Light emitting diode including epitaxial light control features
Epitaxial integration of light control features on LEDs addresses the challenges of precision patterning in PhC structures, enhancing efficiency and directional light emission, suitable for micro-LED displays and other applications.
Patent Information
- Application Number
- JP2024525059
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing LED technologies face challenges in achieving high efficiency and directional light emission due to limitations in fabricating photonic crystal (PhC) structures, which require precise patterning on the wavelength scale and are not suitable for mass production, leading to issues like color mixing, color purity, and thermal stability in micro-LED displays.
The integration of light control features, such as photonic crystals, is achieved epitaxially onto the epitaxial layer of LEDs without physical etching, using selective area growth (SAG) and epitaxial lateral overgrowth (ELO) to reduce defect density and improve crystal quality, allowing for controlled light extraction and directionality.
This method enhances the internal quantum efficiency (IQE) and extraction efficiency (EQE) of LEDs by reducing defects, improving spectral purity and thermal stability, making them suitable for high-resolution displays and other applications.
Smart Images

Figure 2024541943000001_ABST
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 USC Section 119(e) of a co-pending and commonly assigned application, U.S. Provisional Application Docket No. 63 / 273,321 (Attorney Docket No. G&C30794.0811USP1 (UC2022-769-1)), entitled “LIGHT EMITTING DIODES CONTAINING EPITAXIAL LIGHT CONTROL FEATURES,” filed on October 29, 2021 by Srinivas Gandrothula, Shuji Nakamura, and Steven P. DenBaars, which is incorporated herein by reference.
[0002] 1. FIELD OF THEINVENTION The present invention is directed to micro- to macro-sized light emitting diodes (LEDs) with epitaxial light control features, and more specifically, to highly efficient LEDs with photonic crystal (PhC) light extractors. [Background technology]
[0003] 2. Description of Related Art Significant developments in III-nitride LEDs have been identified in the past 30 years. There are two approaches to increasing the efficiency of III-nitride LEDs: the first is to increase the internal quantum efficiency (IQE), which is determined by the crystalline quality of the epitaxial layer structure, and the second is to increase the light extraction efficiency (EQE).
[0004] The IQE for III-nitride LEDs is (10 per square centimeter) 6 The availability of low-dislocation GaN substrates (with a median defect density of dislocations) and advances in metalorganic chemical vapor deposition (MOCVD) techniques have led to significant (>80%) improvements.6 As the transition is further reduced, the IQE will improve.
[0005] C-plane III-nitride devices with significantly improved EQE and output power have been reported using surface roughening methods such as the use of patterned sapphire substrates (PSS) and photoelectrochemical (PEC) etching techniques. Furthermore, the roughened devices demonstrate better performance by having improved output power after packaging compared to conventional devices, mainly due to the dramatic enhancement of photon extraction from the backside of the substrate.
[0006] The effectiveness of this patterning technique generally depends on the crystal orientation and polarity of the surface to be patterned. So far, it has been established only for the nitrogen-polar faces of c-polar 0001 GaN [Appl. Phys. Lett. 84, 855 (2004)], but not for any GaN crystal orientation and polarity, including most semipolar surfaces, nonpolar a-plane, and m-plane surfaces.
[0007] Reactive ion etching (RIE) is another technique for patterning conical features and improving light extraction, regardless of crystal orientation [Applied Physics Express 9, 102102 (2016) (Non-Patent Document 2)].
[0008] The advantage of surface roughening is that there are many available methods to generate randomly roughened surfaces. However, the random nature of photon dynamics does not allow for much control over beam shaping. The use of microlens arrays or PhC arrays with regular periodic structures not only improves light outcoupling, but also provides the ability to tailor the angular intensity distribution.
[0009] Improving the directionality of light emission has been widely investigated, either through the use of microcavities or PhCs. A very promising application of PhC structures is their use to control the propagation of electromagnetic modes in optoelectronic devices. The periodic modulation of the refraction acts as an optical diffraction grating to couple guided modes from the semiconductor device to the air, thus increasing the extraction efficiency and directionality of the LED. The application of gratings for light diffraction in optoelectronic devices requires that the period of the grating is about half the wavelength of the light generated by the device. For GaN-based optoelectronic devices, the period of the grating needs to be about a few hundred nanometers.
[0010] The main difficulty with PhC LEDs is their required precision fabrication. The main challenge in fabricating PhC LEDs is the need to define PhC patterns with their features on the wavelength scale, i.e., hole radii of 100-1,000 nm for the visible spectrum. Commonly used lithography techniques, such as contact lithography, are either limited by the diffraction limit to feature sizes of about 1 μm, or are prohibitively expensive, such as deep UV lithography.
[0011] At the research and development level, electron beam lithography is widely used to define the PhC pattern in a suitable resist. After the resist is developed, it serves as an etching mask to transfer the pattern into the semiconductor. Although electron beam lithography can fabricate feature sizes down to 20 nm with arbitrary patterns, it is not applicable to mass production due to its extremely low throughput.
[0012] A very promising patterning technique is the nanoimprint technique. First, a stamp with an inverse pattern, known as the master, is fabricated. By pressure or capillary forces, the pattern is printed into the resist already cast on the LED surface. After heating and / or UV curing, the stamp is removed and the resist can serve as an etching mask. This patterning process can be done on a wafer scale, thus resulting in high throughput. It is not very flexible, since the master needs to be fabricated first by conventional techniques similar to electron beam lithography, however, any pattern with feature sizes of about 10-20 nm can be printed.
[0013] Thus, there is a need in the art for improved light control features for LEDs.The present invention satisfies that need. [Prior art documents] [Non-patent literature]
[0014] [Non-Patent Document 1] Appl. Phys. Lett. 84, 855 (2004) [Non-Patent Document 2] Applied Physics Express 9,102102(2016) Summary of the Invention [Means for solving the problem]
[0015] The present invention focuses on providing light emitting devices with reduced defect densities that have integrated light control features for extracting, directing, reflecting, refracting, concentrating, or defocusing light emitted from the device. The present invention epitaxially integrates the light control features directly onto the epitaxial layers of the device.
[0016] The method described in this application is different from conventional PhC fabrication. In the present invention, direct etching on semiconductor layers, including active layers, is avoided for PhC fabrication. The present invention also allows the selection of either random rough surfaces or tailored two-dimensional (2D) triangular periodic space lattices for PhC without exposing the device to physical etching methods such as light-emitting reactive ion, plasma, or capacitively coupled etching. The approach described in this invention mitigates possible etch-related damage to quantum wells (QWs) since the patterning is epitaxially formed at an early stage of device layer growth. In addition, the IQE of the device is improved since the epitaxial layers are defect filtered through selective area growth (SAG), also referred to as epitaxial lateral overgrowth (ELO).
[0017] The present invention is applicable to the fabrication of LEDs ranging from macro to micro sizes. 2 for macro-sized LED applications (having a size of about 1 μm 2 The LEDs may be modified for micro-sized LED applications (having a size of 100 nm).
[0018] For example, next-generation displays such as micron-sized LED displays have been intensively researched for their advantages of high wall plug efficiency (WPE) and wide color gamut compared to traditional liquid crystal display (LCD) and organic LED (OLED) displays. However, there are some issues with traditional micron-thick micro LEDs, such as color mixing, color purity, temperature, and color stability.
[0019] To solve these problems, III-nitride-based blue, green, and red PhC cavity microLEDs (PhC cavity μLEDs) with single-mode emission have attracted more attention as potential alternatives. The advantages of PhC cavity μLEDs are spectral purity and thermal stability, since the spectral width and shape are determined by the overlap of the cavity mode with the InGaN QW emission. Another advantage is that the emission of PhC cavity μLEDs is more directional than conventional LEDs. These advantages suggest that PhC cavity μLEDs may be the best fit for display applications.
[0020] Displays based on arrays of μLEDs are also a promising technology for a wide range of applications. In these 2D arrays, each μLED acts as a single pixel of the overall image. These μLED displays can be used in applications ranging from TVs, laptops, smartphones, heads-up displays (HUDs), and augmented / virtual / mixed reality (AR / VR / MR) applications. In these applications, directionality plays a major role, as cross-correlation of light can degrade photographic quality.
