Process and method for steel manufacturing

Indirectly heated reactors for direct reduction of iron ore using hydrogen or carbon monoxide/syngas optimize heat transfer and gas consumption, addressing high emissions and energy intensity in steel production, enabling low-emission steel production from low-grade ores.

JP2024541890AInactive Publication Date: 2024-11-13CALIX LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024523903
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-14
Filing Date
2022-10-18
Publication Date
2024-11-13
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The steel industry faces high CO2 emissions and energy intensity due to current processes, necessitating a shift towards low-emission steel production methods that can utilize low-grade ores and reduce hydrogen consumption.

Method used

The use of indirectly heated reactors for direct reduction of iron ore using hydrogen or carbon monoxide/syngas, optimizing reactor design for efficient heat transfer and reducing gas consumption, and integrating these reactors into steelmaking processes to produce low-emission steel.

Benefits of technology

This approach significantly reduces CO2 emissions and energy intensity, enabling the use of low-grade ores and minimizing hydrogen consumption, while allowing for scalable and flexible production of low-emission steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541890000001_ABST
    Figure 2024541890000001_ABST
Patent Text Reader

Abstract

The present invention provides an externally heated vertical reactor for reducing iron ore, comprising: (a) a reactor tube disposed vertically adjacent to a furnace; (b) an external furnace disposed vertically adjacent to at least one wall of the reactor tube and providing heat conducted through the at least one wall; (c) an inlet at the bottom of the reactor tube, where a reducing gas is heated and injected into the inlet such that the reducing gas rises upward through the reactor tube; (d) a gas outlet disposed adjacent to a top surface of the reactor; (e) a gas filter disposed adjacent an inlet of the gas outlet; and (f) a bed disposed at the bottom of the reactor tube, where reduced iron powder product is collected on the bed at the bottom of the reactor tube.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to the production of iron and steel, including the direct reduction of iron in an indirectly heated reactor. [Background technology]

[0002] The steel industry accounts for approximately 6-8% of the world's CO2 emissions, and in order to mitigate global warming, the steel industry is being asked to reduce its CO2 emissions. According to a report by the World Steel Association, in 2019, for 1.1 billion tons of steel production, the CO2 emission intensity was approximately 1,800 kg of CO2 per ton of steel, and the energy intensity was approximately 19.84 GJ / ton. Since 2010, the CO2 emission intensity increased from 1,800 to 1,830, and the energy intensity slightly decreased from 20.13 GJ / ton to 19.84 GJ / ton. The steel process generally includes the process of making iron from iron ore and the process of making steel, which may be closely integrated when making steel directly from iron ore.

[0003] Those skilled in the art will appreciate that the prior art relating to steel is vast and deep, and that most of the patents relating to processes used in these industries are the result of repeated improvements to processes adopted more than 30 years ago. Today, the energy intensity of current processes is very high, and this high emission intensity is a result of these process developments that use processed coal for combustion, reduction, electrodes, and incorporation into carbon steel. The prior art is defined not by patents and publications, but by the specific technologies that have been developed over time.

[0004] The three main steelmaking processes are sponge iron, in which the gangue in the iron ore is not removed; pig iron production, in which the gangue is removed by slagging; and smelting reduction.

[0005] The three main steelmaking processes that may use this iron, i.e., scrap iron, are open hearth, basic oxygen furnace (BOF), and electric arc furnace (EAF). Steelmaking follows the processes of casting, hot rolling, and cold rolling. Currently, the BOF and EAF processes dominate the industry. Climate change mitigation requires reducing the emission intensity of steelmaking. The process should not require increasing the overall energy intensity of the entire steelmaking process, including the sequestration cost of captured CO2. The process and reactor disclosed herein are primarily directed to low emission steelmaking.

[0006] Reducing emissions intensity can first be achieved by using low-emission iron to replace iron ore in existing processes. Open hearth and converter (BOF) furnaces typically: Direct Reduced Iron (DRI) It can replace up to 30% of sponge iron. The BOF process uses carbon, usually in the form of coke from metallurgical grade coal, for both the iron ore reduction and heating process, and as the carbon source for carbon steel. The CO2 produced in the steelmaking process is produced during the reduction of iron ore to molten iron. Due to the use of coal, the CO2 produced is present as part of the furnace off-gas, known as Blast Furnace Gas (BFG).

[0007] When converting an existing BOF process to produce low-emission steel, Hydrogen Direct Reduced Iron (H-DRI) Using natural gas as a feedstock typically reduces emissions by about 30%. Replacing coal with natural gas can reduce emissions intensity. Emissions can be reduced to about 600 kg CO2 / tonne. This is not enough to mitigate climate change and reach the goal of achieving zero emissions by 2050.

[0008] Although the replacement of steel scrap by DRI in the EAF process can be up to 100%, replacement is currently limited to DRI produced from high-grade ores because EAFs cannot tolerate large amounts of gangue from low-grade ores. New EAF designs, such as the Submerged Arc Furnace (SAF), are being developed to overcome this limitation. To meet current market needs and reduce emissions, it is desirable to adopt a low-carbon DRI process that uses low-grade ores.

[0009] To produce carbon steel, carbon needs to be added to create enough cementite, Fe3C, for strength. To reduce CO2 emissions from steelmaking, it is also necessary to reduce emissions from cementite production. Another source of CO2 emissions in steelmaking is from the use of lime from limestone and other carbonates such as dolomite, which are often used to optimize the Ca:Mg ratio for slagging. A further source of CO2 emissions is from the transportation of iron ore. There are many sources of CO2 emissions in the steelmaking supply chain. However, the largest contribution to CO2 emissions is from the use of fossil fuels in the current DRI and BOF processes.

[0010] Over time, new steelmaking processes will be developed to produce lower-emission steel, driven by the need to reduce emissions to reach the zero-emission targets needed to mitigate climate change. One or more embodiments of the processes and reactors disclosed herein may relate to low emission iron for both iron and steel production.

[0011] As the global supply of high-grade iron ore is dwindling, developments to reduce emissions intensity and maintain energy efficiency should preferably allow for the use of lower-grade ores in the production of iron and steel. One or more embodiments of the process and reactor disclosed herein provide a process for the production of iron and steel at low ore levels for both iron and steelmaking. It can be used to beneficiate low-grade ores.

[0012] The roadmap for producing low-emissions-intensity steel is based primarily on low-emissions electricity, and the use of hydrogen gas for the iron reduction process. The Roadmap also acknowledges that low-grade iron ore is inevitable due to the ongoing shortage of high-grade iron ore. There are fundamental reasons why the mainstream BOF process, which uses coke, cannot be adapted to produce low-emission steel. The Roadmap excludes “end-of-pipe” processes such as carbon capture and storage (CCS) for iron or steelmaking, as these processes have generally proven uneconomical for commodity products such as steel. The primary means of producing low-emission steel has therefore turned its attention to a process known as H-DRI, which modifies the current DRI process to produce sponge iron using low-emission hydrogen instead of a mixture of hydrogen and carbon monoxide (syngas) derived from natural gas. A promising means of producing low-emission steel from sponge iron H-DRI is to use renewable electricity to run the EAF process. Beneficiation of low-grade iron ore is often implied to be achievable. Many H-DRI processes have been developed.

[0013] Prospective H-DRI processes can be categorized into two approaches: (a) Pellets reduction. The first approach being developed for low-emission DRI processes is to adapt successful DRI processes, such as the MIDREX (low pressure) and HYL (high pressure) processes. This pellet DRI process uses a shaft furnace where iron ore pellets are slowly reduced into sponge iron pellets. This is a proven technology for DRI. Low emissions may be achieved using hydrogen instead of syngas as the reducing agent. Such processes are called H-DRI, and the Swedish HYBRIT process (https: / / www.hybritdevelopment.se / en / ) is an example. In this process, hot H-DRI pellets are produced from high-grade ore and injected directly into the EAF process for steel. Process modifications must take into account the conversion of the process from an exothermic reaction using syngas to an endothermic reaction using hydrogen. (b) Particle reduction The second approach of the H-DRI process has the advantage of eliminating the pelletizing process used in (a) by using particle flash reduction of the particles. One example of particle reduction is Flash Iron Making Technology (FIT), which has been developed on a bench scale, based on the use of a suspension reactor in which preheated iron ore powder, typically less than 30 microns, is entrained in a downward co-flow of hydrogen and oxygen. The hydrogen combustion heats the powder to a sufficiently high temperature, typically above 1300 °C, that the reduction process is essentially complete with a residence time of about 5 seconds. The FIT process using a flash reactor is reported in "A Novel Flash Ironmaking Process", US DOE, Office of Energy Efficiency and Renewable Energy, 2018. The short residence time is due to a number of factors: the high particle flow due to entrainment of the downward gas in the solid-gas co-flow, the high temperature of the process produces very high gas velocities, and the mixing of the combustion and reducing gas streams further increases the gas velocities. To The main advantage of the FIT process is that it increases the temperature of the reaction, and the generation of steam from the combustion drives the reaction to higher temperatures, as the steam accelerates the reverse reaction. As a net result of the high temperature and gas velocity, residence times of about 5 seconds can be achieved in a reactor about 19 m high. Although the FIT process temperature is below the melting point of iron, it has been reported that the reaction time increases due to strong sintering of the particles, which blocks the pores within the particles and prevents hydrogen gas from reaching the reduction reaction interface within the particles. Another example of particle reduction is the adoption of the HIsmelt process with hydrogen. The HISmelt process is a commercial EAF steelmaking process in which droplets of sponge iron, produced by the combustion of oxygen and syngas and the reduction of the syngas, are injected into a molten steel bath. The molten sponge iron droplets are made from iron ore particles injected into a hot cyclone collector. The cyclone is developed from the combustion of syngas with oxygen to activate the reduction process with hydrogen and carbon monoxide, the temperature of which is high enough to produce molten sponge iron. Within the molten bath, gangue is removed by slagging to produce pig iron, or, if the iron ore is of high grade, the molten iron may be injected into the EAF. In the HIsarna process, the synthesis gas is replaced by hydrogen. Another example of particle reduction is the FINEX process, which uses usually two or three successive fluidized beds to produce iron by heating particles smaller than 70 μm by combustion of syngas and oxygen and reducing them with excess syngas. The effect of agglomeration can be mitigated by modifying the process by modifying the particle size distribution. This fluidized bed approach to hydrogen conversion has been developed in many such processes, such as HYFOR (less than 150 μm), CICORED (100-2000 μm), and FINMET (50-8000 μm) technologies, which are mainly differentiated by different particle sizes as shown in the figure. It should be noted that particles in the range of less than 250 μm are commonly referred to as ultra-fine.

