Plant and process for forming polymers
The described process addresses polymer degradation and VOC separation issues by using multiple heat exchangers to reduce heat exposure and phase separation, improving polymer quality and regulatory compliance.
Patent Information
- Application Number
- JP2024531067
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-23
- Filing Date
- 2022-11-17
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-11-17
AI Technical Summary
Existing polymerization processes face challenges in efficiently separating polymers from volatile organic compounds (VOCs) while minimizing polymer degradation due to high temperatures and mechanical shear, leading to production inefficiencies and non-compliance with regulatory standards.
A process involving a reactor effluent mixed with a concentrated polymer solution, passing through multiple heat exchangers before entering a phase separator, reduces heat exposure and polymer degradation by distributing heat exchange at lower temperatures, thereby minimizing phase separation and residence time.
This approach significantly reduces the production of off-spec polymers, shortens transition times between polymer grades, and enhances compliance with environmental regulations by minimizing VOCs, while maintaining polymer quality.
Smart Images

Figure 2024542263000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 63 / 282,424, filed November 23, 2021, the entire disclosure of which is incorporated herein by reference.
[0002] Field The present disclosure relates to plants and processes for forming polymers. [Background technology]
[0003] background A continuous solution polymerization process generally involves adding a catalyst to a mixture of monomer, comonomer, and solvent to form a reaction mixture. The reaction mixture may be backmixed to provide a homogenous polymer. The heat of the polymerization reaction, called the exotherm, may be absorbed by the reaction mixture. Alternatively, or in addition, the heat of reaction may be removed by a cooling system, for example, by external cooling of the reactor vessel walls, or by internally located heat exchange surfaces cooled by a heat exchange fluid. During the course of the polymerization, most of the monomer is consumed and the polymer formed remains dissolved in the solvent used during the polymerization. Typically, the higher the concentration of polymer, the higher the viscosity of the polymerization reaction mixture containing the polymer, solvent, and unreacted components. After polymerization, the reaction mixture moves from the polymerization reactor to a finishing section where the polymer, solvent, and unreacted monomers are separated (e.g., by devolatilization). In this finishing process, the solvent and unreacted monomers are gradually removed from the reaction mixture until the polymer can be formed into solid pellets or bales. The separated solvent and monomers can be recycled to the polymerization reactor. Polymer devolatilization is a technique for improving polymer quality and is used in the industrial production of adhesives, elastomers, surface coatings, and plastic materials (e.g., thermosets and thermoplastics). In the devolatilization process, volatile components such as monomers, oligomers, additives, and solvents involved in the polymerization as well as by-products can be devolatilized from the polymer. Devolatilization processes can remove residual volatile organic compounds (VOCs) from the polymer to facilitate compliance with government regulations.
[0004] One method for separating polymers from volatile organic compounds is by evaporation, where the polymer solution is heated above the vaporization temperature of the volatile components. The equipment and methods utilized often depend on the viscosity of the polymer solution, and these devices often have high initial and operating costs. To obtain high polymer output, very large equipment and high consumption of mechanical energy are usually required. Furthermore, these equipment subject the polymer to high temperatures and mechanical shear, which can potentially cause degradation of the polymer's physical properties. Furthermore, techniques that heat the polymer solution in a heat exchange zone involve exposing the polymer solution to high temperatures for extended periods of time. Such exposure to heat can cause thermal degradation of the heat-sensitive polymer, resulting in discoloration of the polymer and / or loss of properties such as impact strength. Furthermore, techniques that avoid degradation of the heat-sensitive polymer can result in low production. For example, the polymer typically undergoes mild temperatures and long residence times in the devolatilizer. When this occurs, production is compromised due to low flow rates through the devolatilizer.
[0005] When the effluent is removed from the polymerization reactor, heat can be introduced to the effluent from the polymerization reactor by a heat exchanger before the reactor effluent is introduced into the devolatilization vessel. However, such a heat exchanger must provide substantial heat for the subsequent devolatilization to occur in the devolatilization vessel, which promotes polymer decomposition and fouling in the lines transporting the reactor effluent and in the devolatilization vessel. Alternatively, the concentrated polymer removed from the devolatilization vessel may be recycled directly to the devolatilization vessel through a line connected to the heat exchanger. This heat exchanger must provide substantial heat for the devolatilization to occur, which results in polymer decomposition and fouling in the recycle lines and in the devolatilization vessel. Furthermore, the heat exchanger must maintain high pressure while operating at high temperatures to prevent undesirable phase separation of the mixture of polymer and volatiles inside the heat exchanger.
[0006] Furthermore, the presence of the recycle line (and the presence of recycled concentrated polymer in the devolatilization vessel due to the polymer recycle) significantly increases the residence time of the devolatilization process compared to a vessel without a recycle line. This residence time can be even longer if the size of the recycle heat exchanger must be large due to the large amount of heat required (provided by the recycled concentrated polymer). For example, a recycle of 725,000 lb / hr or more of recycled concentrated polymer from the devolatilization vessel is typically provided (via a line) to a heat exchanger (operating with a heat addition of 55 MMBtu / hr or more to the recycle stream) before the heated recycled polymer is directly reintroduced into the devolatilization vessel. Such additional heating not only accelerates the degradation of the polymer, but in plants producing multiple different grades of polymer, it also makes the transition time between the production of different polymer grades very long and expensive (due to the large amount of polymer present in the recycle line when the recycle line is shut down to transition to a different polymer grade). For example, there is a need for devolatilization plants and processes that allow for short transition times between polymer grades in a manner that also reduces the amount of off-spec material produced (e.g., cracked polymer and less-recycled concentrated polymer in the recycle line). Summary of the Invention
[0007] overview In some embodiments, a process for forming a polymer includes providing a feed having one or more olefin monomers and a solvent. The process includes introducing the feed into a reactor together with a catalyst to form a reaction mixture. The process includes removing a reactor effluent from the reactor and mixing the reactor effluent with a first concentrated polymer solution in a mixer or line to form a mixture. The process includes introducing the mixture into a heat exchanger to form a heated mixture, and introducing the heated mixture into a pressure let down valve before introducing the heated mixture into a phase separator. The process includes removing a second concentrated polymer solution from the phase separator. The process includes introducing the second concentrated polymer solution into a mixer or line. In some embodiments, a plant for forming a polymer includes a polymerization reactor coupled to a phase separator. The plant includes a heat exchanger and a pressure let-down valve disposed between the polymerization reactor and the phase separator. The heat exchanger is coupled to the polymerization reactor and the pressure let-down valve. The pressure let-down valve is coupled to the phase separator. The plant includes a stream stripper coupled to the phase separator and in line at a location upstream of the heat exchanger and the pressure let-down valve. These and other features and characteristics of the viscosity modifiers of the present disclosure, as well as their advantageous applications and / or uses, will be apparent from the following detailed description.
[0008] So that the above-mentioned features of the present disclosure may be understood in detail, a more particular description of the disclosure briefly summarized above may be had by reference to embodiments, some of which are illustrated in the accompanying drawings, which, however, illustrate only exemplary embodiments of the present disclosure and should not be considered as limiting the scope of the present disclosure, since the present disclosure may admit of other equally effective embodiments. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic layout of a plant and process flow for polymerization and devolatilization in accordance with an embodiment. [Diagram 2] 2 is a schematic layout of a portion of the plant and process flow of FIG. 1 (during normal operation mode) in accordance with an embodiment. [Figure 3A] 1 shows a phase separator of a plant and process flow according to an embodiment. [Figure 3B] 1 shows a phase separator of a plant and process flow according to an embodiment. [Figure 4] 1 is a heat exchanger according to an embodiment. [Diagram 5] 1 is a plate heat exchanger according to an embodiment. [Figure 6] 1 is a plate heat exchanger according to an embodiment. [Figure 7] 1 is a plate heat exchanger according to an embodiment.
[0010] To facilitate understanding, wherever possible, the same reference numerals have been used to designate identical elements common to the figures. The figures may not be to scale and may be simplified for clarity. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Detailed Description The present disclosure relates to plants and processes for forming polymers. In some embodiments, a process for forming a polymer includes providing a feed having one or more olefin monomers and a solvent. The process includes introducing the feed into a reactor with a catalyst to form a reaction mixture and removing a reactor effluent from the reactor. The process includes mixing the reactor effluent with a first concentrated polymer solution in a mixer or line to form a mixture. The process includes introducing the mixture into a heat exchanger to form a heated mixture. The process includes introducing the heated mixture into a pressure let-down valve followed by introducing the heated mixture into a phase separator. The process includes removing a second concentrated polymer solution from the phase separator. The process includes introducing the second concentrated polymer solution into a mixer or line.
[0012] In some embodiments, a plant for forming a polymer includes a polymerization reactor coupled to a phase separator. The plant includes a heat exchanger and a pressure let-down valve disposed between the polymerization reactor and the phase separator. The heat exchanger is coupled to the polymerization reactor and the pressure let-down valve, and the pressure let-down valve is coupled to the phase separator. The plant includes a stream stripper coupled to the phase separator and in line at a location upstream of the heat exchanger and the pressure let-down valve.
[0013] The disclosed plant and process provide a reactor effluent mixed with a recycle stream of concentrated polymer solution (from a phase separator, also called a devolatilizer). This mixture may pass through a heat exchanger before entering the phase separator. Heat exchange may also be accomplished using a heat exchanger disposed within the phase separator. Because heat exchange is provided to the mixture at two or more locations, each of the two or more heat exchange processes (of the two or more heat exchangers) can be performed at a lower temperature than a conventional single heat exchanger, resulting in a reduction in the amount of off-spec (e.g., degraded polymer) in the polymer product produced. Otherwise, the addition of all the heat in the first heat exchanger would significantly increase the heat exchanger outlet temperature, leading to undesirable phase separation of the effluent. Furthermore, providing a large amount of heat to the phase separator itself would otherwise make the vessel oversized.
[0014] Furthermore, the heat exchanger disposed in the devolatilization vessel of the present disclosure provides heat to the concentrated polymer solution exiting the phase separator, which, in addition to mixing the concentrated polymer solution with the reactor effluent prior to the first heat exchange, results in a reduction in the amount of heat that can be used for the first heat exchange (further reducing polymer degradation). Because the first heat exchange (between the reactor effluent and the recycled concentrated polymer solution) does not require as much heat, less recycled concentrated polymer solution can be used during the normal operating mode of the plant. Because less recycled concentrated polymer solution can be used during the normal operating mode, this results in a reduction in the amount of off-spec generated (e.g., decomposed polymer and less recycled concentrated polymer solution in the recycle line), as well as a reduction in the transition time between polymer grades. For example, in some embodiments, the plants and / or processes of the present disclosure employ a recycle of up to 500,000 lb / hr, e.g., up to 400,000 lb / hr, e.g., from about 100,000 lb / hr to about 400,000 lb / hr, e.g., from about 200,000 lb / hr to about 300,000 lb / hr, of concentrated polymer recycled from the devolatilization.
[0015] Additionally, the presence of recycled concentrated polymer solution in the first heat exchanger results in the reduction or elimination of phase separation of the mixture (liquid-liquid or gas-liquid) inside the heat exchanger that would otherwise cause heat transfer and operational problems. Due to the transition mode, the disclosed plants and processes allow for the recycle stream of concentrated polymer solution to be closed off so that there is no significant amount of off-spec (e.g., concentrated polymer stuck inside the recycle line and heat exchangers in the line) during the grade transition. In other words, the devolatilization can have a reduced devolatilization residence time, e.g., a reduced devolatilization residence time of 1 / 3 or more compared to conventional devolatilization processes. Additionally, the heat exchangers of the present disclosure (e.g., disposed within the devolatilization vessel) can have a tube-and-tube design in which tubes are grouped together in bundles to form, for example, 8000 m 2 Compared to conventional tube bundles, the heat exchanger of the present disclosure can provide a significant distribution of the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution) and increase the gas-liquid interface of the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution).