[0021] The present invention proposes the use of ELO technique to obtain defect filtered crystalline quality (no visible defects). Light emitting regions are defined on the wings of the ELO region to ensure reduced defect area. Light control features are deployed in the early stages of ELO by shaping either the growth limiting mask or the host substrate to ensure no physical damage to the performance of the QW region or device layers.
[0022] The invention begins by shaping the desired features on a growth limiting mask that is deposited on a substrate and allowing a first ELO layer to epitaxially take on the shape of the desired features, the first ELO layer typically serving as the n-type layer for the device. The invention can be realized using a homogenous host substrate, as well as the material of the device layers, or a substrate with a III-nitride template, such as an ELO III-nitride template, including sapphire, Si, SiC, SiN, Ga 2 O 3 , LiAlO 2 Such a method can be achieved using a foreign substrate such as a host substrate, a semiconductor substrate, or a semiconductor memory device. Alternatively, the desired features can be formed on the host substrate prior to depositing the ELO mask. In this scenario, when reusing the host substrate, the feature formation step can be avoided since the features will remain intact upon removal of the device layers from the host substrate.
[0023] The present invention relates to a compound having the formula Ga x Al y In z The present invention focuses on the use of the III-nitride material system, including the alloy composition of InGaN, where 0≦x≦1, 0≦y≦1, 0≦z≦1, and x+y+z=1. The majority of current research attention is focused on InGaN-based LEDs, although some work also exists on AlGaN LEDs emitting in the UV-A wavelengths. As a result, the present invention focuses on InGaN LEDs, but most of the techniques described herein should be applicable to AlGaN LEDs as well.
[0024] Since the bandgaps of GaN and InN are 3.4 eV and 0.7 eV, respectively, and alloys in the InGaN material system can theoretically cover the entire visible spectrum, one of the most important advantages of the InGaN material system is the ability to tune the emission wavelength by varying the compositional ratio of indium and gallium in the active region.
[0025] In addition, current InGaN materials, especially for display applications, are grown on sapphire or silicon (Si) substrates using MOCVD. Depending on the reactor dimensions, the wafer diameter can be scaled from 2 inches to 6 inches for sapphire substrates and up to 18 inches for Si substrates, making this scalability ideal for mass production with low material costs.
[0026] The inventive approach uses the ELO technique, which in principle can be adapted to any of the substrates mentioned above, so scalability is not an issue in applying the inventive technique. In addition, the light-emitting area of the device includes the wing regions of the ELO layer, which are known for better crystal quality compared to growing the device layers directly on the substrate or their template. Thus, increased efficiency will be possible by following the inventive approach.
[0027] Conventional LEDs (larger than 300 μm on at least one side) usually have a large light-emitting area at the top of the device to reduce the carrier concentration in the active region and to avoid the effect of efficiency droop. Due to this large light-emitting area, non-radiative centers such as crystal defects may not play a major role in the device operation. However, when the light-emitting area is about 100 μm×100 μm to 10 μm×10 μm or smaller, defects present in the active region may significantly degrade the performance. The present invention solves these problems and provides better crystal quality and improved efficiency, even on homogeneous substrates.
[0028] To overcome the limitations in the prior art as described above, as well as other limitations that will become apparent upon reading and understanding of this specification, the present invention discloses a method of fabricating light control features, such as inducing or extracting features epitaxially on a device layer by patterning a growth-limiting mask that is deposited on a host substrate, which can be a III-nitride substrate, a foreign substrate, or a III-nitride template deposited on a foreign substrate.
[0029] Specifically, the present invention implements the following steps: an island-shaped III-nitride semiconductor layer is grown on a substrate using a pre-patterned growth-limiting mask and an ELO method, where the pattern on the growth-limiting mask provides the desired light control characteristics; a III-nitride ELO layer is grown on the substrate and then over the growth-limiting mask; fabrication of device layers on the III-nitride ELO layer is performed on the wings of the III-nitride ELO layer, which have good crystal quality in terms of dislocation density and stacking faults; the light-emitting aperture is at least partially confined to the wings of the III-nitride ELO layer, and therefore a good crystal quality layer can be guaranteed.
[0030] Front-end fabrication such as mesa formation and pad and n-pad processing are performed on the wings of the III-nitride ELO layer, and then the device units are picked from the host substrate and placed on a carrier or submount. The devices can be removed from the substrate by an elastomeric stamp, or a vacuum chuck, or adhesive tape, or simply by bonding or attaching them to a separate carrier or submount.
[0031] Important aspects of the present invention include the following: Light extraction and / or directionality is controlled. The light control features are placed behind the III-nitride ELO layer, so that the p-side of the device other than from the light control features does not need to be as thick as is the case with many existing devices. · The roughening or periodic patterning on the device layer is performed without the use of chemical etchants. · Surface roughening or periodic patterning on the device layer is performed without the use of physical etching. Patterning features on the epitaxial layers, especially on the n-GaN side of the device, avoids the need for a thick p-GaN layer, which is generally resistive and any physical etching for the light control features would damage the device layers. The low defect density epitaxial layer improves the electrical conductivity of the subsequent p-GaN epitaxial layer grown on top of it. Patterning of features close to the active area, for example within a vicinity of less than 25 μm, is performed substantially without involving the host substrate. Light control features are formed on the wings of the III-nitride ELO layer prior to growth of the active region of the device. The present invention fabricates the light emitting area on the wings of III-nitride ELO layers, thereby providing better crystal quality in the light emitting area, which improves performance. The present invention relates to a substrate with a template, such as a III-nitride template, including sapphire, Si, SiC, SiN, Ga 2 O 3 , LiAlO 2 Foreign substrates such as GaN, ... and GaN may be utilized to expand manufacturability to industrial needs. · The present invention can be utilized to increase yields by making smaller footprint devices that are constrained to the wings of III-nitride ELO layers. The substrate can be reused for processing the next batch of devices after the III-nitride ELO layer and device layers have been removed. The method is independent of the crystal orientation of the substrate. Light control features can also be processed on the host substrate and then deposition of the ELO mask can be performed.
[0032] Several possible designs using this method are illustrated in the detailed description of the invention below. The present invention, when combined with the cross-referenced invention relating to removing semiconductor devices from semiconductor substrates described above, has many advantages over conventionally manufacturable device elements. [Brief description of the drawings]
[0033] Reference is now made to the drawings in which like reference numbers represent corresponding parts throughout.
[0034] [Figure 1A] 1(a) and 1(b) are schematic illustrations of a substrate, a growth-limiting mask, and different possible designs for the growth-limiting mask according to an embodiment of the present invention. [Figure 1B] 1(a) and 1(b) are schematic illustrations of a substrate, a growth-limiting mask, and different possible designs for the growth-limiting mask according to an embodiment of the present invention.
[0035] [Figure 1C] 1(c) and 1(d) are schematic diagrams of III-nitride ELO and device layers grown from patterned growth-limiting masks according to embodiments of the present invention. [Figure 1D] 1(c) and 1(d) are schematic diagrams of III-nitride ELO and device layers grown from patterned growth-limiting masks according to embodiments of the present invention.
[0036] [Figure 2A] FIG. 2(a) is a step-by-step illustration of fabricating a PhC pattern on a growth-limiting mask for subsequent growth of a III-nitride ELO layer according to an embodiment of the present invention.
[0037] [Figure 2B] FIG. 2(b) is a microscope image of the colloid used to pattern the growth-limiting mask.
[0038] [Figure 2C]FIG. 2(c) shows an atomic force microscope (AFM) scan and two panchromatic cathodoluminescence (CL) microscope images of the ELO III-nitride layer when a planar growth-limiting mask without any colloidal pattern is used.
[0039] [Figure 2D] FIG. 2(d) shows an AFM scan and two panchromatic CL microscope images of the ELO III-nitride layer when a growth-limiting mask with a colloidal pattern is used.
