HOT-ROLLED STEEL SHEET AND ITS MANUFACTURING METHOD
A controlled alloy composition and manufacturing process for high-strength hot-rolled steel sheets with 80% autotempered martensite and balanced microstructures address the challenge of achieving both high yield strength and shape straightening properties, resulting in a steel sheet with improved uniformity and stability.
Patent Information
- Application Number
- JP2024530023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-22
- Filing Date
- 2022-11-07
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-11-07
AI Technical Summary
Existing methods for manufacturing high-strength hot-rolled steel sheets struggle to achieve both high yield strength and excellent shape straightening properties, particularly for sheets with yield strengths of 900 MPa or more, due to rapid phase transformation during cooling which leads to poor shape quality.
A specific alloy composition and controlled manufacturing process involving reheating, hot rolling, and precise cooling conditions are employed to create a microstructure with 80% autotempered martensite and controlled austenite, bainite, and ferrite fractions, adhering to certain relational expressions to ensure uniformity and strength.
The method results in a high-strength hot-rolled steel sheet with excellent shape straightening properties, maintaining a wave height of 10 mm or less and yield strength of 900 MPa or more, while ensuring material uniformity and stability.
Smart Images

Figure 2024542247000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet and a manufacturing method thereof. [Background technology]
[0002] High-strength hot-rolled steel sheets are used in a variety of applications, including boom arms for special-purpose vehicles such as cranes and concrete pump trucks, and frames for trucks and trailers. The thickness of steel sheets used for such applications is generally around 3 to 10 mm, and high-strength hot-rolled steel sheets, which are thicker than general automotive steel sheets, are required to have not only high yield strength to support the design load, but also excellent shape quality for part processing and stability. In particular, when high-strength hot-rolled steel sheets have excellent shape quality, they have the advantage of being able to improve the stability of large structures because their quality remains sound even after processing.
[0003] Patent Document 1 is a technology that aims to minimize residual stress and ensure quality shape by controlling the alloy composition and annealing and cooling conditions, while Patent Document 2 is a technology that aims to ensure quality shape by controlling the alloy composition and annealing and cooling conditions and adding a heat treatment process.
[0004] However, the above Patent Documents 1 and 2 include an annealing process that can apply various cooling conditions as a manufacturing method for cold-rolled steel sheets, but hot-rolled steel sheets are manufactured without additional processes after hot rolling, unlike cold-rolled steel sheets, and therefore the shape quality of the steel sheets is significantly deteriorated even if shape correction is performed due to the rapid phase transformation during cooling and high yield strength. Furthermore, while it is possible to actually manufacture general high-strength hot-rolled steel sheets so as to obtain target physical properties, it is practically difficult to improve the shape quality through commonly used shape correction in the case of high-strength hot-rolled steel sheets with a yield strength of 900 MPa or more.
[0005] For this reason, there is a demand for the development of a technique that can increase the shape correctability of high-strength hot-rolled steel sheet having high yield strength. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Publication No. 10-1228753 [Patent Document 2] Korean Patent Publication No. 10-1568495 Summary of the Invention [Problem to be solved by the invention]
[0007] One aspect of the present invention is to provide a high-strength hot-rolled steel sheet excellent in shape correctability and a manufacturing method thereof. [Means for solving the problem]
[0008] One embodiment of the present invention provides a hot-rolled steel sheet having a microstructure containing, by weight%, 0.06-0.12% C, 0.004-0.4% Si, 0.8-2.0% Mn, 0.01-0.05% Al, 0.05-1.0% Cr, 0.001-0.3%, 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other unavoidable impurities, satisfying the following Relational Formula 1, and containing, by area%, 5-15% austenite, 80% or more autotempered martensite, and the balance being one or more of bainite and ferrite. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20
[0009] Another embodiment of the present invention provides a hot-rolled steel sheet containing, by weight %, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other inevitable impurities, satisfying the following Relational Formula 1, having a microstructure containing, by area %, 80% or more of autotempered martensite and the balance being one or more of fresh martensite, bainite and ferrite, and having a wave height in the longitudinal direction of the steel sheet of 10 mm or less. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20
[0010] Another embodiment of the present invention has, in weight percent, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0. The present invention provides a method for producing a hot-rolled steel sheet, the method including the steps of: reheating a slab containing 0.001-0.005% Cu, the balance Fe and other unavoidable impurities, and satisfying the following relational expression 1, at 1200-1350°C; hot rolling the reheated slab at 800-1200°C to obtain a hot-rolled steel sheet so as to satisfy the following relational expression 2; and primarily cooling, secondary cooling and coiling the hot-rolled steel sheet so as to satisfy the following relational expressions 3-6. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20 [Relationship 2] FDT≧896-251[C]+37.5[Si]-31.6[Mn]-7.16[Cr]+29.5[Mo]+129[Ti]-107[Nb] [Relationship 3] MTL ≤ MT ≤ MTU [Relationship 4] CRL≦ICR [Equation 5] TCR≦80℃ / sec [Equation 6] MTL-100≦CT (However, in the above Relational Formulas 2 to 6, FDT means the surface temperature of the hot-rolled steel sheet at the end of hot rolling, MT means the surface temperature of the hot-rolled steel sheet at the end of the first cooling and the start of the second cooling, MTL means 430-380[C]-13.4[Si]-47.3[Mn]-16.0[Cr]-24.2[Mo], MTU means 481-358[C]-16.6[Si]-45.6[Mn]-15.2[Cr]-24.1[Mo], ICR means the first cooling rate of the hot-rolled steel sheet surface from FDT to MT, CRL means 10[2.9-(0.1[C]+0.9[Mn]+0.5[Cr]+1.2[Mo])]+10, TCR means the average cooling rate of the hot-rolled steel sheet surface from FDT to CT, and CT means the coiling temperature.)