[0014] In summary, all of the prior art approaches for H-DRI disclosed above use combustion oxygen for heating and excess hydrogen for reduction within the reactor.

[0015] The H-DRI process involves producing low-emission hydrogen, known as blue hydrogen, from fossil fuels, which may produce hydrogen and carbon monoxide, converting the carbon monoxide to CO2 and hydrogen using steam, separating the CO2 gas from the hydrogen, compressing or liquefying the CO2 to around 100 bar, and transporting and sequestering the CO2 in geological reservoirs where it is converted into carbonate rocks over a long period of time. All of these process steps are proven technologies, but are costly to produce.

[0016] Alternatively, low-emission hydrogen, called green hydrogen, can be produced from renewable electricity such as solar, wind or hydroelectric power using electrolysis of water. Current trends suggest that green hydrogen will be the lowest cost because of the simpler process, the falling cost of electrolyzers and the falling cost of renewable electricity from wind and solar. Green hydrogen is being pursued in the HYBRIT project.

[0017] The challenge with adapting processes that use fossil fuels is that the additional cost of hydrogen production is generally not offset by process improvements. Also, many such processes are not adapted for the use of low-grade ores, such as those required for the use of EAFs. The costs of pelletizing iron ore for processing in shaft furnaces are not negligible, and require, for example, the use of bentonite or biomass as a binder to inhibit pellet crushing in the shaft furnace floor.

[0018] It is noted that the DRI process can produce hot sponge iron, which can be used in steelmaking to produce sponge iron briquettes using the Hot Briquetted Iron (HBI) process. HBI processing is used to inhibit oxidation of the briquettes, including inhibiting oxidation and spontaneous combustion during transportation of the iron for steelmaking. HBI sponge iron is a product that steelmakers sell to steelmakers as a feedstock that can feed into the steelmaking process. Thus, HBI produced using H-DRI can be used to lower the emission intensity of steelmaking, whether by any of the processes mentioned above. It is understood that H-DRI can be processed into low emission sponge iron briquettes using the HBI process.

[0019] If the H-DRI product is injected directly into molten iron for slagging to produce pig iron ingots for use in a BOF or EAF, or, in the case of high-grade ores, directly into an EAF to produce steel, then HBI is not required. Many of the particle-based approaches for H-DRI discussed above produce iron that can be directly injected into the EAF steelmaking process when high-grade iron ore is used to produce the H-DRI.

[0020] It should be noted that EAF technology has been developed primarily for batch reprocessing of steel scrap. Continuous EAF processes are being developed so that H-DRI pellets, briquettes, or ingots can be continuously processed into steel. Summary of the Invention [Problem to be solved by the invention]

[0021] As mentioned above, the use of hydrogen in the reduction of iron ore turns the reduction process into an endothermic reaction, whereas for carbon-based fuels the reaction is generally slightly exothermic. The above-mentioned hydrogen-based processes for iron and steelmaking have been appreciated by those skilled in the art who understand that the production of hydrogen, in its many forms, is energy intensive. There is a need to develop processes that minimize the consumption of hydrogen.

[0022] In this disclosure, it is shown that indirectly heated reactors may be used to process iron ore in hydrogen-carbon monoxide / syngas (DRI reactor) or hydrogen (H-DRI reactor). H-DRI reduces CO2 emission intensity.

[0023] An indirectly heated reactor has been previously described by Sceats et al. (a) A CO2 reduction process for the calcination of carbonate materials by Sceats et al., in WO 2016 / 077863, “Process and Apparatus for Manufacture of Calcined Compounds for the Production of Calcined Products,” and references therein, and in Australian Patent Application Publication Nos. 2020904492 and 20201902810, “Process and Methods for the Calcination and Minerals,” and references therein, WO 2015 / 077818, “Process and Apparatus for Manufacture of Portland Cement,” and references therein. (b) the processing of powders exhibiting a phase change in Australian Patent Application Publication No. 2020902858, "A Method for Pyroprocessing of Powers" and references therein; and (c) Australian Patent Application Publication No. 2021902040, "Processes and Method of Calcination of Minerals", for the processing of materials to produce materials for use in batteries. Here, these disclosures recognize that indirect heating means that heat is generated externally from the reaction vessel and may come from a combustion reaction in a furnace surrounding the reactor or may use resistively or inductively heated electrical elements, and that heat transfer to the reactor may be from such a furnace through steel or other heat conductive elements to separate the heating and process. This prior art on indirectly heated reactors does not disclose the applications and advantages of using such indirectly heated reactors for iron or steel making. This indirectly heated prior art discloses the production of low emission lime or low emission dolime that can be used in place of conventional lime or dolime for low emission slagging processes to remove gangue from iron or steel making processes.

[0024] Some aspects of the present disclosure are and to provide one or more means for optimizing the design of an indirectly heated reactor for producing DRI iron, preferably H-DRI iron. may be related.

[0025] Another aspect of the present disclosure is and providing one or more means for using electrical power to provide indirect heat to a DRI or H-DRI reactor. may be related.

[0026] Further aspects of the present disclosure include , low-grade iron ore using such indirectly heated DRI or H-DRI reactors This may be related to upgrades.

[0027] Further aspects of the present disclosure include , may relate to a carburization process of iron particles, which is intended to passivate the iron and provide carbon in the production of mild and carbon steels, thereby allowing carbon sequestration in the carbon steel, especially when the carbon source is CO2 that would otherwise be emitted. Mild steel contains about 0.03-0.15% by weight carbon, and carbon steel contains 0.3-1.5% by weight. It is noted that a carburization process of iron using carbon monoxide CO is disclosed in US Patent No. 5,869,018 by Stephens.

[0028] Further aspects of the present disclosure include To provide a means for scaling up an indirectly heated DRI or H-DRI reactor to increase production capacity. may be related.

[0029] Further aspects of the present disclosure include Integrating indirectly heated DRI or H-DRI reactors into the steelmaking process may be related.

[0030] Further aspects of the present disclosure include Integrating indirectly heated DRI or H-DRI reactors into the steelmaking process may be related.

[0031] The discussion of prior art throughout this specification should in no way be considered as an admission that such prior art is widely known or forms part of the common general knowledge in the art. [Means for solving the problem]

[0032] This disclosure generally relates to indirectly fired direct reduced iron (DRI) and hydrogen direct reduced iron (H-DRI) reactors for iron and steel making using carbon monoxide / syngas or hydrogen as the reductant, respectively. The use of hydrogen is desirable to reduce CO2 emissions. References to a DRI reactor in this disclosure include references to a H-DRI reactor, where the context permits.

[0033] In a first aspect, a process for reducing iron ore is disclosed herein. The process can include introducing a powder including iron ore such that the powder falls downwardly in a reactor tube. The process can also include introducing a reducing gas into the reactor tube. The reducing gas can be introduced into the reactor tube such that the falling powder and the reducing gas assume a dilute flow region. The process can further include indirectly heating the reactor tube to heat the falling powder and the reducing gas to a temperature at which the falling powder is reduced.

[0034] In some embodiments, 0.5 to 1.0 kg m -2 s -1 The powder may be dispensed as a flux in the range of

[0035] In some embodiments, the average velocity of the powder falling downward may be less than 3.0 m / s and greater than 0.2 m / s.

[0036] In some embodiments, the particle size distribution of the powder, including the iron ore, may be in the range of 25 μm to 250 μm. In these embodiments, the flux, average velocity and particle size distribution may be selected such that the downwardly falling powder and reducing gas assume a dilute flow regime.

[0037] In some embodiments, the residence time of the downward falling powder may be about 10 to 50 seconds.

[0038] In some embodiments, the process may further include collecting the resulting reduced iron powder product from the bottom of the reactor tube.

[0039] In some embodiments, the process may further include collecting the exhaust gas.

[0040] In some embodiments, the exhaust gas may contain entrained powder particles. In these embodiments, the process may further include extracting the particles from the gas stream and re-injecting the particles into the reactor tube.

