EUV active films for EUV lithography

EUV active photoresists with metal alkoxides address sensitivity and blurring issues in conventional photoresists, providing high absorption and etch resistance for precise nanoscale patterning with reduced environmental impact.

JP2024542124APending Publication Date: 2024-11-13TOKYO ELECTRON LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024526777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-09
Filing Date
2022-11-07
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Conventional photoresists used in photolithography systems have low sensitivity and high blurring issues at EUV wavelengths, limiting their effectiveness in patterning sub-10 nm features, and they also pose environmental and toxicity concerns.

Method used

Development of EUV active photoresists containing a network of metal alkoxides terminated with alkoxy groups, which respond to EUV exposure, offering higher absorption and etch resistance, and can be formed using dry processes for precise nanoscale patterning.

Benefits of technology

The EUV active photoresists exhibit improved sensitivity, reduced thickness, and better etch resistance, enabling precise nanoscale patterning with lower environmental impact and improved process control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542124000001_ABST
    Figure 2024542124000001_ABST
Patent Text Reader

Abstract

A method for processing a substrate, the method comprising the steps of forming an extreme ultraviolet (EUV) active photoresist film on the substrate, the photoresist film comprising a network of metal oxides terminated with alkoxy groups, and patterning the EUV active photoresist film by EUV lithography.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of and priority to U.S. Patent Application No. 17 / 522,563, filed November 9, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates generally to extreme ultraviolet (EUV) lithography, and in particular embodiments to EUV active films and methods of forming the same. [Background technology]

[0003] Generally, semiconductor devices, such as integrated circuits (ICs), are fabricated by successively depositing and patterning layers of dielectric, conductive, and semiconducting materials on a semiconductor substrate to form a monolithically integrated network of electronic components and interconnect elements (e.g., transistors, resistors, capacitors, metal lines, contacts, and vias). Each successive technology node reduces costs by shrinking minimum feature sizes and roughly doubling component packing density.

[0004] A common patterning method is to use a photolithography process to expose a coating of photoresist on a target layer to a pattern of actinic radiation, and then transfer the relief pattern to the target layer or an underlying hard mask layer formed on the target layer. With this technique, the minimum feature size is limited by the resolution of the optical system. Therefore, feature size scaling for 7nm and 5nm technology nodes may require 13.5nm extreme ultraviolet (EUV) lithography. Innovations in EUV photolithography technology may be required to meet the cost and quality requirements for patterning in the sub-10nm node region. Summary of the Invention [Means for solving the problem]

[0005] According to one embodiment of the present invention, a method for processing a substrate includes forming an extreme ultraviolet (EUV) active photoresist film on a substrate, the photoresist film comprising an alkoxy-terminated metal oxide network, and patterning the EUV active photoresist film by EUV lithography.

[0006] According to one embodiment of the present invention, a method of processing a substrate in a plasma processing chamber includes exposing the substrate in the plasma processing chamber to a first vapor including an EUV metal precursor, exposing the substrate in the plasma processing chamber to a second vapor including an alcohol having a hydrogen in a beta position relative to oxygen, exposing the substrate in the plasma processing chamber to a third vapor including an oxidizer to form a photoresist film including an EUV metal alkoxide on the substrate, and patterning the photoresist film by EUV lithography.

[0007] According to one embodiment of the present invention, a method of extreme ultraviolet (EUV) lithography includes forming an EUV-active photoresist layer on a substrate, the EUV-active photoresist layer comprising a network of tin oxide terminated with alkoxy groups; exposing the substrate to EUV radiation through an optical mask containing a pattern to form exposed regions of the EUV-active photoresist layer, where one or more alkoxy groups in the exposed regions undergo beta hydrogen elimination to produce tin hydroxide by eliminating an alkene; and developing the EUV-active photoresist layer. [Brief description of the drawings]

[0008] For a more complete understanding of the present invention, and the advantages thereof, reference is now made to the following descriptions taken in conjunction with the accompanying drawings, in which:

