Selective leaching
The method selectively dissolves Cu and Ni/Co from lithium-ion battery alloys while keeping Fe in a residue, addressing inefficiencies in existing separation methods by enhancing solution concentration and reducing impurities and downstream processing needs.
Patent Information
- Application Number
- JP2024532521
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-13
AI Technical Summary
Existing methods for recycling lithium-ion battery alloys fail to effectively separate iron (Fe) from copper (Cu), nickel (Ni), and cobalt (Co) without introducing additional impurities or requiring extensive downstream processing, leading to inefficiencies and increased waste.
A method involving the use of an oxidizing agent under controlled acidic conditions to selectively dissolve Cu and one or more of Ni and Co from alloy powders while minimizing Fe dissolution, using stoichiometric amounts of acid without neutralizing reagents, allowing for efficient separation of Fe into a solid residue.
This approach enhances the concentration of valuable metals in the leaching solution, reduces the need for downstream processing, and minimizes the introduction of impurities, thereby optimizing the recovery process and reducing operational costs.
Smart Images

Figure 2024542277000001 
Figure 2024542277000002 
Figure 2024542277000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of hydrometallurgy and describes a method for selectively dissolving metals such as copper, nickel or cobalt under acidic and oxidizing conditions, while excluding iron, from alloys originating from recycled batteries. [Background technology]
[0002] During the life cycle of a lithium-ion battery, various waste and scrap materials are generated that need to be recycled due to environmental concerns and due to the valuable metals contained in these batteries.
[0003] Waste formation already starts during the manufacturing of lithium-ion batteries. Due to high quality standards and low efficiency of the process, different parts of the lithium-ion battery are rejected or discarded at different process steps. During the manufacturing process, these discarded materials can vary from off-spec cathode powder, to electrode foils, anodes, separators or cathode foil combinations, to battery cells without electrolyte, battery cells with electrolyte, charged battery cells and modules. From the point of view of waste management and recycling, the complexity of these materials increases towards the end of the manufacturing process as more and more materials are added to the product. Discarded battery cells contain most of the elements in the periodic table, e.g. Ni, Co, Mn, Li, Fe, Al, V, P, F, C, Ti or Mg in the cathode, Li, Ti, Si, C, Al or Cu in the anode, Li, F, P or VOC in the electrolyte, Al, Fe, Cu, Ni, Cr or Cl or Br containing plastics in the casing and more depending on the technological development in the lithium-ion battery industry.
[0004] Besides all of these lithium-ion battery manufacturing waste products, batteries also end up as waste at the end of the consumer stage. In terms of material complexity, these end-of-life batteries are comparable to discarded battery cells at the end of the manufacturing process. They can be even more complicated, as the collection and sorting of end-of-life batteries is not 100% selective for lithium-ion batteries. This means that lithium-ion battery recyclers must also deal with a small percentage of all kinds of other batteries, such as alkaline, Ni-Cd, NiMH or Zn batteries, that may be mixed with lithium-ion batteries.
[0005] WO2020212546 describes a scheme for recovering valuable metals from spent rechargeable batteries or their scrap, starting with a pyrometallurgical refining operation of the waste fraction. The refining operation separates the elements Ni, Co, Mn, Cu and Fe from impurities, which are rejected into a slag, to produce a metal alloy containing most of Ni, Co, Mn, Cu and Fe from the feed. The metal alloy fraction is then separated from the slag, converted to powder and further processed in a hydrometallurgical operation. After dissolution of the complete alloy in acidic conditions, Cu is first removed by cementation, which precipitates as metallic copper. Fe is then removed in a separate step by oxidation with O2 and addition of Na2CO3 as a neutralizing agent to produce an Fe-precipitate.
[0006] Such a procedure of sequential Cu-cementation and Fe-precipitation from Ni- and / or Co-bearing solutions is common practice. In fact, most Fe removal operations rely on the extraction of insoluble Fe at low free acid concentrations. 3+The process relies on the precipitation of the compounds. This is described, for example, in Monhemius et al. ("The iron elephant: A brief history of hydrometallurgists' struggles with element no. 26", CIM Journal 8(4): pp. 197-206, 2017). Such processes typically use a combination of an oxidizing agent to promote the conversion of ferrous iron to ferric iron, and a basic reagent to neutralize the free acid, to promote the precipitation of ferric compounds at low free acid concentrations. Common oxidizing agents are air, O2, H2O2, and Cl2. Stronger oxidizing agents, such as hypochlorites, persulfates, or permanganates, can also be applied. Hydroxides or carbonates, especially NaOH, Na2CO3, Mg(OH)2, Ca(OH)2, CaCO3, NH4OH, or (NH4)2CO3, are usually used as neutralizing agents.
[0007] Besides Fe, many other impurities may be present in the feed solution, such as Cr, Al, As, Sb, Sn, W or Cu. These elements may be hydrolyzed and precipitated together with Fe. Hydrolysis procedures use, for example, sodium hydroxide, lithium hydroxide, ammonia, potassium hydroxide or calcium hydroxide. In all these cases, additional elements such as K, Ca, Na, Li or NH4 are introduced into the solution by neutralizing reagents, which is a clear disadvantage when aiming for a high purity operation.
[0008] WO2019090389 presents a way to avoid the introduction of additional contaminants by neutralizing compounds. As part of the flowsheet for converting Ni metal powder feed to nickel sulfate solution, hydrolysis is described for the removal of impurities, including Fe, by neutralization. Ni hydroxide is used as a neutralizing reagent to replace the more traditional alkaline bases. It is specifically mentioned that sodium hydroxide or potassium hydroxide bases are avoided, as these bases typically lead to alkaline contamination. Ni hydroxide is prepared in a separate operation by precipitating Ni from a portion of the purified solution using sodium hydroxide. In this way, sodium does not enter the mainstream of the operation, but sodium hydroxide consumption remains. Despite the use of Ni-containing metal feed in the mainstream, the additional equipment for producing Ni hydroxide makes this essentially a two-stage process.