[0041] In some embodiments, the process may further include scrubbing the exhaust gas to remove gaseous reaction products from the exhaust gas. The scrubbed gas may be re-injected into the reactor tube.

[0042] In some embodiments, the reactor tube may be heated to reach a temperature of 700° C. to 900° C. within the reactor tube.

[0043] In some embodiments, heating may be controlled along the length of the reactor tube to maintain a temperature between 700° C. and 900° C. within the length of the reactor tube.

[0044] In some embodiments, the reducing gas may include carbon monoxide, hydrogen, methane, or mixtures thereof. In some of these embodiments, the reducing gas may include hydrogen. Using hydrogen as the reducing gas may advantageously reduce the carbon dioxide emissions of the process.

[0045] In some embodiments, the reducing gas may be tangentially injected into the reactor tube, such as by tangential injection. In some of these embodiments, the reducing gas may be tangentially injected into the reactor tube at a pressure of about 105 kPa.

[0046] In some embodiments, when considering walls, gas, and particle radiation emissions, the solid volume fraction is about 1×10 for a radiation penetration depth of about 1 meter. -4 In some of these embodiments, the walls of the reactor tube may be heated to a temperature between 1100°C and 1700°C.

[0047] In some embodiments, the process may include indirectly heating the reactor using external combustion.

[0048] In some embodiments, the process may include indirectly heating the reactor using electrical power.

[0049] In some embodiments, the process may further include pre-heating the iron ore-containing powder and / or the reduction gas using waste heat from other processes, such as water condensers and other processes related to the reduction of iron ore.

[0050] In some embodiments, the degree of reduction of the powder comprising iron ore may be 95% or greater.

[0051] In some embodiments, the iron ore-containing powder may include hematite, magnetite, goethite, siderite, or other iron-based minerals and mixtures thereof that require reduction of the iron in order to process the mineral.

[0052] In some variations, the collected reduced iron powder may be subjected to further processing to produce high grade iron ingots.

[0053] In some of these variations, further processing may include injecting the collected reduced iron powder into a heated tank to produce molten iron. Further processing may also include mixing a slagging agent, such as lime, with the molten iron in the tank to form a slag, which floats to the top of the tank, is drained, and cooled. Further processing may further include removing the molten iron from the heated tank. Further processing may further include cooling and processing the removed molten iron to produce high grade iron ingots.

[0054] In other variations, such as when the iron ore comprises impermeable iron ore, the process may include an initial oxidation stage in which the iron ore is oxidized to create porous hematite ore, which may then be charged into the reactor tube.

[0055] In some of these other variations, the oxidation step may involve the process of the first aspect in which the reducing gas is replaced with oxygen or air.

[0056] In some embodiments, the collected reduced iron powder may be subjected to further processing to produce cementite. For example, the further processing may include a second reduction process comprising the process of the first aspect, where the reducing gas comprises carbon dioxide, carbon monoxide, and hydrogen, and the reactor temperature and the relative proportions of carbon dioxide and carbon monoxide in the reducing gas are selected such that a portion of the iron is converted to cementite.

[0057] In some of these embodiments, prior to the second reduction process, the collected reduced iron powder is subjected to a process to form a high grade iron powder. The resulting powder may be fed into the reactor tube of the reduction process.

[0058] Also disclosed herein is a process for reducing iron ore, the iron ore comprising low-grade hematite or goethite. The process may comprise a first reduction process comprising the reduction process of the first embodiment. In the first reduction process, the process may be controlled to substantially limit the degree of reduction to produce a ferromagnetic product, such as magnetite. The process may also comprise cooling the resulting ferromagnetic product using a flash quench process. The process may further comprise magnetically separating the gangue from the cooled ferromagnetic product. The process may further comprise feeding the cooled ferromagnetic product into a second reduction process comprising the reduction process of the first embodiment.

[0059] In a second aspect, an externally heated vertical reactor for reducing iron ore is disclosed herein. The reactor may comprise a vertically oriented reactor tube. The reactor may also comprise a hopper disposed adjacent to an upper end of the reactor tube and configured to input a powder comprising iron ore such that the powder falls downwardly within the reactor tube. The reactor may further comprise a reducing gas input disposed along the reactor tube from a bottom of the reactor tube for inputting a reducing gas into the reactor tube. The reactor may further comprise a heating element disposed vertically adjacent to at least one wall of the reactor tube and configured to provide heat conducted through the at least one wall, thereby heating the powder and gas within the reactor tube to a temperature at which the powder and gas are reacted. The reactor may further comprise a gas outlet disposed adjacent to an upper end of the reactor tube. The reactor may further comprise a reduced iron powder output disposed at a bottom of the reactor tube.

[0060] In some embodiments of the second aspect, the reactor may further include a deflector plate within the reactor tube configured to deflect the gas and the powder. For example, the deflector plate may be disposed within the reactor tube adjacent to the reducing gas inlet.

[0061] In some embodiments of the second aspect, the reducing gas inlet may be positioned to inject the reducing gas tangentially into the reactor tube, such as by tangential injection. In some of these embodiments, the reducing gas inlet may be configured to inject the reducing gas tangentially into the reactor tube at a pressure of about 105 kPa.

[0062] In some embodiments of the second aspect, the reactor may further comprise a gas separator disposed adjacent to the inlet of the gas outlet. The gas separator may be configured to remove entrained powder from the gas.

[0063] In some of these embodiments of the second aspect, the reactor may further comprise a metal tube connected to the gas separator. The metal tube may pass through the center of the reactor tube and may be configured to pass entrained powder removed from the separator through the reactor tube.

[0064] In some of these embodiments of the second aspect, the reactor may further comprise a filter through which the separated exhaust gas passes, where the gas may be scrubbed from the gaseous reaction products.

[0065] In some embodiments of the second aspect, at least one wall of the reactor tube may comprise a steel or ceramic that is stable to hydrogen at about 1050°C.

[0066] In some embodiments of the second aspect, the diameter of the reactor tube may be about 2 m or less. The length of the reactor tube may be 10 to 35 m, and in these embodiments, the residence time of the powder falling downward may be about 10 to 50 seconds. In particular, the residence time may depend on the gas flow direction and the clustering of the iron ore particles.

[0067] In some embodiments of the second aspect, the reactor tubes may be configured such that the heat exchange between the walls of the reactor tubes is less than about 100 kW / m.

[0068] Also disclosed herein is the use of the externally heated vertical reactor of the second aspect in the process for reducing iron ore of the first aspect. In some embodiments, the use of the externally heated vertical reactor may include using about eight such vertical reactors in parallel, where the input powder including the iron ore is distributed to the vertical reactors from a central silo and the reducing gas is distributed from a gas source.

[0069] Other aspects of the present disclosure include the following. (a) An indirectly heated DRI or H-DRI reactor for the reduction of iron ore fines, in which the reactor temperature profile along the reactor wall can be controlled to initiate and maintain the reaction in order to complete the reduction process sufficiently within the residence time of the powder particles in the reactor. (b) Such indirectly heated DRI or H-DRI reactors are fuel agnostic for heating and may be powered by indirect combustion of gas without the normal limitations of direct combustion where the iron ore also reacts with the combustion gases and the impurities therein. (c) Such indirectly heated DRI or H-DRI reactors may use electrical power for heating, using resistive, inductive, or microwave heating. Such reactors may also be explicitly referred to as indirectly heated e-DRI or eH-DRI reactors. Such reactors preferably have the capability to either operate with variable power throughput to allow for rapid shutdown and startup to accommodate the typical fluctuating supply of renewable electricity, to allow for load balancing of grids with fluctuating feed rates of iron ore and reducing gas inputs, or operate with near constant power using energy storage systems such as batteries, heating fluids, or solids to provide heat or power when renewable generation is low. (d) Using such modules of indirectly heated DRI or H-DRI reactors, the process can be scaled up while preferably controlling each reactor by controlling the powder input, reducing gas input, and selected indirect heating input as required. (e) The use of multi-stage indirectly heated DRI or H-DRI reactors, with comminution as required, to allow upgrading of the powder in terms of iron content by magnetic separation of gangue from the partially processed iron powder prior to the final reduction step to high grade iron as described above. (f) The use of indirectly heated DRI or H-DRI reactor segments allows for passivation of the iron surface by the formation of a carbon coating, increasing its oxidation resistance and self-combustion, and allows for the sequestration of carbon in the steel by supplying carbon to the carbon steel. (g) Such indirectly fired DRI or H-DRI reactors are integrated with furnaces for melting iron powder and mixing the molten iron with slagging agents such as low-emission lime / dryme to produce high-grade pig iron ingots. (h) A means of integrating an indirectly fired DRI or H-DRI reactor consuming high grade iron in either briquette or ingot form with an EAF process, including flux addition, to produce iron or steel.

[0070] Reactor Control with Indirect Heating It would be advantageous if at least one embodiment of the process and reactor disclosed herein could provide indirect heating of powders and gases in a DRI or H-DRI reactor process, where combustion and reduction occur simultaneously within the reactor vessel, improving control of the DRI or H-DRI process as compared to existing technology for DRI or H-DRI processing for iron and steel making.