[0040] [Figure 2E] FIG. 2(e) shows a scanning electron microscope (SEM) image and AFM scan of the growth-limiting mask with colloidal patterns.
[0041] [Figure 2F] FIG. 2( f ) shows a microscope image of an ELO III-nitride layer grown on the growth-limiting mask with the colloidal pattern, an SEM image of a portion of the ELO III-nitride layer, and an AFM scan of a portion of the ELO III-nitride layer.
[0042] [Figure 2G] FIG. 2(g) shows an SEM image and AFM scan of a planar growth restriction mask without a colloidal pattern.
[0043] [Figure 2H] FIG. 2(h) shows a microscope image of an ELO III-nitride layer grown on a planar growth-limiting mask, an SEM image of a portion of the ELO III-nitride layer, and an AFM scan of a portion of the ELO III-nitride layer.
[0044] [Figure 2I] Figure 2(i) is a collection of microscope, SEM, and AFM images of the front and back sides of III-nitride ELO layers for planar and patterned growth-limiting masks when different colloid sizes are used to generate the patterns.
[0045] [Figure 3A] 3(a), 3(b), and 3(c) are schematic diagrams of macro-sized LED vertical pad configurations according to embodiments of the present invention. [Figure 3B] 3(a), 3(b), and 3(c) are schematic diagrams of macro-sized LED vertical pad configurations according to embodiments of the present invention. [Figure 3C] 3(a), 3(b), and 3(c) are schematic diagrams of macro-sized LED vertical pad configurations according to embodiments of the present invention.
[0046] [Figure 3D] 3(c), 3(d), and 3(e) are schematic diagrams of macro-sized LED side pad configurations according to embodiments of the present invention. [Figure 3E] 3(c), 3(d), and 3(e) are schematic diagrams of macro-sized LED side pad configurations according to embodiments of the present invention. [Figure 3F] No description available.
[0047] [Figure 4A] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4B] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4C] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4D]4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4E] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4F] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4G] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4H] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4I] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention. [Figure 4J] 4(a), 4(b), 4(c), 4(d), 4(e), 4(f), 4(g), 4(h), 4(i), and 4(j) illustrate the fabrication of micro-sized LEDs with PhC for display applications according to an embodiment of the present invention.
[0048] [Figure 5A]5(a) and 5(b) are schematic diagrams illustrating structures used to maximize vertical light extraction in a PhC LED according to an embodiment of the present invention. [Figure 5B] 5(a) and 5(b) are schematic diagrams illustrating structures used to maximize vertical light extraction in a PhC LED according to an embodiment of the present invention.
[0049] [Figure 6A] 6(a) and 6(b) are schematic diagrams illustrating light extraction features epitaxially integrated on the n-side of an LED according to an embodiment of the present invention. [Figure 6B] 6(a) and 6(b) are schematic diagrams illustrating light extraction features epitaxially integrated on the n-side of an LED according to an embodiment of the present invention.
[0050] [Figure 7A] 7(a) and 7(b) are schematic diagrams illustrating light extraction features epitaxially integrated on the n-side of an LED according to an embodiment of the present invention. [Figure 7B] 7(a) and 7(b) are schematic diagrams illustrating light extraction features epitaxially integrated on the n-side of an LED according to an embodiment of the present invention.
[0051] [Figure 8] FIG. 8 is a flow chart of a process for realizing a light-emitting device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0052] In the following description of the preferred embodiment, reference is made to specific embodiments in which the present invention may be practiced. It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.
[0053] (overview) This invention describes a method to fabricate semiconductor devices such as LEDs by designing the growth restriction mask accordingly. Using ELO, the invention can grow homogeneous substrates such as GaN, or sapphire, Si, SiC, SiN, Ga 2 O 3 , LiAlO 2 The method can be easily applied to foreign substrates such as GaN, ...
[0054] 1(a) illustrates an embodiment of the present invention, which includes providing a III-nitride based host substrate 101, such as a bulk GaN substrate 101, and then a growth-limiting mask 102 is formed on the substrate 101. Specifically, the growth-limiting mask 102 is placed in direct contact with the substrate 101, or it is placed indirectly through an intermediate layer grown, such as by MOCVD, which is a template made of III-nitride based semiconductor deposited on the substrate 101. The present invention uses SiO 2 as the growth-limiting mask 102. 2 , SiN, SiON, TiN, etc., can be used, but are not limited to these materials.
[0055] A growth-limiting mask 102 is deposited over a host substrate 101 and etched to form an opening area 103, the remaining portion of the growth-limiting mask 102 including a nanometer-scale pattern, the opening area 103 having a width x and separating the remaining portion of the growth-limiting mask 102 with a nanometer-scale pattern having a width y.
[0056] Photomask lithography and etching can be performed to create the open areas 103 as well as non-grown regions (not shown). Alternatively, plasma-enhanced chemical vapor deposition (CVD), sputtering, ion beam deposition (IBD), etc. can also be used.
[0057] Nanometer-scale patterns can be formed on the growth-constraining mask 102 using a technique called colloidal lithography [J. Vac. Sci. Technol., B35, 011201 (2017)]. Alternatively, nanoimprinting, electron beam lithography, holography, interference lithography, etc. can be used.
[0058] Two designs for the growth restriction mask 102 are proposed in FIG. 1(b), namely, a hybrid mask 102A or a patterned mask 102B, where the hybrid mask 102A is a combination of smooth regions 104A and patterned regions 104B, and the patterned mask 102B consists of patterned regions 104B without smooth regions 104A.
[0059] 1(c) further illustrates the embodiment of FIG. 1(a) where an epitaxial III-nitride layer 105, such as an n-type GaN-based layer 105, is grown by ELO on the GaN substrate 101 and the growth limiting mask 102. Growth of the ELO III-nitride layer 105 occurs first in the open areas 103 on the GaN-based substrate 101 and then laterally from the open areas 103 over the growth limiting mask 102.
[0060] In one embodiment, the growth of ELO III-nitride layer 105 is stopped or interrupted before the ELO III-nitride layer 105 in adjacent opening areas 103 can coalesce on top of growth limiting mask 102, resulting in non-growth regions 106. In another embodiment, the growth of ELO III-nitride layer 105 in adjacent opening areas 103 coalesces on top of growth limiting mask 102.
[0061] Additional III-nitride semiconductor device 107 layers are deposited on or above the ELO III-nitride layer 105 and may include an active region, a p-type layer, an electron blocking layer (EBL), and cladding layers, and other layers. This results in the device 107 being shaped as a rod.
[0062] When ELO methods are used, defects can be filtered out. An illustration of a dislocation is also shown in FIG. 1(c), where a defect 108 in the growth of ELO III-nitride layer 105 from opening area 103 originates from host substrate 101, but wing regions in ELO III-nitride layer 105 on either side of defect 108 are visually defect-free.
[0063] The light emitting regions of the elements 107 are processed on both sides of the open region 109, preferably between the aperture area 103 and the non-grown region 106. By doing so, each bar of elements 107 will possess an array of twin or identical light emitting apertures (not shown) on either side of the open region 109 along the length of the bar. Alternatively, the open region 109 may be etched to produce separate elements 107 along the bar, each of the elements 107 possessing one or more light emitting apertures (not shown) on either side of the open region 109 along the length of the bar.
[0064] III-nitride elements 107 may be separated from host substrate 101 by etching regions 110 between adjacent bars to expose at least growth limiting mask 102. Regions 110 may be etched to separate the bars of element 107 from adjacent bars of element 107.
[0065] Furthermore, the present invention proposes several approaches to realize light control features for the light emitting element 107. Exemplary fabrication steps related to the present invention are described in further detail below.
[0066] Step 1: Start by forming the desired shape on the growth limiting mask 102, which can be achieved by: Placing the growth limiting mask 102 on the host substrate 101. The growth limiting mask 102 is patterned using nanoimprint lithography, or the desired shape can be transferred onto the growth limiting mask 102 using photolithography + wet etching, or photolithography + dry etching, or colloidal lithography.