[0009] Another approach to separate Ni and / or Co from impurities coexisting in the feed is by selective leaching of the feed: selected impurities are dissolved to a lesser extent or these selected impurities are preferentially rejected into the solid residue. This is described, for example, in WO2019064996, where a battery alloy is subjected to a leaching operation in the presence of a sulfiding agent, thus preferentially dissolving Ni, Co and Fe while leaving most of the Cu in the residue, which is then separated from the other elements by solid / liquid filtration.
[0010] WO2019102765 presents a different approach based on electroleaching of alloys from battery smelting ("battery alloys"), selectively dissolving Ni, Co and Fe from these alloys while simultaneously electrodepositing Cu onto the cathode. In this way, Cu is separated during leaching of the battery alloy, avoiding that a large part of the Cu from the feed ends up in the leachate.
[0011] The documents cited above highlight different methods of leaching alloys. All have in common that the Fe contained in those alloys is completely dissolved together with the other metals. Therefore, separation of most of the Fe from the other dissolved metals in the feed requires a separate downstream treatment of the leachate.
[0012] In conventional schemes for processing alloy powders, Fe is first dissolved in a leaching operation and then removed from solution in downstream Fe removal. For example, when leaching alloy powders using H2SO4, Fe is initially dissolved as FeSO4 during leaching via the following reaction: Fe+H2SO4+1 / 2 O2→FeSO4+H2O.
[0013] It is then oxidized and precipitated during Fe removal as, for example, FeOOH by: 2 FeSO4+H2SO4+1 / 2 O2 →2 Fe2(SO4)3+H2O and Fe2(SO4)3+4 H2O →2 FeOOH(s)+3 H2SO4.
[0014] The acid released during Fe precipitation is typically neutralized using, for example, Ca(OH)2 or NaOH and converted to the CaSO4 or Na2SO4 salts: H2SO4+Ca(OH)2 → CaSO4+2 H2O or H2SO4+2 NaOH → Na2SO4+2 H2O.
[0015] In such conventional schemes, Fe is first consumed during leaching in a stoichiometric amount of acid. In a subsequent Fe removal operation, this acid is neutralized with caustic compounds such as carbonates or hydroxides of Na, K, Mg, Ca, Li, or ammonia. The reaction products are often ammonium, alkali, or earth-alkali salts. These reaction products may ultimately remain in the product solution and introduce additional impurities such as Na, K, Mg, Ca, Li, NH4. Alternatively, these reaction products may ultimately remain in the Fe residue and introduce additional impurities and increase the mass of this residue, which is often considered waste.
[0016] CN105063349A uses a catalyst such as ammonium sulfate, ammonium persulfate, copper sulfate or ferrous sulfate, and adds more than a stoichiometric amount of acid to dissolve Ni, Co and Cu, thereby producing H in the presence of oxygen. 2 SO 4 This invention discloses a method for recovering Cu, Ni and Co from refined alloys by [Prior art documents] [Patent documents]
[0017] [Patent Document 1] International Publication No. 2020 / 212546 [Patent Document 2] International Publication No. 2019 / 090389 [Patent Document 3] International Publication No. 2019 / 064996 [Patent Document 4] International Publication No. 2019 / 102765 [Non-patent literature]
[0018] [Non-Patent Document 1] Monhemius et al., “The iron elephant: A brief history of hydrometallurgists'struggles with element no. 26,” CIM Journal 8(4): pp. 197–206, 2017. Summary of the Invention [Means for solving the problem]
[0019] The present invention discloses a method for dissolving Ni and / or Co and Cu from metal battery alloys while simultaneously preventing the complete dissolution of the Fe contained in such alloys, where instead some of this Fe is rejected to a solid residue and separated by solid / liquid separation.
[0020] The key to the method is the use of an alloy powder containing Cu with reducibility and one or more of Ni and Co, combined with the use of an oxidizing agent, all in a single operation. Cu and Fe are separated. The presented method therefore advantageously combines materials and reaction conditions that are typically not used or used in combination. The introduction of additional impurities into the method is limited or even completely avoided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] A first embodiment is a method for the separation of Fe from Cu and one or more of Ni and Co contained in an alloy powder having more than 1% by weight of Cu, comprising the steps of: - contacting the alloy powder, under oxidizing conditions, with a stoichiometric amount of acid solution chosen between a minimum suitable for dissolving 50% of all metallic elements other than Fe and a maximum suitable for dissolving 100% of all metallic elements other than 50% of Fe, thereby obtaining a leach solution containing a majority of Cu and of one or more of Ni and Co, and a residue containing a majority of Fe; - separating the leachate from the residue; A method is described, including:
[0022] By "alloy powder" is meant a metal alloy in powder form, i.e. a mixture of zero-valent metals. The alloy powder should preferably contain more than 90% by weight, more preferably 95% or even 98% Cu, Co, Ni, Mn and Fe in total. In practice, the alloy may contain other elements, in particular oxygen, as impurities introduced during the manufacturing process or by subsequent contact with the environment. This is particularly relevant when fine powders are manufactured and / or handled without an inert atmosphere, possibly resulting in considerable oxidation of the reactive powder. The alloy powder preferably contains at least 25% by weight Co and Ni in total. The alloy powder preferably contains at least 1% by weight Fe, since prior separation during leaching does not make industrial sense below that limit. This alloy powder may be a mixture of particles with different individual compositions. In this case, when referring to the composition, we mean the average composition of all the particles.
[0023] The amount of acid solution is referred to as "stoichiometric" because it can be derived from the stoichiometry of the dissolution reactions involved. This assumes that the composition of the alloy is at least approximately known, which is typically the case in industrial practice.
[0024] The method can be optimized by selecting alloy powders containing the elements Ni and / or Co, which will at least partially dissolve, thereby enhancing the value of the solution.