[0071] Hydrogen Reduction It would be advantageous if at least one embodiment of the process and reactor disclosed herein could reduce the amount of hydrogen used in the H-DRI process. The production costs of green or blue hydrogen are high Possible Therefore, It would be advantageous to provide an H-DRI process that minimizes the use of hydrogen. Advantageously, the use of indirect heating can reduce the demand for hydrogen and oxygen. The paradigm developed in this disclosure allows the use of hydrogen for the reduction of iron. The advantage is that indirect heating can be provided from either low-cost combustion or electrical heating. Such cost savings can offset the energy required to crush as-mined iron ore to a powder size for processing in such indirectly heated reactors.

[0072] Processing of Iron Ore Fines It would be advantageous if at least one embodiment of the process and reactor disclosed herein could provide an iron ore reduction process that could be used to process iron ore fines, such as those having a particle size of less than about 200 μm.Such fines are produced at many stages from mining to iron and steel making and provide a convenient source of powder that cannot be easily processed in shaft furnaces or fluidized beds.

[0073] Processing of low-grade iron ore. At least one embodiment of the process and reactor disclosed herein uses low-grade iron ore as a feedstock, Iron processing that can upgrade the quality of iron by removing gangue for use in steelmaking In this regard, it would be advantageous to provide a process for: Many processes for the beneficiation of iron ore using indirectly heated DRI or H-DRI reactors It may be related to providing.

[0074] Carbon Sequestration in Steel. Depending on the end user, it may be necessary to add carbon to iron to produce mild carbon steel. In this regard, aspects of the present disclosure include: A process for carburizing or partially carburizing DRI or H-DRI during the production of steel. Regarding , a process that allows for the sequestration of carbon in the steel.

[0075] Reactor Scale-Up At least one embodiment of the process and reactor disclosed herein comprises: To process large amounts of iron ore Can be scaled up Indirectly Heated DRI or H-DRI Reactor It would be advantageous to provide

[0076] In summary, the present disclosure Aspects Indirect heating The present invention may involve the use of a conventional DRI or H-DRI reactor, which may use different methods for indirect heating and different reducing gases, may employ reactor controls that result in high thermal efficiency, and may be utilized for the processing of iron ore fines, upgrading of low grade iron ores, carburization and passivation of iron with carbon. The reactors disclosed herein may also be suitable for scale-up, for example by using modules of such reactors.

[0077] CO 2 At least one embodiment of the process and reactor disclosed herein reduces CO 2 It would be advantageous to provide a process for the production of iron or steel with reduced emissions. In embodiments of these aspects, the H-DRI reactor may use renewable electricity for heating and green hydrogen, zero-emission lime and dry lime for slagging, and iron carburization for carbon sequestration.

[0078] It is acknowledged that indirectly heated reactors such as drop tubes have been used for laboratory evaluation of materials, however, the prior art of Sceats et al. demonstrates that indirectly heated reactors can be deployed on a commercial scale for a variety of applications.

[0079] One or more embodiments of the processes and reactors of the present disclosure relate to the commercial application of indirect heating to DRI and H-DRI reactors, including the use of electric heating to e-DRI and eH-DRI reactors (herein referred to as e-DRI and eH-DRI reactors).

[0080] Disclosed herein is a process for reducing iron ore that can include the use of an indirectly heated DRI or H-DRI reactor, which can include the use of hydrogen for reduction and renewable electricity for indirect heating, which together can reduce the emissions intensity to near zero as an eH-DRI reactor.

[0081] A process for beneficiation of low-grade iron ore using an indirectly heated DRI or H-DRI reactor configuration is also disclosed herein.

[0082] CO in iron for carbon steel production and iron passivation 2 Also disclosed herein is a process for isolating

[0083] Also disclosed herein is a method for scaling up a process for reducing iron ore using several such indirectly heated DRI or H-DRI reactor modules for iron and steel making.

[0084] Further aspects of the process and reactor will become apparent from the description and drawings. [Brief description of the drawings]

[0085] Embodiments of the process and reactor will be better understood and readily apparent to those skilled in the art from the following written description, by way of example only, in conjunction with the drawings in which: [Figure 1] 1 is a schematic diagram of an exemplary embodiment of an indirectly heated DRI reactor operated at a commercial scale, in this example the indirect heating is a furnace system using any fuel and the reducing gas in the reactor is a mixture of gases such as CO, H2, or syngas. [Diagram 2] FIG. 2 is a schematic diagram of an exemplary embodiment of an indirectly heated DRI reactor (eH-DRI reactor) in which indirect heat is provided by electric power and hydrogen gas is used as the reducing gas. The embodiment of FIG. 2 can achieve near zero emissions when renewable electric power is used. [Diagram 3] FIG. 1 is a schematic process flow of an embodiment for upgrading low-grade iron ore using a segmented indirectly heated DRI or H-DRI reactor, where a first segment is used to produce magnetic ferrous material that enables magnetic separation of the gangue, and a second segment is used to complete the reduction to iron. [Figure 4] 1 is a schematic process flow of an embodiment for upgrading low-grade iron ore in which iron powder from an indirectly fired DRI or H-DRI reactor is converted into DRI powder and injected into a molten iron bath where a slagging agent is injected to extract gangue and produce pig iron ingots. [Diagram 5]Schematic process flow of an embodiment for passivating iron ore with cementite to provide carbon for mild and carbon steel production using a segmented indirectly heated DRI or HDI reactor, where in the first segment DRI is produced and a coating of iron is produced by injecting CO2 and hydrogen gas to deposit a layer of cementitious Fe3C. This CO2 can be used to sequester carbon in the steel and reduce the CO2 footprint of the steel. [Figure 6] 1 is a schematic process flow of an embodiment in which iron powder from an indirectly fired DRI or H-DRI reactor module is used to produce DRI powder, which is injected into a molten iron bath and a slagging agent such as lime is injected to extract gangue and produce pig iron ingots for steelmaking. [Figure 7] FIG. 6 is a schematic process flow of an embodiment for steel making used to produce sponge iron briquettes using the HBI process to produce iron from an indirectly heated module of a DRI or H-DRI reactor that may use the beneficiation and passivation processes of FIGS. 4-5. [Figure 8] FIG. 7 is a schematic diagram of an embodiment for integrating a DRI or H-DRI reactor into a module for injecting powder or ingots into an EAF process for steelmaking, which may use the beneficiation and passivation processes of FIGS. 4-6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0086] Preferred embodiments of the process and reactor will now be described with reference to the accompanying drawings and non-limiting examples. Indirectly Heated DRI and H-DRI Reactors

[0087] When producing steel using known techniques for DRI processing, and the tests described for developing the H-DRI process, the reducing gas always serves two roles: first, to provide heat by combustion with injected oxygen to raise the temperature of the gas and solids to initiate the reduction reaction, and, if necessary, to provide additional heat for the reduction of iron ore to iron with hydrogen; second, to provide the gas for reduction. In some cases, the combustion / reduction process includes coal as a fuel.

[0088] Current DRI processes have been developed for iron and steel making processes, and the most commercially developed use pellets or fine / lump iron ore as the feedstock. In these DRI reactors, a bed of slowly moving pellets is reduced by a reducing gas in a shaft kiln. Heat from combustion is adsorbed on the pellet surface, and the diffusion of heat and reducing gas through the pellets is generally the rate-limiting process for the reduction reaction. Typical residence times to achieve uniform reduction in such a packed bed are on the order of a few hours.

[0089] In one or more embodiments of the reactor disclosed herein, heat may be supplied to the reactants from indirectly heated reactor walls rather than from a combustion within the reactor. However, indirect heating is not useful for packed bed reactors because heat penetration from the heated reactor surface into the moving packed bed is limited to the area near the hot surface and the resulting temperature gradient is very high. To make the DRI for such H-DRI reactors, iron ore should be injected as particles and used, and the volume solids fraction of particles should be about 10 to achieve uniform reduction throughout the reactor. -4 This is the order.

[0090] This low volumetric solid fraction is such that the radial penetration depth is ideally equivalent to about 1 m of the reactor tube radius and the temperature distribution throughout the reactor is preferably nearly uniform. In the prior art of Sceats et al., many chemical and physical reactions have been found to be fast enough with such small particles because the heat and mass transport within the particles is fast enough that the increased reaction rate due to the use of small particles compared to pellets offsets the lower volume fraction. Thus, the product flux is similar to that of a packed bed of pellets or a fluidized bed of particles with combustion gases in the reactor. The residence time of the powder particles in the indirectly heated reactor is preferably less than about 50 seconds. The fast reaction times are due to the fact that the mass flow rate of iron ore in the indirectly heated reactor with small particles is similar to that of a moving bed of pellets used in conventional DRI reactors, and therefore the product flux through the reactor cross section is also similar.

[0091] Indirect heating of the falling stream of particles is compared to a fluidized bed. The advantage of indirect heating is that the tendency of the bed to collapse due to fluctuations is eliminated, with fluidized beds being particularly susceptible to particle agglomeration. It is recognized that indirectly heated reactors can be more expensive than fluidized beds for equivalent heat transfer. When indirectly heated reactors are operated with falling powder and rising gas, there is a tendency for fine particles to be elutriated from the reactor, but this is overcome by reinjecting such particles into the reactor, as used in circulating fluidized beds. The advantage of an indirectly heated reactor is that the absence of rising combustion gas reduces the gas flow rate, reducing the extent of elutriation.