[0067] Step 2: A plurality of stripe-shaped opening areas 103 are opened on the substrate 101, the substrate 101 being a group III nitride semiconductor, or the substrate 101 being sapphire, Si, SiC, SiN, Ga 2 O 3 , LiAlO 2 or the substrate 101 comprises a template that has been prepared using a growth-limiting mask 102.
[0068] Step 3: Multiple ELO III-nitride layers 105 are grown on the substrate 101 using the growth-limiting mask 102 such that the growth extends in a direction parallel to the stripe-shaped opening areas 103 of the growth-limiting mask 102. The ELO III-nitride layers 105 take the shape (not shown) of a pattern designed on the growth-limiting mask 102, and the designed pattern is transferred to the interface between the ELO III-nitride layers 105 and the growth-limiting mask 102.
[0069] Step 4: Light emitting devices 107, such as LEDs, are fabricated by conventional lithography methods on the wing regions of the ELO III-nitride layer 105 that are primarily covered by the flat surface regions.
[0070] Step 5: The devices 107 are separated and isolated on the host substrate 101.
[0071] Step 6: The submount is attached to the element 107.
[0072] Step 7: The growth limiting mask 102 and any protective layers used are dissolved using a chemical etchant such as hydrofluoric acid (HF) or buffered hydrofluoric acid (BHF).
[0073] Step 8: The device 107 is separated from the host substrate 101.
[0074] Step 9: The resulting device 107 is packaged.
[0075] (Forming a growth restriction mask) In one embodiment, a III-nitride layer 105, which may be a GaN-based layer, is grown by ELO on a III-nitride substrate 101, such as an m-plane GaN substrate 101, and a SiO 2 , and the ELO III-nitride layer 105 may or may not coalesce on top of the growth-limiting mask 102 .
[0076] The growth limiting mask 102 is made up of stripe-shaped opening areas 103 with a width x, and the SiO 2 The stripes have a width y of 1-20 μm and a spacing of 10-100 μm. If a non-polar substrate 101 is used, the open area 103 is <0001> The aperture areas 103 are oriented along the [-1014] or
[1014] axis, respectively, if a semi-polar (20-21) or (20-2-1) substrate 101 is used. Other surfaces with aperture areas 103 oriented in other directions may be used as well.
[0077] When using III-nitride substrate 101, the present invention can obtain a high quality ELO III-nitride layer 105. As a result, the present invention can also facilitate obtaining a device 107 with reduced defect density, such as reduced dislocations and stacking faults.
[0078] Furthermore, these techniques can be used on any substrate, including sapphire, Si, SiC, SiN, Ga, etc., as long as they allow for growth of the ELO III-nitride layer 105 through the growth limiting mask 102. 2 O 3 , LiAlO 2 It can be used together with the hetero substrate 101 such as the above.
[0079] (Pattern growth restriction mask) Before etching the opening areas 103 onto the growth-limiting mask 102, pre-processing is performed on the growth-limiting mask 102 to form one or more desired patterns of light control features for light extraction or controllability.
[0080] 1(d) illustrates one embodiment that may be used with two different designed patterns, although other designed patterns may be used as well. In this embodiment, a first designed pattern is defined to improve light extraction from the macro LED, and a second designed pattern is defined to improve the directionality of the emitted light using a photonic crystal (PhC) cavity.
[0081] In both cases, the element 107 includes both an n-side surface 111 and a p-side surface 112, and the designed pattern 113 is fabricated on the n-side surface 111, which is the light-emitting surface. Fabrication of the element 107 is performed on the p-side surface 112, and includes deposition of an n-pad 114 and a p-pad 115.
[0082] (Growing epitaxial layers onto a substrate using a growth limiting mask) The III-nitride semiconductor device 107 layers are grown on or above the ELO III-nitride layer 105 in the planar surface areas on the wings of the ELO III-nitride layer 105. In one embodiment, conventional methods are used for epitaxial growth of the III-nitride semiconductor device 107 layers, such as MOCVD. In one embodiment, the III-nitride semiconductor device 107 layers are separated from each other because the MOCVD growth of the ELO III-nitride layer 105 is stopped before adjacent ones of the ELO III-nitride layers 105 can coalesce. In another embodiment, the ELO III-nitride layers 105 are made to coalesce and a post etch is performed to remove the unwanted regions 110.
[0083] Trimethylgallium (TMGa), trimethylindium (TMIn), and triethylaluminum (TMAl) are used as III-element sources. Ammonia (NH3 ) is used as raw gas to supply nitrogen. Hydrogen (H 2 ) and nitrogen (N 2 ) is used as a carrier gas for the III-element source. It is important to include hydrogen in the carrier gas to obtain a smooth surface epilayer.
[0084] Salts and bis(cyclopentadienyl)magnesium (Cp 2 Mg) are used as n-type and p-type dopants. Pressure settings are typically 50-760 Torr. III-nitride based semiconductor layers are generally grown at temperatures ranging from 700-1,250°C.
[0085] For example, the growth parameters include: TMG at 12 sccm, NH 3 is 8 slm, the carrier gas is 3 slm, and SiH 4 is 1.0 sccm, and the V / III ratio is about 7,700.
[0086] (ELO of Limited Area Epitaxy (LAE) III-Nitride Layers) In the prior art, some pyramidal hillocks have been observed on the surface of m-plane III-nitride films following growth (see, for example, U.S. Patent Application Publication No. 2017 / 0092810). In addition, wavy surfaces and recessed areas appear on the growth surface, which aggravates the surface roughness. This is a very serious problem. For example, some papers have shown that a smooth surface can be achieved by controlling the deviation angle (>1 degree) of the growth surface of the substrate, and by controlling the N 2By using carrier gas conditions, it can be obtained. However, these are very restrictive conditions for mass production due to high production costs. Furthermore, GaN substrates have a large deviation angle variation with respect to their origin from their fabrication method. For example, if a substrate has a large deviation angle distribution in-plane, it will have different surface morphology at these points within the wafer. In this case, the yield is reduced by the large deviation angle distribution in-plane. Therefore, it is necessary that the technique does not depend on the deviation angle distribution in-plane.
[0087] The present invention, as described below, solves these problems. 1. The growth area is limited by the area of the growth limiting mask 102 from the edge of the substrate 101. 2. The substrate 101 is a non-polar or semi-polar III-nitride substrate 101 with a tilt orientation ranging from -16 degrees to +30 degrees from the m-plane towards the c-plane and the C-plane. Alternatively, the substrate 101 is a heterosubstrate on which a III-nitride based semiconductor layer is deposited with a tilt orientation ranging from +16 degrees to -30 degrees from the m-plane towards the c-plane. 3. The rod of element 107 has a long side perpendicular to the a-axis of the Group III nitride semiconductor crystal. 4. During MOCVD growth, a hydrogen atmosphere can be used.
[0088] In the present invention, a hydrogen atmosphere can be used during non-polar and semi-polar growth. Using this condition is preferred because hydrogen can prevent excessive growth at the edges of the open areas 103 from occurring in the initial growth stages.
[0089] These results have been obtained under the following growth conditions:
[0090] In one embodiment, the growth pressure ranges from 60 to 760 Torr, but preferably the growth pressure ranges from 100 to 300 Torr to obtain a wide width for the island-shaped III-nitride semiconductor layer; the growth temperature ranges from 900 to 1,200° C.; the V / III ratio ranges from 10 to 30,000; TMG is 2 to 20 sccm; NH 3 ranges from 0.1 to 10 slm; the carrier gas is hydrogen gas only or both hydrogen and nitrogen gas. To obtain a smooth surface, the growth conditions for each facet need to be optimized by conventional methods.
[0091] After growth for about 2-8 hours, the ELO III-nitride layer 105 had a thickness of about 1-50 μm and a bar width of about 50-150 μm.