[0025] Unlike conventional schemes, a neutralizing reagent is not used in the present method, so no dilution of the product solution occurs due to the introduction of a neutralizing reagent, and the costs associated with the use of caustic compounds typically used as neutralizing reagents are avoided.
[0026] Unlike conventional schemes, caustic compounds such as hydroxides of Na, K, Mg, Ca, Li, or ammonia are not used in the present process. Therefore, no additional impurities are introduced into the solution. This eliminates the need for downstream operations to separate impurities such as Na, K, Mg, Ca, Li, NH4 from valuable elements such as Co and / or Ni.
[0027] Unlike conventional schemes, Fe does not consume acid during the leaching operation, so the optimized process achieves the best possible use of the acid from the leaching operation and the acid generated in the process. Such acid is used to dissolve additional Cu, Ni and / or Co present in the alloy powder.
[0028] Unlike the conventional scheme, in the present method Fe is not dissolved during leaching first and then removed in a separate unit operation. Instead, most of the Fe is not dissolved during leaching. The inventors have found that this allows the concentration of other metals in the leach solution to be increased. To avoid unwanted precipitation and solids scaling when handling the leachate, the total concentration of elements in the solution after leaching should be below their maximum combined solubility. Since most of the Fe is not dissolved, the Fe concentration in the solution after leaching is lower in the present method compared to the conventional scheme where most or all of the Fe is dissolved. As a result, higher concentrations of other elements can be targeted without exceeding the maximum combined solubility of all elements in the solution. This can be achieved by increasing the amount of alloy powder per volume in the leaching operation. This allows the reactor size to be reduced for a given volume of alloy powder, since more alloy can be processed per volume. It also reduces the volumetric flow rate of the product solution, thereby reducing the footprint or increasing the capacity of downstream unit operations.
[0029] The presence of at least a minimum amount of Cu is essential. Already, a concentration of at least 1% Cu in the alloy has been found to be a suitable minimum to achieve a commercially viable process. It is actually believed that Cu has a catalytic effect in the current process.
[0030] In a further embodiment, the alloy powder also contains Mn.
[0031] A "major portion" of an element means 50% by weight or more of the amount of that element entering the process.
[0032] In a further embodiment according to the first embodiment, the stoichiometry of the acidic solution in the contacting step is determined to dissolve all metal elements except Fe.
[0033] However, this amount is somewhat theoretical. In practice, the desired elements are not dissolved quantitatively, and Fe is necessarily dissolved to a limited extent. The amount of acid defined as the lower limit allows the dissolution of Fe to be minimized while ensuring the dissolution of most of Ni, Co, Mn, and Cu. The amount defined as the upper limit allows the dissolution yield of Ni, Co, Mn, and Cu to be optimized while keeping most of the Fe in the residue.
[0034] It is acceptable to dissolve at least 50% of all metal elements other than Fe, but it is preferred to dissolve a higher amount of valuable metal, such as at least 90%, 95% or even 98% of the valuable metal.
[0035] On the other hand, the present method limits the amount of acid to dissolve no more than 50% of the Fe, preferably no more than 25% of the Fe, and even more preferably no more than 10% of the Fe.
[0036] In this way, the process allows the separation of most of the Fe from other valuable metals without the need to first completely dissolve it. This advantageously reduces the amount of acid required for the process, while avoiding post-treatment operations to treat the dissolved Fe. The following examples illustrate excellent leaching yields, especially of Co and Ni, but also of Cu, while minimizing the amount of Fe in solution.
[0037] In a further embodiment, the alloy powder originates from the recycling of lithium ion batteries or their waste materials using a pyrometallurgical process.
[0038] Battery alloys, especially when originating from lithium ion batteries or waste materials thereof processed by pyrometallurgy, are likely to contain Cu and one or more of Ni and Co. In this way, the required minimum concentration of Cu is always present, while the value of Ni and / or Co in particular makes the process industrially interesting.
[0039] Lithium ion batteries or their waste products include new or discarded lithium ion batteries, spent or end-of-life batteries, manufacturing or battery scrap, battery components such as electrode foils, electrolytes, separators, casing materials and electrode materials, or pre-processed battery materials, resulting in a very complex waste stream. The metals of interest in such waste streams are typically copper, nickel and / or cobalt, which end up as alloys when processed by pyrometallurgy.
[0040] In a further embodiment, the alloy powder is obtained by milling or atomization.
[0041] Compared to conventional schemes that aim at complete dissolution of the alloy, the amount of acid added in the present method is more limited. As a result, the average acidity during the leaching process is lower. As a result, the process conditions are milder. However, the inventors have surprisingly found that alloy powders containing Cu and one or more of Ni and Co are sufficiently reactive to dissolve under these mild conditions, resulting in high dissolution yields of Cu, Ni and / or Co. Such powders can be obtained by grinding or atomization, in particular by grinding or spray atomization, e.g. water jet atomization. This is in contrast to larger particles such as granules or other large agglomerates of alloys that cannot be efficiently used in the current method due to their lower reactivity, explained by their lower specific surface area.
[0042] The use of alloy powders allows processing in conventional stirred reactors, which allow good process rates by facilitating mass and energy transfer through full or partial suspension of the powder, and these reactors also allow good distribution of the oxidizing agent, both when using a gaseous reagent such as oxygen or a liquid reagent such as hydrogen peroxide.
[0043] In a further embodiment, the alloy powder has a particle size distribution with a D90 of less than 800 μm and / or a D50 of less than 300 μm.
[0044] D50 and D90 refer to the distribution by number. The particle size distribution of the alloy powder is measured by laser diffraction. Laser diffraction can be performed according to ISO 13320:2020. Particles with D90 above 800 μm and / or D50 above 300 μm require more mixing power for suspension in the stirred reactor. This increases the energy consumption and wear of the equipment, making such coarser powders less preferred in the process.
[0045] In a further embodiment, the acid in the acidic solution is either H2SO4 or HCl.