[0016] Polymerization conditions In some embodiments, a process for forming a polymer is provided, the process comprising: (a) providing a feed having one or more monomers and a solvent; (b) introducing the feed into a reactor along with a catalyst; and (c) removing a reactor effluent from the reactor for further processing. In one or more embodiments, the reactor can be a single reactor or multiple reactors, for example, two reactors arranged in parallel or series. One or more of the reactors can be a loop reactor. Additionally or alternatively, the reactor is a continuous stirred tank reactor. In one or more embodiments, the two reactors are arranged in parallel or series, and the ratio of the internal volume of the first reactor to the internal volume of the second reactor can have a minimum ratio value of 50:50, 55:45, 60:40, 65:35, 70:30, 80:10, 85:15, or 90:10, and a maximum ratio value of 55:45, 60:40, 65:35, 70:30, 80:20, 85:15, 90:10, or 95:5, as long as the maximum ratio value is greater than the minimum ratio value. The reaction mixture from the two reactors is combined and then sent to a phase separator.
[0017] The monomers and catalysts may be fed to the reactor by any suitable unit or device. The plant may include a feed supply unit for feeding a feed having one or more olefin monomers in a solvent, e.g., a hydrocarbon solvent. The plant of the present disclosure may also include a catalyst supply unit suitable for feeding a catalyst to the reactor. A feed supply unit suitable for feeding one or more olein monomers in a solvent to the reactor may be any suitable device, but will typically include a feed conduit for each monomer, a feed conduit for a recycle solvent, and a feed conduit for a fresh solvent. Each of these conduits may be fed to a common feed conduit before entering the reactor. One or more pumps may be used to feed the feed to the reactor or reactors and pressurize the feed to the desired pressure. A catalyst supply unit suitable for feeding a catalyst to the reactor may be any suitable device, but will typically include a feed conduit for the catalyst and, optionally, one or more pumps for feeding the catalyst to the reactor or reactors.
[0018] The solvent used for the polymerization can be any suitable solvent, such as hexane and / or isohexane. For example, the solvent is a non-polar solvent that does not coordinate or interact with the catalyst, in the sense that it does not inhibit the catalytic action of the catalyst system. The process of the present application can use low boiling alkane solvents, or mixtures thereof, which may be linear or branched, for example, having 4 to 10 carbon atoms, preferably 5 to 7 carbon atoms, optionally in mixtures with other alkanes of higher or lower molecular weight. The polymers may be derived from monomers containing monoolefins such as ethylene or propylene or other higher alpha olefins having 4 to 10 carbon atoms. This combination gives a mixture that can be easily separated in a liquid phase separator.
[0019] The operating pressure of the reactors described herein can be 8 MPa or more, 9 MPa or more; 10 MPa or more, 12 MPa or more, or 14 MPa or more. The upper pressure is not strictly constrained, but can typically be 20 MPa or less, e.g., 18 MPa or less, or 15 MPa or less, or 14 MPa or less, or 12 MPa or less. In some embodiments, the pressure is sufficient to keep the reaction mixture in a single phase and provide a working pressure to transport the fluids through the plant. The feed temperature may vary depending on the available exotherm and the degree of monomer conversion desired to reach the polymerization temperature. In some embodiments, the temperature is 40° C. or less, or 20° C. or less, or 0° C. or less, or -20° C. or less. The polymerization temperature may vary depending on the desired molecular weight of the polymer, allowing for the influence of any chain transfer agents, such as added hydrogen. In a series reactor process, the temperature in the series of reactors may be increased progressively in increments depending on the nature of the polymerization occurring in the reactors. In some embodiments, the polymerization temperature for polymers containing predominantly (e.g., 50 wt. % or more) ethylene-derived units is at least 100° C., or at least 150° C., or 200° C. or more, depending on the particular polymer being synthesized. The temperature should not exceed the polymerization decomposition temperature or the temperature at which the catalyst can sustain the polymerization reaction.
[0020] Overall, the exotherm can result in a temperature difference between the inlet and outlet temperatures of the polymerization reactor of from 50° C. to 220° C. or even 250° C. In one or more embodiments, feeding the feed at minus 40° C. and letting the exotherm increase the temperature to 210° C. can result in the process producing lower molecular weight polymers. For higher molecular weight polymers, it may be necessary to limit the temperature increase by warmer feeds and / or lower reactor temperatures to avoid excessive viscosity of the reactor solution, which would degrade the mixing performance of the reactor and thereby result in a non-uniform polymer. The monomer concentration may depend on the type and molecular weight of the polymer desired, the associated conversion of monomer to polymer, and the operating temperature. For example, the monomer concentration may be greater than 10 wt%, or 15 wt%, or less than 80 wt%, 70 wt%, or 60 wt%. The total vapor pressure of all components may be less than 100 wt% of the reactor pressure at the stream temperature to avoid the formation of vapor bubbles.
[0021] The polymerization can be carried out using any suitable catalyst, such as a Ziegler-Natta catalyst, a single-site catalyst (SSC), or a metallocene catalyst. In one or more embodiments, an SSC or metallocene catalyst can be used. The term "metallocene" refers to one or more cyclopentadienyl moieties combined with a transition metal of the Periodic Table of Elements. As used herein, the numbering convention of the Periodic Table of Elements is used as described in CHEMICAL AND ENGINEERING NEWS, 63(5), 27 (1985). Metallocene catalysts generally contain a transition metal from Groups 3-10 of the periodic table and at least one ancillary ligand that remains bound to the transition metal during polymerization. In some embodiments, the transition metal is used in its cationic state and is stabilized by a cocatalyst or activator. In some embodiments, a metallocene from Group 4 of the periodic table, such as titanium, hafnium, or zirconium, is used in the polymerization in its monovalent cationic state and with one or two ancillary ligands.
[0022] In some embodiments, the catalyst is a bulky ligand transition metal catalyst. The "bulky ligand" contains a variety of bonded atoms, such as carbon atoms, forming a group that may be cyclic with one or more heteroatoms. The bulky ligand may be a metallocene-type cyclopentadienyl derivative, which may be mononuclear or polynuclear. One or more bulky ligands may be bonded to the transition metal atom. Other ligands may be, for example, hydrocarbyl or halogen leaving groups that are bonded or coordinated to the transition metal and are removable, for example, by a cocatalyst or activator. Removal of any of the ligands leads to the creation of a coordination site where an olefin monomer may be inserted into the polymer chain. In some embodiments, the transition metal atom is a group 4, 5 or 6 transition metal, such as a group 4 atom, of the periodic table of elements.
[0023] The metallocene catalyst can be used with a cocatalyst, which can be an alumoxane, such as methylalumoxane, having an average degree of oligomerization of 4-30 as determined by vapor pressure osmometry. The alumoxane can be modified to provide solubility for linear alkanes or used in a slurry, but typically can be used from a toluene solution. The solution can contain unreacted trialkylammonium, and the alumoxane concentration can typically be expressed as moles of Al per liter, which includes any trialkylaluminum that has not reacted to form oligomers. When used as a cocatalyst, the alumoxane can typically be used in molar excess to the transition metal, such as a molar ratio of 50 or more, such as 100 or more, such as 1000 or less, such as 500 or less. The SSC may be selected from the wide range of SSCs available to tailor the type of polymer made and its associated process window such that under process conditions an activity of at least 40,000 g, such as at least 60,000 g, or even more than 100,000 g, of polymer per gram of SSC (or metallocene) may be produced. By being able to produce different polymers at different operating windows with the selection of the appropriate catalyst, the SSC and auxiliary catalyst components may be used in smaller amounts, and in some cases with the use of small amounts of scavengers.
[0024] The metallocene may be used with a cocatalyst, which may be a non-coordinating anion (the term "non-coordinating anion" as used herein includes weakly coordinating anions, the coordination of which may be weak enough in any event evident from the progress of the polymerization to allow insertion of the unsaturated monomer component). The non-coordinating anion may be provided and reacted with the metallocene in any suitable manner. A precursor of a non-coordinating anion may be used with the metallocene provided in a reduced valence state. This precursor may undergo an oxidation-reduction reaction. The precursor may be an ion pair, and the precursor cation may be neutralized and / or removed in some manner. The non-coordinating anion may be a halogenated, tetraaryl-substituted, non-carbon-based Group 10-14 anion, particularly one having a fluorine group replacing a hydrogen atom on an aryl group or an alkyl substituent on the aryl group.
[0025] In some embodiments, useful Group 10-14 cocatalyst complexes derived from ionic salts include tetracoordinate Group 10-14 anion complexes, where the anion can be represented by the formula: [(M)Q 1 Q 2 ...Q i ] - where M is one or more Group 10-14 metalloids or metals, preferably boron or aluminum, and each Q is a suitable non-coordinating anion [(M)Q 1 Q2 ...Q i ] - or a sufficient number of Q's are effective ligands to provide an electronic or static effect that provides [(M)Q 1 Q 2 ...Q i ] - is an effective non-coordinating or weakly coordinating anion. Exemplary Q substituents include, in particular, fluorinated aryl groups, preferably perfluoroaryl groups, and substituted Q groups having substituents in addition to fluorine substitution, such as fluorinated hydrocarbyl groups. Preferred fluorinated aryl groups include phenyl, biphenyl, naphthyl, and derivatives thereof. The non-coordinating anion may be used in approximately equimolar amounts relative to the transition metal component, for example at least 0.25, preferably 0.5, especially 0.8, and for example up to 4, preferably 2, especially 1.5.
[0026] Representative metallocene compounds may have the formula: L A L B L C i MDE In the formula, L A is a substituted cyclopentadienyl or heterocyclopentadienyl ancillary ligand π-bonded to M; L B L A or J, a heteroatom ancillary ligand σ-bonded to M; L A Ligand and L B The ligands may be covalently linked together via a Group 14 element linking group; C i is an optional neutral non-oxidizing ligand having a coordinate bond to M (i is equal to 0 to 3); M is a Group 4 or 5 transition metal; and D and E independently each have a σ bond to M and are optionally connected to each other or to L. A Or L BThe monoanionic ligand is a labile monoanionic ligand bridged by a transition metal component, which can be displaced by a suitable activator to allow insertion of a polymerizable monomer or macromonomer for coordination polymerization onto the vacant coordination site of the transition metal component.
[0027] Representative nonmetallocene transition metal compounds that can be used as the SSC also include tetrabenzylzirconium, tetrabis(trimethylsilylmethyl)zirconium, oxotris(trimethylsilylmethyl)vanadium, tetrabenzylhafnium, tetrabenzyltitanium, bis(hexamethyldisilazide)dimethyltitanium, tris(trimethylsilylmethyl)niobium dichloride, and tris(trimethylsilylmethyl)tantalum dichloride. Further organometallic transition metal compounds suitable as olefin polymerization catalysts according to the embodiments described herein will be any Group 3-10 compound that can be converted to a catalytically active cation by ligand abstraction and stabilized by a non-coordinating or weakly coordinating anion that is sufficiently labile to be displaced in its active electronic state by an olefinically unsaturated monomer such as ethylene. Metallocenes that are biscyclopentadienyl derivatives of group 4 transition metals, preferably zirconium or hafnium, can be used, for example, as disclosed in WO99 / 41294. These can be derivatives that contain fluorenyl and cyclopentadienyl ligands, advantageously linked by a single carbon and silicon atom, for example, as disclosed in WO99 / 45040 and WO99 / 45041. In some embodiments, the Cp ring is unsubstituted and / or the bridge contains alkyl substituents, preferably alkylsilyl substituents, to aid the alkane solubility of the metallocene, for example, as disclosed in WO00 / 24792 and WO00 / 24793. Other possible metallocenes include those described in WO01 / 58912.
