Dissimilar metal joint and resistance welding method thereof

The described resistance welding method for dissimilar metal joints addresses the issue of low weld strength and brittle intermetallic compounds by using a laminated structure and a sputtering process to evacuate light metals, resulting in high-quality, mechanically strong joints between steel and aluminum or magnesium alloys.

JP2024541826AActive Publication Date: 2024-11-13SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024521284
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-21
Filing Date
2022-08-17
Publication Date
2024-11-13
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

Conventional resistance welding methods for dissimilar metal joints, particularly between steel and aluminum or magnesium alloys, result in low weld strength and the formation of brittle intermetallic compounds, leading to cracks and reduced mechanical integrity.

Method used

A resistance welding method involving a laminated structure with a first class metal plate made of pure iron or iron-based alloys and a second class metal plate with a melting point below 800°C, utilizing a sputtering process to evacuate the second class metal from the welding area, followed by a welding step to form a metallurgical bond between the first class metal plates.

Benefits of technology

The method achieves high-quality joining of dissimilar metals with improved mechanical strength, reduced electrode wear, and wide applicability to various metal combinations, including steel and light metals like aluminum and magnesium, without the formation of brittle intermetallic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541826000001_ABST
    Figure 2024541826000001_ABST
Patent Text Reader

Abstract

The present invention provides a method for resistance welding of dissimilar metal joints, the method comprising the steps of: an outer layer made of iron or an iron-based alloy; and an inner layer having a density of 5 g / cm 3 The present invention welds a laminated structure made of a metal having a melting point of less than 800°C or a light metal having a melting point of less than 800°C. The resistance welding method includes a sputtering step, in which the light metal or low melting point metal in the middle of the laminated structure is detached in the form of sputtering, and a direct joint structure of iron or iron-based alloy layers is formed in the weld interface to complete the welding. The present invention can avoid the formation of brittle intermetallic compounds in the weld interface of dissimilar joints, improve the mechanical performance of the joint, and realize reliable joint between dissimilar metals. The present invention further provides a dissimilar metal joint.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of welding, and more particularly to a dissimilar metal joint and a resistance welding method thereof. [Background technology]

[0002] With the ever-increasing demand for energy saving and emission reduction, lightweight design has become an important issue facing the automobile industry. In a few luxury brand products, design methods such as all-aluminum body have already appeared. However, all-aluminum body is expensive, difficult to maintain, and its price is not widely accepted by ordinary consumers. Therefore, in mainstream products on the market, the main body of the car body structure, especially the structural members such as A-pillar, B-pillar, door reinforcement plate and side member, is still mainly made of steel, and high-strength steel and even ultra-high-strength steel are increasingly used to replace traditional ordinary steel. In addition, automobile enterprises and consumers gradually find that the use of light alloy materials including aluminum alloy and magnesium alloy in shock absorbers, wheelhouse end plates, floors, engines and body exterior coating members is an acceptable solution in terms of both cost and performance. Therefore, the manufacturing method of automobiles that combines steel and light metal is becoming more and more popular. The importance of the joining process of steel and light metal dissimilar joints is becoming apparent.

[0003] In the conventional manufacturing process of the body-in-white, resistance welding is often used to perform resistance welding joints on steel plates. However, the physical properties of steel, especially high-strength steel, are significantly different from those of aluminum alloys and magnesium alloys, and the melting point of steel is generally above 1400°C, while the melting point of aluminum alloys and magnesium alloys is often below 700°C. In the conventional resistance welding process, defects such as a large amount of porosity and cracks are generated in the welded joint between steel and aluminum or magnesium alloy, and a large amount of brittle iron-aluminum or iron-magnesium intermetallic compounds are formed in the welded area, which greatly affects the mechanical strength of the joint.

[0004] Some prior art uses a three-layer composite structure of steel workpiece-aluminum workpiece-steel workpiece or a steel part-aluminum workpiece-steel workpiece, of which the steel part is generally a specially designed rivet, including specially made solid, hollow and semi-hollow rivets. When these are combined and welded, the welding area is first heated or the steel part is driven to rotate at high speed and held in contact with the aluminum part, the intermediate aluminum plate is softened or semi-molten at high temperature, and the welding equipment is provided with a larger pressure to push the softened or semi-molten aluminum alloy out of the welding area, and the welding means is then completed directly between the outermost steel plate or steel part and the steel workpiece. However, the inventors have found that in this process, the heated high-temperature aluminum alloy is in contact with the steel plate for a long time, resulting in the formation of a large amount of brittle intermetallic compounds, and the high-temperature plastic aluminum alloy is also difficult to be efficiently pushed out of the welding area, which affects the quality of the weld. The reason for this is that when dissimilar metals such as aluminum and steel are welded together, iron has a high solid solubility in aluminum, but aluminum is hardly capable of forming a solid solution in iron, so a large amount of solid solution cannot be formed between iron and aluminum. As a result, a large amount of brittle iron-aluminum intermetallic compounds (such as FeAl3, Fe2Al5, FeAl2, FeAl, Fe3Al, etc.) is rapidly formed in the weld seam during welding. These brittle intermetallic compounds usually have a layered structure and are distributed in the weld interface. When the compound layer is subjected to external stress, it is very easy to generate cracks and promote crack growth, which is thought to have a significant adverse effect on the final joint strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-328774 [Patent Document 2] JP 2003-236673 A Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to provide a method for resistance welding of dissimilar metal joints, which solves the problems of low weld strength, the presence of a large amount of brittle intermetallic compounds at the weld interface, and the tendency for cracks to occur when dissimilar metals are welded by resistance spot welding. [Means for solving the problem]

[0007] Another object of the present invention is to provide a dissimilar metal joint having a reliable bond.

[0008] According to one aspect of the embodiment of the present invention, there is provided a method for resistance welding a dissimilar metal joint, the method comprising: welding a dissimilar metal laminate structure, the laminate structure including a first class metal plate and a second class metal plate, the first class metal plate being pure iron or an iron-based alloy, and the second class metal plate being a metal having a density of 5 g / cm 3 The second metal is an element or alloy having a melting point of less than 800°C. The outer plate of the stack structure is a first class metal plate, and the second class metal plate is located between the first class metal plates. The resistance welding method includes a step of discharging the second class metal plate from a welding area and a welding step, and the step of discharging the second class metal plate includes a sputtering step. In the sputtering step, a sputtering ring current and an electrode pressure are applied to the stack structure to heat the stack structure in the welding area, the second class metal melts and is separated from the welding area in the form of sputtering under the action of pressure, and the first class metals approach each other under the action of resistance heat and pressure, where the second class metal plates are completely scattered in at least a part of the welding area. In the welding step, a welding interface is formed in which only the first class metal plates are in contact with each other in at least a part of the welding area, and a metallurgical bond is generated at the welding interface.

[0009] Optionally, the sputtering current comprises one or more current pulses, preferably 2-5, and the duration of a single current pulse is less than or equal to 200 ms, preferably 50 ms-120 ms.

[0010] Furthermore, the sputtering current intensity I1 = K1 * I0, where I0 is the current intensity when resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧ 4√t, t is the thickness of the thinner one of the first class metal plates, and the range of possible values ​​for K1 is 0.8 to 3.5.

[0011] Optionally, in the sputtering step, after the second class metal plate is separated from the welding area in a sputtering manner, a welding interface is formed by contacting only the first class metal plate, and it is preferable that the thickness of the second class metal layer remaining at the welding interface is ≦0.15 mm, and the equivalent diameter of the welding interface is ≧0.5 times the electrode end face diameter, and the thickness of the second class metal layer remaining therein is ≦0.05 mm.

