic, coordination, condensation, and addition.
[0098] As an embodiment of the present invention, the olefin polymer may be produced by a gas phase polymerization method, a solution polymerization method, a slurry polymerization method, etc. Preferably, the polymerization of the olefin monomer may be carried out by gas phase polymerization, specifically, the polymerization of the olefin monomer may be carried out in a gas phase fluidized bed reactor.
[0099] When the olefin polymer is produced by a solution polymerization method or a slurry polymerization method, examples of the solvent that can be used include C tetrahydrofuran such as pentane, hexane, heptane, nonane, decane, and their isomers. 5-12 Examples of the solvent include, but are not limited to, aliphatic hydrocarbon solvents; aromatic hydrocarbon solvents such as toluene and benzene; chlorine-substituted hydrocarbon solvents such as dichloromethane and chlorobenzene; and mixtures thereof.
[0100] [Example] The present invention will be described in more detail below with reference to examples and comparative examples. However, the following examples are merely for the purpose of illustrating the present invention, and the scope of the present invention is not limited to these examples.
[0101] Manufacturing Example 1 1.7g of the transition metal compound of formula 1-1, 0.76g of the transition metal compound of formula 3-1, and 3.5g of the transition metal compound of formula 5-2 were mixed with 951.2g of 10% by weight toluene solution of methylaluminoxane (MAO) (Al / Zr=150) in a glove box and stirred at room temperature for 1 hour. Meanwhile, 230g of silica (XP2402) was put into a reactor, and 1,000ml of purified toluene was added and mixed. The above-mentioned transition metal compound solution was poured into the obtained silica slurry and stirred in an oil bath at 75°C for 3 hours. After the loading was completed and the solid / liquid were sufficiently separated, the supernatant was removed. The supported catalyst was washed three times with toluene and dried in a vacuum at 30°C for 10 hours to obtain 320g of a free-flowing powdered hybrid supported catalyst.
[0102] Manufacturing Example 2 1.4g of the transition metal compound of formula 1-1, 0.63g of the transition metal compound of formula 3-1, and 2.72g of the transition metal compound of formula 4-1 were mixed with 825g of 10% by weight toluene solution of methylaluminoxane (MAO) (Al / Zr=150) in a glove box and stirred at room temperature for 1 hour. Meanwhile, 200g of silica (XP2402) was put into a reactor, and 1,000ml of purified toluene was added and mixed. The above-mentioned transition metal compound solution was poured into the obtained silica slurry and stirred in an oil bath at 75°C for 3 hours. After the loading was completed and the solid / liquid were sufficiently separated, the supernatant was removed. The supported catalyst was washed three times with toluene and dried in a vacuum at 60°C for 10 hours to obtain 280g of a free-flowing powdered hybrid supported catalyst.
[0103] Production Example 3 A free-flowing powdery hybrid supported catalyst (280 g) was obtained in the same manner as in Preparation Example 2, except that 1.4 g of the transition metal compound of formula 1-1, 1.25 g of the transition metal compound of formula 3-1, and 2.2 g of the transition metal compound of formula 4-1 were used.
[0104] Production Example 4 280 g of a free-flowing powdery hybrid supported catalyst was obtained in the same manner as in Preparation Example 2, except that 1.3 g of the transition metal compound of Chemical Formula 2-1, 0.63 g of the transition metal compound of Chemical Formula 3-1, 2.72 g of the transition metal compound of Chemical Formula 4-1, and 824 g of a 10 wt % toluene solution of methylaluminoxane (MAO) were used.
[0105] Production Example 5 A free-flowing powdery hybrid supported catalyst (280 g) was obtained in the same manner as in Preparation 1, except that 1.4 g of the transition metal compound of formula 1-1, 0.63 g of the transition metal compound of formula 3-1, and 2.72 g of the transition metal compound of formula 5-2 were used.
[0106] Working Example Using each of the supported catalysts obtained in the above Production Examples, ethylene and 1-hexene were copolymerized in a continuous gas-phase fluidized bed reactor. Hydrogen was added to adjust the molecular weight of the polymer. The polymerization conditions are summarized in Table 1 below. For comparison, 8380 resin manufactured by Hanwha Solutions, which is produced using a nonmetallocene catalyst, was used as Comparative Example 2.
[0107] [Table 1]
[0108] Test Example The physical properties of the olefin polymers produced using the supported catalysts obtained in the Examples and Comparative Examples were measured as follows. The measurement results are shown in Tables 2 and 3 below.
[0109] (1) Melt flow ratio (MFR) According to ASTM D1238, the melt index was measured at 190°C under a load of 21.6 kg and 2.16 kg, and the ratio (MI 21.6 / MI 2.16 ) was sought.
[0110] (2) Density Measured according to ASTM D1505.