[0028] WO 97 / 03992, which is incorporated herein by reference, describes catalysts in which a single Cp species and a phenol are linked by a C or Si bond, e.g. Me 2C(Cp)(3-tBu-5-Me-2-phenoxy)TiCl 2 WO2001 / 05849, which is incorporated herein by reference, discloses Cp-phosphinimine catalysts, such as (Cp)((tBu) 3 P=N-)TiCl 2 has disclosed. Other suitable metallocenes may be, for example, bisfluorenyl derivatives or non-bridged indenyl derivatives which may be substituted at one or more positions of the fused ring with moieties which have the effect of increasing the molecular weight and indirectly allow polymerization at higher temperatures, as described in EP0693506 and EP0780395. When using the above catalysts, the total catalyst system generally further comprises one or more organometallic compounds as scavengers. The scavengers include those compounds that are effective for removing polar impurities from the reaction environment and for enhancing catalyst activity. Impurities may be inadvertently introduced with any of the polymerization reaction components, particularly with the solvent, monomer and catalyst feed, and may adversely affect the activity and stability of the catalyst, reducing or even eliminating the catalyst activity, especially when ionized anion precursors activate the catalyst system. Impurities or catalyst poisons include water, oxygen, polar organic compounds, metal impurities, etc. Some embodiments incorporate steps to remove these poisons before their introduction into the reaction vessel, for example by chemical treatment or careful separation techniques after or during the synthesis or preparation of the various components, but still some small amount of organometallic compounds will usually be used in the polymerization process itself.
[0029] The scavenger may be an organometallic compound, such as the Group 13 organometallic compounds of U.S. Patents 5,153,157 and 5,241,025, International Publication Nos. WO 91 / 09882, WO 94 / 03506, WO 93 / 14132, and WO 95 / 07941. Exemplary compounds include triethylaluminum, triethylborane, triisobutylaluminum, tri-n-octylaluminum, methylalumoxane, and isobutylalumoxane. Alumoxanes may be used in scavenging amounts with other means of activation, such as methylalumoxane and triisobutylalumoxane with boron-based activators. The amount of scavenger to be used with the catalyst compound may be minimized to an amount effective to enhance activity during the polymerization reaction (or an amount necessary to activate the catalyst compound if used in a dual role), since excess amounts may act as catalyst poisons.
[0030] Polymerizations giving a wide variety of polymer types and molecular weights are achievable. Generally speaking, the polymers are derived from either ethylene or propylene as the major (e.g., greater than 50 wt%) component. The polymers may contain preferably 5 mol % to 40 mol % of comonomers to modify crystallinity and flexibility. The comonomers may be alpha-olefins (this term includes cyclic olefins, e.g., styrene) having 2 to 20 carbon atoms, such as ethylene (for polymers consisting primarily of propylene-derived units), propylene, 1-butene, 1-hexene, and 1-octene. Amounts of dienes, such as hexadiene, vinylnorbornene, ethylidenenorbornene (ENB), norbornadiene, etc., may be included to promote the formation of longer branches themselves resulting from unsaturation and / or polymerized monomer-derived units.
[0031] In the case of plastomers, the polymers that can be produced may include the following aspects: the comonomer is an alpha olefin having 3-15 carbon atoms, such as 4-12 carbon atoms, such as 4-10 carbon atoms. Ethylene may be polymerized with at least two comonomers to form a terpolymer. Ethylene may be polymerized in a ratio of 70 mol% to 99.99 mol%, such as 70 mol% to 97 mol%, such as 80 mol% to 95 mol% ethylene and 0.01 mol% to 30 mol%, such as 3 mol% to 30 mol%, such as 5 mol% to 20 mol% comonomer. The molecular weight distribution of the polymer can be determined with a Waters gel permeation chromatograph equipped with an Ultra Stillagel column and a refractive index detector. The operating temperature of the instrument may be set at 145°C, the elution solvent may be trichlorobenzene, and the calibration standards may include 16 polystyrenes of precisely known molecular weight ranging from a molecular weight of 500 to a molecular weight of 5.2 million, and a polyethylene standard, NBS 1475.10. The molecular weight distribution of the plastomer produced may have a narrow molecular weight distribution, i.e. Mw / Mn may be 3 or less, such as 2.5 or less. The MI of the polymer may be 0.01 dg / min to 200 dg / min, such as 0.1 dg / min to 100 dg / min, such as 0.2 dg / min to 50 dg / min, such as less than 10 dg / min. The plastomer may have a molecular weight distribution of 0.85 g / cm 3 ~0.93g / cm 3 , e.g. 0.87g / cm 3 ~0.92g / cm 3 , e.g. 0.88g / cm 3 ~0.91g / cm 3 The density of the sintered body may be 0.01 to 0.01.
[0032] The processes described herein may include copolymerization reactions including polymerization of one or more monomers, such as alpha olefin monomers of ethylene, propylene, 1-butene, 1-pentene, 1,4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, and cyclic olefins, such as styrene. Other monomers include polar vinyl, diene, norbornene, acetylene, and aldehyde monomers. In the case of elastomers, the polymers that can be produced include ethylene-alpha olefin-diene elastomers (EODE) with high Mw and diene content greater than 0.3 wt%, e.g., greater than 2 wt%. These polymers can be largely amorphous and have low or zero heat of fusion. As used herein, the term "EODE" encompasses elastomeric polymers that include ethylene, alpha olefins, and one or more non-conjugated diene monomers. The non-conjugated diene monomers can be linear, branched, or cyclic hydrocarbon dienes having 6 to 15 carbon atoms. Examples of suitable non-conjugated dienes are straight-chain acyclic dienes such as 1,4-hexadiene and 1,6-octadiene; branched-chain acyclic dienes such as 5-methyl-1,4-hexadiene; 3,7-dimethyl-1,6-octadiene; 3,7-dimethyl-1,7-octadiene and mixed isomers of dihydromyricene and dihydroocinene; monocyclic alicyclic dienes such as 1,4-cyclohexadiene and 1,5-cyclododecadiene; and polycyclic fused and bridged ring dienes such as tetrahydroindene, bicyclo-1,5-(2,2,1)-hepta-2,5-diene; alkenyl, alkylidene, cycloalkylidene norbornenes such as 5-methylene-2-norbornene (MNB); 5-propenyl-2-norbornene, 5-isopropylidene-2-norbornene, 5-(4-cyclopentenyl)-2-norbornene, 5-cyclohexylidene-2-norbornene, 5-vinyl-2-norbornene, and norbornadiene.
[0033] Suitable dienes for use in preparing ethylene-propylene-diene elastomers (EPDM) can be 1,4-hexadiene (HD), 5-ethylidene-2-norbornene (ENB), 5-vinylidene-2-norbornene (VNB), 5-methylene-2-norbornene (MNB), and dicyclopentadiene (DCPD). In at least one embodiment, the dienes are 5-ethylidene-2-norbornene (ENB) and 1,4-hexadiene (HD), for example, the EOD elastomer can contain from 20 wt% to 90 wt% ethylene, for example, 30 wt% to 85 wt% ethylene, for example, 35 wt% to 80 wt% ethylene, based on the weight of the EOD elastomer. Alpha olefins suitable for use in preparing elastomers with ethylene and dienes can be propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 1-dodecene. In at least one embodiment, the alpha olefin is incorporated into the EODE polymer at 10 wt% to 80 wt%, such as 20 wt% to 65 wt%, based on the weight of the EODE polymer. Non-conjugated dienes are typically incorporated into the EODE polymer at 0.5 wt% to 20 wt%, such as 1 wt% to 15 wt%, such as 2 wt% to 12 wt%, based on the weight of the EODE polymer. If desired, multiple dienes, such as HD and ENB, can be incorporated simultaneously with the total diene incorporation within the above limits. In at least one embodiment of the present disclosure, the elastomer can be a low viscosity polymer, such as low viscosity Vistamaxx™ (LVV).
[0034] In at least one embodiment, a suitable elastomer may be a copolymer of two monomers. The copolymer may be a relatively high Mw, low crystallinity, and low ash elastomer. The copolymer may be a high Mw ethylene-alpha olefin copolymer. The ethylene-alpha olefin copolymer may be a copolymer of ethylene and an alpha olefin, not necessarily propylene, that exhibits elastomeric properties. Alpha olefins suitable for use in preparing ethylene-containing elastomers include C 3 -C 10The alpha olefin may be an alpha olefin. Illustrative non-limiting examples of the alpha olefin are propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 1-dodecene. In at least one embodiment, multiple alpha olefins may be incorporated. The ethylene-alpha olefin copolymer may contain 20 wt% to 90 wt% ethylene, such as 30 wt% to 85 wt% ethylene, such as 35 wt% to 80 wt% ethylene. In at least one embodiment, the elastomer can be a propylene-based polymer having predominantly (greater than or equal to 50 wt %) propylene-derived units.
[0035] In at least one embodiment, the propylene-based polymer may be composed of propylene, at least one comonomer, and optionally a diene. The comonomer may be ethylene or an alpha-olefin. The comonomer may be ethylene and a linear or branched C 4 -C 30 Suitable linear alpha olefins include ethylene and C 4 -C 8Alpha olefins include ethylene, 1-butene, 1-hexene, and 1-octene, such as ethylene or 1-butene. Suitable branched alpha olefins include 4-methyl-1-pentene, 3-methyl-1-pentene, and 3,5,5-trimethyl-1-hexene. In at least one embodiment, the propylene copolymer can be a random copolymer, as that term is defined herein below. Dienes may also be included in the propylene-based polymer. In at least one embodiment, dienes include linear acyclic dienes such as 1,4-hexadiene and 1,6-octadiene; branched acyclic dienes such as 5-methyl-1,4-hexadiene; 3,7-dimethyl-1,6-octadiene; 3,7-dimethyl-1,7-octadiene and mixed isomers of dihydromyricene and dihydroocinene; monocyclic alicyclic dienes such as 1,4-cyclohexadiene and 1,5-cyclododecadiene; and polycyclic fused and bridged ring dienes such as tetrahydroindene, methyl ether ... bicyclo-1,5-(2,2,1)-hepta-2,5-diene; alkenyl, alkylidene, cycloalkylidene norbornenes such as 5-methylene-2-norbornene (MNB); non-conjugated dienes which are 5-propenyl-2-norbornene, 5-isopropylidene-2-norbornene, 5-(4-cyclopentenyl)-2-norbornene, 5-cyclohexylidene-2-norbornene, 5-vinyl-2-norbornene, and norbornadiene. Propylene-based polymers can include 1,4-hexadiene (HD), 5-ethylidene-2-norbornene (ENB), 5-vinylidene-2-norbornene (VNB), 5-methylene-2-norbornene (MNB), and dicyclopentadiene (DCPD).
[0036] In at least one embodiment, the propylene-based polymer may have a crystallinity of 2% to 65%. Within this crystallinity range, alternative limits of crystallinity may be from about 5% to about 50%, such as from about 10% to about 45%, such as from about 15% to about 40%. The crystallinity of the propylene-based polymer is derived from isotactic (or alternatively syndiotactic) polypropylene sequences in the copolymer. In at least one embodiment, the amount of propylene may be from 65 wt% to 95 wt%, such as from about 70 wt% to 92%, such as from about 80 wt% to 89 wt%. In at least one embodiment, the propylene-based polymer has a single broad melting transition. Samples of the propylene-based polymer may exhibit secondary melting peaks or shoulders adjacent to the main peak, the combination of which is collectively considered a single melting point, i.e., a single broad melting transition. The height of these peaks is considered the melting point. In at least one embodiment, the propylene-based polymer has a melting point of 25°C to 110°C, e.g., 30°C to 105°C, e.g., 35°C to 90°C.
[0037] The propylene-based polymer may be a crystallizable random copolymer with a narrow composition distribution. The intermolecular composition distribution of the polymer is determined by thermal fractionation in a solvent. A suitable solvent may be a saturated hydrocarbon, such as isohexane or hexane. The thermal fractionation procedure is described below. In at least one embodiment, about 75 wt% or more, such as about 85 wt% of the polymer is separated into one or two adjacent soluble fractions, with the remainder of the polymer in the previous or subsequent fraction. Each of these fractions has a composition (wt% ethylene content) that differs from the average wt% ethylene content of the propylene-based polymer by 20% or less (relative), such as 10% or less (relative). For the purposes of this disclosure, a propylene-based polymer may be considered to have a "narrow" composition distribution if it passes the fractionation test described above. The length and distribution of stereoregular propylene sequences in suitable propylene-based polymers can be consistent with substantially random statistical copolymerization. Without being bound by theory, the length and distribution of sequences are related to the reactivity ratio of copolymerization. As used herein, the term "substantially random" refers to a copolymer whose product of reactivity ratios is about 2 or less. In contrast, in stereoblock structures, the length of PP sequences is longer than that of substantially random copolymers with similar composition. The reactivity ratio and sequence distribution of the polymer position the ethylene residues relative to the adjacent propylene residues. 13 C NMR can be used to determine the randomness and narrow composition distribution of the crystallizable copolymers. In order to produce crystallizable copolymers with the requisite amount of randomness and narrow composition distribution, it would be desirable to use (1) a single-site catalyst and (2) a well-mixed loop polymerization reactor that allows only a single polymerization environment for substantially all of the polymer chains of the appropriate propylene-based polymer. Suitable propylene-ethylene copolymers are described in US Pat. No. 6,635,715, the contents of which are incorporated herein by reference.