[0012] Optionally, the welding step applies a welding current and electrode pressure to the laminated structure, the welding current having an intensity less than or equal to an intensity of the sputtering current.

[0013] Furthermore, the welding current intensity I2=K2*I0, where I0 is the current intensity when the first class metal plates in the dissimilar metal joint are individually resistance-welded to form a weld nugget cross-sectional diameter ≧4√t, t is the thickness of the thinner plate among the first class metal plates, and the range of values ​​that K2 can take is 0.5 to 2.5. Controlling the welding current intensity can ensure the weld strength of the dissimilar joint obtained by the resistance welding method.

[0014] Optionally, the interval between the sputtering current and the welding current is between 0 ms and 200 ms.

[0015] Optionally, the method further comprises a tempering step after the welding step, in which an electrode provides a tempering current to the welded area. The tempering process can improve the mechanical performance of the joint.

[0016] Furthermore, the tempering current intensity I3=K3*I0, where I0 is the current intensity when resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧4√t, t is the thickness of the thinner plate among the first class metal plates, and the range of possible values ​​for K3 is 0.4 to 1.8.

[0017] Optionally, the method further includes a preheating step prior to the sputtering step, in which an electrode provides a preheating current to the area to be welded. The preheating process can melt the aluminum alloy or magnesium alloy in the intermediate layer faster and facilitate the occurrence of the sputtering process.

[0018] Furthermore, the preheating current intensity I4 = K4 * I0, where I0 is the current intensity when resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧ 4√t, t is the thickness of the thinner one of the first class metal plates, and the range of values ​​that K4 can take is 0.2 to 1.3.

[0019] Optionally, the welding method further comprises a preheating step before the sputtering step, in which an electrode provides a preheating current to an area to be welded, and a tempering step after the welding step, in which an electrode provides a tempering current to the welded area, wherein a sputtering current intensity I1=K1*I0, a welding current intensity I2=K2*I0, a preheating current intensity I4=K4*I0, and a tempering current intensity I3=K3*I0, K1 having a range of possible values ​​of 0.8-3.5, K2 having a range of possible values ​​of 0.5-2.5, K4 having a range of possible values ​​of 0.2-1.3, and K3 having a range of possible values ​​of 0.4-1.8, and K1≧K2≧K3≧K4.

[0020] Furthermore, the welding current, the preheating current and the tempering current each have at least one electric pulse, and the application time is 800 ms or less, preferably 200 to 700 ms.

[0021] Furthermore, there is an interval of 0 to 200 ms, preferably 5 to 80 ms, between the welding current or the preheating current and the sputtering current, and between the tempering current and the welding current.

[0022] Optionally, a plating layer is present on at least one surface of the first type metal sheet, and the plating layer is a zinc-based plating layer or an aluminum-based plating layer.

[0023] Optionally, the structural form of the laminated structure is a three-layer group or a five-layer group, in which two outer layer groups of the three-layer group are single layers or adjacent overlapping layers of a first class metal plate, while an inner layer group is a single layer or adjacent overlapping layers of a second class metal plate, and the two outer layer groups and an intermediate layer group of the five-layer group are single layers or adjacent overlapping layers of a first class metal plate, and another two layer groups are single layers or adjacent overlapping layers of a second class metal plate, located between the outer layer groups and the intermediate layer group, respectively, and in the welding step, the adjacent first class metal plates are welded by direct contact with each other under electrode pressure.

[0024] Furthermore, at least two layers of the first type metal plates in the laminated structure are formed by bending the same metal plate, and the bending position is outside the welding area.

[0025] Optionally, the second type metal plate is any one of aluminum, aluminum alloy, magnesium, and magnesium alloy, or a combination of at least two layers of the aluminum, aluminum alloy, magnesium, and magnesium alloy.

[0026] Optionally, the first class metal plate has a tensile strength of 2500 MPa or less, a micro Vickers hardness of 650 Hv or less, and a single layer thickness range of 0.5 mm to 2.5 mm.

[0027] Optionally, the thickness of the single layer or adjacently overlapped second class metal plates between adjacently spaced first class metal plates is ≦4.5 mm, and the total thickness of the single layer or adjacently overlapped first class metal plates is ≦5.5 mm.

[0028] Optionally, the single layer or adjacent overlapping layers of the first class metal plate satisfy the condition that the product A of the plate thickness (unit: mm) and tensile strength (unit: MPa) satisfies 100≦A≦5000.

[0029] Optionally, one of the two outer plates of the laminate structure has a smaller value of the product of plate thickness (in mm) and tensile strength (in MPa) than the other plate.

[0030] According to another aspect of the embodiment of the present invention, a dissimilar metal joint is provided, the dissimilar metal joint having a laminated structure and including a first class metal plate and a second class metal plate, the first class metal plate being pure iron or an iron-based alloy, and the second class metal plate being a metal having a density of 5.0 g / cm 3 or a melting point of less than 800°C, the outer plate of the laminated structure is a class 1 metal plate, and the class 2 metal plate is located between the class 1 metal plates. Here, from the appearance of the dissimilar metal joint, the thickness of the indentation region of the electrode end surface of the dissimilar metal joint is less than the sum of the thicknesses of the class 1 metal plates, the thickness of the joint structure gradually increases from the edge of the indentation region of the electrode end surface to the outside, and finally presents the original stack structure of the combination, and from the cross section of the dissimilar metal joint, the indentation region of the electrode end surface and its surrounding material are characterized by being thin in the middle and thick on both sides, the intermediate indentation region of the indentation region of the electrode end surface is composed only of the class 1 metal plate, and between the class 1 metal plates, interatomic bonds are generated at the interface to form a permanent joint, the thickness of the stack structure gradually increases from the edge of the indentation region to the outside, and the second class metal plate gradually increases from a small thickness to the original thickness of the second class metal plate between the class 1 metal plates.

[0031] Optionally, a "jet-like" solidification structure is present between the first type metal plates outside the indentation area due to molten sputtering of the second type metal plates.

[0032] Optionally, an intermetallic compound (IMC layer) is generated at the contact interface between the second type metal plate and the first type metal plate in an indentation edge region of the electrode end surface.

[0033] Furthermore, at least two layers of the first type metal plate in the laminated structure are formed by bending the same metal plate, and the bending is located outside the welding area.

[0034] According to yet another aspect of the embodiment of the present invention, there is provided a dissimilar metal joint obtained by the resistance welding method of any of the above embodiments. Effect of the Invention

[0035] The beneficial effects of the embodiments of the present invention are as follows:

[0036] (1) The sputtering feature of the method of the present invention realizes effective discharge of light metal in stack structure, and avoids the adverse effect of light metal on joint bonding. In the general knowledge in this field, sputtering in the resistance welding spot welding process is a defect to be avoided, but in the present invention, the sputtering phenomenon is utilized. By applying a sputtering current to the welding area, the second class metal located in the intermediate layer is rapidly melted, and the molten liquid metal instantly breaks through the plastic deformation area around the liquid area under the joint action of the electrode pressure and the current heating, and leaves the welding area in the form of sputtering, so that only a small amount of the second class metal plate exists in the welding area, and even the second class metal plate does not exist, thereby realizing the close contact between the first class metal, avoiding the generation of a large amount of brittle intermetallic compound (IMC layer) in the welding interface in the subsequent welding stage, and effectively improving the quality of the welding. The method of the present invention is simple, highly efficient, has a wide range of application, and has high joint quality.