[0009] [Figure 1] FIG. 1 illustrates the reaction of a tin precursor with an alcohol to form a tin alkoxide, according to various embodiments. [Figure 2A] FIG. 2 is a cross-sectional view of a substrate during a two-step generation of tin alkoxide according to one embodiment, showing the substrate as the tin precursor is deposited. [Figure 2B] FIG. 2 is a cross-sectional view of a substrate during a two-step production of tin alkoxide according to one embodiment, showing the substrate at a subsequent step of reacting the deposited tin precursor with an alcohol to produce the tin alkoxide. [Figure 2C] 1 is a cross-sectional view of a substrate during one-step generation of tin alkoxide according to an alternative embodiment. [Figure 2D] 4 is a cross-sectional view of a substrate during deposition of pre-formed tin alkoxide according to another embodiment. [Diagram 3] 1A-1D illustrate the oxidation of tin alkoxide to form an extreme ultraviolet (EUV) active photoresist, according to various embodiments. [Figure 4A] FIG. 2 is a cross-sectional view of a substrate during a tin alkoxide oxidation step according to one embodiment, showing the substrate upon deposition of an oxidizing agent. [Figure 4B] 2A-2C are cross-sectional views of a substrate during a tin alkoxide oxidation step according to one embodiment, and illustrate the substrate upon completion of formation of an EUV active photoresist layer. [Figure 4C] 1A-1C are cross-sectional views of a substrate during one-step formation of an EUV active photoresist layer according to an alternative embodiment. [Figure 5A] FIG. 2 shows an exemplary chemical structure of an EUV-active photoresist containing alkoxy groups, according to various embodiments; [Figure 5B] FIG. 2 shows an exemplary chemical structure of an EUV-active photoresist containing alkoxy groups, according to various embodiments; [Figure 5C] FIG. 2 shows an exemplary chemical structure of an EUV-active photoresist containing alkoxy groups according to various embodiments; FIG. 3 shows cyclohexyl alkoxide. [Figure 6A]FIG. 1 illustrates a process flow chart for a method of forming an EUV active photoresist layer according to various embodiments. FIG. 2 illustrates the process flow for some embodiments. [Figure 6B] FIG. 1 illustrates a process flow diagram for a method of forming an EUV active photoresist layer according to various embodiments, and shows a process flow for an alternative embodiment. [Figure 7] FIG. 1 illustrates reactions that may occur during an EUV exposure step in an EUV lithography process, in which alkoxy groups of an EUV-active photoresist are converted to hydroxy groups by β-hydrogen elimination, according to various embodiments. [Figure 8A] 1A-1D are cross-sectional views of a substrate during an EUV exposure step in an EUV lithography process according to various embodiments, illustrating the substrate at the start of EUV exposure. [Figure 8B] 1A-1D are cross-sectional views of a substrate during an EUV exposure step in an EUV lithography process according to various embodiments, showing the substrate after EUV exposure. [Figure 9] FIG. 1 illustrates a reaction that may occur during an optional post-exposure bake (PEB) in which hydroxy groups of the reacted EUV-active photoresist condense to release water molecules. [Figure 10] FIG. 2 is a cross-sectional view of a substrate after an EUV exposure step and PEB. [Figure 11A] 1A-1C are cross-sectional views of a substrate after a development step according to various alternative embodiments, including a substrate according to an embodiment without a PEB. [Figure 11B] 1A-1C are cross-sectional views of a substrate after a development step according to various alternative embodiments, including a substrate with a PEB alternative embodiment. [Figure 12A] 1A-1C are cross-sectional views of a substrate at various intermediate stages of an EUV lithography process according to an alternative embodiment, showing the substrate after an EUV exposure step and a deposition step to form a material layer. [Figure 12B] 1A-1D are cross-sectional views of a substrate at various intermediate stages of an EUV lithography process, including after a development step, in accordance with an alternative embodiment. [Figure 12C] 1A-1C are cross-sectional views of a substrate at various intermediate stages of an EUV lithography process according to yet another embodiment, showing the substrate after an EUV exposure step and a deposition step to form a material layer. [Figure 12D] 1A-1D are cross-sectional views of a substrate at various intermediate stages of an EUV lithography process, including showing the substrate after a development step, according to yet another embodiment. [Figure 13] FIG. 1 illustrates a process flow chart of a method of EUV lithography processing in accordance with various embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] This application relates to a method of photolithography process, and more particularly, to a method of forming an extreme ultraviolet (EUV) active photoresist containing metal alkoxide moieties for EUV photolithography process. EUV lithography techniques, for example using UV wavelength of 13.5 nm, can provide great advantages in patterning sub-10 nm features due to its high optical resolution. However, one of the main engineering challenges for EUV lithography is that photoresists developed for conventional photolithography systems may not be effective enough. For example, chemically amplified resists (CAR) or similar polymer resists commonly used in 193 nm lithography tend to have low absorption coefficients at 13.5 nm and therefore may have low sensitivity. Furthermore, diffusion of photoactive species in CAR may result in blurring and increased line edge roughness. Therefore, development of a new class of photoresists for EUV lithography with better performance may be desirable. An embodiment of the present application discloses a method of forming an EUV active photoresist layer containing a network of metal alkoxides, particularly metal oxides terminated with alkoxy groups. The alkoxide group of the metal alkoxide in various embodiments responds to EUV exposure to induce a change in material properties, and the EUV-active photoresist in various embodiments can be designed based on this EUV-active property of the metal alkoxide group.

[0011] The methods described in the present disclosure may advantageously enable metal alkoxide-containing extreme ultraviolet (EUV) active photoresists with high EUV absorptivity and therefore better resist sensitivity compared to conventional chemically amplified resists (CARs). Higher EUV absorptivity may enable a reduction in the thickness of the photoresist required for acceptable performance. The metal alkoxide-containing EUV active photoresists described in the present disclosure may also advantageously exhibit better etch resistance than conventional CARs. Furthermore, the methods herein may enable uniform chemical composition of the metal alkoxide-containing EUV active photoresists, which may be beneficial in reducing blurring or line edge roughness issues. Furthermore, the EUV active photoresists according to various embodiments of the present disclosure may be formed on a substrate and developed by dry or wet processes. While conventional techniques used for applying and developing CARs are based on wet processes, dry processes for forming and developing EUV active photoresists may enable better process control at the nanoscale than wet processes, for example, to form features with critical dimensions of a few nanometers or sub-nanometers. Conventional spin-on processes for deposition and wet processes using developers are also applicable to the methods of the present disclosure.

[0012] The EUV active photoresists formed by the methods described in this disclosure are based on metal oxide networks terminated with alkoxy groups (i.e., metal-oxygen-metal and metal-oxygen-carbon bonds), which advantageously have lower toxicity and environmental impact compared to, for example, organometallic compounds having metal-carbon bonds.