[0011] Another embodiment of the present invention is a steel sheet having, by weight percent, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, and the balance. The present invention provides a method for producing a hot-rolled steel sheet, the method including: reheating a slab containing Fe and other unavoidable impurities and satisfying the following relational expression 1 at 1200 to 1350°C; hot rolling the reheated slab at 800 to 1200°C so as to satisfy the following relational expression 2 to obtain a hot-rolled steel sheet; primary cooling, secondary cooling and coiling of the hot-rolled steel sheet so as to satisfy the following relational expressions 3 to 6; and leveling the coiled hot-rolled steel sheet. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20 [Relationship 2] FDT≧896-251[C]+37.5[Si]-31.6[Mn]-7.16[Cr]+29.5[Mo]+129[Ti]-107[Nb] [Relationship 3] MTL ≤ MT ≤ MTU [Relationship 4] CRL≦ICR [Equation 5] TCR≦80℃ / sec [Equation 6] MTL-100≦CT (However, in the above Relational Formulas 2 to 6, FDT means the surface temperature of the hot-rolled steel sheet at the end of hot rolling, MT means the surface temperature of the hot-rolled steel sheet at the end of the first cooling and the start of the second cooling, MTL means 430-380[C]-13.4[Si]-47.3[Mn]-16.0[Cr]-24.2[Mo], MTU means 481-358[C]-16.6[Si]-45.6[Mn]-15.2[Cr]-24.1[Mo], ICR means the first cooling rate of the hot-rolled steel sheet surface from FDT to MT, CRL means 10[2.9-(0.1[C]+0.9[Mn]+0.5[Cr]+1.2[Mo])]+10, TCR means the average cooling rate of the hot-rolled steel sheet surface from FDT to CT, and CT means the coiling temperature.) Effect of the Invention
[0012] According to one aspect of the present invention, there is provided a high-strength hot-rolled steel sheet excellent in shape correctability and a method for manufacturing the same. [Brief description of the drawings]
[0013] [Figure 1] 1 is a graph showing the relationship between the yield strength and the wave height after leveling for Examples 1 to 6 and Comparative Examples 1 to 10. [Diagram 2] These are photographs of the microstructure of Example 16 before (left) and after (right) leveling, observed by EBSD and an electron microscope, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In order to manufacture a hot-rolled steel sheet having high strength and excellent shape straightening, the above physical properties must be secured simultaneously during the hot rolling process without undergoing an additional heat treatment process. In general, a steel material having high strength must contain a low-temperature transformation phase such as martensite or bainite in order to secure strength, and in order to secure such a low-temperature transformation phase, the steel must be cooled at a high cooling rate and a low cooling stop temperature during the cooling process in the hot rolling process. However, in this case, the corrugation height of the hot-rolled steel sheet is very large, and the yield strength is also increased, making shape straightening difficult.
[0015] The present inventors have completed the present invention based on the discovery that a hot-rolled steel sheet having high yield strength and excellent shape correctability can be produced by precisely controlling the alloy composition and production conditions.
[0016] The present invention will be described below. First, the alloy composition of the present invention will be described. The contents of the alloy compositions described below are expressed in terms of weight percent.
[0017] C: 0.06-0.12% C is the most economical and effective element for strengthening steel, and when the amount of C added is increased, the fraction of martensite and bainite increases, and the tensile strength and yield strength increase. In particular, the strength of tempered martensite or martensite is absolutely affected by the C content. If the C content is less than 0.06%, it is difficult to obtain a sufficient strengthening effect compared to the yield strength to be obtained in the present invention, and if it exceeds 0.12%, there is a problem that the martensite becomes too hard, so that brittleness increases and shape correction property decreases, and there is also a defect that weldability and material uniformity deteriorate. Therefore, the C content is preferably in the range of 0.06 to 0.12%. The lower limit of the C content is more preferably 0.065%, and more preferably 0.07%. The upper limit of the C content is more preferably 0.115%, and more preferably 0.110%.