[0037] (2) The sputtering step of the present invention can be performed with multiple pulses, which can achieve the effect of heating and discharging the light metal multiple times, thereby realizing the maximum discharge of the light metal in the stack structure, and thereby fulfilling the bonding of the stack structure containing multiple layers of light metal.

[0038] (3) The method of the present invention can realize high-quality joining of light metals and steel plates with a stack structure with multiple layers spaced apart, and is not limited by the type, composition and processing method of the light metal and the strength of the steel plate, and can realize joining including, for example, magnesium alloys, aluminum alloy cold-rolled plates, aluminum alloy profiles, aluminum castings, and cases where ultra-high strength hot-formed steel is present in between.

[0039] (4) Compared with the conventional direct resistance spot welding method of steel and aluminum, the method of the present invention can avoid direct contact between the electrode and the light metal, thereby greatly improving the service life of the electrode and the joining quality of the joint.

[0040] (5) Compared with the same kind of conventional technology, the method of the present invention does not require specialized manufacturing of steel metal parts with locking features, does not require piercing light metal or steel members, and has a very wide application market. [Brief description of the drawings]

[0041] [Figure 1] FIG. 2 is a schematic diagram of a laminated structure of an embodiment of a dissimilar metal joint. [Figure 2a] FIG. 13 is a schematic diagram of a laminated structure of another embodiment of a dissimilar metal joint. [Figure 2b] FIG. 11 is a schematic diagram of a laminated structure of yet another embodiment of a dissimilar metal joint. [Diagram 3] FIG. 11 is a schematic diagram of a laminated structure of yet another embodiment of a dissimilar metal joint. [Figure 4] FIG. 2 is a schematic diagram of current, electrode pressure and time in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 5a] 1A-1D are schematic diagrams illustrating the evolution of a weld joint at different welding stages in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 5b] 1A-1D are schematic diagrams illustrating the evolution of a weld joint at different welding stages in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 5c] 1A-1D are schematic diagrams illustrating the evolution of a weld joint at different welding stages in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 5d]1A-1D are schematic diagrams illustrating the evolution of a weld joint at different welding stages in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 5e] 1A-1D are schematic diagrams illustrating the evolution of a weld joint at different welding stages in an embodiment of a method for resistance welding of dissimilar metal joints. [Figure 6] FIG. 1 is a schematic diagram showing the structure of a welded joint of one embodiment of a dissimilar metal joint. [Figure 7] FIG. 11 is a structural schematic diagram of a welded joint of another embodiment of a dissimilar metal joint. [Figure 8a] 1A to 1C are structural schematic diagrams of welded joints of two other different embodiments of dissimilar metal joints. [Figure 8b] 1A to 1C are structural schematic diagrams of welded joints of two other different embodiments of dissimilar metal joints. [Figure 9] FIG. 2 is a diagram showing a peeling fracture surface structure of a welded joint in Example 1 of a resistance welding method for a dissimilar metal joint. [Figure 10] FIG. 4 is a cross-sectional metallographic diagram of a welded joint in Example 2 of a resistance welding method for a dissimilar metal joint. [Figure 11] FIG. 11 is a tensile shear load-displacement curve diagram of a welded joint in Example 2 of the resistance welding method for dissimilar metal joints. [Figure 12] FIG. 11 is a cross-sectional metallographic diagram of a welded joint in Example 4 of the resistance welding method for dissimilar metal joints. [Figure 13] FIG. 11 is a tensile shear load-displacement curve diagram of a welded joint in Example 4 of the resistance welding method for dissimilar metal joints. [Figure 14] FIG. 11 is a cross-sectional metallographic diagram of a welded joint in a fifth embodiment of a resistance welding method for a dissimilar metal joint. [Figure 15] FIG. 11 is a tensile shear load-displacement curve diagram of a welded joint in Example 5 of the resistance welding method for a dissimilar metal joint. [Figure 16] FIG. 11 is a cross-sectional metallographic diagram of a welded joint according to a seventh embodiment of the resistance welding method for a dissimilar metal joint. [Figure 17] FIG. 13 is a tensile shear load-displacement curve diagram of a welded joint in Example 7 of the resistance welding method for dissimilar metal joints. [Figure 18] FIG. 11 is a cross-sectional metallographic diagram of a welded joint according to an eighth embodiment of the resistance welding method for a dissimilar metal joint. [Figure 19]FIG. 13 is a tensile shear load-displacement curve diagram of a welded joint in Example 8 of the resistance welding method for a dissimilar metal joint. [Figure 20] FIG. 2 is a cross-sectional metallographic diagram of a welded joint according to an embodiment of a method for resistance welding a dissimilar metal joint. [Figure 21] FIG. 16 is a cross-sectional metallographic diagram of a welded joint according to a tenth embodiment of the resistance welding method for a dissimilar metal joint. [Figure 22] FIG. 15 is a cross-sectional metallographic diagram of a welded joint in Example 11 of the resistance welding method for dissimilar metal joints. [Figure 23] FIG. 12 is a cross-sectional metallographic diagram of a welded joint in Example 12 of the resistance welding method for dissimilar metal joints. [Figure 24] FIG. 2 is a cross-sectional metallographic diagram of a welded joint according to a comparative example of a resistance welding method for a dissimilar metal joint. [Diagram 25] FIG. 1 is a tensile shear load-displacement curve diagram of a welded joint in a comparative example of a resistance welding method for a dissimilar metal joint. [Figure 26] FIG. 1 is a schematic diagram of each region of a dissimilar metal joint. The purpose of the above drawings is to explain the technical idea of ​​the present invention so as to facilitate the understanding of those skilled in the art, and the drawings only include parts related to the technical features of the present invention, and do not show the whole and all details of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] Hereinafter, the embodiments of the present invention will be described in more detail with reference to the drawings using specific examples.

[0043] The present invention will be further described below with reference to specific examples. It should be understood that these examples are merely for the purpose of illustrating the present invention, and do not limit the scope of the present invention. In addition, the drawings are schematic, and therefore the relevant dimensions of the method and joint of the present invention are not limited to the dimensions or proportions of the schematic. In addition, in the claims and specification of this patent, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or suggest that any such actual relationship or sequence exists between these entities or operations. In addition, the terms "comprise", "include", or any other variation are intended to include a non-exclusive inclusion, whereby a process, method, article, or device that includes a set of elements not only includes those elements, but also includes other elements not expressly listed, or includes elements inherent to such process, method, article, or device. The terms "upper", "lower", "outer", "inner", and the like are only used to relatively describe the relative positional relationship, and do not have any specific inner or outer limitations. Absent more limitations, an element qualified by the phrase "comprising a" does not exclude the presence of other identical elements in the process, method, article, or device that includes the element.