[0046] The use of either H2SO4 or HCl is preferred, although other acids are theoretically possible. Many hydrometallurgical flowsheets are based on one of these two, making the process easy to integrate into existing operations.
[0047] In a further embodiment, the contacting step comprises: - mixing the alloy powder with a first amount of an acidic solution corresponding to 50% to 95% of the selected stoichiometric amount, thereby obtaining a suspension comprising a liquid phase and a solid phase; - oxidizing the suspension; and - acidifying the suspension with a second amount of an acidic solution, whereby the sum of the first and second amounts corresponds to 100% of the determined stoichiometric amount. This will be implemented in stages.
[0048] The first amount of acid can be added fairly quickly to save time, because precise determination ensures that a relatively large, but still substoichiometric, portion of the total amount of acid determined is added.Then, the second amount of acid, typically less than the first amount, is added more slowly to achieve better process control.This embodiment is therefore an efficient multi-step process.
[0049] Between the addition of the first amount of acidic solution and the addition of the second amount of acidic solution, oxidizing conditions are maintained. During this intermediate step, the metal in the suspension will continue to oxidize and the suspension will move toward thermodynamic equilibrium. As a result, less metal needs to be oxidized during the second addition step. The rate of metal dissolution in the second addition step is less limited by the oxidation reaction, which is typically the reaction with the lowest reaction rate. The intermediate equilibrium allows for faster system reaction during the second addition and allows for more precise process control when adding the acid.
[0050] A further embodiment is a method for the separation of Fe from Cu and one or more of Ni and Co contained in an alloy powder having more than 1 wt.% Cu, comprising the steps of: - contacting the alloy powder under oxidizing conditions with a stoichiometric amount of an acidic solution suitable to dissolve at least 50% of all metallic elements other than Fe and at most 100% of all metallic elements other than 50% of Fe, thereby obtaining a leach solution containing a majority of Cu and one or more of Ni and Co and a residue containing a majority of Fe, wherein the acid in the acidic solution is H2SO4 and the contacting step is - determining the stoichiometric amount of acid solution to dissolve 100% of all metallic elements other than Fe; - mixing the alloy powder with an acidic solution in an amount corresponding to 50% to 100% of the determined stoichiometric amount, thereby obtaining a suspension containing liquid and solid phases; - oxidizing the suspension to a redox potential of more than 320 mV Ag / AgCl at a temperature of more than 50° C.; provided that if the concentration of Fe in the liquid phase is less than 0.5 g / L, acidifying the suspension by adding an acidic solution under oxidizing conditions at a temperature above 50° C. until the concentration of Fe is between 0.5 g / L and 3 g / L; - However, if the pH of the liquid phase is greater than 3, acidifying the suspension by adding an acidic solution at a temperature greater than 50°C under oxidizing conditions until the pH is between 1.5 and 3. and - separating the leachate from the residue; A method is described, including:
[0051] The "step of determining the stoichiometry" of the acid solution is - at least 50% of all metallic elements in the alloy other than Fe, and - at most 100% of all metallic elements in the alloy other than 50% of Fe, or in other words, half of the iron plus at most 100% of all non-ferrous metals in the alloy "Means physical or mental activity to determine the amount of acid needed to dissolve a substance."
[0052] The physical activity may involve chemical analysis of a sample of the alloy. The mental activity may be an empirical evaluation with similar alloys, a calculation, or any other approximation of the approximate required stoichiometry. The calculation or approximation may be based on the premise that the metallic elements in the alloy dissolve as divalent cations. The following reaction illustrates the stoichiometry when using either sulfuric or hydrochloric acid: M+H2SO4+1 / 2O2→MSO4+H2O, or M+2HCl+1 / 2O2→MCl2+H2O, where M is Ni, Co, Mn, Cu, and Fe.
[0053] This embodiment is preferred because the second amount of acid can be added more precisely by monitoring the pH and / or dissolved Fe, which is particularly useful when the composition of the starting material is not precisely known.
[0054] In the present process, the addition of the first amount of acid is carried out at a temperature above 50° C. Higher temperatures such as 60° C. or 70° C. are beneficial for the reaction rate and accelerate the process. Depending on the reactor characteristics, the temperature may increase during leaching as a result of the heat generated by the dissolution reaction, which is exothermic.
[0055] In a preferred embodiment, the addition of the second amount of acid according to any of the above provisos is carried out at a temperature above 75° C. In this step too, higher temperatures are beneficial for the reaction rate and accelerate the process.
[0056] The first proviso advantageously addresses the situation where the concentration of Fe in solution is very low. At concentrations below 0.5 g / L Fe, the inventors found that not enough alloy powder was dissolved, resulting in lower dissolution yields of valuable elements such as Ni and Co. Acidification will dissolve some Fe, but will increase the leaching yields of Cu, Co and / or Ni, among others. The upper limit of 3 g / L Fe helps to avoid over-acidification.
[0057] The second proviso advantageously addresses the situation where the pH of the solution is too high. At a pH above 3, increasing amounts of Cu, Co and / or Ni are observed in the residue, resulting in unacceptable losses of these valuable metals. The lower pH limit of 1.5 helps to avoid over-acidification, which would result in dissolution of too much or all of the Fe.
[0058] Staged addition with any one of the above proviso allows for faster and more precise process control. Adding all the acid in one stage runs the risk of adding too much acid and dissolving too much Fe.
[0059] The equilibration begins by mixing the first amount of acid solution with the alloy powder and continues during all successive additions. Successive additions of acid solution minimize the risk of adding too much acid, but take longer. The method is also designed to find a balance between adding the first amount of acid solution quickly (preferably close to stoichiometry for all metal elements other than Fe) and saving time, while avoiding adding too much acid that would result in dissolution of too much Fe.