[0018] Silicon: 0.004 to 0.4% Si is an element that deoxidizes molten steel, exerts a solid solution strengthening effect in the matrix, delays the formation of coarse carbides to concentrate C, and is advantageous in retaining austenite even after cooling when certain cooling conditions are met. If the Si content is less than 0.004%, the effect of delaying the formation of carbides is insufficient, making it difficult to retain austenite, and the process cost of controlling the Si content is excessively high. If the Si content exceeds 0.4%, red scale due to Si is formed on the steel sheet surface during hot rolling, resulting in extremely poor surface quality of the steel sheet, as well as reduced bendability and material uniformity, ultimately resulting in poor shape correctability. Therefore, the Si content is preferably in the range of 0.004 to 0.4%. The lower limit of the Si content is more preferably 0.01%, further preferably 0.03%, and most preferably 0.05%. The upper limit of the Si content is more preferably 0.25%, further preferably 0.18%, and most preferably 0.15%.
[0019] Mn: 0.8-2.0% Mn, like Si, is an element effective in solid solution strengthening steel, and increases the hardening ability of steel, facilitating the formation of low-temperature transformation structures such as martensite and bainite during cooling. However, if the Mn content is less than 0.8%, the effect is excessively low, and the insufficient hardening ability is supplemented with other elements, resulting in a large burden of increased alloy costs. On the other hand, if the Mn content exceeds 2.0%, segregation develops significantly at the center of the thickness during slab casting in the continuous casting process, and microstructures are formed non-uniformly in the thickness direction during cooling, resulting in poor material uniformity and poor shape correctability. In addition, it weakens grain boundaries and excessively increases the brittleness of steel. Therefore, the Mn content is preferably in the range of 0.8 to 2.0%. The lower limit of the Mn content is more preferably 0.9%. The upper limit of the Mn content is more preferably 1.8%, and even more preferably 1.7%.
[0020] Al: 0.01 to 0.05% Al is a component added mainly for deoxidation, and if its content is less than 0.01%, the above effect becomes insufficient. On the other hand, if the Al content exceeds 0.05%, AlN is formed by bonding with nitrogen, which makes it easy for corner cracks to occur in the slab during continuous casting, and defects due to the formation of inclusions are likely to occur. In addition, it may also have an adverse effect on shape correction. Therefore, the Al content is preferably in the range of 0.01 to 0.05%. The lower limit of the Al content is more preferably 0.015%, and even more preferably 0.02%. The upper limit of the Al content is more preferably 0.045%, and even more preferably 0.04%.
[0021] Cr: 0.05~1.0% Cr strengthens the steel through solid solution and increases the hardening ability of the steel during cooling, suppressing the formation of ferrite, while at the same time helping the formation of low-temperature transformation structures such as martensite and bainite. If the Cr content is less than 0.05%, the above effects are not obtained or are excessively small. On the other hand, if the Cr content exceeds 1.0%, segregation at the thickness center begins to develop significantly, as with Mn, and the microstructure in the thickness direction becomes non-uniform, deteriorating the material uniformity and shape correctability. In addition, the formation of bainite is promoted more than the tempered martensite targeted by the present invention, making it difficult to ensure strength. Therefore, the Cr content is preferably in the range of 0.05 to 1.0%. The lower limit of the Cr content is more preferably 0.07%, and even more preferably 0.1%. The upper limit of the Cr content is more preferably 0.9%.
[0022] Mo: 0.001 to 0.3% Mo increases the hardening ability of steel and facilitates the formation of low-temperature transformation structures such as martensite and bainite, and it is known that these effects are as strong as those of Mn. However, unlike Mn, Mo strengthens grain boundaries to suppress brittleness while increasing strength. If the Mo content is less than 0.001%, the above effects cannot be obtained sufficiently, and if it exceeds 0.3%, it may cause regions in which the material uniformity and shape correctability are partially deteriorated due to the precipitates growing coarsely by combining with C formed during coiling after hot rolling. In addition, since Mo is an expensive element, it is disadvantageous in terms of manufacturing costs and is harmful to weldability. Therefore, the Mo content is preferably in the range of 0.001 to 0.3%. The lower limit of the Mo content is more preferably 0.03%, further preferably 0.05%, and most preferably 0.07%.
[0023] P: 0.001 to 0.05% P is an element that has a high solid solution strengthening effect, but generates brittleness due to grain boundary segregation, which inhibits material uniformity and shape correctability. If the P content exceeds 0.05%, as described above, sudden breakage may occur during shape correction due to brittleness due to grain boundary segregation, and shape correctability may deteriorate. It is advantageous to control the P content to be as small as possible, but manufacturing to less than 0.001% requires high manufacturing costs and is economically disadvantageous. Therefore, the P content is preferably in the range of 0.001 to 0.05%. The lower limit of the P content is more preferably 0.002%, even more preferably 0.003%, and most preferably 0.005%. The upper limit of the P content is more preferably 0.03%, even more preferably 0.02%, and most preferably 0.015%.