[0044] The dissimilar metal joint has a laminated structure as shown in Figure 1, and the laminated structure includes first class metal plates 3, 5 and a second class metal plate 4. The first class metal plates 3, 5 may be referred to as the upper plate 3 and the lower plate 5, respectively, and the second class metal plate 4 may be referred to as the inner plate 4. The upper plate 3 is made of the first class metal, the inner plate 4 is made of the second class metal, and the lower plate 5 is made of the first class metal. Regarding the upper plate 3 and the lower plate 5, the first-class metal from which the plate material is manufactured is pure iron or an iron-based alloy, and the specific plate material can be selected from a number of points, for example, in terms of mechanical properties, its tensile strength is 2500 MPa or less, its micro Vickers hardness is 650 Hv or less, and in terms of dimensions, the thickness of the single layer is in the range of 0.5 mm to 2.5 mm, or the value A of the product of the plate thickness (unit: mm) and the tensile strength (unit: MPa) is between 100 and 5000. In consideration of these points, in a preferred embodiment, the A values ​​of the upper plate 3 and the lower plate 5 are not equal. Either surface of any of the first-class metal plates may be a bare plate, or may have an aluminum-based or zinc-based plating layer, such as a zinc plating layer, an aluminum silicon plating layer, a zinc aluminum plating layer, or a zinc nickel plating layer, or a lead tin plating layer. Regarding the inner plate 4, the second-class metal from which the plate material is manufactured is a metal having a density of 5 g / cm 3 The specific plate material can be selected from a number of viewpoints. For example, in terms of components, any one of aluminum, aluminum alloys, magnesium, and magnesium alloys, or a combination of at least two layers, may be selected. In terms of dimensions, the thickness shall be 4 mm or less.

[0045] The upper plate 3, the inner plate 4 and the lower plate 5 are single-layer plate structures, and in other embodiments, they may be composite structures in which multiple layer plates are adjacently stacked, and such composite structures in which multiple layer plates are adjacently stacked may be made of different plate materials that each meet the above-mentioned limiting conditions. In order to help improve the quality of the welding, regardless of the form of the stacked structure, it is preferable that the total thickness of the first class metal plate is 5 mm or less, and the total thickness of the second class metal plate is 4 mm or less.

[0046] The upper plate 3, the inner plate 4 and the lower plate 5 of the dissimilar metal joint can be installed as a multi-layer structure. In the dissimilar metal joint (before welding) shown in FIG. 2a, the upper plate 3 has a three-layer structure, and the lower plate 5 has a two-layer structure. In the dissimilar metal joint (before welding) shown in FIG. 2b, the inner plate 4 has a two-layer structure. Here, the multi-layer structures of the upper plate 3, the inner plate 4 and the lower plate 5 may be made of the same type of material, or may be a combination of multiple different types of materials that satisfy the parameter restrictions in the above-mentioned embodiment. For example, the multi-layer structures of the upper plate 3 and the lower plate 5 may be any combination of laminations of low carbon steel and pure iron, and the multi-layer structure of the inner plate 4 may be any combination of laminations of one or at least two of aluminum, aluminum alloy, magnesium, and magnesium alloy.

[0047] As shown in Fig. 3, another type of dissimilar metal joint may be a five-layer composite structure consisting of an upper plate 3 and a lower plate 5 made of a first-class metal, an inner plate 4 made of a second-class metal, and an inner plate 13 made of a first-class metal, in which each layer may be a single plate or a composite structure in which multiple layers of plates are adjacently stacked. For such a structure, in the welding step, the adjacent and spaced first-class metal plates, i.e., the upper plate 3 and the inner plate 13, and the inner plate 13 and the lower plate 5, are welded in contact with each other.

[0048] Hereinafter, the welding process of the embodiment of the resistance welding method for dissimilar metal joints will be described by taking the three-layer laminated structure provided in FIG. 1 as an example. In the resistance welding process, the upper electrode 1 and the lower electrode 2 apply current and electrode pressure to the laminated structure. In FIG. 5, the horizontal axis is time (ms), and the vertical axis is electrode pressure (N) or current (kA), where the dashed line indicates the change in pressure over time, and the solid line indicates the change in current over time. The resistance welding process includes a preheating stage from t1 to t2, a sputtering stage from t3 to t4, a welding stage from t5 to t6, and a tempering stage from t6 to t7. In each stage, the upper electrode 1 and the lower electrode 2 apply corresponding preheating current I4, sputtering current I1, welding current I2, and tempering current I3 to the laminated structure, respectively. The electrode pressure changes stepwise with time in FIG. 4. In the sputtering step, a sputtering current and an electrode pressure are applied to the stack structure to heat the stack structure in the welding area, the second class metal melts and leaves the welding area in the form of sputtering under the action of pressure, and the first class metal approaches each other under the action of resistance heat and pressure, whereby the second class metal plates are completely scattered in at least a part of the welding area. In the welding step, a welding interface is formed in which only the first class metal plates are in contact in at least a part of the welding area, and a metallurgical bond is generated at the welding interface. In another embodiment, the electrode pressure shown in Table 1 can be kept unchanged throughout the entire welding process.

[0049] Here, the sputtering current and the electrode pressure are applied by a welding electrode, and the welding electrode has an electrode end surface. In the sputtering process, the completely scattered second-class metal plate includes a situation where a trace amount of the second-class metal remains at the weld interface formed by contacting the first-class metal plate, and the trace amount of the second-class metal remains mixed with the plating layer or base element on the surface of the first-class metal, so that when the cross section of the welded point is observed with the naked eye, only a stack structure made of the first-class metal is seen, and in the subsequent process of continuing welding, the trace amount of the second-class metal remains completely fuses and enters the weld nugget formed by the first-class metal plate, and does not affect the quality of the weld, that is, the trace amount of the second-class metal plate remains cannot form a brittle intermetallic compound with the first-class metal plate, and does not affect the performance of the weld nugget.

[0050] The mixture of the first class metal and the second class metal elements at the weld interface and the situation where the original contact surface is fused and disappears due to the joining of only the first class metal are the occurrence of metallurgical bonding. Metallurgical bonding includes diffusion bonding and weld nugget bonding in the examples described below.

[0051] First, the reference current intensity I0 is defined. I0 is the current intensity when single-pulse resistance welding is performed individually on the upper sheet 3 and the lower sheet 5 to form a weld nugget with a cross-sectional diameter ≧4√t, where t is the thickness of the thinner sheet.

[0052] An optional pre-pressure step is applied before the electrodes apply current to the laminate structure, which brings the stacked workpieces into intimate contact and reduces the resistance between the sheets. The pre-pressure pressure is as shown in FIG. 5 and can be lower than the electrode pressure in the sputtering and welding stages described below.

[0053] In the preheating stage, as shown in FIG. 5a, the electrode applies a preheating current to the laminated structure to make the contact of the stacked workpieces closer and reduce the resistance between the plates. The preheating current has at least one electric pulse, and the duration is generally less than 800 ms, preferably 200-700 ms. The preheating current is preferably such that no sputtering occurs, and the preheating current intensity I4 numerically satisfies I4=K4*I0, and the range of possible values ​​of K4 is 0.2-1.3. In some embodiments, the preheating stage can be omitted and still complete welding on the laminated structure.

[0054] In the sputtering stage, as shown in Figures 5b and 5c, the electrodes apply a sputtering current to the laminated structure, and under the action of the sputtering current, the inner plate 4 material in the welding area is melted into liquid metal 6, some of which forms spatters 7 and leaves the welding area, forming an area where the second metal does not exist between the first metal plates 3 and 5. The first metal plates 3 and 5 are softened by heat under the action of the current, and are brought close to each other in the middle by the pressure of the upper electrode 1 and the lower electrode 2, and contact each other in the area where the second metal does not exist to form a welding interface 8. The second metal 4 is pressed and deformed, and the thickness of the second metal left at the welding interface 8 is generally ≦0.15 mm, and in a preferred state, the thickness is ≦0.05 mm, and the equivalent diameter of the welding interface 8 is usually more than 0.5 times the end face diameter of the upper electrode 1 or the lower electrode 2. The sputtering current intensity I1 numerically satisfies I1=K1*I0, and the range of possible values ​​for K1 is 0.8 to 3.5. The sputtering current may be a single pulse or multiple pulses, the number of pulses is preferably 2 to 5, and the duration of a single pulse is 200 ms or less, preferably 50 ms to 120 ms.