[0092] (Making elements) The elements 107 are fabricated in the flat surface areas on the wings of the ELO III-nitride layer 105 by conventional methods, and various element 107 designs are possible. For example, only front-end processing such as p-pads and n-pads may be required to realize the LEDs, which can be performed along either the length or width of the wings of the ELO III-nitride layer 105. Alternatively, the interface can be used as an n-pad 114 by partially depositing metal over the top of the pattern 113, or by creating space for the n-pad 114 through the use of a hybrid mask 102A.
[0093] (Forming a structure for separating element units) The purpose of this step is to isolate the ELO III-nitride layer 105 and III-nitride semiconductor device 107 layers from the host substrate 101. At least two methods can be used to transfer the device 107 onto a carrier or submount. In one method, the ELO III-nitride layer 105 and III-nitride semiconductor device 107 layers are separated from the host substrate 101 by etching the open areas 109 and the areas 110 between adjacent rods using a selective etching mask to expose at least the growth limiting mask 102. The separation of the layers 105, 107 can also be performed, for example, via scoring lines with a diamond-tipped or laser scriber, or using tools such as RIE or ICP (inductively coupled plasma) etching, but is not limited to these methods, and other methods can also be used to isolate the device 107.
[0094] The method described in [Srinivas Gandrothula et al., 2020 Appl. Phys. Express, 13, 041003] may be used, or alternatively, a support carrier such as a submount may be used to lift off the fabricated element 107 from the host substrate 101.
[0095] (Definition of terms) III-nitride substrates The III-nitride substrate 101 may comprise any type of III-nitride substrate 101, so long as it allows for the growth of III-nitride semiconductor layers through the growth-limiting mask 102. This includes any GaN substrate 101 sliced from bulk GaN on the {0001}, {11-22}, {1-100}, {20-21}, {20-2-1}, {10-11}, {10-1-1} plane, etc., or other planes, and AlN crystalline substrates.
[0096] Hetero Substrate Furthermore, the present invention also relates to sapphire, Si, SiC, SiN, Ga 2 O 3 , LiAlO2 A hetero-substrate 101 such as a GaN or III-nitride based semiconductor layer can be used. For example, a GaN template or other III-nitride based semiconductor layer can be grown on the hetero-substrate 101 prior to deposition of the growth-limiting mask 102. The GaN template or other III-nitride based semiconductor layer is typically grown on the hetero-substrate 101 to a thickness of about 2-6 μm, and then the growth-limiting mask 102 is placed on the GaN template or other III-nitride based semiconductor layer.
[0097] Growth restriction mask The growth limiting mask 102 is SiO 2 , SiN, SiON, Al 2 O 3 , AlN, AlON, MgF, ZrO 2 , TiN, or other dielectric layers, or refractory or noble metals, such as W, Mo, Ta, Nb, Rh, Ir, Ru, Os, Pt, etc. The growth limiting mask 102 can be a layered structure selected from the above materials. It can also be a multi-stacking layer structure selected from the above materials.
[0098] In one embodiment, the thickness of the growth limiting mask 102 is about 0.05 to 3 μm. The width of the growth limiting mask 102 is preferably greater than 5 μm, and more preferably, the width is greater than 10 μm. The growth limiting mask 102 can be deposited by, but is not limited to, sputtering, e-beam evaporation, plasma enhanced chemical vapor deposition (PECVD), ion beam deposition (IBD), and the like.
[0099] On the m-plane freestanding GaN substrate 101, the growth limiting mask 102 comprises a plurality of opening areas 103, which are arranged in a first direction parallel to the 11-20 direction of the substrate 101 and in a second direction parallel to the 0001 direction of the substrate 101, periodically with intervals extending in the second direction. The length of the opening areas 103 is, for example, 200 to 35,000 μm, the width is, for example, 2 to 180 μm, and the spacing between the opening areas 103 is, for example, 20 to 180 μm. The width of the opening areas 103 is typically constant in the second direction, but may be varied in the second direction as necessary.
[0100] On the c-plane freestanding GaN substrate 101 , the open areas 103 are disposed in a first direction parallel to the 11-20 direction of the substrate 101 and in a second direction parallel to the 1-100 direction of the substrate 101 .
[0101] On a semi-polar (20-21) or (20-2-1) GaN substrate 101, the open areas 103 are oriented parallel to [-1014] and [10-14], respectively.
[0102] Alternatively, a heterosubstrate 101 can be used. When a c-plane GaN template is grown on a c-plane sapphire substrate 101, the open area 103 is in the same direction as the c-plane GaN template.
[0103] When the m-plane GaN template is grown on the m-plane sapphire substrate 101, the open area 103 is in the same direction as the m-plane GaN substrate. By doing this, the m-plane cleavage plane can be used to split the bar 107 of the element using the c-plane GaN template, and the c-plane cleavage plane can be used to split the bar of the element 107 using the m-plane GaN template, which is preferred.
[0104] Group III nitride semiconductor layer The ELO III-nitride layer 105 and III-nitride semiconductor device 107 layers may contain In, Al, and / or B as well as other impurities such as Mg, Si, Zn, O, C, H, and the like.
[0105] The III-nitride semiconductor device 107 layer generally comprises three or more layers including at least one of an n-type layer, an undoped layer, and a p-type layer. The III-nitride semiconductor device 107 layer specifically comprises a GaN layer, an AlGaN layer, an AlGaInN layer, an InGaN layer, etc. When the device 107 has multiple III-nitride semiconductor device 107 layers, the distance between adjacent III-nitride semiconductor device 107 layers is generally 30 μm or less, preferably 1 μm or less, but is not limited to these figures. Several electrodes are arranged at predetermined positions according to the type of the semiconductor device 107.
[0106] Semiconductor Device The semiconductor element 107 may be, for example, but is not limited to, a Schottky diode, a light emitting diode, a semiconductor laser, a photodiode, a transistor, etc. The present invention is particularly useful for micro LEDs and VCSELs. The present invention is particularly useful for semiconductor lasers that require a smooth area for cavity formation.
[0107] Alternative Embodiments The following describes alternative embodiments of the present invention.
[0108] (First embodiment) A first embodiment includes a III-nitride based LED with light control features that include attached patterns for light extraction and / or directing, and a method of manufacturing the LED. This embodiment is illustrated in Figures 1(a), 1(b), 1(c), and 1(d).
[0109] A host substrate 101 is provided, and a growth-limiting mask 102 having a plurality of stripe-shaped opening areas 103 is formed on the substrate 101 .
[0110] In this embodiment, the growth-limiting mask 102 is patterned to include structures corresponding to emission wavelengths such as PhC for better light extraction. Alternatively, the same structures can be fabricated on the host substrate 101, and then the growth-limiting mask 102 is placed over the fabricated structures and takes the shape of the structures.
[0111] For proof of concept, feasibility experiments were performed to transfer a pattern onto the interface between the growth-limiting mask 102 and the III-nitride ELO layer 105. Specifically, either a hybrid mask 102A or a patterned mask 102B can be used.
[0112] FIG. 2(a) illustrates the steps performed in the feasibility experiment. A GaN-on-sapphire substrate 101 with a c-plane GaN template was used for this study. As shown in step 1, PhC patterns are deposited on the host substrate 101 using silica colloids 201 as described in [J.Vac.Sci.Technol.,B35,011201 (2017)]. The average diameter size of the colloids 201 is about 500 nm. A microscope image of the colloids 201 with an average diameter of 420 nm is shown in FIG. 2(b). Then, a 500 nm thick SiO 2 with a growth limiting mask 102 is deposited on the host substrate 101 as shown in step 2. 2 The layers were deposited using PECVD.
[0113] Two mask patterns were demonstrated to distinguish the differences: one was a planar growth-limiting mask 102 without any colloidal pattern, and the other was a growth-limiting mask 102 with the colloidal pattern described above.
[0114] 2(c) shows an AFM image and two panchromatic CL microscope images (30 kV, 1.6 nA) of the ELO III-nitride layer 105 when a planar growth-limiting mask 102 without any colloidal pattern is used. The CL microscope image (I) shows the open areas 109 and wings of the ELO III-nitride layer 105, the AFM image is a portion of the CL microscope image (I), and the CL microscope image (II) shows defects in the open areas 109 with no defects present in the wings of the ELO III-nitride layer 105.