[0024] S: 0.001 to 0.005% S is an impurity present in steel, and if its content exceeds 0.005%, it combines with Mn and the like to form nonmetallic inclusions, which easily cause fine cracks when the steel is bent, greatly reducing impact resistance, and impairs material uniformity and shape correctability. On the other hand, it is advantageous to control the S content to be as low as possible, but to produce it to less than 0.001%, it takes a lot of time and energy during steelmaking operations, and productivity decreases. Therefore, the S content is preferably in the range of 0.001 to 0.005%. The lower limit of the S content is more preferably 0.002%. The upper limit of the S content is more preferably 0.004%.
[0025] N: 0.001 to 0.01% The above N, together with C, is a typical solid solution strengthening element, and may form coarse precipitates together with Ti, Al, etc. In general, it is known that the solid solution strengthening effect of N is superior to that of carbon. However, if the content of N exceeds 0.01%, there is a problem that the toughness is greatly reduced. On the other hand, in order to manufacture the above N content to less than 0.001%, it takes a lot of time during steelmaking operation, and the productivity decreases. Therefore, the content of N is preferably in the range of 0.001 to 0.01%. The lower limit of the above N content is more preferably 0.002%, further preferably 0.003%, and most preferably 0.004%. The upper limit of the above N content is more preferably 0.009%, and further preferably 0.008%.
[0026] Nb: 0.001 to 0.05% Nb, together with Ti and V, is a typical precipitation strengthening element, and is effective in improving strength and impact toughness through the effect of refining crystal grains by precipitating during hot rolling and delaying recrystallization. It is also advantageous in retaining austenite under specific cooling conditions. This increase in physical properties can improve shape correction. If the Nb content is less than 0.001%, the above effect cannot be obtained. On the other hand, if the Nb content exceeds 0.05%, there is a problem that the Nb content grows into coarse composite precipitates and deteriorates the material uniformity. Therefore, the Nb content is preferably in the range of 0.001 to 0.05%. The upper limit of the Nb content is more preferably 0.03%, further preferably 0.02%, and most preferably 0.01%.
[0027] Ti: 0.001 to 0.05% Ti, together with Nb and V, is a representative precipitation strengthening element, and forms TiN in steel due to its strong affinity with N. TiN has the effect of suppressing the growth of crystal grains during the heating process for hot rolling, and is advantageous in utilizing B added to improve hardening ability through stabilization of solute N. In addition, Ti that reacts with nitrogen and remains is dissolved in steel and combines with carbon to form TiC precipitates, making it a useful component for additionally improving the strength of steel. If the Ti content is less than 0.001%, the above effect cannot be obtained, while if it exceeds 0.05%, there is a problem that the material uniformity is deteriorated due to the generation of coarse TiN and the coarsening of precipitates during heat treatment. Therefore, the Ti content is preferably in the range of 0.001 to 0.05%. The lower limit of the Ti content is more preferably 0.005%, more preferably 0.01%, and most preferably 0.02%. The upper limit of the Ti content is more preferably 0.04%, and even more preferably 0.03%.
[0028] B: 0.001 to 0.005% B has the effect of improving hardening ability when present in a solid solution state in steel, has the effect of stabilizing grain boundaries to improve the brittleness of steel in low temperature regions, and has the effect of strengthening grain boundaries even in a small amount. If the content of B is less than 0.001%, it is difficult to obtain the above effect, while if it exceeds 0.005%, it may delay recrystallization behavior during hot rolling, greatly increase hardening ability, deteriorate formability, and form coarse precipitates such as BN, which may increase the brittleness of steel. Therefore, the content of B is preferably in the range of 0.001 to 0.005%. The upper limit of the B content is more preferably 0.004%, and even more preferably 0.003%.
[0029] On the other hand, the hot-rolled steel sheet of the present invention preferably satisfies the above-mentioned alloy composition and at the same time satisfies the following relational formula 1 (hereinafter, the left side of the following relational formula 1 may be referred to as "T"), in which the content of each alloy element is expressed in weight percent.
[0030] [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20
[0031] The above-mentioned relational expression 1 is a component relational expression for controlling the microstructure. When the value of T exceeds 20, a sufficient low-temperature structure is obtained, but the uneven distribution of Mn segregation zones and retained austenite increases, making it impossible to obtain uniform physical properties, and therefore, sufficient shape correction effect cannot be obtained. Therefore, the value of T is preferably 20 or less. The value of T is more preferably 19 or less, further preferably 17 or less, and most preferably 16 or less. On the other hand, the smaller the value of T, the more advantageous it is for ensuring a uniform microstructure and physical properties, so the present invention does not particularly limit the lower limit of the value of T.