[0013] Various embodiments of the present disclosure may consist of three processing steps: (i) generation of metal alkoxide molecules, (ii) formation of an EUV-active photoresist layer on a substrate, and (iii) an EUV lithography process using the EUV-active photoresist layer. In the following, step (i) is first described with reference to Figures 1 and 2A-2D, and then step (ii) is described with reference to Figures 3 and 4A-4B. Examples of chemical structures of EUV-active photoresists are shown in Figures 5A-5C. Process flow diagrams for steps (i) and (ii) according to various embodiments are shown in Figures 6A and 6B. Step (iii), the EUV lithography process, may include an EUV irradiation step, an optional post-exposure bake (PEB), and a development step, which are described with reference to Figures 7 and 8A-8B, Figures 9 and 10, and Figures 11A and 11B, respectively. Furthermore, a particular embodiment involving a post-exposure deposition step to form a material layer is described in Figures 12A-12D. An exemplary process flow diagram for an EUV lithography process is described with reference to Figure 13. All drawings are for illustrative purposes only and are not to scale.

[0014] FIG. 1 illustrates the reaction of a metal precursor 10 with an alcohol 11 to produce a metal alkoxide 12, according to various embodiments.

[0015] Metal precursors including EUV metals can be used to form EUV-active photoresists. In this disclosure, EUV metals can refer to metals with high EUV absorption coefficients. In various embodiments, the EUV metals can include tin (Sn), and in other embodiments, can include zirconium (Zr), indium (In), antimony (Sb), bismuth (Bi), or hafnium (Hf). Various embodiments, including figures, are described below using tin as an exemplary metal component for EUV-active photoresists, although in some embodiments, other metals can also be present in the EUV-active photoresist.

[0016] In FIG. 1, the metal precursor 10 may be, in one example, an organotin compound that includes ligands (L1-L4). In various embodiments, these ligands may include amines, carboxylates, or halogens. In some embodiments, some of the ligands may include alkoxy groups. An alcohol 11 reacts with the metal precursor 10 to displace one or more of the ligands to generate one or more alkoxy groups bonded to the metal, in this case tin, thus generating a metal alkoxide 12, in this case tin alkoxide. In this disclosure, the metal alkoxide 12 may refer to a metal compound that includes a metal atom terminated with one or more alkoxy groups. The metal alkoxide 12 can be used as an intermediate to form an EUV-active photoresist that includes a network of metal oxides terminated with alkoxy groups. For example, in FIG. 1, two ligands (i.e., L1 and L3) are exchanged with two alkoxy groups. Without wishing to be bound by any theory, some of the functional groups of the metal alkoxide 12 may be removed, for example, by reacting with moisture. In various embodiments, one or two alkoxy groups per metal atom may be retained to form an EUV-active photoresist. The extent of the ligand exchange may depend on the type and conditions of the process. This ligand exchange reaction to produce the metal alkoxide 12 may be performed by a dry or wet process. For example, the ligand exchange reaction may be performed on a substrate by using deposition techniques such as atomic layer deposition (ALD), chemical vapor deposition (CVD), vapor deposition including physical vapor deposition (PVD), and other plasma processes such as plasma enhanced CVD (PECVD), and other processes. In other embodiments, wet processes such as spin-on processes may also be used.

[0017] In various embodiments, the metal alkoxide 12 may include ethoxide, isopropoxide, tert-butoxide, cyclohexyl alkoxide, cyclohexene alkoxide, or cyclohexadiene alkoxide. The metal alkoxide 12 includes a hydrogen in the β position relative to the oxygen atom of the alkoxy group (i.e., a β hydrogen). The β hydrogen may be an important photoreactive species in EUV lithography. Without wishing to be bound by any theory, this may be because the β hydrogen is necessary for the photoinduced β hydrogen elimination reaction to occur. The β hydrogen elimination reaction may be the basis for the EUV active properties of the photoresist according to various embodiments.

[0018] The alcohol 11 can be selected according to the type of metal alkoxide desired. For example, the alcohol 11 can include ethanol, isopropanol, tert-butanol, or cyclohexanol. In various embodiments, any alcohol having a hydrogen in a β position relative to an oxygen atom can be used. In certain embodiments, the selection of bulky reactive groups can advantageously provide steric hindrance relative to each other and prevent excessive condensation prior to the EUV lithography process. Furthermore, a higher number of hydrogen atoms in the alcohol 11 in a β position relative to the oxygen can improve the probability of removing the β hydrogen, thereby improving the EUV sensitivity. Furthermore, in some embodiments, two or more alkoxides can be used to form an EUV-active photoresist. The use of two or more alkoxides can advantageously allow fine tuning of the overall physical and chemical properties (e.g., bulkiness, carbon to oxygen ratio, and / or hydrophobicity / hydrophilicity) of the resulting EUV-active photoresist. In one embodiment, exposure to moisture (water molecules in the gas phase) can also be performed to adjust the physical and chemical properties of the EUV-active photoresist.

[0019] 2A and 2B show cross-sectional views of a substrate 100 during a two-step generation of a metal alkoxide 12 according to one embodiment.

[0020] In FIG. 2A, in various embodiments, the substrate 100 comprises a semiconductor substrate. In one or more embodiments, the substrate 100 may be a silicon wafer or a silicon-on-insulator (SOI) wafer. In certain embodiments, the substrate 100 may comprise a silicon germanium wafer, a silicon carbide wafer, a gallium arsenide wafer, a gallium nitride wafer, or other compound semiconductors. In other embodiments, the substrate 100 comprises a heterogeneous layer, such as silicon germanium on silicon, gallium nitride on silicon, silicon carbon on silicon, as well as a layer of silicon on silicon or an SOI substrate. The substrate 100 may also include an intermediate layer 110 on the substrate 100, as shown in FIG. 2A. In certain embodiments, the intermediate layer 110 may comprise silicon oxide, silicon nitride, silicon carbonitride (SiCN), silicon oxycarbide (SiOC), or other materials. The intermediate layer 110 may be a layer that is patterned by an etching process after an EUV lithography process.