[0060] "The acid in the acidic solution is H2SO4" means that the majority of the acid in the acidic solution used is H2SO4. Therefore, this does not exclude operations where small amounts of another acid, such as HCl or HNO3, are also present in solution. In such cases, any other acid present in the solution must also be taken into account when determining the stoichiometry.
[0061] In a further embodiment, the acid in the acidic solution is HCl and the contacting step comprises: - determining the stoichiometry of the acid solution according to a first embodiment; - mixing the alloy powder with an acidic solution in an amount corresponding to 50% to 100% of the determined stoichiometric amount, thereby obtaining a suspension containing liquid and solid phases; - oxidizing the suspension to a redox potential of more than 320 mV Ag / AgCl at a temperature of more than 50° C.; provided that if the pH of the liquid phase is greater than 2, acidifying the suspension by adding an acidic solution at a temperature greater than 50° C. under oxidizing conditions until the pH is between 0.5 and 2. This will be implemented in stages.
[0062] Although H2SO4 is perhaps more frequently used in industry, HCl has the same advantages and is therefore an equally preferred option. The inventors have observed that the selectivity for dissolving metals is typically somewhat better when using HCl. They have also observed that under the conditions of the present process, the Fe concentration in the leach solution is very low, making the provisos regarding Fe concentration largely irrelevant. Therefore, in this embodiment, only the provisos regarding pH apply.
[0063] The pH range when using HCl is lower (i.e., more acidic) than that of H2SO4.
[0064] By "the acid in the acidic solution is HCl" we mean that the majority of the acid in the acidic solution used is HCl. Therefore, this does not exclude operations where small amounts of another acid, such as H2SO4 or HNO3, are also present in solution. In such cases, any other acid in the solution must also be taken into account when determining the stoichiometry.
[0065] The option of using HCl or H2SO4 results in two independent embodiments.
[0066] In a further embodiment, the oxidizing conditions in the contacting step are obtained by the addition of H2O2 and / or O2 containing gas. The use of air is possible but will result in a lower process rate compared to the use of O2 gas.
[0067] In a further embodiment, the process is carried out at atmospheric pressure: high pressure leaching is not required, avoiding the use of more expensive autoclaves.
[0068] In a further embodiment, the acidic solution in the contacting step is obtained by acid leaching of a solid starting material containing Ni and / or Co. These elements will end up in the leaching solution together with the metals introduced by the dissolved alloy powder. Fe may also be present in this acidic solution, but the Fe concentration is preferably less than 3 g / L, preferably less than 2 g / L, more preferably less than 1 g / L. If less Fe is present in the starting solution, more Fe dissolution from the alloy powder can be tolerated. Allowing more Fe dissolution from the alloy powder can be beneficial to maximize the dissolution yield of Ni, Co and / or Cu.
[0069] In a further embodiment, the alloy powder and the solid starting material have the same composition. This preferred setup helps to avoid the introduction of further impurities while contributing to the overall yield of pure valuable metals such as Ni and / or Co. This includes processing schemes where the solid starting material is the same alloy powder. In such schemes, the acidic starting solution may come from a recycle stream from a unit operation downstream of the leaching operation. Optionally, Fe may be removed from this recycle stream before it is used as the acidic starting solution in the leaching operation in order to limit the Fe concentration in the starting solution.
[0070] In a further embodiment, the mixing, oxidation, and acidification steps are operated sequentially as a continuous process.
[0071] Compared to batch processes, such continuous processes make it possible to increase the process intensity in industrial setups.
[0072] In a further embodiment, the leach solution obtained in the step of separating the leach solution from the residue is further treated in an electrowinning step to separate Cu from other metals contained in said solution, in particular from Ni and / or Co.
[0073] Electrowinning can be carried out, for example, directly in the leach solution ("direct EW") or can be combined with solvent extraction ("SX-EW").
[0074] In a further embodiment, the residue obtained in the step of separating the leach solution from the residue is used as starting material for steel making.
[0075] The following examples illustrate the invention.
[0076] Example 1 This example describes an embodiment using a two-stage addition of sulfuric acid, where the second addition is triggered by a pH-related criterion.
[0077] The CoNiCuFeMn-alloy originates from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser diffraction: the average particle size has a D50 of 96 μm and a D90 of 298 μm.
[0078] The elemental composition by mass is 59% Co, 9.5% Ni, 0.3% Mn, 25% Cu, and 5.1% Fe.
[0079] 252 g of this alloy powder is added to a beaker with 1.4 L of demineralized water. Upon mixing a suspension is formed which is heated to 65° C. O2 is sparged into the suspension at 75 L / hr.
[0080] The stoichiometric amount of acid to dissolve all metal elements except Fe is determined to be 3.93 mol H2SO4, which can be derived directly from Table 1a. This corresponds to 772 mL of an acidic aqueous solution containing 500 g / L H2SO4.
[0081] [Table 1]
[0082] Choose to add 69% of the amount determined above to the suspension. This corresponds to 530 mL of acidic aqueous solution. Add the solution slowly over a period of 3 hours while sparging.
[0083] The temperature is then increased to 82° C. while continuing to sparge. The redox potential rises to 326 mV Ag / AgCl and the pH to 4.03. The liquid is sampled and the Fe concentration is measured to be 0.6 g / L.
[0084] This Fe level is not below the threshold of 0.5 g / L: therefore, no further acidification is caused by Fe-related criteria.
[0085] The pH is above the threshold of 3: this triggers the need for further acidification according to pH-related criteria. Aim for a pH between 1.5 and 3.
[0086] Therefore, an additional amount of the acidic aqueous solution is added slowly to the suspension over a period of 3 hours at a temperature of 80° C. while sparging O2 into the suspension at 75 L / hr. When the pH stabilizes at 2.7, the process step is considered complete. An additional amount of 250 ml of the acidic solution is then added.
[0087] In total, 780 mL of 500 g / L H2SO4 solution was used, which is the amount of acidic solution suitable to dissolve at least 50% of all metal elements except Fe, and corresponds to a stoichiometric amount suitable to dissolve 98% of all metal elements except 50% of Fe.