[0038] Commercially available examples of polymers formed by the processes and plants of the present disclosure include Vistamaxx™ copolymers from ExxonMobil Chemical Company, Tafmer™ elastomers from Mitsui Chemicals, and Versify™ elastomers from Dow Chemical Company. For example, Vistamaxx™ is a propylene-based elastomer that enhances the performance and processability of films, compounds, nonwovens, and molded / extruded products. Vistamaxx™ free-flowing pellets are easy to incorporate, and the broad compatibility allows for dry blending operations. Vistamaxx™ offers a wide range of applications, such as: 1) nonwovens (elasticity, softness, and toughness; delivered with drop-in processing capabilities); 2) films (elasticity, sealability, toughness, and tack); 3) polymer modification and compounding (impact strength, clarity, flexibility / stiffness, softness, high filler loading). Vistamaxx™ copolymers are copolymers of propylene and ethylene. Vistamaxx™ is a propylene-rich (>80%), semi-crystalline material with high amorphous content. The synthesis of Vistamaxx™ polymers is typically based on Exxpol™ technology from ExxonMobil Chemical. Vistamaxx™ 6102 ("VM6102") has a viscosity of 0.862 g / cm 3 %, a melt index of 1.4 g / 10 min (at 190° C., 2.16 kg), an MFR of 3 g / 10 min, and an ethylene content of 16 wt %. Vistamaxx™ 3980 propylene-ethylene performance polymer ("VM3980") is available from ExxonMobil Chemical Company. VM3980 has an ethylene content of 9 wt%, the remainder being propylene. Properties of VM3980 include: 3 (ASTM D1505); melt index of 3.6 g / 10 min (ASTM D1238; 190°C, 2.16 kg); melt mass flow rate of 8 g / 10 min (230°C, 2.16 kg); Shore D hardness (ASTM D2240) of 34; and Vicat softening temperature (VST) of 77.3°C.
[0039] Vistamaxx™ 6502 (VM6502) is a polymer with isotactic propylene repeat units in a random ethylene distribution; the polymer has a viscosity of 0.865 g / cm 3 density of 45.2 g / 10 min; melt mass flow rate (230° C., 2.16 kg); and an ethylene content of 13.1 wt %. Vistamaxx™ 3000 propylene-ethylene performance polymer ("VM3000") is available from ExxonMobil Chemical Company. VM3000 has 11 wt% ethylene with the remainder being propylene. Properties of VM3000 include: 3 density (ASTM D1505); melt index (ASTM D1238; 190°C, 2.16 kg) of 3.7 g / 10 min; melt mass flow rate (230°C, 2.16 kg) of 8 g / 10 min; Shore D hardness (ASTM D2240) of 27; and Vicat softening temperature (VST) of 65.1°C. Vistamaxx™ 3588 propylene-ethylene performance polymer ("VM3588") is available from ExxonMobil Chemical Company. VM3588 has an ethylene content of 4 wt%, the remainder being propylene. Properties of VM3588 include: 3 (ASTM D1505); melt mass flow rate (230°C, 2.16 kg) of 8 g / 10 min; Shore D hardness (ASTM D2240) of 50; and Vicat softening temperature (VST) of 103°C. Vistamaxx™ 6202 ("VM6202") has a viscosity of 0.863 g / cm 3 %, a melt index of 9.1 g / 10 min (at 190° C., 2.16 kg), an MFR of 20 g / 10 min, and an ethylene content of 15 wt %. Vistamaxx™ 3020 ("VM3020") has a viscosity of 0.874 g / cm 3%, a melt index of 1.1 g / 10 min (at 190° C., 2.16 kg), an MFR of 3 g / 10 min, and an ethylene content of 11 wt %. The disclosed plants and processes provide for transitions between different grades of polymer, e.g., Vistamaxx™ grades of polymer, with reduced amounts of off-specification (e.g., degraded polymer and / or non-degraded polymer outside the desired specification range) in a manner that also results in reduced transition times between polymer grades and reduced amounts of recycle polymer in the recycle line, as compared to conventional plants and processes.
[0040] Plant and process flow FIG. 1 is a plant (100) and process flow for polymerization and devolatilization according to an embodiment. As shown in FIG. 1, a monomer stream (101) and a catalyst compound stream (102) may be introduced into the plant 100 and mixed to form a solution. A solvent (e.g., isohexane) is also present. The solution of monomer and catalyst compound may travel through a cooler or heater (103) to reach an appropriate temperature. The cooled or heated solution of monomer and catalyst compound may then be pumped via pump (104) to a first heat exchanger (105) in the reaction zone. Prior to introduction into the first heat exchanger, the catalyst compound may be contacted with an activator as described herein (not shown) to form a catalyst system. In some embodiments, the catalyst compound is contacted with an activator just prior to entering the first heat exchanger.
[0041] The catalyst system contacts the monomer in solution in the first heat exchanger (105) to obtain the polymer. The monomer, catalyst system, and polymer may flow through the first heat exchanger (105) in a cross-flow direction relative to the first heat exchanger (105). A portion of the monomer, catalyst system, and polymer exiting the first heat exchanger (105) may be recycled back to the first heat exchanger (105), and another portion of the monomer, catalyst system, and polymer exiting the first heat exchanger (105) may be pumped by another pump (106) to a second heat exchanger (107) in the reaction zone. A portion of the monomer, catalyst system, and polymer exiting the second heat exchanger (107) may be recycled back to the second heat exchanger (107), and another portion of the monomer, catalyst system, and polymer exiting the second heat exchanger (107) may be transferred to a phase separator / devolatilizer vessel (14). Additionally or alternatively, an activator may be introduced into the recycle stream (not shown). Although the first heat exchanger (105) and the second heat exchanger (107) are shown in series, they may alternatively be in parallel.
[0042] In the phase separator (14), the monomers and / or solvent are separated from the polymer. The concentrated polymer solution can exit the lower portion of the phase separator (14) and is passed to a stream splitter (70). This stream splitter (70) distributes the concentrated polymer solution into a first stream that is transferred via line (72) to the low pressure separator (34). In the low pressure separator (34), the evaporated solvent and monomers are separated from the further concentrated polymer solution exiting the phase separator (14). The stream splitter (70) also distributes the concentrated polymer solution into a second stream (recycle stream), which is transferred via line (74) to line (11) at a location upstream of the heat exchanger (not shown) for mixing with the reactor effluent. In some embodiments, a third separator (not shown) may be utilized. The third separator is typically operated at a lower pressure and higher temperature than the separator (34). In some embodiments, the third separator may be operated at a pressure of from about 667 Pa (5 Torr) to about 5333 Pa (40 Torr) and / or a temperature of from about 130°C to about 220°C.
[0043] A heater (109) in line (72) to form a heated concentrated polymer solution. A portion of the heated concentrated polymer solution may be recycled to the phase separator (14). The remaining portion of the heated concentrated polymer solution may be further heated in a heater (110) in line (72) to keep the heated concentrated polymer solution in the molten phase before being transferred to the low pressure separator (34) to remove any residual monomer and / or solvent from the heated concentrated polymer solution. A more concentrated polymer solution (up to about 100% polymer) exits the bottom of the low pressure separator (34) which may be (1) processed in a third stage devolatilization (e.g., low pressure separator) (not shown) or (2) mixed with additional suitable additives (112) and cooled in a cooler (113) before being sent to pelletization and packaging. Similarly, the more concentrated polymer solution exits the third stage devolatilization vessel (not shown) and may be mixed with suitable additives (112), cooled in a cooler (113), and then sent to pelletization and packaging.
[0044] Conditions in the phase separator (14) during devolatilization can include a temperature of about 150° C. to about 180° C. (e.g., average temperature of the interior volume of the phase separator), a pressure of about 75 psig to about 150 psig, and / or a mass flow rate (e.g., of the first and / or second concentrated polymer solution) of about 200 to about 1000 tonnes / hr, e.g., about 250 tonnes / hr to about 775 tonnes / hr. The polymer content of the reactor effluent entering the phase separator (14) can be about 10 wt % to about 25 wt %. The polymer content of the effluent of phase separator (14) entering low pressure separator (34) is from about 25 wt% to about 45 wt%. Low pressure separator (34) may be operated at a temperature of from about 180° C. to about 200° C. and a pressure of from about 25 psig to about 50 psig. The polymer content of the effluent exiting the low pressure separator (34) may be from about 80 wt% to about 95 wt%, for example, from about 88 wt% to about 91 wt%. If a third stage devolatilization is performed, the third separator (not shown) may be operated at a temperature of from about 200° C. to about 220° C. and a pressure of from about 20 torr (0.39 psig) to about 50 torr (0.97 psig). The effluent exiting the third separator may have less than about 500 wppm volatile organic compounds (VOCs).
[0045] The monomer and solvent exiting the top of the phase separator (14) may then be cooled in a cooler (114) and transferred to a condenser (115). The concentrated monomer and / or solvent exits the bottom of the condenser (115) and is transferred to a mixed feed drum (120) so that it may be fed back into the system. The non-condensable gases (e.g., hydrogen gas, ethylene gas) exit the top of the condenser (115) and may be transferred to a compressor (118) and another cooler (119) to convert the gas to a liquid which may then be transferred to the mixed feed drum (120) for reuse in the system. Similarly, the monomer and / or solvent exiting the top of the low pressure separator (34) may pass through a compressor (116), another cooler (117), compressor (118) and a cooler (119) to form a liquid which may then be transferred to the mixed feed drum (120) for reuse in the system.
[0046] Non-limiting polymerization example Table 1 shows exemplary polymerization processes for making low molecular weight plastomers, high molecular weight elastomers, and high propylene content ethylene copolymers polymerized as described above. In some embodiments, the plant is operated at one or more of the conditions shown in Table 1.
[0047] [Table 1]
[0048] To make plastomers using the plant of FIG. 1, the feed temperature can be reduced to 0° C. by a heater / cooler (103). An aluminum alkyl is added as a scavenger in an amount appropriate to the poison content of the feed. The pressure is increased to 120 bar by a centrifugal pump. Then, the feed, which mainly contains solvent and has a partial pressure of ethylene and propylene or butene or hexene or octene comonomers up to 50 bar, enters the first heat exchanger (105) (e.g., the first reactor of a series of reactors). Catalyst and activator are added to the first heat exchanger (105 / 107) in amounts that result in the desired polymerization temperature, which is related to the desired molecular weight of the polymer being formed. The heat of polymerization is generated without the use of hydrogen (H 2 The temperature is then increased to 150-200°C (although a second reactor may be used) to form a plastomer. At the exit of the second series reactor, the polymer concentration is in the range of 10-25 wt%. Water is then fed via a line (not shown) to quench the polymerization reaction, which would otherwise continue in the presence of residual catalyst, unreacted monomer, and elevated temperature. The heat exchangers first raise the temperature, and the concentrated polymer solution in the recycle line (74) (in addition to the heat exchangers located in the phase separator (14), described in more detail below) causes a further temperature increase. A rapid pressure drop occurs as the polymerization mixture enters the phase separator (14) through the let-down valve (18) (in FIG. 2) with a fast pressure drop. The pressure difference between the outlet of the reactor pump and the outlet of the let-down valve (18) is responsible for forcing the feed and polymerization mixture to flow through the heat exchangers (105 / 107) and line (11) containing the heat exchanger (12).