[0021] In various embodiments, prior to deposition of the metal precursor 10, the substrate 100 may be optionally processed by a pretreatment step to improve the deposition step. In some embodiments, a plasma or thermal process may be performed to chemically or physically modify the composition of the surface end groups of the intermediate layer 110. For example, the optional pretreatment may be a plasma treatment using a hydrogen-containing reducing agent. In one embodiment, a plasma treatment using molecular hydrogen (H2) may be performed.

[0022] 2A , the metal precursor 10 can be deposited as a layer on the intermediate layer 110 by a dry or wet process. In certain embodiments, without wishing to be bound by any theory, a portion of the metal precursor 10 can chemically bond to the surface of the intermediate layer 110. For example, one of the ligands (L1-L4) of the metal precursor 10 can react with a surface hydroxy group of the intermediate layer 110.

[0023] In Figure 2B, in a subsequent step, an alcohol 11 is delivered to the substrate 100 from a vapor or solution and reacts with the absorbed metal precursor 10 to produce a metal alkoxide 12, as also shown in Figure 1. The method according to this embodiment may be particularly advantageous when applied to atomic layer deposition (ALD), allowing the metal alkoxide 12 to be grown with high uniformity layer by layer.

[0024] Furthermore, in certain embodiments, the above two steps (i.e., deposition of metal precursor 10 and reaction with alcohol 11) can be repeated consecutively by alternating exposure to metal precursor 10 and alcohol 11 to enable layer-by-layer growth for precise film thickness control and film uniformity. In one embodiment, the two exposures may overlap in time, while in other embodiments they may not, and a purge or degassing step may be inserted between the exposure steps. The purge or degassing step may be beneficial to ensure that chemical reactions at the surface are limited, while the overlapping exposures may aid in faster film growth.

[0025] In certain embodiments, the thickness of the layer of metal alkoxide 12 may be between about 15 nm and about 40 nm. In general, metal alkoxide-containing EUV photoresist films can be advantageously thinner than conventional CARs due to their higher etch resistance and higher sensitivity.

[0026] FIG. 2C shows a cross-sectional view of substrate 100 during one-step generation of metal alkoxide 12 according to an alternative embodiment.

[0027] 2C, the metal precursor 10 and the alcohol 11 can be simultaneously delivered from vapor or solution to the substrate 100 in a single step, and the metal alkoxide 12 can be produced and deposited on the intermediate layer 110. Such an embodiment can be advantageous when applied to, for example, chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD), allowing for the continuous growth of a layer of metal alkoxide 12 in a single step.

[0028] FIG. 2D shows a cross-sectional view of substrate 100 during deposition of pre-formed metal alkoxide 12 according to another embodiment.

[0029] The metal alkoxide 12 may be already prepared or available in a separate process and may be used in this embodiment, where the metal alkoxide 12 may be delivered directly to the substrate from a vapor or solution to form a layer on the intermediate layer 110 as shown in FIG. 2D.

[0030] Although FIGS. 2A-2D show the deposition as only a two-step or one-step process, in various embodiments, the production of a layer of metal alkoxide 12 may be accomplished by repeating any of the above processes to achieve a desired thickness of the layer.

[0031] FIG. 3 illustrates the oxidation of a metal alkoxide 12 to form an extreme ultraviolet (EUV) active photoresist 14, according to various embodiments.

[0032] 4A-4B show cross-sectional views of substrate 100 during the oxidation step described in FIG. 3, according to one embodiment.

[0033] Oxidation of the metal alkoxide 12 forms metal-oxygen-metal bonds by displacing one or more of the ligands of the metal alkoxide 12 to form a condensed network of alkoxy-terminated tin oxide. In FIG. 3, oxidation removes the ligands L2 and L4 of the metal alkoxide 12 as by-products. The resulting condensed network of alkoxy-terminated metal oxide may function as an EUV-active photoresist 14, as described further below. Unlike previously known tin-based photoresists, the EUV-active photoresist 14 does not contain metal-carbon bonds. Advantageously, metal alkoxides, such as tin alkoxides, are generally less toxic and raise fewer concerns regarding environmental issues during manufacture.

[0034] In various embodiments, an oxidizing agent 13 can be used for the oxidation. In certain embodiments, the oxidizing agent 13 can include dioxygen (O2), ozone (O3), water, air, or hydrogen peroxide (H2O2). Although two alkoxy groups are shown for each metal atom in Figure 3, depending on the structure and degree of oxidation of the metal alkoxide 12, the metal atom can be bonded to one, two, or three alkoxy groups.

[0035] In certain embodiments, a plasma process in a plasma processing chamber can be employed for oxidation, in one embodiment, oxidation can be performed by exposing the metal alkoxide 12 to oxygen radicals generated to form a metal oxide network.

[0036] In Figure 4A, an oxidizing agent 13 can be provided from a vapor or solution to induce oxidation of the metal alkoxide 12. As a result, a layer of EUV active photoresist 14 is formed on the intermediate layer 110 due to the oxidation of the metal alkoxide 12, as shown in Figure 4B.

[0037] FIG. 4C illustrates a cross-sectional view of a substrate during one-step formation of an EUV active photoresist layer according to an alternative embodiment.

[0038] 4C, the oxidation step can be combined with a step of generation of a metal alkoxide 12 (by providing a metal precursor 10 and an alcohol 11) and can be performed in a single step in a processing chamber, where an EUV-active photoresist layer 14 can be formed directly on the intermediate layer 110. This single step can be performed by a wet or dry process.

[0039] In various embodiments, after the EUV active photoresist layer 14 is formed on the substrate 100, an optional post-apply bake may be performed to remove any excess solvent from the wet process, residual volatile by-products from the dry process, or both, so that the substrate 100 is ready for an EUV lithography process for patterning.