[0088] The solid and liquid fractions are then separated by filtration. 2.0 L of leachate solution is obtained. The mass of the residue is 67.2 g and the water content is 62%. Both compositions are shown in Table 1b, together with the leachate yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0089] [Table 2]
[0090] This example shows how nearly all Co, Ni, Mn and Cu can be dissolved in high yields, while 72% of Fe reports to the residue, which contains only trace amounts of the most valuable metals Co and Ni.
[0091] Example 2 This example represents an embodiment using a single addition of sulfuric acid. No further acidification is effected by either an Fe-related or a pH-related criterion.
[0092] The CoNiCuFeMn-alloy originates from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser diffraction: the average particle size has a D50 equal to 102 μm and a D90 equal to 274 μm.
[0093] The elemental composition by mass is 32% Co, 12% Ni, 2.3% Mn, 26% Cu, and 26% Fe.
[0094] 5543 g of alloy powder is added to a 60 L reactor along with 38 L of demineralized water. Upon mixing a suspension is formed which is heated to 60° C. O2 is sparged into the suspension at 400 L / hr.
[0095] The stoichiometric amount of acid to dissolve all metal elements except Fe is determined to be 66.45 mol H2SO4, which can be derived from Table 2a. This corresponds to 4.90 L of an acidic solution with 1330 g / L H2SO4.
[0096] [Table 3]
[0097] Choose to add 99% of the amount determined above to the suspension. This corresponds to 4.85 liters of aqueous acid. While sparging, add the solution slowly over a period of 4.5 hours.
[0098] After adding the acidic aqueous solution, the redox potential in the suspension is measured to be 216 mV vs Ag / AgCl, and the pH is 1.6.
[0099] The temperature is then increased to 80°C while continuing to sparge. The redox potential rises to 340mV vs Ag / AgCl and the pH to 2.9. The liquid is sampled and the Fe concentration is measured to be 1.9g / l.
[0100] The pH does not exceed the 3.0 threshold and the Fe level does not fall below the 0.5 g / l threshold. This means that no further acidification is caused by either the Fe-related or the pH-related criteria. Therefore, no additional acid solution is added. This means that in total, 4.85 L of 1330 g / L H2SO4 solution is consumed. This corresponds to the stoichiometric amount suitable for dissolving 83% of all metallic elements except 50% of Fe.
[0101] The solid and liquid fractions are then separated by filtration. 35 L of leachate solution is obtained. The mass of the residue is 9387 g with a water content of 69%. Both compositions are shown in Table 2b, together with the leachate yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0102] [Table 4]
[0103] This example shows how it is possible to dissolve almost all the Co, Ni, Mn and most of the Cu, while 95% of the Fe appears in the residue. In comparison to example 1, a second addition of acid is not necessary, since neither the claimed dissolved Fe nor the pH provisos are triggered.
[0104] Example 3 This example represents an embodiment using two-stage addition of sulfuric acid, the second addition being driven by an Fe-related standard.
[0105] The CoNiCuFeMn-alloy comes from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser: the average particle size has a D50 equal to 143 μm and a D90 equal to 296 μm.
[0106] The elemental composition by mass is 19% Co, 44% Ni, 7.8% Mn, 22% Cu, and 5.8% Fe.
[0107] 4638 g of alloy powder is added to a 60 L reactor along with 42 L of demineralized water. Upon mixing a suspension is formed which is heated to 60° C. O2 is sparged into the suspension at 350 L / hr.
[0108] The stoichiometric amount of acid to dissolve all metal elements except Fe is determined to be 72.37 moles of H2SO4, which can be derived directly from Table 3a. This corresponds to 5.33 L of aqueous acid solution containing 1330 g / L H2SO4.
[0109] [Table 5]
[0110] Choose to add 90% of the amount determined above to the suspension. This corresponds to 4800 mL of the acidic aqueous solution. While sparging, add the solution slowly over a period of 5.5 hours.
[0111] After adding the acidic aqueous solution, the redox potential of the suspension is measured to be 370mV vs Ag / AgCl, and the pH is measured to be 0.5. The liquid is sampled, and the Fe concentration in the liquid at this point is measured to be 5.5g / L.
[0112] The temperature is then increased to 80° C. while continuing to sparge. The liquid is sampled and the Fe concentration is monitored hourly. After 10 hours, the Fe concentration is measured to be 0.42 g / L.
[0113] This Fe level is below the threshold of 0.5 g / L: this triggers the need for further acidification according to the Fe-related criteria. Aim for an Fe concentration of 2.5 g / l.
[0114] Therefore, an additional amount of the aqueous acid solution is slowly added to the suspension over a period of 4 hours, at a temperature of 80° C., while sparging O2 into the suspension at 350 L / hr. The process steps are considered to be complete when the targeted Fe concentration of 2.5 g / l is reached. An additional amount of 570 ml of the acid solution is then added. At this point, the pH is measured to be 2.0.
[0115] In total, 5370 mL of 1330 g / L H2SO4 solution was used, which corresponds to a stoichiometric amount suitable for dissolving 101% of all metal elements except Fe, which also corresponds to a stoichiometric amount suitable for dissolving 97% of all metal elements except 50% of Fe.
[0116] The solid and liquid fractions are then separated by filtration. 42 liters of leach solution are obtained. The residue weighs 3408 g and has a water content of 86%. Both compositions are shown in Table 3b, together with the leach yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0117] [Table 6]
[0118] This example shows how almost all Co, Ni, Mn and Cu can be dissolved in high yields, while 61% of Fe appears in the residue, which contains only trace amounts of the most valuable metals Co and Ni.
[0119] Example 4 This example illustrates a different approach to adding the acid solution.
[0120] The CoNiCuFeMn-alloy originates from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser diffraction: the average particle size has a D50 of 162 μm and a D90 of 458 μm.