[0115] 2(d) shows an AFM image and two panchromatic CL microscope images of the ELO III-nitride layer 105, where a growth-limiting mask 102 with a colloidal pattern was used. The CL microscope image (III) shows the open areas 109 and wings of the ELO III-nitride layer 105, the AFM image is a portion of the CL microscope image (III), and the CL microscope image (IV) shows defects in the open areas 109 with no defects present in the wings of the ELO III-nitride layer 105.
[0116] FIG. 2(e) shows an AFM scan of the growth limiting mask 102 with the colloidal pattern.
[0117] FIG. 2( f ) shows a microscope image of the ELO III-nitride layer 105 grown on the growth-limiting mask 102 with the colloidal pattern and an AFM scan of a portion of the ELO III-nitride layer 105 .
[0118] In the AFM scans of Figures 2(e) and 2(f), the PhC patterns defined by the colloids have a triangular spatial lattice structure with sizes within the subwavelength range of the desired visible region (400 nm to 700 nm).
[0119] Next, as shown in step 3 of Figure 2(a), parallel stripes are formed by etching the growth-limiting mask 102 and colloids 201 with open areas 103. A III-nitride ELO layer 105 is then grown using MOCVD and allowed to extend into the patterned growth-limiting mask 102, followed by III-nitride based semiconductor device 107 layers such as MQWs 202, as shown in step 4 of Figure 2(a).
[0120] The experimental demonstration of step 4 can be seen in Figures 2(c) and 2(d), where images (I) and (III) are epilayers grown on planar and patterned growth-limiting masks 102, respectively. Illustrations of open windows and wings are also depicted on the epilayers for better understanding. An AFM scan of the top surface morphology is shown in the side window.
[0121] Panchromatic CL measurements revealed that threading dislocations (TDs) on the epitaxial layer are shown in images (II) and (IV) for the planar growth-limiting mask 102 and the patterned growth-limiting mask 102, respectively. As can be seen, all dislocations (defects) appear along the open windows of the epitaxial layer 105, and no visible defects are identified on the wings in both cases, which indicates a better crystal quality for the wings.
[0122] Therefore, when devices 107 are fabricated on these wings, their IQE will be improved, thereby improving the lifetime of devices 107. As above, the low defect density crystalline layer also helps in maintaining the spectral purity of devices 107 when high carrier injection is introduced. In general, the spread of their emission wavelength, called the full width at half maximum (FWHM), will not increase, as is found in conventional devices fabricated on planar substrates.
[0123] As can be seen in Figures 2(c) and 2(d), for images (II) and (IV), despite the presence of a PhC pattern underneath the ELO III-nitride layer 105, the quality of the wings in terms of dislocations and surface morphology is similar to the ELO III-nitride 105 grown on the unpatterned growth limiting mask 102.
[0124] The inventors have confirmed successful transfer of the PhC pattern onto the growth limiting mask 102 and onto the interface 111 of the ELO layer 105, as shown in Figures 2(e), 2(f), 2(g), and 2(h), and the ELO layer 105 is removed from the host substrate 101 using the method described in [S. Gandrothula, Appl. Phys. Express 13, 041003 (2020)].
[0125] The interface of the ELO layer 105 has been experimentally scanned using AFM, and the results can be seen in Figures 2(e), 2(f), 2(g), and 2(h) as the epilayer interfaces. The pattern on the interface of the ELO layer 105 has been copied from the pattern on the growth limit mask 102.
[0126] 2(i) is a collection of microscope, SEM, and AFM images of the front and back sides of III-nitride ELO layer 105 for planar growth-limiting mask 102 and patterned growth-limiting mask 102 when different colloid sizes are used to generate the patterns. Specifically, image 203 is a microscope image showing the colloid particle size, image 204 is a microscope image of the back side of ELO III-nitride layer 105, image 205 is a SEM image of the back side of ELO III-nitride layer 105, image 206 is an AFM scan of the back side of ELO III-nitride layer 105, and image 207 is an AFM scan of the pattern on growth-limiting mask 102.
[0127] Second Embodiment The second embodiment is about achieving macro-sized, highly efficient LEDs for solid-state lighting applications such as residential, automotive, entertainment, etc. Grown entirely in MOCVD, they are approximately 0.05 mm 2 ~0.1mm 2 A device 107 layer with an area of is produced on the wings of the ELO layer 105. For this to happen, the entire area of the growth limiting mask 102 is covered with a PhC pattern such as that shown in FIG. 1(b) with either a hybrid mask 102A or a patterned mask 102B, and then a III-nitride epitaxial layer 105 is grown using MOCVD. A mesa is etched for the LED, metal contacts are deposited, and then the LED is extracted from the host substrate 101 and packaged.
[0128] As shown in Figures 3(a), 3(b), 3(c), 3(d), 3(e), and 3(f), the LEDs can be packaged in a number of different ways depending on the pad configuration and / or mounting method.
[0129] 3(a), 3(b), and 3(c) illustrate a vertical pad configuration, where the element 107 resides on a cup reflector 301, with one of the metal contacts 302 placed on the extraction feature when a PhC patterned mask 102B is used, or on the flat area 104A along the extraction feature 104B when a hybrid mask 102A is used. Another metal contact 303 is placed on the bottom of the element 107. All of these elements are then encapsulated in an epoxy hemisphere 304, with a cathode 305 and an anode 306 extending outside of the hemisphere 304 for electrical connection to a power supply (not shown).
[0130] FIG. 3(b) shows the MQWs 202, contacts 302, 303, and current spreading lines 307 as well as the extraction of light from the extraction features.
[0131] FIG. 3( c ) shows a ZnO submount 308 with rear side roughening that is used to mount the element 107 in the hemisphere 304 after the substrate 101 has been removed from the element 107 .
[0132] 3(d), 3(e), and 3(f) illustrate a side pad configuration, where the element 107 resides on a cup reflector 301 and both metal contacts 302 are placed on the bottom of the element 107. All of these elements are then encapsulated in an epoxy hemisphere 304, with the cathode 305 and anode 306 extending outside the hemisphere 304 for electrical connection to a power supply (not shown). In this embodiment, the metal contacts 302, 303 are placed on the side of the element 107 opposite the light extraction features when a PhC patterned mask 102B is used, or when a hybrid type mask 102A is used.
[0133] FIG. 3( f ) shows the ZnO submount 308 with rear side roughening that is used to mount the device 107 within the hemisphere 304 after the substrate 101 is removed.
[0134] (Third embodiment) A third embodiment is directed to a PhC cavity micro-sized LED for display applications.
[0135] Next-generation displays such as micro light-emitting diode displays are being intensively researched due to their advantages of high wall plug efficiency and wide color gamut compared to conventional LCD and OLED displays. However, there are some problems with conventional thickness LEDs, such as color mixing, color purity, temperature, and color stability. To solve these problems, III-nitride-based blue, green, and red PhC cavity LEDs have attracted more attention as potential alternatives. The advantages of PhC cavity LEDs include spectral purity and thermal stability, since the spectral width and shape are determined by the overlap of the cavity mode with the InGaN QW emission. Another advantage is that the emission of PhC cavity LEDs is more directional than conventional LEDs. Furthermore, the PhC cavity or PhC on the p-side of the LED would damage the device layers or increase the operating characteristics. Researchers [Appl. Phys. Lett. 96, 031108 (2010)] have reported n-side PhC by incorporating it into an LED, but such an approach increases defects and greater growth control is required. Ideally, the PhC or PhC cavity should be close to the light-emitting region (i.e., QW) to extract most of the escape modes of light.
[0136] For display applications, microLEDs smaller than about 20 μm on at least one side have been reported to be less efficient due to damage associated with plasma etching when defining the mesa. 6 cm -2 It has been found that epitaxial layers having threading dislocation densities less than 100 nm are less resistant to damage from plasma etching.