[0032] The remaining component of the present invention is iron (Fe). However, since unintended impurities may be inevitably mixed from raw materials or the surrounding environment during normal manufacturing processes, it is not possible to exclude them. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them will not be specifically mentioned in this specification.
[0033] In this case, the inevitable impurities may contain Ni: 0.01% or less. The Ni is an expensive element, and the present invention has the advantage of being economical because excellent shape correction properties can be ensured without adding Ni. The Ni content is more preferably 0.008% or less, even more preferably 0.006% or less, and most preferably 0.005% or less.
[0034] The hot-rolled steel sheet of the present invention preferably has a microstructure before shape correction by leveling, which contains, in area %, 5 to 15% austenite, 80% or more autotempered martensite, and at least one of the remaining bainite and ferrite. The austenite reduces the yield strength to allow shape correction to be performed well, and at the same time, transforms into martensite after leveling to improve strength. If the austenite fraction is less than 5%, it is difficult to fully obtain the above effect, and if it exceeds 15%, there is a drawback that a sufficient low-temperature structure cannot be secured, and the strength of the finally obtained steel sheet decreases. The lower limit of the austenite fraction is more preferably 6%, and even more preferably 7%. The upper limit of the austenite fraction is more preferably 13%, even more preferably 11%, and most preferably 10%. The autotempered martensite exhibits the effect of providing ductility advantageous for localized and limited deformation such as shape correction, and at the same time providing high strength. If the fraction of the autotempered martensite is less than 80%, there is a drawback in that the strength of the finally obtained steel sheet is excessively low. It is more preferable that the fraction of the autotempered martensite is 82% or more. The more the autotempered martensite is formed, the more advantageous it is in terms of ensuring strength, but one or more of bainite and ferrite may be inevitably formed in the manufacturing process. Meanwhile, autotempered martensite has almost the same structure as tempered martensite formed through a short-time tempering treatment at a low temperature without a separate tempering treatment, and is characterized in that fine epsilon carbides are formed in the laths.
[0035] In the hot-rolled steel sheet of the present invention, the microstructure after shape correction by leveling preferably contains, in area %, 80% or more of autotempered martensite, and the remainder being one or more of fresh martensite, bainite, and ferrite. By transforming the austenite before leveling into martensite after leveling, not only the shape correctability but also superior strength can be ensured.
[0036] In addition, the hot-rolled steel sheet of the present invention after leveling has excellent shape straightening properties, with a wave height in the longitudinal direction of the steel sheet being 10 mm or less. Here, the wave height means the height from a valley to a peak when the steel sheet has a wave shape in the longitudinal direction.
[0037] As described above, the hot-rolled steel sheet provided before and after leveling preferably has a prior austenite average grain size of 10 to 30 μm. If the prior austenite average grain size is less than 10 μm, there is a drawback that the hardenability is reduced and sufficient low-temperature structure cannot be secured, and if it exceeds 30 μm, there is a drawback that retained austenite cannot be formed in the steel sheet due to the excessively large hardenability, and ductility is greatly reduced. The lower limit of the prior austenite average grain size is more preferably 12 μm, even more preferably 15 μm, and most preferably 17 μm. The upper limit of the prior austenite average grain size is more preferably 28 μm, and even more preferably 26 μm.
[0038] In addition, the above-mentioned hot-rolled steel sheet after leveling can have excellent strength, with a yield strength of 900 MPa or more.
[0039] Hereinafter, a method for producing a hot-rolled steel sheet according to an embodiment of the present invention will be described. Meanwhile, the method for producing a hot-rolled steel sheet according to an embodiment of the present invention may use a process in which continuous casting and hot rolling are directly connected.
[0040] First, the slab satisfying the above-mentioned alloy composition and Relational Formula 1 is reheated at 1200 to 1350°C. If the reheating temperature is less than 1200°C, the precipitates are not sufficiently redissolved, the formation of precipitates is reduced in the process after hot rolling, coarse TiN remains, and it is difficult to eliminate the segregation generated during continuous casting by diffusion. On the other hand, if the reheating temperature exceeds 1350°C, abnormal grain growth of austenite grains causes a decrease in strength and uneven structure, so the reheating temperature is preferably in the range of 1200 to 1350°C. The lower limit of the reheating temperature is more preferably 1220°C, even more preferably 1230°C, and most preferably 1250°C. The upper limit of the reheating temperature is more preferably 1330°C, even more preferably 1310°C, and most preferably 1300°C.