[0049] Comparing the use of this plant with the row marked Elastomer in Table 1, it can be seen that the polymerization temperature is lower than for the plastomer, and the reactor effluent coming out of the reactor is less (its viscosity will be similar to that of the plastomer), but the same separation process and plant can be used to give somewhat less output (reflecting the less efficient polymerization process at lower temperatures). With two reactors in series, it may be preferable for the first reactor to operate at a temperature of 0-110°C and the second reactor to operate at a temperature of 40-140°C, for example the first reactor to operate at a temperature of 10-90°C and the second reactor to operate at a temperature of 50-120°C, for example the first reactor to operate at a temperature of 20-70°C and the second reactor to operate at a temperature of 60-110°C. With proper control of process conditions and poison levels, temperatures of this order of magnitude can be obtained using only one reactor or even two reactors under the same process conditions. The same is true for the row in Table 1 marked "Major Propylene Content Copolymer" where the temperature is lowered to allow the less reactive propylene monomer to form a sufficiently high molecular weight.
[0050] The disclosed plants and processes allow for polymerization and subsequent polymer separation to result in polymers of a wide variety of average molecular weights and comonomer contents over a wide range of temperatures and with catalysts suitable for operation at high and low operating temperatures. The disclosed process plants are capable of producing plastomers, elastomeric, and / or predominantly propylene content copolymers by simply varying the polymerization starting materials (e.g., catalyst, monomer, and / or comonomer) and process conditions.
[0051] Figure 2 is a portion of a plant (100) during a normal operating mode according to an embodiment. As shown in Figure 2, line (11) carries reactor effluent to be mixed with concentrated polymer solution in recycle line (74). The reactor effluent and concentrated polymer solution can be mixed directly and enter line (11). Or, as shown in Figure 2, after being mixed via mixer (76), the mixture can continue to move via line (11) to heat exchanger (12). As mentioned above, the plant of the present disclosure may be operated under a normal operating mode in which the concentrated polymer solution in recycle line (74) is mixed with the reactor effluent in line (11). Alternatively, during a transition mode, only the reactor effluent is fed to the phase separator (14) via line (11) and the recycle of the concentrated polymer solution is stopped. For example, valves (310a) and / or (310b) (each shown in an open position in FIG. 2) may be in a closed position to stop mixing of the concentrated polymer solution in recycle line (74) with the reactor effluent in line (11). A transition mode may be implemented when transitioning between polymer grades or between entirely different polymers.
[0052] During normal operation or transition mode, the reactor effluent in line (11) entering mixer (76) has a temperature of from about 54.44° C. (130° F.) to about 165.56° C. (330° F.), for example from about 60° C. (140° F.) to about 160° C. (320° F.), a pressure of from about 3.792 MPa (550 psig) to about 5.516 MPa (800 psig), for example from about 3.999 MPa (580 psig) to about 4. a pressure of 482 MPa (650 psig), a mass flow rate of about 181,440 t (400 Mlb) / hr to about 317,520 t (700 Mlb) / hr, for example about 226,800 t (500 Mlb) / hr to about 272,160 t (600 Mlb) / hr, a steam content of about 0 wt%, and / or a polymer content of about 5 wt% to about 35 wt%, for example about 10 wt% to about 30 wt%. The concentrated polymer solution in recycle line (74) (from stream splitter (70)) entering mixer (76) may be at a temperature of from about 200°F to about 300°F, for example from about 215°F to about 280°F, and at a pressure of from about 550 psig to about 800 psig, for example about 580 psig. 100 psi (4.482 MPa) (650 psig) or less, a mass flow rate of about 350 Mlb / hr to about 630 Mlb / hr, e.g., about 450 Mlb / hr to about 540 Mlb / hr, a steam content of about 0 wt.%, and / or a polymer content of about 20 wt.% to about 60 wt.%, e.g., about 25 wt.% to about 50 wt.%.
[0053] From mixer (76), the reactor effluent (or a mixture of reactor effluent and concentrated polymer solution) is transferred to heat exchanger (12). During the normal operating mode (where the reactor effluent and concentrated polymer solution are mixed), the mixture of reactor effluent and concentrated polymer solution in line (11) between mixer (76) and heat exchanger (12) is maintained at a temperature of from about 150°F to about 310°F, for example from about 180°F to about 280°F, and at a pressure of from about 550 psig to about 800 psig, for example from about 3. The pressure may be from about 580 psig (999 MPa) to about 650 psig (4.482 MPa), a mass flow rate from about 800 Mlb / hr to about 1200 Mlb / hr, e.g., from about 1025 Mlb / hr to about 1075 Mlb / hr, a steam content of about 0 wt%, and / or a polymer content of from about 10 wt% to about 30 wt%, e.g., from about 18 wt% to about 22 wt%. During the transition mode (reactor effluent and concentrated polymer solution are not mixed), the reactor effluent in line (11) between mixer (76) and heat exchanger (12) has a temperature of from about 54.44°C (130°F) to about 165.56°C (330°F), for example from about 60°C (140°F) to about 160°C (320°F), and a pressure of from about 3.792 MPa (550 psig) to about 5.516 MPa (800 psig), for example about 3.999 MPa (5 a mass flow rate of from about 400 Mlb / hr to about 700 Mlb / hr, e.g., from about 500 Mlb / hr to about 600 Mlb / hr, a steam content of about 0 wt%, and / or a polymer content of from about 5 wt% to about 35 wt%, e.g., from about 10 wt% to about 30 wt%.
[0054] From the heat exchanger (12), the mixture of reactor effluent and concentrated polymer solution in line (11) is transferred to the letdown valve (18) from the heat exchanger (12). During a normal operating mode, the mixture of reactor effluent and concentrated polymer solution in line (11) transferred from the heat exchanger (12) to the letdown valve (18) is maintained at a temperature of from about 220°F to about 360°F, for example from about 240°F to about 340°F, and at a pressure of from about 400 psig to about 600 psig, for example about 435 psi g) to about 550 psig; a mass flow rate of about 400 Mlb / hr to about 1100 Mlb / hr, for example about 500 Mlb / hr to about 1060 Mlb / hr; a steam content of about 0 wt.% to about 1 wt.%, for example about 0 wt.%, and / or a polymer content of about 10 wt.% to about 50 wt.%, for example about 15 wt.% to about 40 wt.%. During the transfer mode, the reactor effluent in line (11) transferred from heat exchanger (12) to letdown valve (18) is maintained at a temperature of from about 220°F to about 350°F, for example from about 240°F to about 330°F, and at a pressure of from about 400 psig to about 600 psig, for example from about 435 psig to about 3792 MPa. a (550 psig), a mass flow rate of about 400 to about 600 t / hr, for example about 450 to about 560 t / hr, a steam content of about 0 wt.% to about 1 wt.%, for example about 0 wt.%, and / or a polymer content of about 5 wt.% to about 35 wt.%, for example about 10 wt.% to about 30 wt.%.
[0055] Through the let-down valve (18), the mixture of reactor effluent and concentrated polymer solution in line (11) is transferred to the phase separator (14) through the let-down valve (18). During normal operation, the mixture of reactor effluent and concentrated polymer solution in line (11) transferred to the phase separator (14) through the let-down valve (18) has a temperature of from about 170°F to about 300°F, for example from about 200°F to about 270°F, a pressure of from about 50 psig to about 200 psig, for example from about 70 psig to about 1.1 MPa, and a pressure of from about 50 psig to about 200 psig. a pressure of 72 MPa (170 psig), a mass flow rate of about 158,760 t (350 Mlb) / hr to about 498,960 t (1100 Mlb) / hr, for example about 181,440 t (400 Mlb) / hr to about 498,960 t (1100 Mlb) / hr, a steam amount of about 10 wt% to about 60 wt%, for example about 15 wt% to about 50 wt%, and / or a polymer content of about 10 wt% to about 50 wt%, for example about 15 wt% to about 40 wt%. During the transition mode, the reactor effluent in line (11) being transferred from the letdown valve (18) to the phase separator (14) may be at a temperature of from about 170°F to about 300°F, for example from about 190°F to about 280°F, and at a pressure of from about 50 psig to about 200 psig, for example from about 60 psig to about 117 MPa. 170 psig), a mass flow rate of about 400 to about 700 t / hr, e.g., about 500 to about 272,160 t / hr, a steam content of about 10 wt.% to about 50 wt.%, e.g., about 20 wt.% to about 40 wt.%, and / or a polymer content of about 5 wt.% to about 35 wt.%, e.g., about 10 wt.% to about 30 wt.%.
[0056] From the phase separator (14), the concentrated polymer solution formed in the phase separator (14) is transferred via line (302) to pump (304. During normal operation mode and / or transition mode, the concentrated polymer solution in line (302) transferred from the phase separator (14) to pump (304) may be at a temperature of from about 170°F to about 300°F, for example from about 200°F to about 270°F, at a pressure of from about 50 psig to about 200 psig, for example from about 65 psig to about 160 psig, at a pressure of from about 100 psig to about 150 psig, for example from about 150 psig to about 170 psig, and at a pressure of from about 100 psig to about 150 psig. A mass flow rate of from about 90,720 t (200 Mlb) / hr to about 362,880 t (800 Mlb) / hr, for example from about 99,792 t (220 Mlb) / hr to about 480,816 t (1060 Mlb) / hr, for example from about 99,792 t (220 Mlb) / hr to about 344,736 t (760 Mlb) / hr, a steam amount of from about 0 wt% to about 1 wt%, for example about 0 wt%, and / or a polymer content of from about 20 wt% to about 70 wt%, for example from about 25 wt% to about 60 wt%.
[0057] From pump (304), concentrated polymer solution is transferred via line (306) to stream splitter (70). During normal operation mode and / or transition mode, the concentrated polymer solution in line (306) transferred from pump (304) to stream splitter (70) may be at a temperature of from about 170°F to about 300°F, for example from about 200°F to about 270°F, and at a pressure of from about 500 psig to about 800 psig, for example from about 550 psig to about 750 psig. a mass flow rate of from about 90,720 t (200 Mlb) / hr to about 362,880 t (800 Mlb) / hr, such as from about 99,792 t (220 Mlb) / hr to about 480,816 t (1060 Mlb) / hr, for example from about 99,792 t (220 Mlb) / hr to about 344,736 t (760 Mlb) / hr, a steam content of from about 0 wt% to about 1 wt%, for example about 0 wt%, and / or a polymer content of from about 20 wt% to about 70 wt%, for example from about 25 wt% to about 60 wt%. From the stream splitter (70), the concentrated polymer solution in line (72) is transferred via line (72) to separator (34). During normal operation mode and / or transition mode, the concentrated solution phase in line (72) transferred from stream splitter (70) to separator (34) may be at a temperature of from about 200°F to about 300°F, for example from about 220°F to about 280°F, and at a pressure of from about 500 psig to about 800 psig, for example about 550 psig. ) to about 5.171 MPa (750 psig), a mass flow rate of about 90,720 t (200 Mlb) / hr to about 158,760 t (350 Mlb) / hr, for example about 99,792 t (220 Mlb) / hr to about 122,472 t (270 Mlb) / hr, a steam content of about 0 wt.% to about 1 wt.%, for example about 0 wt.%, and / or a polymer content of about 20 wt.% to about 70 wt.%, for example about 25 wt.% to about 60 wt.%.
[0058] FIG. 3A is a phase separator (14) of a plant (100) according to an embodiment. As shown in FIG. 3A, the phase separator (14) is a static devolatilizer. The phase separator (14) includes a heat exchanger (400) and an inlet (410) for receiving an effluent (402) (e.g., reactor effluent or a mixture of reactor effluent and concentrated polymer solution) from a pressure let-down valve (18) via a line (11). As shown in FIG. 3A, the heat exchanger (400) is partially disposed within the phase separator (14), but may alternatively be disposed entirely within the phase separator (14). The phase separator (14) includes a vessel (403) for receiving a first concentrated polymer solution (421). The vessel (403) includes a lower sump area (404) for collecting a second concentrated polymer solution (422). The vessel (403) has an upper region (405) for discharging the volatile material (406). The vessel (403) has a central region (407) between the lower sump region (404) and the upper region (405). A discharge pump (408) in fluid communication with the lower sump region (404) discharges the second concentrated polymer solution (422) from the vessel (403). An extraction line (409) allows for the discharge of the volatile material (406) from the vessel (403), the extraction line (409) being located in the upper region (405) of the phase separator (14), for example, the extraction line (409) being in the top third portion of the phase separator (14). The heat exchanger (400) has a volatiles discharge area (434) for discharging the volatiles (406) towards the extraction line (409).