[0055] In the welding stage, the electrode applies a welding current to the laminated structure, as shown in FIG. 5d. The strength of the welding current is smaller than that in the sputtering stage, but the electrode pressure is larger than that in the sputtering stage. The welding current may be single-pulsed or multi-pulsed, and the application time is generally less than 800 ms, preferably 200-700 ms. The welding current strength I2 numerically satisfies I2=K2*I0, and the range of possible values ​​of K2 is 0.5-2.5. The first-class metal sheets 3, 5 continue to be heated under the action of the welding current, and the metal at the contact surface 8 melts to form a steel weld nugget 9 with a diameter reaching 3.5√t, and further realize a metallurgical bond between the first-class metal sheets 3, 5. A small amount of intermetallic compound (IMC layer) is formed at the interface where a part of the liquid metal left around the weld interface of the inner sheet 4 contacts the nearby steel. In order to bring the upper sheet 3 and the lower sheet 5 into sufficient contact after sputtering has occurred, an interval of 0 to 200 ms can be set between the sputtering current and the welding current, and is preferably 10 to 70 ms.

[0056] In the tempering stage, as shown in FIG. 5e, the electrode applies a tempering current to the laminated structure to perform a heat-keeping and tempering process on the weld interface, obtain a uniform weld structure, and remove residual stress. The tempering current has at least one electric pulse, and the application time is generally less than 800 ms, preferably 200-700 ms. The tempering current does not preferentially cause sputtering, and the tempering current intensity I3 numerically satisfies I3=K3*I0, and the range of possible values ​​of K3 is 0.4-1.8. In some embodiments, the tempering stage can be omitted and still complete welding on the laminated structure, and the tempering current I3 is generally less than 15 kA, preferably 4-12 kA.

[0057] In the above process, K1, K2, K3, and K4 should satisfy K1≧K2≧K3≧K4.

[0058] The current is provided by the welding electrode, and the specific value may be an effective current, a peak current, or an average current, which is easily understood in the art. The welding electrode functions as a part of a resistance welding device. The resistance spot welding device can be realized by a commercial frequency welding machine, a medium frequency welding machine, or an AC welding machine, which are widely applied in industry. Here, the resistance spot welding device may be a stationary spot welding device, or a robot-driven automated device, which generally includes a welding clamp with a C-shape, an X-shape, and other types of structural shapes, and is usually realized by a robot or an automated member. The welding electrode may be made of any material having electrical and thermal conductivity, for example, a copper alloy, such as a copper alloy including a copper chromium (CuCr) alloy, a copper chromium zirconium (CuCrZr) alloy, a copper alloy with aluminum oxide particles, or other various copper alloys that can be used as an electrode material, and its welding surface may be a spherical surface, a cross section, and other special shape surfaces, for example, an electrode cap having an end surface with a protruding structure or a concave structure on the surface.

[0059] According to the specific circumstances of different embodiments, the time interval between the preheating current and the sputtering current, between the sputtering current and the welding current, and between the welding current and the tempering current can be set, and the setting range of the interval is 0-200 ms, preferably 5-80 ms. During the interval period, the welding electrode maintains a pressure holding state.

[0060] In some other embodiments, for example, when the upper and lower plates 3 and 5 are made of thick hot-formed steel and the inner plate 4 is made of a very thin aluminum plate, the sputtering stage in the resistance welding process is very short, and the aluminum material constituting the inner plate 4 can be quickly removed from the weld interface in a short time, and the sputtering current I1 and the welding current I2 can be kept equal. Also, the duration of the welding stage is short, and the upper and lower plates 3 and 5 made of hot-formed steel are fixed in the form of diffusion welding without melting in the weld area. In such embodiments, no weld nugget is generated in the joint structure.

[0061] The above-mentioned resistance welding method is not limited to the three-layer stacked structure, but can also be applied to the stacked structures shown in Figures 2a, 2b and 3, where I0 is the current intensity when single-pulse resistance welding is performed individually on the first class metal plates to form a weld nugget cross-sectional diameter ≧4√t, t is the thickness of the thinner plate among the first class metal plates, taking Figure 2a as an example, where t is the thickness of the thinner plate among the three-layer plate in upper plate 3 and the two-layer plate in lower plate 5, and taking Figure 3 as an example, where t is the thickness of the thinner plate among the upper plate 3, the inner plate 13 and the lower plate 5.

[0062] According to the above embodiment, a dissimilar metal joint provided in another aspect of the embodiment of the present invention can be obtained. A typical joint structure is as shown in Fig. 6, in which the dissimilar metal joint has a laminated structure and includes a first class metal plate and a second class metal plate, among which the first class metal plate is pure iron or an iron-based alloy and includes an upper plate 3 and a lower plate 5, and the second class metal plate has a density of 5.0 g / cm 3 It is a single body or alloy with a melting point of less than 800°C or less, including an inner plate 4. From the appearance, the thickness between the indentation areas 10, 11 of the electrode end surface of the dissimilar metal joint is less than the sum of the thicknesses of the first class metal plates 3, 5, and the thickness of the joint structure gradually increases from the edge of the indentation areas 10 and 11 of the electrode end surface to the outside, and finally presents the stack structure of the original combination. From the cross-section of the dissimilar metal joint, the indentation areas 10, 11 of the electrode end surface and the surrounding material are characterized by being thin in the middle and thick on both sides, the middle indentation area of ​​the indentation area of ​​the electrode end surface is only composed of the first class metal plate, and the first class metal plate forms a permanent joint by interatomic bonding at the interface, which may be a solidified weld nugget 9, or may be a metal interface where solid diffusion bonding occurs. The thickness of the laminated structure gradually increases from the edge of the indentation outward, the outer first class metal plate presents a V-shape, and the second class metal plate gradually increases from a small thickness to the original thickness of the second class metal plate between the V-shaped structure formed by the first class metal plate. The second class metal plate deformed in the sputtering process meets the characteristic that the equivalent diameter of the area with a thickness ≦ 0.15 mm within the indentation regions 10 and 11 on the electrode end surface in the joint structure is usually 0.5 times or more the end surface diameter of the upper electrode 1 or the lower electrode 2.

[0063] Typically, between the inner plate 4 and the upper plate 3 or lower plate 5, there exists a jet-like solidified structure formed when the inner plate 4, which is a second-class metal plate, melts during the sputtering process and the sputtering 7 solidifies.

[0064] As shown in Figure 6, in the indentation edge region of the electrode end surface, the surface of the region where the inner plate 4 made of the second class metal plate contacts with the upper plate 3 and the lower plate 5 made of the first class metal plate melts, forming an intermetallic compound (IMC layer) 12. Outside the intermetallic compound 12, the pressed and deformed second class metal plate has an equivalent diameter of the second class metal plate region (including the weld nugget) with a thickness of ≦0.15 mm that is generally 0.5 times or more the end face diameter of the upper electrode 1 or the lower electrode 2. In some embodiments, the IMC layer may be formed by diffusion between the second class metal plate and the first class metal plate.