[0040] 5A-5C show three exemplary chemical structures of a tin alkoxide-containing EUV-active photoresist 14 that can be produced by the methods described above according to various embodiments.

[0041] The size of the alkoxy group may vary in various embodiments. In FIG. 5A, the EUV-active photoresist 14 is based on ethoxide (-OC2H5) groups as an example of a small sized alkoxy group. The use of relatively small sized alkoxy groups may be useful for improving the hydrophilicity of the EUV-active photoresist 14. On the other hand, the use of medium or large alkoxy groups may improve the hydrophobicity of the EUV-active photoresist 14 and provide steric hindrance to prevent excessive condensation prior to the EUV lithography process. In FIG. 5B, the EUV-active photoresist 14 is based on tert-butoxide (-OC4H9) groups as an example of a medium sized alkoxy group. In FIG. 5C, the EUV-active photoresist 14 is based on cyclohexyl alkoxide (-OC6H7) groups as an example of a large sized alkoxy group. 11 ) basis.

[0042] 6A and 6B show process flow diagrams of methods for forming an EUV active photoresist layer according to various embodiments. The process flow can be described using the figures described above (e.g., Figures 2A-2D and 4A-4B), and therefore will not be described again in detail.

[0043] In FIG. 6A, the process flow 60 may begin by exposing the substrate 100 to a vapor containing a metal precursor (block 600A, e.g., FIG. 2A), and then exposing the substrate 100 to an alcohol to generate a metal alkoxide (block 605, e.g., FIG. 2B). Alternatively, a solution containing a metal precursor dissolved in a solvent may be applied by a spin-on process (block 600C, e.g., FIG. 2A), and then the substrate 100 is exposed to an alcohol to generate a metal alkoxide (block 605, e.g., FIG. 2B). The spin-on process may include heating the substrate 100 to remove the solvent used in the process. In either embodiment, after generating the metal alkoxide, the substrate 100 may be exposed to an oxidizing agent to form metal-oxygen-metal bonds (block 610, e.g., FIG. 4A). Once this step is completed, an EUV-active photoresist containing a network of metal oxides terminated with alkoxy groups is formed on the substrate 100, and an EUV lithography process may be performed (block 620). Additionally, in other embodiments where a metal alkoxide is already available (e.g., FIG. 2D ), process flow 60 may begin with exposing the substrate to a vapor containing the metal alkoxide (block 600B) or applying a solution containing the metal alkoxide (block 600D), followed by oxidation (block 610) and an EUV lithography process (block 620) to pattern an EUV active photoresist.

[0044] In FIG. 6B, the process flow 62 may include a cyclic dry process based, for example, on atomic layer deposition (ALD). First, the substrate 100 may be exposed to a first vapor containing an EUV metal precursor 10 (block 630, e.g., FIG. 2A). Then, the substrate 100 may be exposed to a second vapor containing an alcohol 11 (block 640, e.g., FIG. 2B) to form a layer of metal alkoxide 12. These two steps may be repeated by alternating the two exposures to form a layer of metal alkoxide 12. In one embodiment, the two exposures may be alternated with overlap in time, while in other embodiments, they may be separated by a purge step. The substrate 100 may then be exposed to a third vapor containing an oxidizer 13 (block 650, e.g., FIG. 4A) to form metal-oxygen-metal bonds. These three steps (blocks 630, 640, and 650) may also be repeated to obtain a target thickness for the EUV-active photoresist 14. After completing the formation of the EUV active photoresist 14, an EUV lithography process may be performed (block 620) to pattern the EUV active photoresist 14.

[0045] Below, an extreme ultraviolet (EUV) lithography process for patterning an EUV active photoresist is described according to various embodiments.

[0046] FIG. 7 illustrates reactions that may occur during an EUV exposure step in an EUV lithography process, according to various embodiments.

[0047] In FIG. 7, EUV irradiation induces β-hydrogen elimination, and alkoxy groups in the EUV-active photoresist 14 are converted to hydroxy groups in the reacted photoresist 16, which may generate alkenes as by-products. Without wishing to be bound by any theory, at this stage, some of the generated hydroxy groups may further condense and crosslink by dehydration to form additional metal-oxygen-metal bonds. The structural change of the EUV-active photoresist 14 into the reacted photoresist 16 may affect material properties such as solubility and determine the positive / negative type of photoresist.

[0048] 8A and 8B show cross-sectional views of a substrate 100 during an EUV exposure step in an EUV lithography process, according to various embodiments.

[0049] In Figure 8A, a layer of EUV active photoresist 14 is formed on an intermediate layer 110 on a substrate 100. An EUV lithography process may be performed by exposing the substrate 100 to EUV radiation 115 (e.g., 13.5 nm wavelength) through a photomask 125. Thus, the light-induced reaction shown in Figure 7 occurs only in the areas of the EUV active photoresist 14 that are exposed to the EUV radiation 115.

[0050] 8B shows the substrate 100 after the EUV exposure step. The areas of the EUV active photoresist 14 that were exposed to the EUV exposure 115 are converted to reacted photoresist 16. The areas of the EUV active photoresist 14 that were not exposed to the EUV exposure 115 remain unreacted.

[0051] FIG. 9 illustrates reactions that may occur within reacted photoresist 16 during an optional post-exposure bake (PEB).

[0052] FIG. 10 shows a cross-sectional view of the substrate 100 after the EUV exposure step and PEB shown in FIG.

[0053] In various embodiments, a PEB can optionally be performed to further differentiate the material properties of the reacted photoresist 16 from that of the unreacted EUV-active photoresist. In certain embodiments, the PEB can be performed by heating the substrate 100 in a processing chamber under vacuum or flowing gas at a temperature between 70° C. and 250° C., such as in one embodiment at a temperature between 180° C. and 225° C.