[0121] The elemental composition by mass is 38% Co, 9% Ni, 2.2% Mn, 22% Cu, and 27% Fe.
[0122] 250 g of this alloy powder is added to a beaker with 1.7 L of demineralized water. Upon mixing a suspension is formed which is heated to 75° C. O2 is sparged into the suspension at 75 L / hr.
[0123] The stoichiometric amount of acid to dissolve all metallic elements except Fe is not determined in advance. Instead, pH measurement in the liquid is used to control the acid addition with a simple feedback loop that keeps the pH below 2.0. So if the pH drops below this set point of pH 2.0, the acid addition is interrupted. The acid addition is resumed only if the pH increases again above the set point of pH 2.0. This increase in pH is explained by the consumption of free acid during the dissolution of the alloy powder.
[0124] Using this technique, a dilute sulfuric acid solution (500 g / L H2SO4) is added slowly to the suspension over a period of 6 hours at a temperature of 75° C. while sparging O2 through the suspension at 75 L / hr. The process step is considered complete when the pH stabilizes at 2.0 without further acid addition.
[0125] At this point, 688 ml of 500 g / L H2SO4 solution was added. The redox potential in the suspension was 396 mV vs Ag / AgCl. The liquid was sampled and the Fe concentration was measured to be 18 g / l.
[0126] The temperature is then increased to 85° C. while continuing to sparge. The pH decreases despite the fact that no additional acid is added. After 5 hours, the pH in the liquid is 1.4.
[0127] At this point, the solid and liquid fractions are separated by filtration. 2.2 L of leach solution are obtained. The mass of the residue is 167 g and the water content is 49%. Both compositions are shown in table 4a, together with the leach yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0128] [Table 7]
[0129] In this example, 688 ml of 500 g / L H2SO4 solution was added using a pH-based controller to add acid, which corresponds to 3.51 mol of acid. This is the amount of acid solution suitable to dissolve at least 50% of all metal elements except Fe, and corresponds to the stoichiometric amount suitable to dissolve 98% of all metal elements except 50% of Fe. This can be derived directly from Table 4b.
[0130] [Table 8]
[0131] This example shows that using a pH-controlled acid feed, it is possible to add an amount of acid that is stoichiometric to dissolve at least 50% of all metal elements except Fe and at most 100% of the metal elements in addition to 50% of Fe. As a result, nearly all Co, Ni, Mn and Cu are dissolved, while 64% of Fe appears in the residue. The residue contains small amounts of the most valuable metals Co and Ni.
[0132] Compared to Examples 1, 2 and 3, the results of this example are less favorable for two reasons. Firstly, the pH of the product solution is equal to 1.4, which is lower than the preferred range between 1.5 and 3. The fact that this pH further decreases after the end of the acid addition can be explained by the fact that acid is released into the solution during the hydrolysis of the iron, for example according to the following reaction: Fe2(SO4)3+4 H2O→2 FeOOH(s)+3 H2SO4
[0133] Second, the Fe concentration in solution is measured to be 11 g / l, which is much higher than the preferred range between 0.5 g / l and 3 g / l.
[0134] The inventors attribute this less favorable result to the fact that instead of first determining the stoichiometric amount of acid solution that would dissolve 100% of all metal elements except Fe, and then limiting the acid to a maximum of 100% of that amount in the first acid addition step, the use of a pH-based controller for the acid addition resulted in the addition of a larger amount of acid. As a result, the system progressed to a less favorable condition that could no longer be corrected by the addition of additional acid.
[0135] Comparative Example 5 The CoNiCuFeMn-alloy originates from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser diffraction: the average particle size has a D50 of 162 μm and a D90 of 361 μm.
[0136] The elemental composition by mass is 32% Co, 13% Ni, 2.4% Mn, 27% Cu, and 27% Fe.
[0137] 220 g of this alloy powder is added to a beaker with 2 L of demineralized water. Upon mixing a suspension is formed which is heated to 63° C. O2 is sparged into the suspension at 80 L / hr.
[0138] 830 mL of a 500 g / L H2SO4 solution is added slowly to the suspension with sparging over a period of 6 hours. The redox potential is measured to be 447 mV vs Ag / AgCl and the pH is measured to be 1.0.
[0139] The solid and liquid fractions are then separated by filtration. 1.9 L of leachate solution is obtained. The mass of the residue is 35.7 g and the water content is 67%. Both compositions are given in table 5, together with the leachate yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0140] [Table 9]
[0141] This example shows that adding too much acid leads to almost complete dissolution of all metals, including Fe, so that they end up in the leach solution.
[0142] Example 6 This example represents an embodiment using hydrochloric acid.
[0143] The CoNiCuFeMn-alloy originates from a battery refining process. It is converted into a powder by atomization. The particle size distribution is measured by laser diffraction: the average particle size has a D50 of 143 μm and a D90 of 296 μm.
[0144] The elemental composition by mass is 19% Co, 44% Ni, 7.8% Mn, 22% Cu, and 5.8% Fe.
[0145] 390 g of this alloy powder is added to a beaker along with 0.85 L of demineralized water. Upon mixing a suspension is formed which is heated to 60° C. O2 is sparged into the suspension at 75 L / hr.
[0146] The stoichiometric amount of hydrochloric acid that will dissolve all metal elements except Fe is determined to be 12.2 mol HCl, which can be derived directly from Table 6a. This corresponds to 1010 mL of an acidic aqueous solution containing 440 g / l HCl.
[0147] [Table 10]
[0148] Choose to add 80% of the amount determined above to the suspension. This corresponds to 810 mL of acidic aqueous solution. The solution is added slowly, with sparging, over a period of 3 hours.
[0149] The redox potential is measured to be 315mV vs Ag / AgCl and the pH is measured to be 2.1.