[0065] In other embodiments, the upper plate 3, inner plate 4, and lower plate 5 in the joint of dissimilar metals may all be single-layered or multi-layered, and may have a three-layer structure as shown in Figure 6, or may have a five-layer structure as shown in Figure 7 by adding an intermediate layer 13 made of a class 1 metal between the inner plate 4 made of multiple layers of class 2 metal plates.

[0066] As shown in Figures 8a and 8b, another type of dissimilar metal joint may be one in which one folded first class metal plate constitutes at least two layers of the stack structure, and the folded portion 14 is located outside the welding area. Such a stack structure may be a three-layer structure as shown in Figure 8a, in which the outer side of the stack structure is made of a first class metal plate 5 with a folded portion 14, and an inner plate 4 made of a second class metal plate is fitted into the folded overlap area, or a five-layer structure as shown in Figure 8b, in which the stack structure includes an upper plate 3 and a lower plate 5 made of a first class metal, of which the lower plate 5 has a folded portion 14, and two inner plates 4 made of a second class metal are inserted between the upper plate 3 and the lower plate 5 and into the space formed by the folded structure of the lower plate 5, respectively.

[0067] In order to more easily understand each region in the above-mentioned welded joint, refer to Figure 26, the welded joint a is a structure including a first class metal plate and a second class metal plate and forms a spot joint, the welded region b includes a region where the welding electrode welds the stack structure and realizes the joint by the effect of resistance heat, the indentation region c of the electrode end surface is a pressure-receiving region formed by the end surface of the welding electrode directly contacting and pressuring the dissimilar metal joint during the welding process, the welded interface region d is a region formed by only the first class metal plates contacting each other after the second class metal is separated, and the welded joint further includes a light metal thinning region e, which is a region where the thickness of the second class metal plate gradually becomes thinner from the original thickness thereof in the vicinity of the welded interface region. Hereinafter, an embodiment of the resistance welding method for dissimilar metal joints will be described with reference to an example.

[0068] Example 1 The upper plate 3 is made of CR210 cold rolled steel with a thickness of 0.8 mm and a tensile strength of less than 400 MPa, the inner plate 4 is made of AA6016 aluminum alloy with a thickness of 0.8 mm, and the lower plate 5 is made of CR420 cold rolled steel with a thickness of 1.0 mm and a tensile strength of less than 600 MPa. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are as shown in Table 1. After welding was completed, the peeling fracture surface was as shown in Figure 9, and solidified light metal spatter 7 was present at the interface between the inner plate 4 and the lower plate 5, circling the weld point and distributing radially toward the outer periphery. The results of the tensile shear load test of the joint after welding were as shown in Table 2. Since a strong steel-to-steel weld nugget was formed between the first class metal plates 3, 5 and the second class metal plate 4, the tensile shear load test showed that the joint had an extremely high tensile shear strength of about 3775N.

[0069] Example 2 The upper plate 3 is made of CR210 cold rolled steel with a thickness of 1.0 mm and a tensile strength of less than 400 MPa, and the inner plate 4 is made of AA5754 aluminum alloy with a thickness of 1.2 mm. Unlike the material selected in Example 1, the inner plate 4 is a 5 series aluminum alloy, and the lower plate 5 is made of CR420 cold rolled steel with a thickness of 1.0 mm and a tensile strength of less than 600 MPa. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are as shown in Table 1, and the cross-sectional metallography of the joint is as shown in Figure 10. After the welding is completed, the joint is subjected to a tensile shear load test, and the tensile shear load-displacement curve is as shown in Figure 11. According to the tensile shear load test, the joint has an extremely high tensile shear strength of about 7292.4 N in the shear tension process at the significant plastic deformation stage. The results of the tensile shear peak load test are shown in Table 2.

[0070] Example 3 A Q&P980 cold rolled steel having a thickness of 1.0 mm and a tensile strength of generally more than 1000 MPa is selected as the upper plate 3, an AA5754 aluminum alloy having a thickness of 1.5 mm is selected as the inner plate 4, and a Q&P1180 cold rolled high strength steel having a thickness of 1.2 mm and a tensile strength of generally more than 1200 MPa is selected as the lower plate 5. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are as shown in Table 1. After the welding is completed, a tensile shear load test is performed on the joint. The test shows that the joint also has an extremely high tensile shear strength of about 7557.6 N. The tensile shear peak load test result is shown in Table 2.

[0071] Example 4 The upper plate 3 is made of CR420 cold rolled steel with a thickness of 1.0 mm and a tensile strength of 600 MPa or less, the inner plate 4 is made of AA6016 aluminum alloy with a thickness of 1.6 mm, and the lower plate 5 is made of Q&P1180 cold rolled high strength steel with a thickness of 1.2 mm and a tensile strength of generally 1200 MPa or more. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are as shown in Table 1, and the cross-sectional metallography of the joint is as shown in Figure 12. After the welding is completed, the joint is subjected to a tensile shear load test, and the tensile shear load-displacement curve is as shown in Figure 13. The tensile shear load test shows that the joint has obvious plastic deformation and has an extremely high strength of about 8995.0 N, and the peak load test result of the tensile shear is shown in Table 2.

[0072] Example 5 The upper plate 3 is made of CR420 cold rolled steel with a thickness of 1.0 mm and a tensile strength of 600 MPa or less, the inner plate 4 is made of AA6016 aluminum alloy with a thickness of 2.0 mm, and the lower plate 5 is made of Q&P1180 cold rolled high strength steel with a thickness of 1.2 mm and a tensile strength of generally 1200 MPa or more. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are shown in Table 1, and the metallography of the joint cross section is shown in Figure 14. After the welding is completed, the joint is subjected to a tensile shear load test, and the tensile shear load-displacement curve is shown in Figure 15. The tensile shear load test shows that the joint has an extremely high tensile shear strength of about 9508.4 N, and the peak load test result of the tensile shear is shown in Table 2.

[0073] Example 6 The upper plate 3 is made of 1.0mm thick Q&P980 cold rolled high strength steel, which generally has a tensile strength of 1000MPa or more, the inner plate 4 is made of 2.0mm thick AA6061 aluminum alloy, and the lower plate 5 is made of 1.4mm thick CR420 cold rolled steel, which has a tensile strength of 600MPa or less, and the surface of the lower plate 5 is coated with zinc. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6mm. The specific welding process parameters are shown in Table 1. After the welding is completed, the joint is subjected to a tensile shear load test. The test results show that the joint has a very high tensile shear strength of about 10437.8N. The tensile shear peak load test results are shown in Table 2.

[0074] Example 7 The upper plate 3 is made of CR420 steel having a thickness of 1.0 mm and a tensile strength of 600 MPa or less, the inner plate 4 is made of AZ31 magnesium alloy having a thickness of 2.0 mm, and the lower plate 5 is made of hot-formed ultra-high strength steel having a thickness of 1.2 mm and a tensile strength of generally 1300 MPa or more. The first welding electrode 1 and the second welding electrode 2 are both ordinary spherical electrodes, and the welding end surface of the electrode is 6 mm. The specific welding process parameters are shown in Table 1. The joint cross-sectional metallography is shown in Figure 16. After the welding is completed, the joint is subjected to a tensile shear load test, and the tensile shear load-displacement curve is shown in Figure 17. The tensile shear load test shows that the joint has an extremely high tensile shear strength of about 6970.0 N, and the tensile shear peak load test results are shown in Table 2.