[0054] Without wishing to be bound by any theory, the PEB causes the hydroxy groups of the reacted photoresist 16 to condense and release water molecules, as shown in FIG. 9. This reaction increases cross-linking within the metal oxide network, i.e., forms additional metal-oxygen-metal bonds. As a result, the baked photoresist 18 (FIGS. 9 and 10) is a more condensed network of hydroxy-terminated metal oxides. The baked photoresist 18 may have different material properties than the initial network of alkoxy-terminated metal oxides (e.g., the unreacted areas of the EUV-active photoresist 14 in FIG. 10) and the reacted photoresist (e.g., the reacted photoresist 16 in FIG. 8B). For example, in various embodiments, the baked photoresist 18 may have a substantially lower solubility than the solubility of the EUV-active photoresist 14. In various embodiments, the solubility of the baked photoresist 18 may be about 5 to about 1.5 times lower, or in other embodiments, 10 to 2 times lower, than that of the EUV-active photoresist 14. Additionally, in one embodiment, the volatility may also be reduced, for example by about 2 times. As a result, the baked photoresist 18 may be more resistant to dry development processes, such as dry etching (e.g., reactive ion etching or atomic layer etching), as compared to the EUV-active photoresist 14. For example, the sputter threshold may be higher for the baked photoresist 18.

[0055] 11A and 11B show cross-sectional views of a substrate 100 after a development step, according to various embodiments.

[0056] After completion of the EUV exposure and optional post-exposure bake (PEB), a development step can be performed to remove portions of the EUV-active photoresist 14 for patterning. The development step can be a wet or dry process. Conventionally, the photoresist can be removed by treating the substrate with a developer to dissolve the reacted areas (for positive resist) or the unreacted areas (for negative resist) of the photoresist. Similar wet processes can be applied to various embodiments. Alternatively, dry processes can be used in other embodiments. Dry processes can include, for example, selective plasma etching processes or thermal processes, advantageously eliminating the use of developer solutions. In certain embodiments, the dry process can be performed using a reactive ion etching (RIE) process or an atomic layer etching (ALE).

[0057] In Figures 11A and 11B, the unreacted areas of the EUV-active photoresist are removed, which is shown for a negative photoresist. The reacted photoresist 16 (Figure 11A) or the baked photoresist 18 (Figure 11B) may be left as a feature on the intermediate layer 110. The feature may be further used as an etch mask to transfer the pattern to the intermediate layer 110. In other embodiments, the EUV-active photoresist may be a positive resist, and the reacted areas (the reacted photoresist 16 or the baked photoresist 18) may be selectively removed by a development step. In certain embodiments related to a positive photoresist, a chemical modification step may be performed to change the chemical structure of the reacted photoresist 16 or the baked photoresist 18 in order to reverse the positive / negative nature of the photoresist. In one embodiment, such a positive photoresist may include a crosslinked metal alkoxide-containing film that undergoes chain scission during EUV exposure.

[0058] 12A and 12C show cross-sectional views of a substrate 100 during a post-exposure deposition step of an EUV lithography process, according to various embodiments.

[0059] 12B and 12D show cross-sectional views of substrate 100 after a post-exposure deposition step followed by a development step according to various embodiments, corresponding to FIGS. 12A and 12C, respectively.

[0060] In some embodiments, after the EUV exposure and before the development step, an area-selective post-exposure deposition step can be optionally inserted to selectively form a material layer 120 on the reacted areas of the EUV photoresist. The material layer 120 can be formed on the reacted photoresist 16 (FIG. 12A) or on the baked photoresist 18 (FIG. 12C). For example, this material layer can be used as a hard mask to improve the selectivity in a subsequent process, such as a development step and / or a plasma etching process to form features in the intermediate layer 110. In a particular embodiment, the post-exposure deposition step can be based on atomic layer deposition (ALD). Surface functional groups of the reacted areas of the EUV photoresist, such as hydroxy groups, can be used to chemically adsorb reactants from the vapor used in the post-exposure deposition step. Other deposition techniques can also be used for the post-exposure deposition step. For example, such techniques can include other plasma processes, such as chemical vapor deposition (CVD), physical vapor deposition (PVD) or even plasma enhanced CVD (PECVD). Alternatively, wet processes can also be used for the post-exposure deposition step. A development step may also be performed after the post-exposure deposition step (Figures 12B and 12D).

[0061] 13 shows a process flow diagram of a method of EUV lithography processing according to various embodiments. The process flow can be described using the figures described above (e.g., Figures 8A-8B, 10, 11A-11B, and 12A-12D), and therefore will not be described again in detail.

[0062] In FIG. 13, process flow 1300 may begin with forming an EUV active photoresist including tin alkoxide on a substrate (block 1310), followed by exposing the substrate to patterned EUV radiation (block 1320). Then, in certain embodiments, a development step may be performed immediately (block 1330). Alternatively, a post-exposure bake (PEB) may be performed (block 1322) after the EUV exposure (block 1320) and before the development step (block 1330). In yet other embodiments, the EUV exposure (block 1320) may be followed by a post-exposure deposition step (block 1324) to form a material layer, followed by a development step (block 1330). In yet another embodiment, the EUV exposure (block 1320) may be followed by a PEB and post-exposure deposition step (blocks 1322 and 1324), followed by a development step (block 1330). The order of these two optional steps may be swapped, and the post-exposure deposition step (block 1324) may occur before the PEB (block 1322).

[0063]

[0023] Exemplary embodiments of the present invention are summarized herein. Other embodiments can be seen throughout this specification and the claims.