[0041] Thereafter, the reheated slab is hot-rolled at 800 to 1200°C to satisfy the following relational expression 2 to obtain a hot-rolled steel sheet. If the hot-rolling temperature exceeds 1200°C, the temperature of the hot-rolled steel sheet becomes high, the size of the crystal grains becomes coarse, and the surface quality of the hot-rolled steel sheet deteriorates. On the other hand, if the hot-rolling temperature is less than 800°C, when the rolling is completed, the elongated crystal grains develop due to excessive recrystallization delay, and the anisotropy becomes severe, and the formability also deteriorates, ultimately resulting in poor material uniformity and shape correctability. The lower limit of the hot-rolling temperature is more preferably 810°C, more preferably 820°C, and most preferably 830°C. The upper limit of the hot-rolling temperature is more preferably 1180°C.
[0042] On the other hand, in the present invention, it is preferable to satisfy the condition of the following Relational Formula 2 during hot rolling (hereinafter, the right side of the following Relational Formula 2 is also referred to as "FDTL"), where FDT means the surface temperature of the hot-rolled steel sheet at the end of hot rolling.
[0043] [Relationship 2] FDT≧896-251[C]+37.5[Si]-31.6[Mn]-7.16[Cr]+29.5[Mo]+129[Ti]-107[Nb]
[0044] If the FDT is lower than the FDTL, ferrite is partially formed on the surface of the steel sheet, which is at a lower temperature than the center of the thickness of the steel sheet, and a sufficient fraction of martensite cannot be formed after cooling, which causes a variation in the material properties between the center and the surface, ultimately resulting in a deterioration in shape correctability. In other words, if Relational Formula 2 is satisfied, high strength and excellent shape correctability can be obtained at the same time.
[0045] Thereafter, the hot-rolled steel sheet is subjected to primary cooling, secondary cooling, and coiling so as to satisfy the following Relational Formulas 3 to 6. In this case, in the following Relational Formulas 3 to 6, MT means the surface temperature of the hot-rolled steel sheet at the end of the primary cooling and the start of the secondary cooling, MTL means 430-380[C]-13.4[Si]-47.3[Mn]-16.0[Cr]-24.2[Mo], MTU means 481-358[C]-16.6[Si]-45.6[Mn]-15.2[Cr]-24.1[Mo], ICR means the primary cooling rate of the hot-rolled steel sheet surface from FDT to MT, CRL means 10[2.9-(0.1[C]+0.9[Mn]+0.5[Cr]+1.2[Mo])]+10, TCR means the average cooling rate of the hot-rolled steel sheet surface from FDT to CT, and CT means the coiling temperature.
[0046] When the MT is greater than the MTU, martensite cannot be formed, and when it is less than the MTL, fine and uniformly distributed austenite cannot be formed. When the ICR is lower than the CRL, sufficient martensite cannot be formed, and ferrite and bainite are formed in large amounts unintentionally, making it impossible to obtain high strength, which suppresses the formation of austenite and deteriorates shape correction. On the other hand, in the present invention, even if the ICR value is extremely high, there is no significant change in the strength of martensite, so the upper limit is not particularly limited. When the TCR is greater than 80°C / sec, a problem occurs in that austenite is exposed to a low temperature before it can be stabilized and disappears. When the CT is less than MTL-100, the coil temperature becomes excessively low, making it difficult to wind in the process. In addition, fine retained austenite formed in the process of generating a large amount of martensite phase, which is excessively hard and brittle, disappears, causing the material of the rolled plate to become non-uniform and the shape to become poor. Meanwhile, in the present invention, the upper limit of the coiling temperature is not particularly limited, but the upper limit may be 350°C in terms of ensuring strength. That is, the fine and uniformly distributed austenite formed by appropriately controlling the cooling and coiling processes is characterized in that it makes straightening easier during shape straightening by leveling, and at the same time, it disappears completely after straightening. The hot-rolled steel sheet manufactured through the above-mentioned process control can have high yield strength while having excellent shape straightening ability.
[0047] [Relationship 3] MTL ≤ MT ≤ MTU [Relationship 4] CRL≦ICR [Equation 5] TCR≦80℃ / sec [Equation 6] MTL-100≦CT
[0048] Thereafter, the method may include a step of leveling the coiled hot-rolled steel sheet. The leveling is for shape correction, and the present invention does not particularly limit the leveling process, and any conventional technique used in the art may be used. Meanwhile, the leveling is a shape correction method in which no reduction is applied to the steel sheet, and therefore, it can be distinguished from skin pass rolling in which a reduction of 0.1 to 2.0% is applied. EXAMPLES
[0049] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are intended to illustrate and embody the present invention, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.
[0050] (Example) A hot-rolled steel sheet was manufactured from a slab having the alloy composition shown in Table 1 below under the conditions shown in Table 2 below. The reheating temperature of the slab was 1250°C, and the thickness of the hot-rolled sheet immediately after hot rolling was 4 mm. Leveling was then performed using a tension leveler. The microstructure, average prior austenite grain size, wave height, and mechanical properties of the hot-rolled steel sheet before and after leveling were measured, and the results are shown in Tables 3 and 4 below, respectively. Meanwhile, in this example, a trace amount of impurities was detected even though Ni was not added.