[0111] (3) Gel Permeation Chromatography A gel permeation chromatography-FTIR (GPC-FTIR) with the model name GPC-6 manufactured by Polymer Char was used. Measurements were performed at a temperature of 160° C., and trichlorobenzene was used as the solvent. The measurement results of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in FIG. 2 to FIG. 7, respectively.
[0112] (4) Shear rate Measurements were performed using a Gottfert RG25 capillary rheometer. Measurement conditions were: circular hole, length 20 mm, effective length 20 mm, diameter / width 2, height 0 mm, run angle 180°, 230°C, piston diameter 15 mm, and capillary diameter 2 mm. Measurements were performed based on the shear rate at which sharkskin and melt fracture occurred, and the shear rate was calculated from the above mathematical formula 1. For the polymers of Examples 1 to 4 and Comparative Examples 1 and 2, the presence or absence of sharkskin and melt fracture depending on the shear rate was observed, and the results are shown in Figures 8 and 9, respectively.
[0113] [Table 2]
[0114] [Table 3]
[0115] As can be seen from Tables 2 and 3 and Figures 2 to 9, the olefin polymers of the Examples (Figures 2 to 5 and Figure 8) within the scope of the present invention, which have a unimodal broad molecular weight distribution with a shoulder, had a high shear rate at which melt fracture or sharkskin appeared, and were excellent in high-speed processability. In contrast, the olefin polymer of Comparative Example 1 (Figures 6 and 9), which has a bimodal molecular weight distribution, suffered from melt fracture at a low shear rate, and had poor high-speed processability. Moreover, the olefin polymers of the Examples showed high-speed processability similar to or better than that of a commercial product (Comparative Example 2; Figures 7 and 9). [Industrial Applicability]
[0116] According to an embodiment of the present invention, an olefin polymer produced by using a hybrid metallocene catalyst has a broad, unimodal molecular weight distribution having a shoulder, and is excellent in high-speed processability.
Claims
1. Density: 0.930 to 0.970 g / cm 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The melt flow ratio (MFR) of the polymer is 30 to 200, the molecular weight distribution is unimodal with a shoulder when measured by gel permeation chromatography (GPC), and melt fracture or shark skin phenomenon occurs when measured by a capillary rheometer. -1 The olefin polymer is as described above. [0010] (mathematical formula 1) In the above mathematical formula: 【number】 is the apparent shear rate (sec -1 ), and V is the volumetric flow rate (mm 3 / sec) and R is the radius of the circular hole capillary (mm).
2. Density is 0.930 to 0.965 g / cm 3 and the melt index (I 2.16 ) is 0.5 to 4.5 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The ratio (MFR) of the melt flow rate to the melt flow rate (MFR) is 30 to 150, and the shear rate at which melt fracture and sharkskin phenomena appear when measured with a capillary rheometer is 700 sec -1 The olefin polymer according to claim 1 .
3. The olefin polymer according to claim 1, produced by polymerization of ethylene and at least one α-olefin in the presence of a hybrid metallocene catalyst, the hybrid metallocene catalyst comprising: (a) at least one first transition metal compound selected from a transition metal compound represented by the following chemical formula 1 and a transition metal compound represented by the following chemical formula 2; (b) at least one second transition metal compound selected from a transition metal compound represented by the following chemical formula 3; (c) at least one tertiary transition metal compound selected from a transition metal compound represented by the following chemical formula 4, a transition metal compound represented by the following chemical formula 5a, and a transition metal compound represented by the following chemical formula 5b; and (d) a co-catalyst compound. 【Chemistry 1】 In the above chemical formula, l1 and m1 each independently represent an integer of 0 to 5. l2, l3, m2, and n1 each independently represent an integer of 0 to 4; m3 and o1 each independently represent an integer of 0 to 2, p is the oxidation state of M, +3, +4, or +5; q is the formal charge of the YZL ligand and is 0, -1, -2, or -3; M is independently titanium (Ti), zirconium (Zr), or hafnium (Hf); M' is titanium, zirconium, or hafnium, each in a formal oxidation state of +2, +3, or +4; X is independently halogen, C 1-20 Alkyl, C 2-20 Alkenyl, C 2-20 Alkynyl, C 6-20 Aryl, C 1-20 Alkyl C 6-20 Aryl, C 6-20 Aryl C 1-20 Alkyl, C 1-20 Alkylamide, or C 6-20 is an aryl amide, Each X' is independently alkyl; Each Q is independently carbon (C), silicon (Si), germanium (Ge), or tin (Sn); Q′ is an anionic leaving group, and each Q′ is independently hydrogen, substituted or unsubstituted C 1-40 Hydrocarbon group, substituted or unsubstituted C 1-40 a heterohydrocarbon group, a heteroatom, or a halogen; L is a Group 15 or 