[0064] Example 1. A method for processing a substrate, comprising the steps of forming an extreme ultraviolet (EUV) active photoresist film on a substrate, the photoresist film comprising a network of metal oxides terminated with alkoxy groups, and patterning the EUV active photoresist film by EUV lithography.

[0065] Example 2. The method of Example 1, wherein one or more of the alkoxy groups contains a hydrogen at the beta position relative to the oxygen.

[0066] Example 3. The method of example 1 or 2, wherein the metal oxide is tin oxide.

[0067] Example 4. The method of any one of Examples 1-3, wherein the alkoxy group comprises ethoxide, isopropoxide, tert-butoxide, cyclohexyl alkoxide, cyclohexene alkoxide, or cyclohexadiene alkoxide.

[0068] Example 5. The method of any one of Examples 1-4, further comprising the step of generating a metal compound from a metal precursor terminated with one or more alkoxy groups, the metal compound being an intermediate for forming a network, the step of generating the metal compound from the metal precursor comprising exposing the substrate to a vapor comprising the metal precursor and exposing the metal precursor to an alcohol, and the step of forming an EUV-active photoresist film comprising exposing the metal compound to an oxidizing agent to form a metal-oxygen-metal bond by displacing one or more of the ligands of the metal compound.

[0069] Example 6. The method of any one of Examples 1-5, wherein the step of forming an EUV-active photoresist film comprises depositing a layer comprising a metal alkoxide on the substrate by exposing the substrate to a vapor comprising a metal alkoxide, and exposing the layer comprising a metal alkoxide to an oxidizing agent to form a metal-oxygen-metal bond by replacing one or more ligands of the metal alkoxide.

[0070] Example 7. The method of any one of Examples 1-6, wherein the oxidizing agent comprises oxygen, ozone, water, air, or hydrogen peroxide.

[0071] Example 8. The method of any one of Examples 1-7, wherein the steam and the oxidant are simultaneously introduced into a process chamber holding the substrate.

[0072] Example 9. The method of any one of Examples 1-8, wherein the forming step includes depositing a layer comprising a metal alkoxide on the substrate by exposing the substrate to a vapor comprising a metal alkoxide in a plasma processing chamber, and oxidizing the layer comprising a metal alkoxide by exposing it to oxygen radicals generated in the plasma processing chamber to form a metal oxide network.

[0073] Example 10. The method of any one of Examples 1-9, wherein the step of patterning the EUV-active photoresist film comprises converting one or more of the alkoxy groups in the exposed EUV-active photoresist film to hydroxy groups, and converting the hydroxy groups to form additional metal-oxygen-metal bonds in the metal oxide network.

[0074] Example 11. A method for processing a substrate in a plasma processing chamber, comprising the steps of exposing the substrate in the plasma processing chamber to a first vapor comprising an EUV metal precursor, exposing the substrate in the plasma processing chamber to a second vapor comprising an alcohol having a hydrogen at a beta position relative to oxygen, exposing the substrate in the plasma processing chamber to a third vapor comprising an oxidizer, thereby forming a photoresist film on the substrate comprising an EUV metal alkoxide, and patterning the photoresist film by EUV lithography.

[0075] Example 12. The method of example 11, wherein the EUV metal is tin, and the step of exposing the substrate to a first vapor comprises chemically adsorbing a tin precursor to the substrate, the step of exposing the substrate to a second vapor comprises reacting an alcohol with the adsorbed tin precursor to produce tin alkoxy groups, and the step of exposing the substrate to a third vapor comprises oxidizing the adsorbed tin precursor to form a tin oxide network comprising tin-oxygen-tin bonds.

[0076] Example 13. The method of example 11 or 12, further comprising alternating between exposing the substrate to a first vapor and exposing the substrate to a second vapor a plurality of times, and performing a purging or degassing step between exposing the substrate to the first vapor and exposing the substrate to the second vapor to remove residual portions of the first vapor, the second vapor, or both.

[0077] Example 14. The method of any one of Examples 11-13, further comprising alternating between exposing the substrate to the first vapor and exposing the substrate to the second vapor a plurality of times, wherein the exposure of the substrate to the first vapor and the exposure of the substrate to the second vapor are overlapped in time.

[0078] Example 15. A method of extreme ultraviolet (EUV) lithography comprising the steps of: forming an EUV-active photoresist layer on a substrate, the EUV-active photoresist layer comprising a network of tin oxide terminated with alkoxy groups; exposing the substrate to EUV radiation through an optical mask comprising a pattern to form exposed regions of the EUV-active photoresist layer, one or more alkoxy groups in the exposed regions undergo beta hydrogen elimination to produce tin hydroxide by eliminating an alkene; and developing the EUV-active photoresist layer.

[0079] Example 16. The method of example 15, further comprising exposing the substrate to EUV radiation followed by a post-exposure bake to form tin-oxygen-tin bonds by condensation of the hydroxy groups of the tin hydroxide.

[0080] Example 17. The method of example 15 or 16, wherein developing the EUV active photoresist layer removes unexposed areas of the EUV active photoresist layer.

[0081] Example 18. The method according to any one of Examples 15 to 17, wherein the step of developing the EUV active photoresist layer is carried out by a wet process.

[0082] Example 19. The method according to any one of Examples 15-18, wherein the step of developing the EUV active photoresist layer is performed by a dry process using a plasma process, a thermal process, or both.

[0083] Example 20. The method of any one of Examples 15-19, further comprising, prior to developing the EUV active photoresist layer, performing an area-selective deposition process to selectively form a material layer on the exposed areas of the EUV active photoresist layer.