[0059] A discharge opening (424) of the heat exchanger (400) discharges the first concentrated polymer solution (421) downwardly towards the lower sump region (404) and towards the second heat exchanger (500) configured to receive the first concentrated polymer solution (421). The second heat exchanger (500) is configured to receive the first concentrated polymer solution (421) via an inlet (520) (which is an inner transition) and provide heat exchange to the first concentrated polymer solution (421) to form a second concentrated polymer solution (422) having a reduced volatile matter content compared to the first concentrated polymer solution (421). The second concentrated polymer solution (422) may exit the heat exchanger (500) via an outlet (530) (which is an outer transition) and travel towards the lower sump region (404). The separated volatile materials produced by the second heat exchanger (500) may exit the second heat exchanger (500) at outlet (540) and travel towards the upper region (405) and ultimately the extraction line (409).
[0060] Heat exchanger (400) and heat exchanger (500) may independently be operated at a temperature of from about 170°F to about 330°F, for example from about 215°F to about 300°F, a pressure of from about 50 psig to about 200 psig, for example from about 60 psig to about 170 psig, and / or a mass flow rate of from about 200 Millibes per hour to about 800 Millibes per hour, for example from about 250 Millibes per hour to about 760 Millibes per hour. Heat exchanger (400) and heat exchanger (500) may independently be operated at from 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr, such as from about 15,825 MJ (15 MMBtu) / hr to about 26,375 MJ (25 MMBtu) / hr, such as from about 18,990 MJ (18 MMBtu) / hr to about 23,210 MJ (22 MMBtu) / hr. "MMBtu / hr" refers to Millions of British Thermal Units. The heat exchanger is utilized in addition to heat exchanger 12, which may be operated at a lower heat input than conventional heat exchangers in conventional recirculation lines, which often operate at about 60 MMBtu / hr. For example, heat exchanger 12 may be operated at about 25 MMBtu / hr to about 50 MMBtu / hr, e.g., about 35 MMBtu / hr to about 40 MMBtu / hr.
[0061] A phase separator having one or more heat exchangers can provide improved devolatilization, especially for highly viscous polymer products containing large amounts of volatiles and / or when the specifications of the final product allow only very low concentrations of residual volatiles. The use of a first heat exchanger and a second heat exchanger each disposed (partially or completely) within the phase separator can provide a reduction in the volatile content of the second concentrated polymer phase exiting the phase separator (compared to the use of only one or no heat exchangers disposed within the phase separator). Additionally, the heat exchangers of the present disclosure may have a bundled tube-tube design, e.g., 8000 m 2 Compared to conventional tube bundles, the heat exchangers of the present disclosure provide a significant distribution of the reactor effluent (or a mixture of reactor effluent and concentrated polymer solution) to increase the heat transfer surface area and gas-liquid interface of the reactor effluent (or a mixture of reactor effluent and concentrated polymer solution). Conditions in the phase separator (14) during devolatilization can include a temperature of about 150° C. to about 180° C. (e.g., average temperature of the interior volume of the phase separator), a pressure of about 75 psig to about 150 psig, and / or a mass flow rate (e.g., of the first and / or second concentrated polymer solution) of about 200 Millibes per hour to about 1000 Millibes per hour, e.g., about 250 Millibes per hour to about 775 Millibes per hour. The second concentrated polymer solution (422) can be transferred from the phase separator (14) via line (302) to pump (304), as described above.
[0062] FIG. 3B is a phase separator (14) of a plant (100) according to an embodiment. As shown in FIG. 3B, the phase separator (14) is a static devolatilizer. The phase separator (14) includes an effluent (402) and an inlet manifold (410) for receiving the effluent (402) (e.g., reactor effluent or a mixture of reactor effluent and concentrated polymer solution) from a pressure let-down valve (18) via a line (11). As shown in FIG. 3B, the inlet manifold (410) is disposed within the phase separator (14) and has a plurality of outlets (480) configured to feed the effluent (402) into an internal cavity of the phase separator (14). For example, the phase separator (14) includes a vessel (403) for receiving a first concentrated polymer solution (421). The vessel (403) has a lower sump area (404) for collecting a second concentrated polymer solution (422). The vessel (403) has an upper region (405) for discharging the volatile material (406). The vessel (403) has a central region (407) between the lower sump region (404) and the upper region (405). A discharge pump (408) in fluid communication with the lower sump region (404) discharges the second concentrated polymer solution (422) from the vessel (403). An extraction line (409) allows for the discharge of the volatile material (406) from the vessel (403), the extraction line (409) being located in the upper region (405) of the phase separator (14), for example, the extraction line (409) being in the top third portion of the phase separator (14).
[0063] The inlet manifold (410) has a volatiles discharge area (434) for discharging the volatiles (406) towards the extraction line (409). The outlet (480) of the inlet manifold (410) discharges the first concentrated polymer solution (421) downwardly towards the lower sump area (404) and a heat exchanger (500) configured to receive the first concentrated polymer solution (421). The heat exchanger (500) is configured to receive the first concentrated polymer solution (421) via one or more inlets (not shown) and provide heat exchange to the first concentrated polymer solution (421) to form a second concentrated polymer solution (422) having a reduced volatiles content relative to the first concentrated polymer solution (421). The second concentrated polymer solution (422) may exit the heat exchanger (500) via one or more outlets (not shown) and travel towards the lower sump area (404). The separated volatile materials produced by the second heat exchanger (500) may exit the second heat exchanger (500) at one or more outlets (not shown) and travel toward the upper region (405) and ultimately the extraction line (409). The heat exchanger (500) may be operated at a temperature of from about 170°F to about 330°F, for example from about 215°F to about 300°F, a pressure of from about 50 psig to about 200 psig, for example from about 60 psig to about 170 psig, and / or a mass flow rate of from about 200 Millibes per hour to about 800 Millibes per hour, for example from about 250 Millibes per hour to about 760 Millibes per hour. Heat exchanger (500) may be operated at from about 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr, such as from about 15,825 MJ (15 MMBtu) / hr to about 26,375 MJ (25 MMBtu) / hr, such as from about 18,990 MJ (18 MMBtu) / hr to about 23,100 MJ (22 MMBtu) / hr. Because it is utilized in addition to heat exchanger (12), heat exchanger (12) of FIG. 1 may be operated at a lower heat input than conventional heat exchangers in conventional recycle lines, which often operate at about 63,300 MJ (60 MMBtu) / hr. For example, heat exchanger (12) can be operated at from about 26,375 MJ (25 MMBtu) / hr to about 52,750 MJ (50 MMBtu) / hr, such as from about 36,925 MJ (35 MMBtu) / hr to about 47,475 MJ (45 MMBtu) / hr.
[0064] A phase separator having one or more heat exchangers can provide improved devolatilization, especially for highly viscous polymer products containing large amounts of volatiles and / or when the specifications for the final product allow only very low concentrations of residual volatiles. The use of a heat exchanger disposed within the phase separator can provide a reduction in the volatile content of the second concentrated polymer phase exiting the phase separator (compared to when a heat exchanger disposed within the phase separator is not used). Additionally, the heat exchangers of the present disclosure may have a bundled tube-tube design, e.g., 8000 m 2 Compared to conventional tube bundles, the heat exchangers of the present disclosure provide a significant distribution of the reactor effluent (or a mixture of reactor effluent and concentrated polymer solution) to increase the heat transfer surface area and gas-liquid interface of the reactor effluent (or a mixture of reactor effluent and concentrated polymer solution). Conditions in the phase separator (14) during devolatilization can include a temperature of about 150° C. to about 180° C. (e.g., average temperature of the interior volume of the phase separator), a pressure of about 75 psig to about 150 psig, and / or a mass flow rate (e.g., of the first and / or second concentrated polymer solution) of about 200 Millibes per hour to about 1000 Millibes per hour, e.g., about 250 Millibes per hour to about 775 Millibes per hour. The second concentrated polymer solution (422) can be transferred from the phase separator (14) via line (302) to pump (304), as described above.
[0065] FIG. 4 is a heat exchanger (550) that can be used as the heat exchanger of FIG. 3A according to an embodiment. The heat exchanger (550) can be the heat exchanger (400) and / or the heat exchanger (500) of FIG. 3. As shown in FIG. 4, the heat exchanger (550) includes a central body (510), two inner transition parts (520), two outer transition parts (530), and three pipe connections (540). One of the two inner transition parts (520) extends from a first end (520a) of the central body (510), and the other extends from a second end (520b) of the central body (510). Each of the two transition parts (530) extends from either outer end (520b) of the respective inner transition part (520). Each connection (540) is integrally formed with and has a pipe wall portion extending from the outer envelope surface of one of the first and second ends (530b, 530c) of the respective outer transition portion (530). The pipe connections (540) are circular and may be adapted to (A) receive the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution), (B) provide an outlet for volatile materials to the phase separator vessel (403), or (C) provide an outlet for the concentrated polymer solution (422). The heat exchanger (550) (e.g., components of the heat exchanger (550), such as the central body (510)) may be formed of steel or a steel alloy. The heat exchanger (550) may have a plurality of channels (not shown) disposed therein. The plurality of channels may form a checkerboard pattern, for example, as described in U.S. Publication No. 2020 / 0300561, the entire contents of which are incorporated herein by reference. The inner transition portion (520) has a major direction length L that is at least three times the maximum width W of any channel disposed within the central body (510).
[0066] Alternatively, the heat exchanger may be a plate-type heat exchanger, such as the heat exchanger of FIG. 3B. The plate-type heat exchanger may have a plurality of first heat exchanger plates and a plurality of second heat exchanger plates, which are connected to each other and arranged side by side such that a first interplate space is formed between each pair of adjacent first and second heat exchanger plates, and a second interplate space is formed between each pair of adjacent second and first heat exchanger plates. The first interplate spaces and the second interplate spaces are spaced apart from each other and arranged side by side in an alternating order within the plate package. Each heat exchanger plate essentially has at least a first porthole and a second porthole, the first porthole forming a first inlet channel to the first interplate space, and the second porthole forming a first outlet channel from the first interplate space. For example, the plate heat exchanger may have a first outlet for the volatiles outlet and a second outlet for the concentrated polymer solution (421) or (422).
[0067] 5-7 show a plate heat exchanger (600). The plate heat exchanger (600) comprises a plurality of heat exchanger plates (601) forming a plate package (602), each of which comprises a main extension plane p (see FIG. 5). The heat exchanger plates (601) are pressed into a shape such that when the plates are placed next to each other in the plate package (602), an interplate space is formed between each pair of plates (601). The interplate space may be formed in whole or in part by a spacing member, e.g. a gasket, provided between the plates, and is arranged to form a plurality of first passages (603) for the reactor effluent (or a mixture of the reactor effluent and the concentrated polymer solution) and a plurality of second passages (604) for a medium (e.g. a heating fluid). The first passages (603) are separated from the second passages (604). Furthermore, the first passages (603) and second passages (604) are arranged alongside one another in an alternating order, e.g., substantially each first passage (603) is surrounded by two second passages (604).
[0068] Plate package (602) includes heat exchanger plates (601) that are connected to one another in any suitable manner, such as by brazing, and the heat exchanger plates (601) are substantially identical except for one of the end plates, which in the disclosed embodiment does not have a porthole. Additionally, plate package (602) includes four port channels (606), (607), (608), and (609). Each port channel (606), (607), (608), and (609) extends through plate (601) except for the one end plate. Two port channels (606) and (607) are in fluid communication with the first passageway (603), where the port channel (606) forms a first inlet port channel and extends to a first inlet (611) for the reactor effluent (or a mixture of the reactor effluent and the concentrated polymer solution) and the port channel (607) forms a first outlet port channel and extends to a first outlet (612) for the volatiles and concentrated polymer solution. Two other port channels (608) and (609) are in fluid communication with the second passageway (604), where the port channel (608) forms a second inlet port channel (608) and extends to a second inlet (613) for the medium (heating fluid) and the port channel (609) forms a second inlet port channel and extends to a second outlet (614) for the medium. It should be noted that the plate heat exchanger device may be of a type having another number of port channels, for example 2 or 6 port channels, and / or another number of passages.