16 element; Y is a Group 15 element; Z is a Group 15 element; Z' is independently -O-, -S-, -N(C 1-40 Hydrocarbon group)-, or -P(C 1-40 a hydrocarbon group)-, R 1 ~R 4 , R 7 , R 8 , R 11 , and R 12 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, wherein each of these independently represents a substituted or unsubstituted, saturated or unsaturated C 4-20 may or may not form a ring, R 5 , R 6 , R 9 , R 10 , R 13 , and R 14 each independently represents a substituted or unsubstituted C 1-20 Alkyl, substituted or unsubstituted C 2-20 Alkenyl, substituted or unsubstituted C 6-20 Aryl, substituted or unsubstituted C 1-20 Alkyl C 6-20 Aryl, substituted or unsubstituted C 6-20 Aryl C 1-20 Alkyl, substituted or unsubstituted C 1-20 Heteroalkyl, substituted or unsubstituted C 3-20 Heteroaryl, substituted or unsubstituted C 1-20 Alkylamide, substituted or unsubstituted C 6-20 Arylamide or substituted or unsubstituted C 1-20 silyl, where R 5 and R 6 , R 9 and R 10 , R 13 and R 14 are each independently linked to each other and are substituted or unsubstituted, saturated or unsaturated C 2-20 may or may not form a ring, R 15 and R 16 are each independently 1-20 a hydrocarbon group or a heteroatom-containing group, where the heteroatom is silicon, germanium, tin, lead, or phosphorus, or R 15 and R 16 may be linked to each other, R 17 is absent or hydrogen, C 1-20 is an alkyl, halogen, or heteroatom-containing group; R 18 and R 19 are each independently an alkyl group, an aryl group, a substituted aryl group, a cyclic alkyl group, a substituted cyclic alkyl group, or a polycyclic ring system; R 20 and R 21 are each independently absent, a hydrogen, an alkyl group, a halogen, a heteroatom, a hydrocarbon group, or a heteroatom-containing group; R x and R y each independently represents a substituted or unsubstituted C 1-40 Hydrocarbon group, substituted or unsubstituted C 1-40 a heterohydrocarbon group, a halogen, or hydrogen; R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d each independently represents a substituted or unsubstituted C 1-40 Hydrocarbon group, substituted or unsubstituted C 1-40 Heterohydrocarbon group, -Si(R e ) 3 , -OSi(R e ) 3 , -Ge(R e ) 3 , -P(R e ) 2 , -N(R e ) 2 , -OR e , -SR e , -NO 2 , -CN, -CF 3 , -OCF 3 , -S(O)R e , -S(O) 2 R e , -N=C(R e ) 2 , -OC(O)R e , -C(O)OR e , -N(R)C(O)R e , -C(O)N(R e ) 2 , halogen, and hydrogen, where R e each independently represents a substituted or unsubstituted C 1-30 A hydrocarbon group or a substituted or unsubstituted C 1-30 Heterohydrocarbon group, where R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d Two or more of may or may not form one or more ring structures.
4. The transition metal compound of Chemical Formula 1 is at least one of transition metal compounds represented by Chemical Formulas 1-1 to 1-8 below, and the transition metal compound of Chemical Formula 2 is a transition metal compound represented by Chemical Formula 2-1 below. The olefin polymer according to claim 3. 【Chemistry 2】 In the above formula, Me is methyl.
5. The olefin polymer according to claim 3, wherein the transition metal compound of the formula 3 is at least one of transition metal compounds represented by the following formulas 3-1 to 3-10. 【Chemistry 3】 【change】 In the above chemical formula, Me is methyl, n-Bu is n-butyl, t-Bu is t-butyl, Ph is phenyl, and p-Tol is p-tolyl.
6. The transition metal compound of Chemical Formula 4 is at least one of transition metal compounds represented by Chemical Formulae 4-1 to 4-2 below, the transition metal compound of Chemical Formula 5a is at least one of transition metal compounds represented by Chemical Formulae 5-1 to 5-4 below, and the compound of Chemical Formula 5b is at least one of transition metal compounds represented by Chemical Formulae 5-5 and 5-6 below. The olefin polymer according to claim 3, 【Chemistry 4】 In the above formula, Me is methyl, t-Bu is t-butyl, and Ph is phenyl.
7. The olefin polymer according to claim 3, wherein the co-catalyst compound comprises at least one selected from the group consisting of a compound represented by the following chemical formula 6, a compound represented by the following chemical formula 7, and a compound represented by the following chemical formula 8: 【Chemistry 5】 (Chemical formula 6) 【change】 (Chemical formula 7) [L-H] + [Z(A) 4 ] - Or [L] + [Z(A) 4 ] - (Chemical formula 8) In the above formula 6, n is an integer of 2 or more, R a is a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, In the above formula 7, D is aluminum (Al) or boron (B), R b , R c , and R d each independently represents a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a halogen-substituted hydrocarbon group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, In the above formula 8, L is a neutral or cationic Lewis base, [L-H] + and [L] + is a Bronsted acid, Z is a Group 13 element, and each A is independently a substituted or unsubstituted aryl group having 6 to 20 carbon atoms or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.