[0084] The present invention has been described with reference to several exemplary embodiments, which are not intended to be construed in a limiting sense. Various modifications and combinations of the exemplary embodiments, as well as other embodiments of the invention, will be apparent to those skilled in the art upon reference to the above description. It is therefore intended that the appended claims cover such modifications or embodiments.

Claims

1. 1. A method of processing a substrate, comprising: forming an extreme ultraviolet (EUV) active photoresist film on the substrate, the photoresist film comprising an alkoxy-terminated metal oxide network; patterning the EUV active photoresist film by EUV lithography; The method includes:

2. The method of claim 1 , wherein one or more of the alkoxy groups contains a hydrogen at the beta position relative to the oxygen.

3. The method of claim 1 , wherein the metal oxide is tin oxide.

4. The method of claim 1, wherein the alkoxy group comprises ethoxide, isopropoxide, tert-butoxide, cyclohexyl alkoxide, cyclohexene alkoxide, or cyclohexadiene alkoxide.

5. The method further includes a step of forming a metal compound having one or more of the alkoxy groups at its terminal end from a metal precursor, the metal compound being an intermediate for forming the network, the step of forming the metal compound from the metal precursor comprising: exposing the substrate to a vapor containing the metal precursor; and exposing said metal precursor to an alcohol; Including, The step of forming an EUV active photoresist film comprises: exposing said metal compound to an oxidizing agent to form a metal-oxygen-metal bond by displacing one or more of the ligands of said metal compound; The method of claim 1 , comprising:

6. The step of forming an EUV active photoresist film comprises: depositing a layer comprising a metal alkoxide on the substrate by exposing the substrate to a vapor comprising a metal alkoxide; and exposing the layer comprising a metal alkoxide to an oxidizing agent to form a metal-oxygen-metal bond by displacing one or more ligands of the metal alkoxide. The method of claim 1 , comprising:

7. The method of claim 6 , wherein the oxidizing agent comprises oxygen, ozone, water, air, or hydrogen peroxide.

8. The method of claim 6 , wherein the vapor and the oxidizer are introduced simultaneously into a processing chamber holding the substrate.

9. The forming step further comprises: depositing a layer comprising a metal alkoxide on the substrate by exposing the substrate to a vapor comprising a metal alkoxide in a plasma processing chamber; and oxidizing the layer comprising a metal alkoxide by exposing it to oxygen radicals generated in the plasma processing chamber to form the network of metal oxides; The method of claim 1 , comprising:

10. The step of patterning the EUV active photoresist film includes: converting one or more of the alkoxy groups in the exposed EUV-active photoresist film to a hydroxy group; and converting said hydroxy groups to form additional metal-oxygen-metal bonds in said metal oxide network; The method of claim 1 , comprising:

11. 1. A method of processing a substrate in a plasma processing chamber, comprising: exposing the substrate in the plasma processing chamber to a first vapor comprising an EUV metal precursor; exposing the substrate in the plasma processing chamber to a second vapor comprising an alcohol having a hydrogen in a beta position relative to oxygen; forming a photoresist film comprising an EUV metal alkoxide on the substrate by exposing the substrate in the plasma processing chamber to a third vapor comprising an oxidizer; patterning the photoresist film by EUV lithography; The method includes:

12. 12. The method of claim 11, wherein the EUV metal is tin, and the step of exposing the substrate to the first vapor comprises chemically adsorbing a tin precursor to the substrate, the step of exposing the substrate to the second vapor comprises reacting the alcohol with the adsorbed tin precursor to produce tin alkoxy groups, and the step of exposing the substrate to the third vapor comprises oxidizing the adsorbed tin precursor to form a tin oxide network comprising tin-oxygen-tin bonds.

13. alternating between exposing the substrate to the first vapor and exposing the substrate to the second vapor a plurality of times; performing a purging or degassing step between said exposure of said substrate to said first vapor and said exposure of said substrate to said second vapor to remove residual portions of said first vapor, said second vapor, or both; The method of claim 11 further comprising:

14. 12. The method of claim 11, further comprising alternating between exposing the substrate to the first vapor and exposing the substrate to the second vapor a plurality of times, wherein the exposing of the substrate to the first vapor and the exposing of the substrate to the second vapor are overlapped in time.

15. 1. A method of extreme ultraviolet (EUV) lithography, comprising: forming an EUV active photoresist layer on a substrate, the EUV active photoresist layer comprising a network of alkoxy terminated tin oxide; exposing the substrate to EUV radiation through an optical mask containing a pattern to form exposed areas of the EUV active photoresist layer, wherein one or more alkoxy groups in the exposed areas undergo beta hydrogen elimination to produce tin hydroxide by eliminating an alkene; developing the EUV active photoresist layer; The method includes:

16. 16. The method of claim 15, further comprising the step of performing a post-exposure bake after exposing the substrate to EUV radiation to condense hydroxy groups of the tin hydroxide to form tin-oxygen-tin bonds.

17. 16. The method of claim 15, wherein developing the EUV active photoresist layer removes unexposed areas of the EUV active photoresist layer.

18. 16. The method of claim 15, wherein developing the EUV active photoresist layer is performed by a wet process.

19. 16. The method of claim 15, wherein developing the EUV active photoresist layer is performed by a dry process using a plasma process, a thermal process, or both.

20. 16. The method of claim 15, further comprising performing an area-selective deposition process to form a material layer selectively over the exposed areas of the EUV active photoresist layer before developing the EUV active photoresist layer.

Citation Information

Patent Citations

  • Method for forming an EUV patternable hard mask

    JP2021523403A

  • Dry-deposited photoresists containing organic coreactants

    JP2023534960A

  • Positive tone development of CVD EUV resist films

    WO2021072042A1