[0150] The temperature is then increased to 80° C. while continuing to sparge. After 4 hours, the redox potential is measured to be 559 mV Ag / AgCl and the pH has risen to 2.3. The liquid is sampled and the Fe concentration is measured to be 0.01 g / L.
[0151] The pH is above the threshold of 2: this triggers the need for further acidification according to pH-related standards when using hydrochloric acid. Aim for a pH between 0.5 and 2.
[0152] Therefore, an additional amount of the acidic aqueous solution is slowly added to the suspension over a period of 4 hours at a temperature of 80° C. while sparging O2 through the suspension at 75 L / hr. The process step is considered to be complete when the pH stabilizes at 1.7. An additional amount of 140 ml of the acidic solution is then added.
[0153] In total, 1010 ml of 440 g / l HCl solution was used, which corresponds to a stoichiometric amount suitable for dissolving 100% of all metal elements except Fe, which also corresponds to a stoichiometric amount suitable for dissolving 97% of all metal elements except 50% of Fe.
[0154] The solid and liquid fractions are then separated by filtration. 1.6 L of leachate solution is obtained. The mass of the residue is 105 g and the water content is 49%. Both compositions are shown in table 6b, together with the leachate yield calculated as the mass of the element contained in the liquid divided by the sum of the amounts of the element contained in the filtrate and in the solid.
[0155] [Table 11]
[0156] This example shows how nearly all Co, Ni, Mn and Cu can be dissolved in high yields using hydrochloric acid, while more than 99% of Fe appears in the residue, which contains only trace amounts of the most valuable metals Co and Ni.
Claims
1. A method for separating Fe from Cu and one or more of Ni and Co contained in an alloy powder having more than 1% by weight of Cu, contacting said alloy powder with a stoichiometric amount of acidic solution, under oxidizing conditions, selected between a minimum suitable for dissolving 50% of all metallic elements other than Fe and a maximum suitable for dissolving 100% of all metallic elements other than 50% of Fe, thereby obtaining a leach solution containing a majority of Cu and a majority of one or more of Ni and Co, and a residue containing a majority of Fe; separating the leach solution from the residue; A method comprising:
2. 2. The method of claim 1, wherein the alloy powder originates from recycling lithium ion batteries or their waste materials using a pyrometallurgical process.
3. 3. The method according to claim 1 or 2, wherein the alloy powder is obtained by milling or atomization.
4. 4. The method according to any one of claims 1 to 3, wherein the alloy powder has a particle size distribution with a D90 of less than 800 μm and / or a D50 of less than 300 μm.
5. The acid in the acidic solution is H 2 SO 4 5. The method of claim 1, wherein the HCl is either HCl or HCl.
6. The contacting step comprises: mixing the alloy powder with a first amount of an acidic solution corresponding to 50% to 95% of a selected stoichiometric amount, thereby obtaining a suspension including a liquid phase and a solid phase; oxidizing the suspension; and acidifying the suspension with a second amount of acidic solution, whereby the sum of the first amount and the second amount corresponds to 100% of the determined stoichiometric amount. The method according to any one of claims 1 to 5, wherein the method is carried out stepwise by:
7. The acid in the acidic solution is H 2 SO 4 and the contacting step is determining the stoichiometric amount of said acidic solution to dissolve 100% of all metallic elements other than Fe; mixing the alloy powder with an amount of the acidic solution corresponding to 50% to 100% of the determined stoichiometric amount, thereby obtaining a suspension containing a liquid phase and a solid phase; oxidizing the suspension to a redox potential of greater than 320 mV Ag / AgCl at a temperature greater than 50° C.; provided that if the Fe concentration in the liquid phase is less than 0.5 g / L, acidifying the suspension by adding an acidic solution under oxidizing conditions at a temperature above 50° C. until the Fe concentration is between 0.5 g / L and 3 g / L; provided that if the pH of the liquid phase is greater than 3, acidifying the suspension by adding an acidic solution at a temperature greater than 50° C. under oxidizing conditions until the pH is between 1.5 and 3. The method according to any one of claims 1 to 5, wherein the method is carried out stepwise by:
8. the acid in the acidic solution is HCl, and the contacting step comprises:
2. Determining the stoichiometry of the acid solution according to claim 1; mixing the alloy powder with an amount of the acidic solution corresponding to 50% to 95% of the determined stoichiometric amount, thereby obtaining a suspension containing a liquid phase and a solid phase; Oxidizing the suspension to a redox potential of greater than 320 mV Ag / AgCl at a temperature greater than 50° C.; and provided that if the pH of the liquid phase is greater than 2, acidifying the suspension by adding an acidic solution at a temperature greater than 50° C. under oxidizing conditions until the pH is between 0.5 and 2. The method according to any one of claims 1 to 5, wherein the method is carried out stepwise by:
9. The oxidizing conditions in the contacting step are 2 O 2 And / or O 2 9. The method according to claim 1, wherein the method is obtained by the addition of an enriched gas.
10. 10. The process according to any one of claims 1 to 9, wherein the process is carried out at atmospheric pressure.
11. 11. The method according to any one of claims 1 to 10, wherein the acidic solution in the contacting step is obtained by acid leaching of a solid starting material containing Ni and / or Co.
12. The method of claim 11 , wherein the alloy powder and the solid starting material have the same composition.
13. 9. The process of any one of claims 6 to 8, wherein the mixing, oxidation, and acidification steps are operated sequentially as a continuous process.
14. 14. The method according to any one of the preceding claims, wherein the leach solution obtained in the step of separating the leach solution from the residue is further treated in an electrowinning step to separate Cu from other metals contained in the solution, in particular from Ni and / or Co.
15. 2. Use of the residue according to claim 1 as starting material for steel making.
Citation Information
Patent Citations
Method for separating copper from nickel and cobalt
WO2019064996A1
Production of high purity nickel sulfate
WO2019090389A1
Method for treating lithium ion battery waste
WO2019102765A1
Process for the preparation of precursor compounds for lithium battery cathodes
WO2020212546A1