[0092] One premise of the process and reactor disclosed herein is that the flux of iron from an indirectly heated reactor using a reducing gas is similar to the reduction of a packed bed of iron ore pellets or a fluidized bed of particles where direct heating is used by combustion of a portion of the reducing gas in the reactor. This approach has been validated by processing a wide range of iron ores in an indirectly heated reactor.

[0093] In terms of energy efficiency, the radiation of heat from the indirect furnace into the reactor is offset by radiation losses from the furnace exterior to the surrounding air. This is minimized by using refractory to surround the exterior of the furnace. Thick refractories store energy and may slow the system's response to heater temperature changes. Some applications require fast response, so refractories with low thermal mass are used. Indirectly heated DRI and H-DRI reactors therefore have energy efficiencies comparable to existing processes.

[0094] The advantage is that these reactors offer more flexible operation to accommodate variations in either heat, iron ore fines, or reducing gas mass flow rates, and the heating energy can be generated by any combustion process, and electricity, or a combination thereof.

[0095] In one embodiment of the present disclosure, the use of an indirectly heated DRI or H-DRI reactor for reducing iron ore on a commercial scale is disclosed. The basic principle of iron ore reduction is that the iron ore must be heated to initiate the reduction reaction in a reducing gas such as carbon monoxide or hydrogen. In the prior art, the iron oxide is heated by injecting oxygen into a reducing gas of H2 and CO, and the combustion of the reducing gas is induced to provide heat. At a certain temperature, set by the properties of the iron ore, the reduction process of iron ore with excess CO and H2 begins. The reduction of iron ore with CO is exothermic and the reduction with H2 is endothermic, so a balance can be achieved by controlling the gas composition. In general, combining the oxidation combustion process and the reduction process in the same reactor results in constraints on the control of the process. This is further complicated by the need to introduce the iron ore as pellets or to introduce complex fluidized beds to limit the emission of fines in the exhaust gas stream. Over the years, the steel industry has developed energy-efficient means to operate this process and scaled it up in large reactors such as BOFs.

[0096] The use of indirect heating of the iron ore eliminates the need to carry out a combustion process within the reactor to supply heat. Heat transfer from combustion in an external furnace is via a thermally conductive medium such as a steel or ceramic wall. The ability to control the temperature distribution along the reactor improves control of the process, whereas traditional processes require the injection of reducing gas or oxygen at various points along the reactor.

[0097] One consequence of indirect heating is that the reduction process is independent of a heat source. Therefore, lower-grade fuels, which contain substances that would adversely affect the quality of the iron if used in an internal combustion reduction process, may be used for combustion in the external furnace. Another consequence is that air may be used to burn the fuel, rather than an expensive oxy-combustor.

[0098] Ideally, the particle size in the indirectly heated reactor should be less than 250 μm, which can be achieved by crushing and grinding the ore; the preferred range of 250 μm can be easily achieved using low-cost crushers and grinders for mined iron ore. 。

[0099] In FIG. 1, a schematic diagram of an indirectly heated DRI or H-DRI reactor for producing sponge iron powder is shown, with iron ore powder injected from the top of the reactor and reducing gas injected at the bottom to provide a counterflow of gas. The reducing gas can be CO, or H2, or a mixture thereof. The reactor mainly consists of a reactor tube 101 and a combustion furnace 102, which can be powered by gas or gas-solid combustion process. A preferably dried and preheated iron ore concentrate powder input 103 is injected into a hopper 104 to form a bed of powder, which is injected into an injection tube 106 at the top of the reactor by a rotary valve 105 to form a downward plume of powder. At the bottom of the reactor, a flow of reducing gas 107 is injected tangentially into the reactor as a swirling flow at a pressure of about 105 kPa. The rising gas and falling powder are heated by an external combustion furnace through the reactor wall. The segmented combustor can provide the desired reaction temperature along the reactor so that in this configuration the reducing gas is consumed by the iron ore at a controlled rate. This is important because the reaction can be endothermic, exothermic, or a mixture of both depending on the reducing gas composition and the reduction kinetics at any point in the reactor. Throughout the reduction process, as the reducing gas rises through the reactor it is converted to steam and CO2. As mentioned above, the reducing gas injected into the reactor exceeds the amount consumed so that the reduction reaction can proceed to completion. At the top of the reactor, the exhaust gas steam is exhausted from the top of the reactor, carrying the powder fines and is separated from the gas by a cyclone 108 and filter 109 to obtain the exhaust gas steam 110. The exhaust gas is cooled by the falling powder. The gas is cooled by the falling powder and the entrained fines are collected in the bed in the cone 111 and reinjected into the reactor through the fines reinjection tube 113 using a rotary valve 112. All the powder processed as sponge iron is cooled by gas injected into the bottom of the reactor, collected in a bed of cone 114 at the bottom of the reactor, and discharged from the reactor through rotary valve 115 as sponge iron 116.The exhaust gas stream 110, which typically contains steam, CO2, and unreacted reducing gas, is cooled and water and CO2 are extracted using known processes used in the petrochemical industry. Excess reducing gas is recycled to the reactor as part of the reducing gas stream 107. The desired process temperature should preferably be low so that the reaction rate is not inhibited by either sintering of the particle surface area or melting of the iron, which would retard the diffusion of hydrogen into the oxide. The residence time in the reactor is preferably less than 50 seconds, and typically ranges from 10 to 50 seconds. 。

[0100] The fast process times of the reactors mean that the material volumes in the reactors are of the order of tens of kilograms, so that the feed rates of the iron feed ore and reducing gas can be changed very rapidly to keep up with the energy available from heat production.

[0101] Thus, one or more embodiments of the present disclosure can include directly heating iron ore particles flowing down the reactor in a dilute flow region where the volume fraction of the particles is small enough that radiation from the reactor walls can penetrate the powder dust and gases. o Considering walls, gas, and particle emissions at temperatures on the order of 10°C, the radiation penetration depth is on the order of 1 meter, and the volumetric solid fraction is about 10 -4 The need for a low solids volume fraction of the particles in the powder means that the residence time of the particles in reactors 8 to 30 m high is of the order of 10 to 50 seconds, with the particles flowing downward in a countercurrent of reducing gas. The primary consideration is therefore the rate of the iron reduction reaction, and ensuring that the reaction can be completed within the required residence time.

[0102] The short residence times considered above have certain advantages. Iron, when formed at the process temperatures of interest, is known to form iron "hairs" that can diffuse through the particles quickly and cause agglomeration of the iron particles. This is a known risk that creates challenges in fluidized bed reactors, as the agglomeration or "sticking phenomena" can cause the bed to collapse, which can result in the reactor being shut down and the time to re-establish fluidization being too long for commercial operation. The process and reactor disclosed herein are intended to provide a method for the preparation of non-fluidized bed processes. Recruitment is doing.

[0103] Taking the above into consideration, the application criteria is whether the iron ore particles can be processed into sponge iron within about 10 to 50 seconds. For reasons considered below, the process temperature is preferably 700 to 900 oC range. This low temperature prevents the "sticking phenomenon" common in gas-based DRI reactors such as fluidized beds. The reduction kinetics of iron ore has been intensively studied. The kinetics of the direct reduction reactions of hematite to magnetite and magnetite to wustite are known to occur very quickly compared to the slower reduction of wustite to iron, which is the rate determining step. The definitive study by Liu et al. (W. Liu, J. Y. Lim, M. A. Sausedo, A. N. Hayhurst, S. A. Scott, and J. S. Dennis), "Kinetics of the reduction of wustite (umlaut) by hydrogen and carbon dioxide for the chemical looping production of hydrogen", Chem. Eng. Sci. 120, 149-166 (2014), considers the reduction kinetics. The study shows that even with about 5% hydrogen, the reaction is very fast in this temperature region, and the results, when extrapolated to initially 100% hydrogen at the bottom of the reactor and about 60% hydrogen at the top of the reactor, ensure that the reaction is completed in less than 5-10 seconds for particles up to about 250 μm. This reaction rate is fast enough for use in dilute flow reactors that process iron ore particles in hydrogen. More detailed calculations show that the heat exchange between the hot walls of the reactor is less than about 100 kW / m, which is less than the rate of about 200 kW / m required for the highly endothermic reaction. It may be concluded that neither the chemical kinetics of the reduction nor the heat transfer from the hot reactor walls are limitations of the process described herein. Experiments performed in an indirectly heated reactor support these conclusions.

[0104] The requirements considered above limit the reactor to tubes with a diameter of up to a few meters. Due to the very fast reaction rate of a few seconds, the flux of sponge iron leaving the tube is similar to that of a typical DRI reactor using a moving bed of pellets, with respect to the cross section of the tube, since the reaction rate in such a bed is of the order of a few hours. Those skilled in the art will appreciate that the flux of sponge iron leaving the tube is approximately 3 ms -1It will be appreciated that a dilute flow of powder at a velocity of less than 1000 rpm will result in much less wear to the reactor material than a moving bed of pellets. It will be apparent to those skilled in the art that an indirectly heated DRI or H-DRI plant has the advantage of simplifying the iron and steel making process by eliminating the need for a pelletizing plant. In order to transition away from the carbon-intensive iron and steel making process, it is important to be able to reduce costs by eliminating manufacturing processes such as pelletizing. The ability to make iron or steel from iron ore concentrate has many such advantages.