[0137] As shown in Figures 4(a) and 4(b), the light emitting device 401 is composed of high crystal quality layers on the wings of the ELO III-nitride layer 105, so that the device 401 suitable for display applications will contain substantially fewer defects or no defects at all. In addition, extraction features 402 such as PhCs or PhC cavities (e.g., with disordered PhC periodicity) can be formed on the growth constraining mask 102. The micro-LEDs 401 including PhC cavities without encapsulation have x, y, and h dimensions of less than 20 μm and can serve as light sources or pixels in display applications. The PhCs 402 act as light guiding structures and suppress color mixing with neighboring elements. This is the most desirable property for microdisplays that require higher density integration of light sources, such as AR / VR applications.
[0138] As shown in Figures 4(c) and 4(d), a growth limiting mask 102 for a PhC cavity 403 is placed on a host substrate 101, which contains an array 404 of one or more individual units of PhC 403, and the PhC design can be a defect-introduced PhC 405 or a regular PhC 406.
[0139] As shown in FIGS. 4( e and 4 ( f ), adjacent ones of PhC 402 may be separated by regions 407 , which may correspond to non-coalesced, non-grown regions 106 of ELO III-nitride layer 105 .
[0140] As shown in Figures 4(g) and 4(h), an entire bar 408 of element 107 can be selected and separated from the substrate 101, or selected ones of elements 409 can be selected and separated from the substrate 101.
[0141] As shown in FIGS. 4(i) and 4(j), the element 107 may be mounted onto a display panel 410 or other carrier using bottom contacts 411 and / or top contacts 412.
[0142] This embodiment provides a solution to realize a directional light source with good quality for display applications. Also, fabricating a PhC or a PhC cavity on a conventional thin flip-chip design is nearly impossible because it degrades the p-side material. In addition, approaches such as thinning the substrate 101 and then placing the PhC on the substrate 101 side are time-consuming.
[0143] The methods described herein not only provide a PhC on the n-side of the device layer, but also provide a device epitaxial layer with negligible threading dislocations.
[0144] (Fourth embodiment) In the fourth embodiment, to maximize the vertical light extraction of the PhC LED, it is essential to keep some distance between the light-emitting active area and the light-guiding features, which corresponds to the wavelength of the light in the material. In that case, the ratio of intensity in the ejection mode to the guided mode is increased when compared to thick LEDs. To realize this application, the present invention can be modified as follows:
[0145] 5(a) and 5(b), ELO III-nitride layer 105 is grown on growth-limiting mask 102 and host substrate 101, and light extraction features such as PhC or PhC cavities formed by colloids 201 are used to pattern growth-limiting mask 102. Polishing is then performed on ELO III-nitride layer 105 to line 501, resulting in a thickness t, where t is comprised of the thickness of growth-limiting mask 102, colloids 201, and ELO III-nitride layer 105 with the transferred PhC features.
[0146] Next, III-nitride semiconductor device 107 layers are grown on ELO III-nitride layer 105. For example, ELO III-nitride layer 105 may comprise one or more n-type layers, and III-nitride semiconductor device 107 layers may include an n-type GaN layer; an InGaN spare layer with 5% indium content; an MQW consisting of 5 periods of 2.5 nm InGaN quantum wells and 13.5 nm GaN barriers as an active region; a 20 nm p-type electron blocking layer (EBL) layer; and 200 nm p-type GaN. The total thickness of the layers is about 500 nm.
[0147] Finally, the substrate 101 is removed and the p- and n-contacts 502, 503 are deposited. Alternatively, the p- and n-contacts 502, 503 can be deposited before removing the substrate 101.
[0148] As with the other embodiments, the processed elements 107 are then consolidated accordingly.
[0149] Fifth embodiment In a fifth embodiment, a larger LED with light extraction features for better EQE is described. As shown in FIG. 6(a), the LED has a length l and a width w, e.g., l×w=about 50,000 μm. 2 After achieving the desired dimensions of the LED element 107 having the above, the LED element 107 with the metallized p-contact 601 on the top of the element 107 is removed from the host substrate 101. The p-contact 601 can be a reflective material such as Ti / Ag / Ni / Au.
[0150] 6(b), the open regions 109 are the connections between the ELO III-nitride layer 105 and the host substrate 101 where dislocations on the host substrate 101 are still present, but where the dislocations do not propagate into the wings of the ELO III-nitride layer 105. The open regions 109 are substantially free of any material from the host substrate 101. With respect to the areas of the open regions 109, when a GaN-on-sapphire template is used as the host substrate 101, the dislocations are not propagated into the wings of the ELO III-nitride layer 105. 8 ~10 9 cm 2When a GaN-on-silicon template is used as the host substrate 101, the dislocations increase by 10 10 ~10 11 When a larger, bulk free-standing GaN substrate is used as the host substrate 101, the dislocations increase by 10 6 ~10 5 cm 2 It is.
[0151] 6(b), light extraction features 602, which may be concave, are epitaxially integrated on the n-side of the LED element 107, and the relatively higher dislocation density region, open area 109, is a planar surface that may be used to place an n-pad 603. The LED element 107 is then packaged as described above.
[0152] Alternatively, as shown in Figures 7(a) and 7(b), the LED element 107 has a metallized n-contact 701 on the open area 109, which is a relatively higher dislocation density region and a planar surface. The element 107 may include concave light control features 702 or convex light control features 703, which are epitaxially integrated on the n-side of the LED element 107 using a growth limiting mask 102. A metallized p-contact 704 is formed on the n-side of the LED element 107. The relatively higher dislocation density regions are deposited over the open areas 109 and the planar surfaces. The LED device 107 is then packaged as described above.
[0153] Sixth embodiment The sixth embodiment describes large scale fabrication of integrated light extraction features for LEDs 107 on foreign substrates 101, such as GaN on sapphire, GaN on silicon, template on substrate, etc. The light extraction features are formed on the growth limit mask 102 or on the foreign substrate 101. The ELO III-nitride layer 105 then accepts the shape of the features without adding threading dislocations to the wings of the ELO III-nitride layer 105. Macro- to micro-sized LEDs 107 can be fabricated as described above.
[0154] This particular embodiment is advantageous when large size substrates 101 such as sapphire (6 inches or larger) or Si (12 inches or larger) are used to reduce production costs.
[0155] To date, fabrication of conventional LEDs has been attempted using GaN-on-sapphire and GaN-on-silicon substrates; however, there have been no reports addressing the LED's crystalline quality or light-control features near the active region. The present embodiment primarily addresses such issues.
[0156] (Process Step) 8 is a flow chart illustrating a method 800 of fabricating a semiconductor device in accordance with the present invention. Specifically, FIG 8 illustrates a method 800 of fabricating an LED with epitaxial light control features.
[0157] Block 801 represents the step of providing a substrate 101. In this step, the substrate comprises a III-nitride substrate or a foreign substrate with a III-nitride template deposited thereon.
[0158] Block 802 represents the step of forming a growth-limiting mask 102 on or above the substrate 101. Specifically, the growth-limiting mask 102 is deposited directly on the substrate 101 or directly on a III-nitride template that is deposited on the substrate 101. The growth-limiting mask 102 is typically an insulating film (e.g., SiO 2 , SiN, SiON, TiN, etc.) and are deposited by, for example, plasma-enhanced chemical vapor deposition (CVD), sputtering, ion beam deposition (IBD), etc.
[0159] Block 803 represents the step of designing light control features in the growth-limiting mask 102. Specifically, one or more patterns 113 are formed on the growth-limiting mask 102 or the host substrate 101 using colloidal lithography, nanoimprinting, electron beam lithography, holography, or interference lithography. Preferably, the patterns 113 are formed on the growth-limiting mask 102 or the host substrate 101 and then epitaxially transferred to at least the interface between the III-nitride ELO layer 105 and the growth-limiting mask 104 without etching or damaging the III-nitride ELO layer 105 or the III-nitride semiconductor device 107 layers.
[0160] The pattern 113 may comprise a hybrid mask 102A consisting of smooth regions 104A and patterned regions 104B, or a patterned mask 102B consisting of patterned regions 104B without smooth regions 104A.