[0075] Example 8 A Q&P980 steel with a thickness of 1.0 mm and a tensile strength generally above 1000 MPa is selected as the upper plate 3, a 6061 aluminum alloy profile with a thickness of 2.4 mm is selected as the inner plate 4, and a hot-formed ultra-high strength steel with a thickness of 1.4 mm is selected as the lower plate 5. The specific welding process parameters are shown in Table 1, and the joint cross-sectional metallography is shown in Figure 18. After welding is completed, a tensile shear load test is carried out on the joint, and the tensile shear load-displacement curve is shown in Figure 19. The tensile shear load test shows that the joint has an extremely high tensile shear strength of about 9883.4 N, and the peak load result of the tensile shear test is shown in Table 2.

[0076] Example 9 A 1.0 mm thick Q&P980 steel was used as the upper plate 3, a 1.6 mm thick AA6061 aluminum alloy was used as the inner plate 4, and a combination of a 1.2 mm thick hot-formed steel with a tensile strength of 2000 MPa and a 1.2 mm thick Q&P1180 hardened steel with a tensile strength of 1180 MPa was selected as the lower plate 5, of which the hot-formed steel was used as the upper layer of the lower plate 5, and the Q&P1180 steel was used as the lower layer of the lower plate 5. The welding was performed by using three 16 kA pulses as the sputtering current I1, each pulse lasting 80 ms and spaced 20 ms apart, cooling for 30 ms after the sputtering current, applying a 13 kA welding current I2, and welding lasting for 300 ms. The metallographic diagram of the resulting joint is shown in FIG. 20. In this embodiment, I0 was 8.2 kA (welding time 280 ms). The weld nugget structure 9 consisted entirely of steel and contained no bright intermetallic compounds.

[0077] Example 10 DP780 steel with a thickness of 1.0 mm was used as the upper plate 3, AZ31 magnesium alloy with a thickness of 2.0 mm was used as the inner plate 4, and a combination of hot-formed steel with a thickness of 1.4 mm and a tensile strength of 2000 MPa and Q&P1180 hardened steel with a thickness of 1.2 mm and a tensile strength of 1180 MPa was selected as the lower plate 5, of which the hot-formed steel was used as the upper layer part of the upper plate 5, and the Q&P1180 steel was used as the lower layer part of the lower plate 5. For welding, three 19 kA pulses were used as the sputtering current I1, each pulse lasting 80 ms and spaced 20 ms apart, and the sputtering current was cooled for 30 ms after the sputtering current, and a 13 kA welding current I2 was applied and welded for 400 ms. The metallographic diagram of the joint obtained is shown in FIG. 21. In this embodiment, I0 was 8.7 kA (welding time 280 ms). The weld nugget structure 9 consisted entirely of steel and contained no bright intermetallic compounds.

[0078] Example 11 A DP780 steel plate with a thickness of 1 mm was used as the upper plate 3, a 5754 aluminum alloy plate with a thickness of 0.8 mm and an AA6061 aluminum alloy plate with a thickness of 1.6 mm were used as the inner plates 4, and a Q&P1180 hardened steel plate with a thickness of 1.2 mm and a tensile strength of 1200 MPa was inserted as the inner plate 13. A DP780 steel plate with a thickness of 1 mm was used as the lower plate 5 to form a five-layer composite structure, of which the 5754 aluminum alloy was positioned above the inner plate 13 and the AA6061 aluminum alloy was positioned below the inner plate 13. A 6kA preheat current I4 was used for 100ms preheating, followed by three 20kA pulses as sputtering current I1, each lasting 85ms and spaced 20ms apart, with 30ms cooling after the sputtering current, and a 15kA welding current I2 was applied and lasted 400ms to perform welding, the joint metallography of which is shown in Figure 22, where in this example I0 was 8.6kA (welding time 300ms). The weld nugget structure 9 consisted entirely of steel and did not contain any bright intermetallic compounds.

[0079] Example 12 DP780 steel with a thickness of 1 mm was selected as the upper plate 3, 5754 aluminum alloy with a thickness of 0.8 mm and AA6061 aluminum alloy with a thickness of 1.6 mm were combined as the inner plate 4, and Q&P1180 hardened steel with a thickness of 1.2 mm and a tensile strength of 1200 MPa was selected as the lower plate 5. A 6 kA preheating current I4 was used to perform preheating for 100 ms, followed by three 21 kA pulses as the sputtering current I1, each pulse lasting 80 ms and spaced 20 ms apart, followed by 30 ms cooling after the sputtering current, and a 15 kA welding current I2 was applied and welded for 380 ms. The metallography of the resulting joint is shown in FIG. 23, where I0 was 8.5 kA (welding time 280 ms) in this example. The weld nugget structure 9 was entirely made of steel and did not contain any bright intermetallic compounds.

[0080] (Comparative Example) For comparison with the embodiment of the present invention, in this embodiment, a conventional resistance spot welding method is used to weld aluminum steel dissimilar metals. During welding, the first welding electrode and the second welding electrode are both spherical, the spherical radius is 100 mm, and the diameter of the welding surface of the spherical electrode is 10 mm. The optimized preferred welding parameters are selected for welding. The welding parameters adopted are welding pressure 5600 N, welding current 17 kA, welding time 100 ms, 5 pulse currents, interval between pulse currents 20 ms, and maintained for 300 ms after welding. The joint metallography is shown in FIG. 24. For welding, 1.2mm thick Q&P1180 steel is selected as the first metal plate 5, and 1.6mm thick AA6016 is selected as the second metal plate 4. After welding, a tensile shear load test is carried out on the joint. The test result is shown in Table 2 and FIG. 25. The joint tensile shear peak load is only 3265.8N, which is much lower than the peak load of the joint of the present invention. As can be seen from the load-displacement curve, the joint displacement is very small, about 0.3mm, and the brittleness is obvious, which is much smaller than the joint provided in the present invention.

[0081] [Table 1]

[0082] [Table 2]

[0083] It should be understood that the above examples, together with the drawings, are intended to allow those skilled in the art to better understand the technical idea of ​​the present invention, and do not specifically limit the embodiments and protection scope of the present invention. Within the scope of the claims of the present invention, modifying or replacing related parts, materials, and method steps, and combining different embodiments when no conflict occurs, all belong to the protection scope of the present invention.

Claims

1. A resistance welding method for a dissimilar metal joint for welding a dissimilar metal laminate structure, the laminate structure including a first class metal plate and a second class metal plate, the first class metal plate being pure iron or an iron-based alloy, and the second class metal plate being a metal having a density of 5 g / cm 3 a metal alloy having a melting point of less than 800° C. or less than 800° C., an outer plate of the laminated structure is a first class metal plate, the second class metal plate is located between the first class metal plates, and the resistance welding method includes a step of removing the second class metal plate from a welding area and a welding step, The step of discharging the second type metal plate includes a sputtering step, In the sputtering step, a sputtering current and an electrode pressure are applied to the stack structure to heat the stack structure in the welding area, the second metal melts and is separated from the welding area in the form of sputtering under the action of pressure, and the first metals approach each other under the action of resistance heat and pressure, whereby the second metal plate is completely scattered in at least a part of the welding area; a welding interface is formed in which only the first type metal plate is in contact with the first type metal plate in at least a portion of the welding area, and a metallurgical bond is generated at the welding interface.

2. 2. The method of resistance welding of dissimilar metal joints according to claim 1, characterized in that the sputtering current comprises one or more, preferably 2 to 5, current pulses, the duration of a single said pulse being less than or equal to 200 ms, preferably between 50 ms and 120 ms.