[0105] The example in Figure 1 is an indirectly heated DRI (H-DRI) reactor, which does not explicitly address the need for CO2 emission reduction in iron production. Emission reduction in the furnace can be achieved by using hydrogen as the injected reducing gas or by using low-emission fuels such as biomass or waste. However, for large industrial plants, it is generally not possible to utilize large amounts of biomass or waste. An alternative approach that simplifies the heating process is to use renewable electricity for heating, which is discussed below.

[0106] In FIG. 2, a schematic diagram of a preferred embodiment of an indirectly heated eH-DRI reactor for producing sponge iron powder from iron ore powder using hydrogen as the reducing gas is shown. The reducing gas is H2. The reactor mainly consists of a reactor tube 101 and an array of electric furnace elements 102. A preferably dried and preheated iron ore concentrate powder input 103 is injected into a hopper 104 to form a bed of powder, which is then injected into an injection tube 106 at the top of the reactor by a rotary valve to form a downward plume of powder. Along the reactor, a flow of hydrogen 107 is injected tangentially into the reactor as a swirling flow at a pressure of about 105 kPa. In this embodiment, the electric furnace has several such injector elements 102, which can also preheat hydrogen for injection into the reactor, in combination with a deflector plate 108 that deflects the gas and particles. The turbulent flow can help break up the gas and particle flows to suppress the formation of powder agglomerates, enhance the heat exchange between the gas and the particles, and increase the residence time. The rising gas and falling powder are heated through the reactor walls by an electric furnace to reach the desired reaction temperature, and the reducing gas is consumed by the iron ore in the reduction process, resulting in the formation of sponge iron at the bottom of the reactor. Throughout the reduction process, hydrogen gas is converted to steam as it rises through the reactor. As mentioned above, hydrogen gas is always in excess of the amount consumed so that the reduction reaction can proceed to completion. The gas stream is exhausted from the top of the reactor, carrying the powder fines and is separated from the gas by a cyclone 109 and a filter 110 to obtain an exhaust gas steam 111. The fines are collected in a bed in a cone 112 and are reinjected into the reactor through a fines reinjection pipe 114 using a rotary valve 113. All the powder processed as sponge iron is collected in a bed in a cone 115 at the bottom of the reactor and discharged from the reactor through a rotary valve 116, releasing hot sponge iron 117. The exhaust gas stream 111, consisting of steam and hydrogen, is cooled such that the water is easily extracted to form liquid water, leaving hydrogen gas with minimal steam. The excess hydrogen gas is recycled to the reactor as part of the reducing gas stream 107.The desired reactor temperature should preferably be low so that the reaction rate is not inhibited by either sintering of the surface area or melting of the iron. 。

[0107] The injection of gas streams and the use of plate deflectors along the reactor can be used in any application of indirectly heated reactors. It is well known that countercurrent gas and powder flows are organized in the reactor tube to minimize interactions, so that downward flowing particles tend to accumulate near the walls, while gas moves upwards at high speed in the middle of the tube. This means that the advantage of the rising gas slowing down the powders and increasing their residence time, facilitating gas-particle heat transfer, is lost. At the top of the reactor, such a separation can be useful as it can reduce the entrainment of fines in the exhaust. Particles and gases can be deflected by plates in the tube, but the plates can become fouled. Simple approaches such as an inner tube can break the symmetry and create an annular reactor, and tubes can be used to inject gas in a different way than described in Figure 2. Hydrogen injection does not deflect particles significantly due to the low momentum of hydrogen. The most desirable approach is to use a deflector plate, as shown in Figure 2, which is washed with a hydrogen jet and prevents fouling of the plate. Pulsed gas systems are routinely used in filter systems and may be used for this purpose. The spacing of such devices should be less than the length required to re-establish steady flow in the pipe. The details of this will depend on the process details.

[0108] As in the embodiment of Figure 2, very fast shutdown or startup can be achieved through the use of electrically powered elements. The reactor is designed to use renewable electricity, which is not generated all the time. In peak solar or wind conditions, the cost is very low. This allows the reactor throughput to be scaled up or down to match the availability and cost of electricity, and green hydrogen will have a similar reaction.

[0109] One approach to mitigating variable energy is to use a reactor design that can switch between combustion or renewable electricity, or a variable mix of each.

[0110] Another approach is to store the electricity in batteries or store the heat and convert the heat to electricity to maintain the required power for a period of time, especially needed to fill the gap in renewable electricity from solar and wind farms. In the long term, the average cost of renewable electricity is expected to fall below the cost of fossil fuels on a MWhr basis. Therefore, the electricity can be used to heat the reactor in a 24 / 7 operation to produce hydrogen by electrolysis. In that case, it is always more advantageous to use the electricity for electrical heating than to use electrolysis to make hydrogen for combustion and generate heat by combustion.

[0111] In Figures 1 and 2, the heated wall for heat transfer can be either: (a) Carbon steel has negligible carbon which can lead to attack by hydrogen leading to embrittlement and fracture, and has a hardness of about 1100 to support its own weight as a vertical reactor tube. o A metal alloy of steel that exhibits strength at temperatures of 0.4 °C, preferably an alloy of nickel and chromium with the addition of silica, under the proper conditions the steel forms a passivation layer of chromium and silica oxides. Note that these oxide layers are stable in hydrogen, with the presence of small amounts of steam in the reactor. Furthermore, the alloy should be in the austenitic phase, which inhibits hydrogen diffusion. When such metals are used for heat transfer, electric elements are deployed in the furnace to irradiate the steel, while still gas conditions maintain an oxidizing environment. Such a system requires that the temperature can be raised quickly, the steel tubes are mounted so that they can be easily replaced, bellows and counterweights are used to relieve stress on the steel, thermal expansion and creep are addressed, and the gas pressure in the reactor must be maintained at a positive gauge pressure to inhibit buckling. (b) Ceramic materials may be used in the reactor design where they have the added advantage of being able to encapsulate electrical heating elements. Such elements may be subject to thermal shock and the operation of the reactor must take this into account.

[0112] FIG. 1 illustrates an embodiment using indirect heating by combustion, and FIG. 2 illustrates an embodiment using indirect heating using electrical power. It is noted that the indirectly heated reactors described above, and in particular the indirectly heated H-DRI reactor, can be applied to the processing of a wide range of ferrous or ferric containing iron ores, which contain elements such as manganese, nickel, copper, and chromium, and require an initial iron reduction step. Subsequent processing can include hydrometallurgical extraction processes, or deeper reduction processes such as Al-thermal reduction. An advantage of the indirectly heated reactors described herein is that the products from this initial reduction step, which are typically used for flotation and acid-base extraction processes, are porous, allowing for efficient extraction. CO 2 emissions reduction

[0113] CO in steel production 2 The process and reactor paradigm described herein for reducing emissions can be based on indirect heating. Near zero emission intensity can be achieved by using: (a) iron ore fines, preferably having a particle size of less than about 250 μm; and (b) green hydrogen or blue hydrogen using CCS for the direct reduction of iron ore to iron; and (c) Renewable electricity should be used for indirect heating of reactants and products to initiate the reduction reactions and for providing energy to drive the endothermic hydrogen reduction of iron ore to iron.

[0114] Because indirect heating is agnostic to the heating source, there are many ways to configure the reactor between the embodiments of FIG. 1 (combustion heated) and FIG. 2 (electrical heated) to achieve the degree of emissions reduction desired. Iron ore beneficiation and use of indirectly heated DRI or H-DRI reactors

[0115] Beneficiation of low-grade iron ore can be achieved by crushing the low-grade iron ore into small particles and extracting the gangue by various processes based on known techniques using the density difference between the iron ore and the gangue, or in the case of magnetite, by using a magnetic separator. In this section, iron ore beneficiation processes including the use of indirectly heated DRI or H-DRI reactors are described.

[0116] It is well known that reduction roasting of low-grade hematite ores can be used to enhance the magnetic separation of gangue from magnetite produced by roasting, because magnetite is a ferromagnetic material with high magnetic susceptibility. Therefore, reducing hematite to magnetite can improve the separation of gangue. The magnetic properties of iron ores depend on their thermal history through particle morphology and particle size, so the detailed process flow of the ore beneficiation varies greatly. Conventional magnetic reduction roasting is carried out on a time scale of several hours. Considering that the particle size for particle reduction is less than about 250 μm, the roasting time is very short, on the order of a few seconds, and the temperature is kept lower than the reduction temperature of magnetite to wustite and about 600 for flash roasting. o A temperature of 0.5C is selected. The product is cooled by flash quenching, preferably in an inert atmosphere to inhibit reoxidation, until the Curie temperature is reached and the magnetic susceptibility increases as the temperature decreases. Flash quenching can cause distortions in the powder particles, which can result in the release of further gangue by further comminution of the more porous magnetite.

[0117] FIG. 3 shows a schematic process flow for upgrading low-grade hematite ore 301. The hematite ore 301 is crushed by a crusher / grinding machine 302 to a size for injection into a first segment 303 of an indirectly heated H-DRI reactor which operates to produce hot magnetite 304 powder using hydrogen as a reducing agent. This reduces the hematite to magnetite, flash-cooled in nitrogen (not shown), and injected into a second crushing machine 305 to release gangue and magnetite, which powder is injected into a magnetic separator 306 to release a gangue vapor 307 and a high-grade porous magnetite stream 308. The porous magnetite ore is reduced in a second H-DRI segment 309-310 to produce high-grade hot iron 311. Since the reduction process of hematite to magnetite is very fast compared to the overall reduction to iron, the initial size of the crushing grinding circuit may be larger than the <250 μm specified for iron production. Therefore, the process described in FIG. 3 may be repeated to release the gangue in the crushing stage.