[0051] The microstructure was measured through an Electron Back-Scattered Diffraction (EBSD) tester in an electron microscope.
[0052] The average prior austenite grain size was measured using an optical microscope after a test piece taken from the hot-rolled steel sheet produced as above was immersed in a solution prepared by mixing 200 ml of a supersaturated aqueous picric acid solution and 10 ml of a 10% aqueous sodium dodecylbenzenesulfonate solution, to which 10 ml of a 10% aqueous ferric chloride solution was added, for 10 minutes to corrode the test piece.
[0053] The wave height was measured as the maximum difference from the valley to the peak for a steel plate length of 2 m after the hot-rolled coil was unwound.
[0054] The yield strength (YS), tensile strength (TS) and elongation at break (El) were measured by taking JIS No. 5 test pieces from the hot rolled coil in the direction parallel to the rolling direction.
[0055] [Table 1]
[0056] [Table 2]
[0057] [Table 3]
[0058] [Table 4]
[0059] As shown in Tables 1 to 4 above, in the case of Examples 1 to 6, which satisfy all of the alloy compositions, relational expressions, and manufacturing conditions proposed by the present invention, it can be seen that the mechanical properties and shape quality targeted by the present invention are ensured.
[0060] In the case of Comparative Example 1, although the manufacturing conditions of the present invention are satisfied, the C content range of the present invention is exceeded and Relational Formula 1 is not satisfied. Therefore, it can be seen that the wave height after leveling is at a high level due to high strength and low shape correctability.
[0061] In the case of Comparative Example 2, although the production conditions of the present invention were satisfied, the C content did not reach the range of the present invention, and therefore the yield strength was at a low level.
[0062] In the case of Comparative Example 3, although the production conditions of the present invention are satisfied, the Mn content range of the present invention is exceeded and Relational Formula 1 is not satisfied. This leads to deterioration of shape correctability due to increased segregation and embrittlement, and the wave height after leveling is at a high level.
[0063] In the case of Comparative Example 4, although the manufacturing conditions of the present invention are satisfied, the C and Cr content ranges of the present invention are not reached, and Relational Formula 1 is not satisfied. Therefore, it is understood that the yield strength is low and the wave height after leveling is at a high level.
[0064] In the case of Comparative Example 5, although the alloy composition of the present invention is satisfied, not only was an existing hot rolling process using one-stage cooling adopted, but the MT did not satisfy the conditions of the present invention, so that it was not possible to secure an appropriate fraction of austenite before leveling, and the yield strength was also at a low level.
[0065] In the case of Comparative Example 6, since the C content exceeds the range of the present invention and the FDT is lower than the FDTL, it can be seen that the anisotropy increases due to the ferrite formed during rolling, the yield strength is low due to material non-uniformity, and the wave height after leveling is at a high level.
[0066] In the case of Comparative Example 7, although the alloy composition of the present invention is satisfied, the CT does not satisfy the conditions of the present invention, so that the appropriate fraction of austenite before leveling cannot be secured, and the wave height after leveling is at a high level.
[0067] In the case of Comparative Example 8, although the alloy composition of the present invention is satisfied, it is apparent that the ICR is lower than the CRL, and therefore the yield strength is at a low level.
[0068] In the case of Comparative Example 9, although the alloy composition of the present invention is satisfied, the TCR exceeds the condition of the present invention, so that the appropriate fraction of austenite before leveling cannot be secured, and the wave height after leveling is at a high level.
[0069] In the case of Comparative Example 10, although the production conditions of the present invention are satisfied, Relational Expression 1 is not satisfied, and therefore it is understood that the wave height after leveling is at a high level.
[0070] Fig. 1 is a graph showing the relationship between the yield strength and the wave height after leveling for Invention Examples 1 to 6 and Comparative Examples 1 to 10. As can be seen from Fig. 1, it can be confirmed that Invention Examples 1 to 6 simultaneously have a yield strength of 900 MPa or more and a wave height of 10 mm or less.
[0071] Figure 2 shows EBSD and electron microscope photographs of the microstructures before (left) and after (right) leveling for Example 16. As can be seen from Figure 2, in the case of Example 16, the austenite formed before leveling disappears after leveling, and it can be confirmed that the microstructure that the present invention aims to obtain is formed.
Claims
1. The composition contains, by weight, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other unavoidable impurities. The following relational expression 1 is satisfied, A hot-rolled steel sheet having a fine structure containing, by area percentage, 5 to 15% austenite, 80% or more autotempered martensite, and the remainder being one or more of bainite and ferrite. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20
2. The composition contains, by weight, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other unavoidable impurities. The following relational expression 1 is satisfied, The microstructure contains, in terms of area percentage, 80% or more of autotempered martensite, the remainder being one or more of fresh martensite, bainite, and ferrite, A hot-rolled steel sheet having a wave height of 10 mm or less in the longitudinal direction of the steel sheet. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20
3. The hot-rolled steel sheet according to claim 1 or 2, wherein the inevitable impurities include Ni: 0.01% or less.
4. The hot-rolled steel sheet according to claim 1 or 2, wherein the average prior austenite grain size of the hot-rolled steel sheet is 10 to 30 μm.