8. 8. The olefin polymer according to claim 7, wherein the compound represented by Chemical Formula 6 is at least one selected from the group consisting of methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, and butylaluminoxane.
9. The olefin polymer according to claim 7, wherein the compound represented by Chemical Formula 7 is at least one selected from the group consisting of trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylchloroaluminum, triisopropylaluminum, tri-s-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, and tributylboron.
10. The compound represented by Chemical Formula 8 includes triethylammonium tetraphenylboron, tributylammonium tetraphenylboron, trimethylammonium tetraphenylboron, tripropylammonium tetraphenylboron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron, tributylammonium tetrapentafluorophenylboron, N,N-diethylanilinium tetraphenylboron, N,N-diethylanilinium tetrapentafluorophenylboron, diethylammonium tetrapentafluorophenylboron, triphenylphosphonium tetraphenylboron, trimethylphosphonium tetraphenylboron, triethylammonium tetraphenylaluminum, tributylammonium tetraphenylaluminum, trimethylammonium tetraphenylaluminum, tripropylammonium tetraphenylaluminum, trimethylammonium tetraphenylaluminum, 8. The olefin polymer according to claim 7, which is at least one selected from the group consisting of N,N-diethylanilinium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetrapentafluorophenylaluminum, N,N-diethylanilinium tetraphenylaluminum, N,N-diethylanilinium tetrapentafluorophenylaluminum, diethylammonium tetrapentatetraphenylaluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl)boron, triphenylcarbonium tetra(p-trifluoromethylphenyl)boron, and triphenylcarbonium tetrapentafluorophenylboron.
11. The olefin-based polymer according to claim 3, wherein the hybrid metallocene catalyst further comprises a support supporting the hybrid transition metal compound, the cocatalyst compound, or both.
12. The olefin-based polymer according to claim 11, wherein the support comprises at least one selected from the group consisting of silica, alumina, and magnesia.
13. The olefin polymer according to claim 11, wherein the total amount of the mixed transition metal compounds supported on the support is 0.001 to 1 mmole based on 1 g of the support, and the total amount of the co-catalyst compounds supported on the support is 2 to 15 mmole based on 1 g of the support.
14. The method includes a step of polymerizing ethylene and at least one α-olefin in the presence of a mixed metallocene catalyst comprising: (a) at least one first transition metal compound selected from a transition metal compound represented by the following chemical formula 1 and a transition metal compound represented by the following chemical formula 2; (b) at least one second transition metal compound selected from a transition metal compound represented by the following chemical formula 3; (c) at least one third transition metal compound selected from a transition metal compound represented by the following chemical formula 4, a transition metal compound represented by the following chemical formula 5a, and a transition metal compound represented by the following chemical formula 5b; and (d) a co-catalyst compound, to obtain an olefin polymer, wherein the density of the olefin polymer is 0.930 to 0.970 g / cm. 3 and the melt index (I 2.16 ) is 0.1 to 5.0 g / 10 min, and the melt index (I 21.6 ) and the melt index (I 2.16 The ratio (MFR) of the molecular weight distribution to the molecular weight of the polymer is 30 to 200, and when measured by gel permeation chromatography, the molecular weight distribution is unimodal with a shoulder, and when measured by a capillary rheometer, melt fracture and shark skin phenomenon appear. -1 The above is the method for producing an olefin polymer. 【number】 [0025] (Mathematical formula 1) In the chemical formula, l1, l2, l3, m1, m2, m3, n1, o1, p, q, M, M', X, X', Q, Q', L, Y, Z, Z', R 1 ~R 21 , R x , R y , R 22a , R 23a , R 24a , R 25a , R 22b , R 23b , R 24b , R 25b , R 26c , R 27c , R 28c , R 29c , R 26d , R 27d , R 28d , and R 29d is as defined in claim 3, and in the mathematical formula: 【number】 , V, and R are as defined in claim 1.
15. The method for producing an olefin polymer according to claim 14, wherein the α-olefin is at least one selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, and 1-hexadecene.
16. The method for producing an olefin polymer according to claim 15, wherein the α-olefin is 1-hexene.
17. The process for producing an olefin polymer according to claim 14, wherein the polymerization of ethylene and at least one α-olefin is carried out by gas phase polymerization.
Citation Information
Patent Citations
Olefin polymer with excellent processability
JP2017526773A
Ethylene / alpha-olefin copolymer with excellent processability
JP2017536422A