[0118] The energy demands required to convert hematite to magnetite are low and, if necessary, energy can be recovered using standard heat recovery systems. The reactor is an indirectly heated DRI reactor and, if hydrogen is used instead of syngas, no CO 2 This may offset the benefit of reduced emissions. Because the energy consumption of the hematite to magnetite reaction is low, the primary advantage of using an indirectly heated reactor is fine control of the process to minimize sintering of magnetite and specifically inhibit the thermal reaction of iron with gangue to form inseparable iron silicates. Flash quenching is desirable to increase the stress on the cooled magnetite particles and promote particle decrepitation and release of gangue during magnetite comminution. It is recognized that this process separates gangue particle material in the hematite ore or released during the initial crushing / grinding step. The gangue stream may contain magnetite that was insufficiently magnetically separated, and this feed can be further processed to remove such residual iron by multiple passes through the magnetic separation process described in Figure 3. The process of crushing and heat treatment as described in Figure 3 can be repeated until the required grade of ore is achieved.

[0119] Hematite is a commonly low-grade iron ore and was therefore selected as the iron ore to be processed in the two-stage reactor system depicted in Figure 3, although other ores such as goethite and siderite may also be processed.

[0120] Magnetite ores are found in nature, generally as non-porous minerals, and are often associated with geological processes. As for hematite, high-grade magnetite is becoming depleted, increasing the need to beneficiate such ores. Magnetic separation is used, but is incomplete because magnetite ores have low porosity and the gangue is tightly bound within the particles. The small particle size required for the DRI and H-DRI processes mentioned above aids in the release of such tightly bound gangue before injection into the indirectly heated reactors described in the context of Figures 1 and 2.

[0121] Although the small particle size of magnetite favors the release of tightly retained gangue, it has been observed that the length of indirectly heated DRI and H-DRI reactors is larger than for highly porous iron ores such as hematite and goethite, due to the slower reduction rate of low-porosity gangue. The porosity of such minerals can be improved by the process of oxidizing magnetite to hematite in an indirectly heated reactor, where oxygen, or preferably air, is introduced into the indirectly heated reactor by replacing the reducing gas. During the oxidation of magnetite to hematite, the particles decrepitate, expand and crack, resulting in a sufficiently porous material. This material, as synthetic hematite, can be injected into the DRI or HDI reactor for reduction of iron. The energy required to oxidize magnetite is small and the demand for oxygen is low. Oxidation to iron in an indirectly heated reactor is carried out by maximizing the porosity and surface area, resulting in a material that is reduced more quickly than the original magnetite ore. This means a more compact reactor.

[0122] The approach of oxidizing magnetite to porous synthetic hematite allows the release of previously tightly held gangue, which can be injected into the beneficiation process described above in Figure 3 to further beneficiate the ore as described to produce higher grade iron products.

[0123] Those skilled in the art will appreciate that the above processes are generally irreversible processes that depend on the mineralogy of the iron ore. The above processes vary depending on the mineralogy of the iron ore and the demand for high-grade iron, especially sponge iron, which can be fed directly into the EAF with a low emission footprint. Often, the ore needs to be beneficiated to remove phosphorus, in which case the above beneficiation processes can be integrated into known techniques for phosphorus extraction.

[0124] It will be appreciated that those skilled in the art will recognize that an advantage of the beneficiation process described above is that because indirectly heated DRI or H-DRI reactors use particles instead of pellets, a particle-based beneficiation process based on magnetic separation of particles is easily integrated into the production of iron ore using such indirectly heated reactors.

[0125] Another approach to beneficiation is to use a flash slagging approach on the iron powder produced by the DRI or H-DRI reactor. This approach is illustrated in Figure 4. Hot iron particles 401 are injected into a heated bath 402, which melts the particles and slagging is performed by injection of a slagging agent 403, which is not a carbonate material and is preferably made of lime, dolomite or a mixture of both. This material is most preferably made from the calcination of limestone, dolomite or magnesite as described in the prior art by Sceats et al., which allows the CO 2 is recovered and sequestered as a pure gas stream. The process described herein is therefore a low emission process. The Ca / Mg ratio can be optimized to extract the gangue using the best known ratio understood from chemical analysis of the gangue. The slag rises to the top of the vessel and is extracted as stream 404, and the molten iron is removed from the vessel as stream 405 using known slagging techniques to extract these streams and mix the molten iron with slagging agents. In a subsequent process (not shown), the slag is cooled using a heat recovery process, any iron can be recovered using known techniques, and the molten iron is preferably cooled and drawn into ingots, which are a form of pig iron. If desired, coke can be added to the process to facilitate the subsequent production of carbon steel.

[0126] The most desirable use of pig iron ingots is for injection into an EAF to produce steel, because residual gangue in the pig iron is low enough that up to 100% of the pig iron can be processed in the EAF if desired, thereby lowering the demand for scrap iron. It is recognized that there are cases where it may be desirable to run the process as a batch process. The advantages of using the hot powdered sponge iron from DRI and H-DRI reactors are: "Flash slagging" occurs because the slagging agent is in intimate contact with the iron powder, minimizing the diffusion length of reactive components in the gangue and slagging agent. Carbon sequestration in iron

[0127] Carbon derived from coal is used at certain levels in the production of mild or carbon steel to maximize the strength of the steel while retaining ductile properties suitable for processing and use. Mild and carbon steels therefore contain significant amounts of cementitious Fe. 3 HBI is characterized by the presence of 1,000 to 1,000 carbon atoms. Historically, significant amounts of carbon were included in the pig iron raw material. Another reason for adding carbon to HBI is to passivate the surface. Cementite oxidation by ambient air or moisture is slow, so a coating of cementite can retard oxidation. Furthermore, as a result of rapid oxidation, hot iron is pyrophoric, making handling DRI a safety hazard. This may be obviated by the HBI process, which reduces the surface area of ​​the iron and inhibits runaway oxidation, but the process does not inhibit oxidation on the exposed surface after compaction. From this perspective, coating the iron surface with cementite has an advantage. Importantly, the carbon reduces the CO that would otherwise be emitted. 2 If the CO2 emissions from the steelmaking process are derived from carbon dioxide, the emission intensity in the steelmaking process will be reduced. 2 is a small fraction of current steel emissions, but as mentioned above, H-DRI also includes other CO 2 An example of an emission source is CO from limestone, dolomite, or magnesite. 2 emissions, and pure CO using the prior art of Sceats et al. 2 It can be recovered as a stream.

[0128] In the Stephens prior art, CO 2 They teach that a flow of iron can be injected with hydrogen to convert iron to cementite through a reaction mechanism. H 2 +CO 2 ⇔H 2 O+CO 3Fe+H 2 +CO→Fe 3 C+H 2 O Here, the water-gas shift reaction is in equilibrium and H 2 The O partial pressure is assumed to be such that oxidation of iron is inhibited. This technique shows that if one were to attempt to form cementite by reduction of iron ore, the reaction rate would be too slow. 2 , CO, CO 2 The stream may be an off-gas from a steelmaking process.

[0129] In Figure 5, a means of coating the surface of iron particles is considered. In this process, hot DRI 501 from the indirectly heated DRI or H-DRI reactor described above is injected into a second indirectly heated reactor 502, heated in this case by electrical power 503, to produce the required hydrogen / CO 2 The gas mixture 504 is injected at the bottom. External heating is performed to heat the hydrogen / CO 2 / CO / H 2 The O partial pressure is controlled to obtain a fast reaction to form cementite, and the conditions of the cementite reaction mechanism are satisfied for a given input temperature of the iron and gas feed. The exhaust gas 505 is cooled in condenser 506, water is extracted as stream 507, and CO, H 2 , and CO 2 The residual gas stream 508 of the iron is recycled. The extent of reaction of the iron to cementite in the product 509 depends on the residence time of the particles in the reactor and the characteristics of the input iron stream such as porosity and pore distribution, as the resistance of the cementite product layer impedes the reaction rate. The solid product 509 is treated as required for further processes in iron and steel making.

[0130] The extent of reaction of iron to cementite in the product depends on the residence time of the particles in the reactor and the characteristics of the input iron stream, such as porosity and pore distribution, as the resistance of the cementite product layer impedes the reaction rate. Ideally, the cementite product layer under ambient conditions is thick enough to inhibit pyrophoric combustion of the iron, so that the powder may be sufficiently stable, and ideally no HBI process is required for transport to the steel plant. In the production of mild or carbon steel, the amount of carbon that needs to be added in steelmaking may be reduced, preferably to zero.

[0131] Achieving a combination of low-grade iron beneficiation, degree of cementite conversion, and carbon sequestration may reduce the process costs of steel production and lower the carbon footprint of steel. Scaling up production

[0132] A potential drawback of indirectly heated reactors for power gas processes is the need to ensure that radiation from the walls can penetrate the gas and particle cloud. Typically, this limits the diameter of a single tube reactor to about 2 meters. The reactor flux may be the same as a conventional DRI reactor, but the needs of the steel plant mean that such a plant would require multiple reactor tubes to achieve a throughput of up to 5 million tonnes of Fe per year. Due to the simplicity of the reactor design, modules of reactor tubes can be developed. In larger plants, multiple modules may be used.