[0069] With the exception of one end plate, each port channel (606), (608), and (609) is formed by an opening or port hole in each heat exchanger plate (601) in the plate package (602). The port holes forming the port channels (606), (608), and (609) are circular when viewed in the direction of the port channels (606), (608), and (609). Each port channel (606), (608), and (609) is connected to a respective conduit pipe (221), (222), (223), respectively, extending from the plate package (602) for the supply and removal of a medium (e.g., reactor effluent, a mixture of reactor effluent and concentrated polymer solution, volatiles, first / second concentrated polymer solutions, or a heating fluid). For example, pipe (221) and port channel (606) allow for the supply and transport of reactor effluent or a mixture of reactor effluent and concentrated polymer solution to the first passageway (603). Pipe (622) and port channel (608) allow for the supply and transport of a medium (e.g., a heating fluid) to the second passageway (604), and pipe (623) and port channel (609) allow for the discharge and transport of a medium (heating fluid) from the second passageway (604). The plate package (602) has, in use, an upper end and a lower end that is below the upper end with respect to the direction of gravity, with a first inlet (611) near the upper end and a first outlet (612) near the lower end. A second inlet (613) at the lower end operates according to the counter-current principle, while a second outlet (614) is at the upper end. It should be noted that plate heat exchangers can also be designed to operate according to the parallel-current principle.
[0070] The plate heat exchanger is arranged to allow heating of the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution) in the first passage (603) by use of a medium (heating fluid) in the second passage (604). For example, due to the heating of the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution), volatile substances will be removed from the reactor effluent (or a mixture of the reactor effluent and concentrated polymer solution). One or more of the heat exchanger plates may include heat transfer areas having corrugations including ridges and valleys. The port channel (607) forming the first outlet (612) includes or forms a volatiles outlet (631) arranged to allow the release of volatiles of the reactor effluent (or a mixture of the reactor effluent and the concentrated polymer solution) and a liquid outlet (632) arranged to allow the release of the concentrated polymer solution. The liquid outlet (632) is provided in or near the gas outlet (631). In a first embodiment, the first outlet (612) is formed by a porthole. However, the port channel (607) is divided by means of a dividing element (633) extending from said one end plate into the port channel (607) so that an upper volatiles outlet (631) and a lower volatiles outlet (632) are formed. In this way, the volatiles outlet (631) is separated from the concentrated polymer outlet (632).
[0071] The outlet opening of the volatiles outlet (631) has a center point that is at a higher level than the center point of the outlet opening of the liquid outlet (632) in normal use with respect to gravity. Figure 7 shows the dividing element (633) in solid lines extending a short distance into the port channel (607). However, the dashed lines show that the dividing element may extend substantially the full length of the port channel (607). The dividing element (633) may comprise or be formed of a simple sheet that may have a convex, somewhat curved shape when viewed from the gas outlet (631). In this case, concentrated polymer on the dividing element (633) may flow outward and downward from the volatiles outlet (631) or, preferably, the concentrated polymer outlet (632). In an alternative embodiment, the plate heat exchanger does not have a dividing element (633). The volatile material outlet (631) includes or is connectable to a volatile material release conduit (635) extending from the plate package (602) for release and transport of the volatile material. The concentrated polymer outlet (632) includes or is connectable to a release conduit (636), also extending from the plate package (602) and separated from the volatile material release conduit for separate release and transport of the concentrated polymer. The heat exchanger plates substantially delimiting each passage (603) are configured such that the transition between the first passage (603) and the port channel (607) of the first outlet (612) forms a throttling for the heated components of the reactor effluent (or reactor effluent and concentrated polymer solution mixture) flowing into the port channel (607). The throttling is formed by an edge region (646) that extends around at least the first outlet (612) and inwardly toward the central plane of the interplate space that forms the first passage (603).
[0072] Additional Features The present disclosure provides, inter alia, the following aspects, each of which may be considered to include any alternative aspects as appropriate. Clause 1. A process for forming a polymer, comprising: providing a feed having one or more olefin monomers and a solvent; introducing the feed into a reactor along with a catalyst to form a reaction mixture; removing reactor effluent from the reactor; mixing the reactor effluent with a first concentrated polymer solution in a mixer or line to form a mixture; introducing the mixture into a heat exchanger to form a heated mixture; introducing the heated mixture into a pressure let-down valve followed by introducing the heated mixture into a phase separator; removing the second concentrated polymer solution from the phase separator; introducing a second concentrated polymer solution into the mixer or line; The process includes: Clause 2. The process of clause 1, wherein the reactor is a continuous stirred tank reactor. Clause 3. The process of clause 1 or 2, wherein the step of introducing the second concentrated polymer solution into the mixer or line is conducted at a rate of about 500,000 lb / hr or less.
[0073] Clause 4. A second concentrated polymer solution, a first portion being a second concentrated polymer solution introduced into a mixer or line; The second part and 4. The process of any one of clauses 1-3, further comprising the step of introducing the second concentrated polymer solution into a stream splitter configured to distribute the second concentrated polymer solution into The process further comprising the step of introducing the second portion into a second phase separator. Clause 5. The process of any one of clauses 1 to 4, wherein the monomers include octene, butene, propylene and ethylene. Clause 6. When the second concentrated polymer solution is being introduced into the mixer or line, the second concentrated polymer solution Temperatures between approximately 101.67°C (215°F) and approximately 137.78°C (280°F), Pressure of about 3.999MPa (580psig) to about 4.482MPa (650psig), Mass flow rate of approximately 204,120t (450Mlb) / hr to approximately 244,944t (540Mlb) / hr, A steam content of about 0 wt% to about 1 wt%, and Polymer content of about 25wt% to about 50wt% 6. The process according to any one of clauses 1 to 5, comprising: Clause 7. When the heated mixture is being introduced into the pressure let-down valve, the heated mixture Temperatures between approximately 115.56°C (240°F) and approximately 171.11°C (340°F), Pressure of about 2.999MPa (435psig) to about 3.792MPa (550psig), Mass flow rate of approximately 226,800t (500Mlb) / hr to approximately 480,816t (1060Mlb) / hr. A steam content of about 0 wt% to about 1 wt%, and Polymer content of about 15wt% to about 40wt% 7. The process according to any one of clauses 1 to 6, comprising:
[0074] Article 8. Furthermore: stopping the introduction of the second concentrated polymer solution into the mixer or line; ceasing mixing of the reactor effluent with the first concentrated polymer solution; introducing the reactor effluent into a heat exchanger to form a heated reactor effluent; introducing the heated reactor effluent into a pressure let-down valve followed by introducing the heated reactor effluent into a phase separator; removing the third concentrated polymer solution from the phase separator; 8. The process according to any one of clauses 1 to 7, comprising: Clause 9. When the heating reactor effluent is introduced into the pressure let-down valve, Temperatures between about 115.56°C (240°F) and about 165.56°C (330°F), Pressure of about 2.999MPa (435psig) to about 3.792MPa (550psig), Mass flow rate of approximately 204,120t (450Mlb) / hr to approximately 254,016t (560Mlb) / hr, A steam content of about 0 wt% to about 1 wt%, and Polymer content of about 10wt% to about 30wt% 9. The process according to any one of clauses 1 to 8, comprising: Clause 10. When the mixture is introduced into the heat exchanger to form a heated mixture, the heated mixture is Temperatures between approximately 82.22°C (180°F) and approximately 137.78°C (280°F), Pressure of about 3.999MPa (580psig) to about 4.482MPa (650psig), Mass flow rate of approximately 464,940t (1025Mlb) / hr to approximately 487,620t (1075Mlb) / hr, A steam content of about 0 wt% to about 1 wt%, and having a polymer content of about 10 wt% to about 30 wt%, and During the introduction of the reactor effluent into the heat exchanger to form the heated reactor effluent, the heated reactor effluent is Temperatures between about 60°C (140°F) and about 160°C (320°F), Pressure of about 3.999MPa (580psig) to about 4.482MPa (650psig), Mass flow rate of approximately 226,800t (500Mlb) / hr to approximately 272,160t (600Mlb) / hr, A steam content of about 0 wt% to about 1 wt%, and having a polymer content of about 5 wt% to about 35 wt%; 10. The process according to any one of clauses 1 to 9.
[0075] Clause 11. When the heated mixture is introduced into the phase separator, the heated mixture Temperatures between about 83.33°C (200°F) and about 132.22°C (270°F), Pressure of about 0.483MPa (70psig) to about 1.172MPa (170psig), Mass flow rate of approximately 181,440t (400Mlb) / hr to approximately 498,960t (1,100Mlb) / hr, About 15wt% to about 50wt% steam volume, and having a polymer content of about 15 wt% to about 40 wt%, and While the heated reactor effluent is being introduced into the phase separator, Temperatures between approximately 87.78°C (190°F) and approximately 137.78°C (280°F), Pressure of about 0.414MPa (60psig) to about 1.172MPa (170psig), Mass flow rate of approximately 226,800t (500Mlb) / hr to approximately 272,160t (600Mlb) / hr, Steam volume of about 20wt% to about 40wt%, and having a polymer content of about 10 wt% to about 30 wt%; 11. The process according to any one of clauses 1 to 10. Clause 12. When the second portion is introduced into the second phase separator, the second portion Temperatures between approximately 104.44°C (220°F) and approximately 137.78°C (280°F), Pressure of about 3.792MPa (550psig) to about 5.171MPa (750psig), Mass flow rate of approximately 99,792t (220Mlb) / hr to approximately 122,472t (270Mlb) / hr, A steam content of about 0 wt% to about 1 wt%, and Polymer content of about 25wt% to about 60wt% 12. The process according to any one of clauses 1 to 11, comprising:
[0076] Clause 13. The process of any one of clauses 1-12, wherein the step of introducing the heated mixture into the phase separator is performed by introducing the heated mixture into an inlet of the phase separator, and a second heat exchanger is coupled to the inlet of the phase separator. Clause 14. The process of any one of clauses 1-13, wherein the step of introducing the heated mixture into the phase separator further comprises the step of introducing the heated mixture into a third heat exchanger disposed within the phase separator below the second heat exchanger. Clause 15. The process of any one of clauses 1-14, wherein the second heat exchanger comprises a first plurality of tubes and the third heat exchanger comprises a second plurality of tubes. Clause 16. The second heat exchanger comprises: Temperatures between approximately 101.67°C (215°F) and approximately 148.89°C (300°F), A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rate of approximately 113,400t (250Mlb) / hr to approximately 480,816t (1060Mlb) / hr 16. The process according to any one of clauses 1 to 15, wherein the process is operated at Clause 17. The third heat exchanger comprises: Temperatures between approximately 101.67°C (215°F) and approximately 148.89°C (300°F), A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rate of approximately 113,400t (250Mlb) / hr to approximately 344,736t (760Mlb) / hr 17. The process according to any one of clauses 1 to 16, wherein the process is operated at
[0077] Clause 18. The first heat exchanger is operated at about 26,375 MJ (25 MMBtu) / hr to about 52,750 MJ (50 MMBtu) / hr; 18. The process according to any one of clauses 1 to 17. Clause 19. The second heat exchanger is operated at about 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr; and the third heat exchanger is operated at about 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr; 19. The process according to any one of clauses 1 to 18. Clause 20. The first heat exchanger is operated at about 36,925 MJ (35 MMBtu) / hr to about 47,475 MJ (45 MMBtu) / hr; the second heat exchanger is operated at about 18,990 MJ (18 MMBtu) / hr to about 23,100 MJ (22 MMBtu) / hr; and the third heat exchanger is operated at about 18,990 MJ (18 MMBtu) / hr to about 23,100 MJ (22 MMBtu) / hr; 20. The process according to any one of clauses 1 to 19. Clause 21. A phase separator, Temperatures between approximately 104.44°C (220°F) and approximately 148.89°C (300°F), A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rate of approximately 113,400t (250Mlb) / hr to approximately 351,540t (775Mlb) / hr 22. The process of any one of clauses 1 to 21, further comprising the step of operating with.