5. The hot-rolled steel sheet according to claim 2, wherein the hot-rolled steel sheet has a yield strength of 900 MPa or more.
6. a step of reheating a slab containing, in weight percent, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other inevitable impurities, and satisfying the following relational formula 1 at 1200-1350°C; hot rolling the reheated slab at 800 to 1200° C. to obtain a hot-rolled steel sheet so as to satisfy the following Relation 2: a step of primarily cooling, secondary cooling and coiling the hot-rolled steel sheet so as to satisfy the following Relational Expressions 3 to 6. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20 [Relationship 2] FDT≧896-251[C]+37.5[Si]-31.6[Mn]-7.16[Cr]+29.5[Mo]+129[Ti]-107[Nb] [Relationship 3] MTL≦MT≦MTU [Relationship 4] CRL≦ICR [Relationship 5] TCR≦80° C. / sec [Relationship 6] MTL-100≦CT (In the above-mentioned Relational Formulas 2 to 6, FDT means the surface temperature of the hot-rolled steel sheet at the end of hot rolling, MT means the surface temperature of the hot-rolled steel sheet at the end of the first cooling and the start of the second cooling, MTL means 430-380[C]-13.4[Si]-47.3[Mn]-16.0[Cr]-24.2[Mo], and MTU means 481-358[C]-16.6[Si]-45 .6[Mn]-15.2[Cr]-24.1[Mo], ICR means the primary cooling rate of the hot-rolled steel surface from FDT to MT, CRL means 10[2.9-(0.1[C]+0.9[Mn]+0.5[Cr]+1.2[Mo])]+10, TCR means the average cooling rate of the hot-rolled steel surface from FDT to CT, and CT means the coiling temperature.
7. a step of reheating a slab containing, in weight percent, C: 0.06-0.12%, Si: 0.004-0.4%, Mn: 0.8-2.0%, Al: 0.01-0.05%, Cr: 0.05-1.0%, Mo: 0.001-0.3%, P: 0.001-0.05%, S: 0.001-0.005%, N: 0.001-0.01%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, B: 0.001-0.005%, the balance being Fe and other inevitable impurities, and satisfying the following relational formula 1 at 1200-1350°C; hot rolling the reheated slab at 800 to 1200° C. to obtain a hot-rolled steel sheet so as to satisfy the following Relation 2: performing primary cooling, secondary cooling and coiling of the hot-rolled steel sheet so as to satisfy the following Relational Expressions 3 to 6; and leveling the coiled hot-rolled steel sheet. [Relationship 1] (10[C] + [Si] + 2.5[Mn]) / (1.5[Cr] + 2.0[Mo] - 3.2[Nb]) ≦ 20 [Relationship 2] FDT≧896-251[C]+37.5[Si]-31.6[Mn]-7.16[Cr]+29.5[Mo]+129[Ti]-107[Nb] [Relationship 3] MTL≦MT≦MTU [Relationship 4] CRL≦ICR [Relationship 5] TCR≦80° C. / sec [Relationship 6] MTL-100≦CT (In the above-mentioned Relational Formulas 2 to 6, FDT means the surface temperature of the hot-rolled steel sheet at the end of hot rolling, MT means the surface temperature of the hot-rolled steel sheet at the end of the first cooling and the start of the second cooling, MTL means 430-380[C]-13.4[Si]-47.3[Mn]-16.0[Cr]-24.2[Mo], and MTU means 481-358[C]-16.6[Si]-45 .6[Mn]-15.2[Cr]-24.1[Mo], ICR means the primary cooling rate of the hot-rolled steel surface from FDT to MT, CRL means 10[2.9-(0.1[C]+0.9[Mn]+0.5[Cr]+1.2[Mo])]+10, TCR means the average cooling rate of the hot-rolled steel surface from FDT to CT, and CT means the coiling temperature.
Citation Information
Patent Citations
Method for producing superhigh strength hot rolled steel sheet
JP2006274335A
High-strength hot-rolled steel sheet having excellent low temperature toughness, and method for producing the same
JP2011052320A
High strength hot dip zinc-coated steel sheet excellent in formability and impact resistance, and manufacturing method therefor
JP2012031462A
High-strength hot-rolled steel sheet having excellent bending characteristic and low-temperature toughness and method for producing the same
JP2013117068A
High-strength hot-rolled steel sheet with excellent bendability and low-temperature toughness and its manufacturing method
JP2021507107A