3. 3. The method for resistance welding a dissimilar metal joint according to claim 1 or 2, characterized in that the sputtering current intensity I1 = K1 * I0, where I0 is the current intensity when resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧ 4√t, t is the thickness of the thinner plate among the first class metal plates, and the range of possible values ​​for K1 is 0.8 to 3.

5.

4. 2. The method of claim 1, wherein in the sputtering step, after the second type metal plate is separated from the welding area by sputtering, only the first type metal plate is in contact with the second type metal plate to form a welded interface, the thickness of the second type metal layer remaining at the welded interface is ≦0.15 mm, preferably ≦0.05 mm, and the equivalent diameter of the welded interface is ≧0.5 times the electrode end diameter of the welding electrode.

5. 2. The method of claim 1, wherein in the welding step, a welding current and an electrode pressure are applied to the laminated structure, and the intensity of the welding current is equal to or less than the intensity of the sputtering current.

6. 2. The method for resistance welding a dissimilar metal joint according to claim 1, wherein I2=K2*I0, I2 is the intensity of a welding current, I0 is the current intensity when single-pulse resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧4√t, t is the thickness of the thinner plate among the first class metal plates, and K2 can range from 0.5 to 2.

5.

7. 2. The method for resistance welding of dissimilar metal joints according to claim 1, wherein an interval between the sputtering current and the welding current is 0 ms to 200 ms.

8. The method of claim 1 further comprising a tempering step after the welding step, wherein an electrode provides a tempering current to the weld area.

9. The method for resistance welding a dissimilar metal joint according to claim 8, characterized in that the tempering current intensity I3 = K3 * I0, where I0 is the current intensity when single-pulse resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧ 4√t, t is the thickness of the thinner plate among the first class metal plates, and the range of possible values ​​for K3 is 0.4 to 1.

8.

10. 2. The method of claim 1, further comprising a preheating step prior to said sputtering step, wherein an electrode provides a preheating current to an area to be welded.

11. 11. The method for resistance welding of a dissimilar metal joint according to claim 10, wherein the preheating current intensity I4 = K4 * I0, where I0 is the current intensity when single-pulse resistance welding is performed individually on the first class metal plates in the dissimilar metal joint to form a weld nugget cross-sectional diameter ≧ 4√t, t is the thickness of the thinner plate among the first class metal plates, and the range of possible values ​​for K4 is 0.2 to 1.

3.

12. The resistance welding method further includes a preheating step before the sputtering step, in which an electrode provides a preheating current to an area to be welded, a welding step after the sputtering step, and a tempering step after the welding step, in which an electrode provides a tempering current to the weld area, a sputtering current intensity I1=K1*I0, a welding current intensity I2=K2*I0, a preheating current intensity I4=K4*I0, and a tempering current intensity I3=K3*I0, where I0 is the current intensity of the dissimilar metal joint.

2. The resistance welding method for dissimilar metal joints according to claim 1, wherein K1 is a current intensity when single-pulse resistance welding is performed individually on the first class metal plates in the welding process to form a weld nugget cross-sectional diameter ≧4√t, t is a thickness of the thinner one of the first class metal plates, K1 has a range of values ​​from 0.8 to 3.5, K2 has a range of values ​​from 0.5 to 2.5, K4 has a range of values ​​from 0.2 to 1.3, and K3 has a range of values ​​from 0.4 to 1.8, and K1 ≧ K2 ≧ K3 ≧ K4.

13. The method for resistance welding of dissimilar metal joints according to claim 12, characterized in that the welding current, the preheating current and the tempering current each have at least one electric pulse, and the application time is less than 800 ms, preferably 200-700 ms.

14. The method for resistance welding of dissimilar metal joints according to claim 12, characterized in that the intervals between the welding current or the preheating current and the sputtering current, and between the tempering current and the welding current are 0 to 200 ms, preferably 5 to 80 ms.

15. 2. The method for resistance welding a dissimilar metal joint according to claim 1, wherein a plating layer is present on at least one surface of the first type metal plate, and the plating layer is a zinc-based plating layer or an aluminum-based plating layer.

16. 2. The method for resistance welding of dissimilar metal joints according to claim 1, characterized in that the structural format of the laminated structure is a three-layer group or a five-layer group, and the two outer layer groups of the three-layer group are single layers or adjacent overlapping layers of the first type metal plate, while the inner layer group is a single layer or adjacent overlapping layers of the second type metal plate, and the two outer layer groups and the intermediate layer group of the five-layer group are single layers or adjacent overlapping layers of the first type metal plate, and the other two layer groups are single layers or adjacent overlapping layers of the second type metal plate, and are located between the outer layer groups and the intermediate layer group, respectively.

17. 17. The method for resistance welding a dissimilar metal joint according to claim 1 or 16, characterized in that at least two layers of the first type metal plate in the laminated structure are formed by bending the same metal plate, and the bending position is outside the welding area.

18. 17. The method for resistance welding a dissimilar metal joint according to claim 1 or 16, characterized in that the second type metal plate is any one of aluminum, an aluminum alloy, magnesium, and a magnesium alloy, or a combination of at least two layers of the second type metal plate.

19. 2. The method for resistance welding of dissimilar metal joints according to claim 1, wherein the thickness of the single layer or adjacently overlapped second class metal plates between the adjacently spaced first class metal plates is ≦4.5 mm, and the total thickness of the single layer or adjacently overlapped first class metal plates is ≦5.5 mm.

20. 2. The method for resistance welding a dissimilar metal joint according to claim 1, wherein one of the two outer plates of the laminate structure has a smaller value of the product of the plate thickness (unit: mm) and the tensile strength (unit: MPa) than the other plate.

21. The laminated structure includes a first metal plate and a second metal plate, the first metal plate being pure iron or an iron-based alloy, and the second metal plate having a density of 5.0 g / cm 3 a metal alloy having a melting point of less than 800° C., an outer plate of the laminated structure is a first class metal plate, and the second class metal plate is located between the first class metal plates, a thickness of the indentation region of the electrode end surface of the dissimilar metal joint not greater than the sum of the thicknesses of the first class metal plates; an intermediate indentation region of the indentation region of the electrode end surface is made only of the first class metal plate; and an interatomic bond is generated at the interface between the first class metal plates to form a permanent bond; the thickness of the stack structure gradually increases from the edge of the indentation region to the outside; and the thickness of the second class metal plate gradually increases from a small thickness between the first class metal plates to the original thickness of the second class metal plate.

22. The dissimilar metal joint according to claim 21, characterized in that a "jet-like" solidification structure caused by molten sputtering of the second type metal plate is present between the first type metal plate and the second type metal plate outside the indentation area.

23. The dissimilar metal joint according to claim 21, characterized in that an intermetallic compound (IMC layer) is generated at the contact interface between the second type metal plate and the first type metal plate in the indentation edge region of the electrode end surface.

24. 24. The dissimilar metal joint according to claim 21, wherein at least two layers of the first type metal plate in the laminated structure are formed by bending the same metal plate, and the bending is located outside the welding area.

25. A dissimilar metal joint, characterized in that it is obtainable by the method according to any one of claims 1 to 22.

Citation Information

Patent Citations

  • Method for joining different kinds of materials

    JP2003236673A

  • Method for joining dissimilar material

    JP2012055962A

  • Apparatus and method for joining dissimilar metals

    JP2016523718A

  • Resistive spot welding method

    WO2015005134A1

  • Dissimilar material joining method of aluminum and steel

    JP1995328774A