[0078] Clause 22. A plant for forming a polymer, comprising: a polymerization reactor coupled to a phase separator; a heat exchanger and a pressure let-down valve disposed between the polymerization reactor and the phase separator, the heat exchanger being connected to the polymerization reactor and the pressure let-down valve, and the pressure let-down valve being connected to the phase separator; a stream splitter coupled to the phase separator and coupled to the line at a location upstream of the heat exchanger and the pressure let-down valve; Including, plant. Clause 23. The method further comprising: Plant as referred to in clause 22. Clause 24. The method further comprising a vacuum devolatilization extruder coupled to the second phase separator. 2. A plant as referred to in clause 22 or 23. Clause 25. Further comprising one or more valves coupled to the second line, the one or more valves configured to prevent flow of material in the second line from entering the first line at a location upstream of the heat exchanger and the pressure let-down valve. 25. A plant according to any one of clauses 22 to 24. Clause 26. The phase separator includes a second heat exchanger coupled to the inlet of the phase separator. 26. A plant according to any one of clauses 22 to 25. Clause 27. The plant of any one of clauses 22-26, wherein the phase separator further comprises a third heat exchanger disposed within the phase separator below the second heat exchanger.
[0079] Overall, the plants and processes of the present disclosure allow for faster transition times between polymer grades while also reducing the amount of off-specification (e.g., degraded polymer and less recycled concentrated polymer in the recycle line) compared to conventional plants and processes. The terms "consists essentially of" and "consisting essentially of," unless otherwise specified, do not exclude the presence of other steps, elements, or materials, whether specifically mentioned herein or not, unless such steps, elements, or materials affect the basic and novel characteristics of the disclosure, and further, they do not exclude impurities and variations commonly associated with the elements and materials used. For the sake of brevity, only certain ranges are explicitly disclosed herein. However, a range from any lower limit can be combined with any upper limit to describe a range not explicitly described, and a range from any lower limit can be combined with any other lower limit to describe a range not explicitly described, and similarly, a range from any upper limit can be combined with any other upper limit to describe a range not explicitly described. Moreover, any point or individual value between its endpoints is included within the range even if not explicitly described. Thus, any point or individual value can act as its own lower limit or upper limit in combination with any other point or individual value or any other lower limit or upper limit to describe a range not explicitly described. All numerical values within this detailed description are modified by the term "about" to account for experimental error and variations that one of ordinary skill in the art would expect.
[0080] All documents described herein, including any priority documents or test procedures, are incorporated herein by reference to the extent that they do not contradict this text. As is apparent from the general description and specific embodiments above, the forms of the disclosure have been illustrated and described, but various modifications can be made without departing from the spirit and scope of the disclosure. Thus, the disclosure is not intended to be limited thereby. Similarly, the term "comprising" is considered synonymous with the term "including" for purposes of U.S. law. Similarly, whenever a composition, element, or group of elements is preceded by the transitional phrase "comprising," we should understand that we also contemplate the same composition or group of elements having the transitional phrase "consisting essentially of," "consisting of," "selected from the group of consisting of," or "is" preceding the description of the composition, element, or elements, and vice versa. While the present disclosure has been described with respect to certain embodiments and examples, those skilled in the art, having the benefit of this disclosure, may devise other embodiments that do not depart from the scope and spirit of the present disclosure.
Claims
1. 1. A process for forming a polymer, comprising: providing a feed having one or more olefin monomers and a solvent; introducing the feed into a reactor along with a catalyst to form a reaction mixture; removing reactor effluent from the reactor; mixing the reactor effluent with a first concentrated polymer solution in a mixer or line to form a mixture; introducing the mixture into a heat exchanger to form a heated mixture; introducing the heated mixture into a pressure let-down valve and then into a phase separator; removing the second concentrated polymer solution from the phase separator; introducing said second concentrated polymer solution into said mixer or line; The process comprising:
2. 2. The process of claim 1, wherein the reactor is a continuous stirred tank reactor.
3. 3. The process of claim 1 or 2, wherein the step of introducing the second concentrated polymer solution into the mixer or line is conducted at a rate of about 500,000 lb / hr or less.
4. said second concentrated polymer solution; a first portion being the second concentrated polymer solution introduced into the mixer or line; The second part and 4. The process of claim 1, further comprising the step of introducing the second concentrated polymer solution into a stream splitter configured to distribute the second concentrated polymer solution into The process further comprising the step of introducing the second portion into a second phase separator.
5. The process of any one of claims 1 to 4, wherein the monomers include octene, butene, propylene and ethylene.
6. While the second concentrated polymer solution is being introduced into the mixer or line, the second concentrated polymer solution a temperature of about 101.67°C (215°F) to about 137.78°C (280°F); a pressure of about 3.999 MPa (580 psig) to about 4.482 MPa (650 psig); A mass flow rate of about 204,120 t (450 Mlb) / hr to about 244,944 t (540 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and Polymer content of about 25 wt % to about 50 wt % The process according to any one of claims 1 to 5, comprising:
7. While the heated mixture is being introduced into the pressure let-down valve, the heated mixture a temperature of about 240° F. to about 340° F.; a pressure of about 2.999 MPa (435 psig) to about 3.792 MPa (550 psig); A mass flow rate of about 226,800 t (500 Mlb) / hr to about 480,816 t (1060 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and Polymer content of about 15 wt% to about 40 wt% The process according to any one of claims 1 to 6, comprising:
8. moreover, stopping the introduction of the second concentrated polymer solution into the mixer or line; ceasing mixing of the reactor effluent with the first concentrated polymer solution; introducing the reactor effluent into the heat exchanger to form a heated reactor effluent; introducing the heated reactor effluent into the pressure let-down valve followed by introducing the heated reactor effluent into the phase separator; removing the third concentrated polymer solution from the phase separator; The process according to any one of claims 1 to 7, comprising:
9. While the heated reactor effluent is being introduced into the pressure let-down valve, the heated reactor effluent a temperature of about 115.56°C (240°F) to about 165.56°C (330°F); a pressure of about 2.999 MPa (435 psig) to about 3.792 MPa (550 psig); A mass flow rate of about 204,120 t (450 Mlb) / hr to about 254,016 t (560 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and Polymer content of about 10 wt % to about 30 wt % The process according to any one of claims 1 to 8, comprising:
10. When the mixture is introduced into the heat exchanger to form the heated mixture, the heated mixture a temperature of about 180° F. to about 280° F.; a pressure of about 3.999 MPa (580 psig) to about 4.482 MPa (650 psig); A mass flow rate of about 464,940 t (1025 Mlb) / hr to about 487,620 t (1075 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and having a polymer content of about 10 wt % to about 30 wt %; and During the introduction of the reactor effluent into the heat exchanger to form the heated reactor effluent, the heated reactor effluent comprises: a temperature of about 60° C. (140° F.) to about 160° C. (320° F.); a pressure of about 3.999 MPa (580 psig) to about 4.482 MPa (650 psig); A mass flow rate of about 226,800 t (500 Mlb) / hr to about 272,160 t (600 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and having a polymer content of about 5 wt % to about 35 wt %; The process according to any one of claims 1 to 9.
11. While the heated mixture is being introduced into the phase separator, the heated mixture a temperature of about 83.33° C. (200° F.) to about 132.22° C. (270° F.); a pressure of about 70 psig to about 170 psig; A mass flow rate of about 181,440 t (400 Mlb) / hr to about 498,960 t (1,100 Mlb) / hr; A steam content of about 15 wt % to about 50 wt %, and having a polymer content of about 15 wt % to about 40 wt %, and While the heated reactor effluent is being introduced into the phase separator, the heated reactor effluent a temperature of about 87.78°C (190°F) to about 137.78°C (280°F); a pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig); A mass flow rate of about 226,800 t (500 Mlb) / hr to about 272,160 t (600 Mlb) / hr; A steam content of about 20 wt % to about 40 wt %, and having a polymer content of about 10 wt % to about 30 wt %; The process according to any one of claims 1 to 10.
12. While the second portion is being introduced into the second phase separator, the second portion a temperature of about 104.44°C (220°F) to about 137.78°C (280°F); a pressure of about 3.792 MPa (550 psig) to about 5.171 MPa (750 psig); A mass flow rate of about 99,792 t (220 Mlb) / hr to about 122,472 t (270 Mlb) / hr; A steam content of about 0 wt % to about 1 wt %, and Polymer content of about 25 wt% to about 60 wt% The process according to any one of claims 1 to 11, comprising:
13. 13. The process of any one of claims 1 to 12, wherein the step of introducing the heated mixture into the phase separator is performed by introducing the heated mixture into an inlet of the phase separator, and a second heat exchanger is coupled with the inlet of the phase separator.
14. 14. The process of any one of claims 1 to 13, wherein introducing the heated mixture into the phase separator further comprises introducing the heated mixture into a third heat exchanger disposed within the phase separator below the second heat exchanger.
15. The process of any one of claims 1 to 14, wherein the second heat exchanger comprises a first plurality of tubes and the third heat exchanger comprises a second plurality of tubes.
16. The second heat exchanger comprises: a temperature of about 101.67°C (215°F) to about 148.89°C (300°F); A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rates of about 113,400 t (250 Mlb) / hr to about 480,816 t (1060 Mlb) / hr The process according to any one of claims 1 to 15, wherein the process is operated at
17. The third heat exchanger comprises: a temperature of about 101.67°C (215°F) to about 148.89°C (300°F); A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rates of about 113,400 t (250 Mlb) / hr to about 344,736 t (760 Mlb) / hr The process according to any one of claims 1 to 16, wherein the process is operated at
18. the first heat exchanger is operated at about 26,375 MJ (25 MMBtu) / hr to about 52,750 MJ (50 MMBtu) / hr; The process according to any one of claims 1 to 17.
19. the second heat exchanger is operated at about 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr; and the third heat exchanger is operated at about 10,550 MJ (10 MMBtu) / hr to about 31,650 MJ (30 MMBtu) / hr; The process according to any one of claims 1 to 18.
20. the first heat exchanger is operated at about 36,925 MJ (35 MMBtu) / hr to about 42,200 MJ (40 MMBtu) / hr; the second heat exchanger is operated at about 18,990 MJ (18 MMBtu) / hr to about 23,210 MJ (22 MMBtu) / hr; and the third heat exchanger is operated at about 18,990 MJ (18 MMBtu) / hr to about 23,210 MJ (22 MMBtu) / hr; The process according to any one of claims 1 to 19.
21. The phase separator, a temperature of about 220° F. to about 300° F.; A pressure of about 0.414 MPa (60 psig) to about 1.172 MPa (170 psig), and Mass flow rates of about 113,400 t (250 Mlb) / hr to about 351,540 t (775 Mlb) / hr The process of any one of claims 1 to 21, further comprising the step of operating with
22. 1. A plant for forming a polymer, comprising: a polymerization reactor coupled to a phase separator; a heat exchanger and a pressure let-down valve disposed between the polymerization reactor and the phase separator, the heat exchanger being connected to the polymerization reactor and the pressure let-down valve, and the pressure let-down valve being connected to the phase separator; a stream splitter coupled to the phase separator and coupled in line to a location upstream of the heat exchanger and the pressure let-down valve; The plant comprising:
23. 23. The plant of claim 22, further comprising a second phase separator coupled to the stream splitter.
24. 24. The plant of claim 22 or 23, further comprising a vacuum devolatilizing extruder coupled to the second phase separator.
25. 25. The plant of any one of claims 22 to 24, further comprising one or more valves coupled to a second line, the one or more valves configured to prevent flow of material in the second line from entering the first line at a location upstream of the heat exchanger and the pressure let-down valve.
26. A plant according to any one of claims 22 to 25, wherein the phase separator comprises a second heat exchanger connected to an inlet of the phase separator.
27. The plant of any one of claims 22 to 26, wherein the phase separator further comprises a third heat exchanger disposed within the phase separator below the second heat exchanger.
Citation Information
Patent Citations
Production of polyolefin
JP1994263821A
Plants and processes for forming polymers
JP2016164284A
Devolatilization Processes
US20210284764A1
Cited By
Concentration Method and Concentrator Module for Continuous Flow Microreaction System
KR103043259B1