[0133] FIG. 6 shows a top plan view of a module of an indirectly heated H-DRI reactor coupled to an EAF. The eight-tube module 601 includes eight indirectly heated reactor units, such as the reactors of FIG. 1 or FIG. 2. Each reactor can preferably be operated independently. Each reactor feeds hot sponge iron and lime powder to a pond of molten steel in the EAF 603. The EAF is designed as a three-electrode unit with electrodes 604. The EAF is preferably a continuous EAF under development in the industry, where molten steel 605 is withdrawn from the bottom of the EAF and slag 606 is withdrawn from the top of the molten steel. Various means are used to mix the materials in the EAF, and additional materials such as carbon and other metals for alloys are added as needed. Improvements including iron and cementite upgrading may be included in the module design for steelmaking.

[0134] The tube module described in Figure 6 can also be applied to the production of low emission intensity iron briquettes, where the powder at the outlet of each reactor is collected and injected into the HBI plant. Improvements including iron and cementite upgrading may be included in the modular design for steelmaking.

[0135] In iron and steelmaking modules, each reactor may be operable with independent control of each tube, or the input powder may be distributed to the tube bank and the hot iron powder streams may be pooled together. This modular operation option also allows the ability to derive power for production when electricity and hydrogen costs are low. A similar approach may be used to preheat the input streams of powder and reducing gas to the reactors. Such preheating is a known technique and the optimum means of preheating will depend on the integrated design.

[0136] In the claims which follow, as well as in the preceding description of the processes and reactors, unless the context otherwise requires, either by express language or by necessary implication, the word "comprise" or variations such as "comprises" or "comprising" are used in the inclusive sense, i.e., to specify the presence of stated features, but are not used to exclude the presence or addition of further features in various embodiments of the processes and reactors.

Claims

1. 1. An externally heated vertical reactor for reducing iron ore, comprising: (a) a reactor tube disposed vertically adjacent to a furnace, wherein a feed powder of iron ore is fed into a hopper adjacent an upper end of the reactor tube, the feed powder dropping downwardly through the reactor tube, and a feed of reducing gas is injected into a bottom of the reactor tube; (b) an external furnace disposed vertically adjacent to at least one wall of the reactor tube and providing heat conducted through the at least one wall, the conducted heat increasing the temperature of the falling input powder; (c) a feed port at the bottom of the reactor tube, wherein the reducing gas is heated and injected into the feed port such that the reducing gas rises upward through the reactor tube, further increasing the temperature of the falling feed powder such that the iron ore is reduced by the rising reducing gas; an inlet for reaching a reaction temperature of 700°C to 900°C such that the reducing gas is consumed by the iron ore in a reduction reaction to form reduced iron powder product at the bottom of the reactor, and external heat is controlled along the length of the reactor tube to maintain a reaction temperature profile to reduce the iron ore; (d) a gas outlet disposed adjacent to an upper surface of the reactor, where gas exhausted at the top of the reactor forms a flow that entrains unreacted input powder particles, where the unreacted particles are extracted from the gas flow and reinjected into the reactor; (e) a gas filter disposed adjacent the gas exhaust inlet, wherein gas extracted from the reactor tubes scrubs gas reaction products including steam and carbon dioxide, and wherein the scrubbed extracted gas is reinjected into the input gas stream; and (f) a bed disposed at the bottom of the reactor tube, the reduced iron powder product being collected in the bed at the bottom of the reactor tube and vented from the reactor for subsequent processing; An externally heated vertical reactor comprising:

2. 2. The externally heated vertical reactor of claim 1, wherein the reducing gas comprises carbon monoxide, hydrogen, methane, or a mixture thereof.

3. Considering walls, gas, and particle emissions, the volume fraction is about 1x10 for a radiation penetration depth of about 1 meter. -4 3. The externally heated vertical reactor according to claim 1 or 2, wherein the reactor wall is heated to a temperature of 1100 to 1700° C.

4. An external heat source is generated within the furnace from the combustion of solid or gaseous fuels, or from electrical power using resistance, induction, or microwave generation, and is distributed along the length of the reactor such that, taking into account walls, gas, and particle emissions, the volume fraction is about 1×10 for a radiation penetration depth of about 1 meter. -4 and the reactor wall is heated to a temperature of 1100-1700° C.

5. 5. The externally heated vertical reactor according to any one of claims 1 to 4, wherein the iron ore fines can be hematite, magnetite, goethite, siderite, or other iron-based minerals and mixtures thereof that require iron reduction to process said minerals.

6. 6. The externally heated vertical reactor according to any one of claims 1 to 5, wherein said at least one wall of said reactor tube is made of steel or ceramic that is stable to hydrogen at about 1050°C.

7. The reducing gas is hydrogen and the heat source is CO 2 The externally heated vertical reactor according to any one of claims 3 to 5, wherein the power source is renewable power to minimize emission intensity.

8. 8. The externally heated vertical reactor according to any one of claims 1 to 7, wherein the input powder has a particle diameter range of more than 25 μm and less than about 250 μm.

9. 9. The externally heated vertical reactor according to any one of claims 1 to 8, wherein the diameter of the reactor tube is about 2 m or less, the length of the reactor tube is 10-35 m, and the residence time of the iron ore particles flowing downward is about 10-50 seconds, and the residence time depends on the gas flow direction and clustering of the iron ore particles.

10. 10. The externally heated vertical reactor according to any one of claims 1 to 9, wherein the heat exchange between the walls of the reactor is less than about 100 kW / m.

11. 11. The externally heated vertical reactor according to any one of claims 1 to 10, wherein the average velocity of the input powder during its fall through the reactor tube is less than 3.0 m / s and greater than 0.2 m / s.

12. The flux of the input powder in the reactor is 0.5 to 1.0 kg m -2 s -1 The externally heated vertical reactor according to any one of claims 1 to 11, wherein the temperature is within the range of

13. 13. The externally heated vertical reactor according to any one of claims 1 to 12, wherein the input powder and input reducing gas are preheated from waste heat from other processes, such as a water condenser and other processes related to the use of the reduced iron product.

14. 14. The externally heated vertical reactor according to any one of claims 1 to 13, wherein the unreacted input powder particles extracted from the gas stream are re-injected into the reactor tube together with hydrogen through a metal tube passing through the center of the reactor tube, whereby these particles are heated and reduced during their movement towards the bottom of the reactor.

15. The externally heated vertical reactor according to any one of claims 1 to 14, wherein the degree of reduction is 95% or more.

16. A process for reducing an input iron ore fine using the externally heated vertical reactor of any one of claims 1 to 15, wherein the input iron ore fine is low grade hematite or goethite; (a) the process is controlled to substantially limit the extent of reduction to produce a ferromagnetic material, such as magnetite; (b) the powder cooling process is a flash quench process; (c) is used; (d) a magnetic separator is used to separate gangue from the magnetic iron ore product; (e) the magnetic iron ore product is injected into a second reactor according to any one of claims 1 to 15 for processing into iron. process.

17. A process for reducing input iron ore fines using the reactor of any one of claims 1 to 15, comprising the steps of: (a) processing low-grade iron ore particles into iron powder at high temperatures; (b) injecting the hot iron powder into a heated bath to produce molten iron; (c) mixing the molten iron with a slagging agent, such as lime, in the heated vessel so that slag is formed, the slag floats to the top of the vessel, is drained, and is cooled; (d) removing the molten iron from the heated bath, cooling, and processing to produce high grade iron ingots. process.

18. 1. A process for activating impermeable iron ore, comprising: (a) oxidizing iron ore to produce porous hematite ore; (b) reducing the porous hematite ore in an externally heated vertical reactor according to any one of claims 1 to 15 to produce iron ore. process.

19. 19. The process of claim 18, wherein the oxidation process uses an externally heated vertical reactor according to any one of claims 1 to 15, wherein the reducing gas is replaced with air.

20. 1. A process for producing cementite, comprising the steps of: (a) reducing iron ore using an externally heated vertical reactor according to any one of claims 1 to 15 to produce iron particles; (b) optionally incorporating the process of claim 17 to produce high quality iron powder; (c) mixing the iron powder with CO 2 and H 2 16. The externally heated vertical reactor according to claim 1, wherein (d) the reactor temperature and CO 2 The relative compositional proportions of are selected to convert a portion of the iron into cementite. process.

21. 16. The externally heated vertical reactor according to any one of claims 1 to 15, used for beneficiating iron, activating impermeable iron ore or producing a desired proportion of cementite in iron, by using a module of about eight such reactors, where the input iron ore feed is distributed to the reactor from a central silo and the reducing gas is distributed to the reactor from a suitable gas source and can be heat exchanged independently from other elements of the commercial process for electricity or gas heating.

Citation Information

Patent Citations

  • JP1974059718A

  • Process and apparatus for directly reducing particulate iron oxide to metal iron

    JP1978100911A

  • Shaft furnace for metallurgy

    JP1979042313A

  • Induction heating apparatus in verticalltype reducinggannealing furnace

    JP1979042319A

  • The fluidized bed temperature in the fluidized bed reduction process control

    JP1980081697U