[0161] Pattern 113 may comprise a first designed pattern defined to improve extraction of light emitted from the element 107 layer (e.g., when pattern 113 comprises a random rough surface) or a second designed pattern defined to improve directionality of light emitted from the element 107 layer (e.g., when pattern 113 comprises a PhC pattern).
[0162] In one embodiment, a pattern 113 is fabricated on a host substrate 101 and a growth-limiting mask 102 is formed over the pattern 113, the growth-limiting mask 102 incorporating the pattern 103, for example when the pattern 113 comprises a PhC pattern. In this embodiment, the PhC pattern is deposited on the host substrate 101 using colloid 201 and the growth-limiting mask 102 is deposited on the colloid 201, whereby the growth-limiting mask 102 incorporates a PhC pattern. The PhC pattern may comprise one or more PhC cavities, the PhC cavities may comprise an array of one or more PhCs, the PhCs may be regular PhCs or defect-induced PhCs.
[0163] After the pattern 113 is introduced into the growth limiting mask 102, the opening areas 103 separated by the stripes of the growth limiting mask 102 are etched into the growth limiting mask 102. Alternatively, the opening areas 103 can be etched into the growth limiting mask 102 before the pattern 113 is introduced into the growth limiting mask 102.
[0164] Block 804 represents the step of using the ELO and growth limiting mask 102 to grow a III-nitride ELO layer 105 first from the opening areas 103 in the growth limiting mask 102 and then laterally over the growth limiting mask 102, where the III-nitride ELO layer 105 may or may not merge with adjacent (or neighboring) III-nitride ELO layers 105.
[0165] Block 805 represents the step of growing III-nitride element 107 layers on or above the III-nitride ELO layer 105, where the III-nitride element 107 layers are grown on the wings of the III-nitride ELO layer 105, and the III-nitride ELO layer 105 and the III-nitride element 107 layers together comprise island-like III-nitride semiconductor layers 105, 107.
[0166] Pattern 113, formed on growth-limiting mask 102 or host substrate 101, is transferred to at least interface 111 between III-nitride ELO layer 105 and growth-limiting mask 102, and possibly to element 107 layers as well, with pattern 113 having epitaxially integrated light control features for extracting, directing, reflecting, refracting, concentrating, or defocusing light emitted from element 107 layers, such that the light control features are formed before the light emitting layers are formed.
[0167] In one embodiment, the light control features are formed on the n-side surface 111 of the III-nitride ELO layer 105, e.g., the light control features are epitaxially integrated on the back side of the III-nitride ELO layer 105 to minimize the thickness of the p-type layers of the III-nitride semiconductor device 107.
[0168] Block 806 represents the step of fabricating light emitting devices 107, such as LEDs, by conventional lithographic methods on the wing regions of ELO layer 105, which are primarily covered by the planar surface regions.
[0169] Block 807 represents the step of dividing the island III-nitride semiconductor layers 105 , 107 into separate elements 107 or groups of elements 107 to isolate the elements 107 on the host substrate 101 .
[0170] Block 808 represents the step of removing the elements 107 from the substrate 101. This may involve dissolving the growth limiting mask 102 and any protective layers using a chemical etchant such as buffered hydrofluoric acid (BHF) or hydrofluoric acid (HF).
[0171] Block 809 represents the step of transferring the device 107 onto a display panel, submount, or other external carrier. Specifically, this step involves transferring the device 107, including the island-shaped III-nitride semiconductor layers 105, 107, onto a display panel, submount, or other external carrier.
[0172] This step also includes forming lateral or vertical injection configurations for injecting current into the elements 107, and includes depositing n- and p-contacts onto the elements 107. These configurations allow each element 107 in the bar of elements 107 to be processed separately or together with other elements 107.
[0173] Block 810 represents the end result of the method, ie, the completed device 107 .
[0174] (References) The following references are incorporated herein by reference: 1.Appl.Phys.Lett.84,855(2004) 2.Applied Physics Express 9,102102(2016) 3.J.Vac.Sci.Technol.,B 35,011201(2017) 4. U.S. Patent Application Publication No. 2017 / 0092810, filed June 11, 2014, by James W. Raring et al., entitled “Surface morphology of non-polar gallium nitride containing substrates.” 5.Appl.Phys.Express,13,041003(2020) 6.Appl.Phys.Lett.96,031108(2010)
[0175] (Conclusion) The description of the preferred embodiments of the present invention now concludes. The foregoing description of one or more embodiments of the present invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations are possible in light of the above teachings. It is intended that the scope of the present invention be limited not by this detailed description, but rather by the claims appended hereto.
Claims
1. 1. A method, comprising: forming a growth-limiting mask on a host substrate, wherein one or more patterns are formed on the growth-limiting mask or the host substrate; growing one or more epitaxial lateral overgrowth (ELO) layers and device layers on the host substrate using the growth limiting mask; Including, The pattern formed on the growth limiting mask or the host substrate is transferred to at least an interface between the ELO layer and the growth limiting mask, the pattern comprising epitaxially integrated light control features that extract, direct, reflect, refract, concentrate or defocus light emitted from the device layer.
2. The method of claim 1 , wherein the pattern is formed on the growth confinement mask or the host substrate using colloidal lithography, nanoimprinting, electron beam lithography, holography, or interference lithography.
3. The method of claim 1 , wherein the pattern comprises a hybrid mask consisting of smooth and patterned areas, or a patterned mask consisting of patterned areas without smooth areas.
4. The method of claim 1 , wherein the pattern comprises a first designed pattern defined to enhance extraction of light emitted from the device layer.
5. The method of claim 4 , wherein the pattern comprises a random rough surface.
6. The method of claim 1 , wherein the pattern comprises a second designed pattern defined to enhance directionality of light emitted from the device layer.
7. The method of claim 1 , wherein the pattern is fabricated on the host substrate and the growth-limiting mask is formed over the pattern, the growth-limiting mask incorporating the pattern.
8. The method of claim 7 , wherein the pattern comprises a photonic crystal (PhC) pattern.
9. the photonic crystal pattern is deposited on the host substrate using a colloid; The method of claim 8 , wherein the growth-limiting mask is deposited on the colloid, whereby the growth-limiting mask incorporates the photonic crystal pattern.
10. 10. The method of claim 9, wherein the photonic crystal pattern comprises one or more PhC cavities, the PhC cavities comprising an array of one or more PhCs, the PhCs being ordered PhCs or defect-induced PhCs.
11. The method of claim 1 , wherein the device layer is grown on one or more wings of the ELO layer.
12. The method of claim 1 , wherein the pattern is epitaxially formed in the ELO layer without etching or damaging the ELO layer or the device layer.
13. The method of claim 1 , wherein the light control features are formed on an n-side of the ELO layer.
14. The method of claim 13 , wherein the light control features are epitaxially integrated behind the ELO layer to minimize a thickness of a p-type layer of the device layer.
15. The method of claim 1 , wherein the light control features are formed before a light emitting layer is formed.
16. A structure comprising: a growth-limiting mask formed on a host substrate, one or more patterns being formed on the growth-limiting mask of the host substrate; one or more epitaxial lateral overgrowth (ELO) layers and device layers grown on the host substrate using the growth limiting mask; Equipped with The pattern formed on the growth limiting mask or the host substrate is transferred to at least the interface between the ELO layer and the growth limiting mask, the pattern comprising epitaxially integrated light control features that extract, guide, reflect, refract, concentrate or defocus light emitted from the device layer.
Citation Information
Patent Citations
Substrate fine processing method,substrate manufacturing method and light emitting element
CN101454913A
Semiconductor laser element and its manufacturing method
JP2003046189A
Photonic crystal light-emitting device
JP2005317959A
Semiconductor element, and manufacturing method thereof
JP2008053602A
High quality devices growth on pixelated patterned templates
US20140183700A1
Cited By
Optical element substrate, method for manufacturing optical element substrate, and method for manufacturing optical communication substrate
WO2026203285A1
Optical element substrate manufacturing method, optical communication substrate, optical communication device, optical element substrate, and optical communication substrate manufacturing method
WO2026203286A1