Polypropylene composition suitable for packaging applications

A composition of a mixed plastic polypropylene/polyethylene blend from recycled streams, combined with a heterophasic propylene copolymer, addresses the challenge of enhancing mechanical and impact properties in thin-wall injection molding, reducing impurities and odor, and facilitating the use of recycled materials in packaging.

JP2024542494AInactive Publication Date: 2024-11-15BOREALIS AG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529838
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-01
Filing Date
2022-11-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge lies in improving the mechanical and impact properties of heterophasic propylene copolymers derived from post-consumer recycled polyolefin streams while maintaining high melt flow rates and low impurity levels, particularly in thin-wall injection molding applications, where current compositions rely heavily on virgin polymers and face issues with contamination and odor.

Method used

A composition comprising a mixed plastic polypropylene/polyethylene blend from post-consumer recycled streams blended with a heterophasic propylene copolymer, optimized through a multi-step polymerization process using a single-site catalyst system, achieving a balanced mix of mechanical properties, low impurities, and high melt flow rates.

Benefits of technology

The solution results in a composition suitable for thin-wall injection molding with improved mechanical properties, reduced volatile organic compounds (VOC) and semi-volatile organic compounds (FOG) content, and minimal odor, enabling upcycling of recycled materials into high-quality packaging articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542494000001
    Figure 2024542494000001
  • Figure 2024542494000002
    Figure 2024542494000002
  • Figure 2024542494000003
    Figure 2024542494000003
Patent Text Reader

Abstract

The present invention relates to a composition obtained by blending 50-95% by weight, preferably 55-90% by weight, more preferably 60-88% by weight of a mixed plastic polypropylene / polyethylene blend, component (A), with 5-50% by weight, preferably 10-45% by weight, more preferably 12-40% by weight of a heterophasic propylene copolymer, component (B) (all percentages are based on the total composition), a process for the manufacture of said composition, an article comprising said composition, the use of said composition in the manufacture of an article, and a method for the manufacture of said composition, comprising the steps of: 2 (230°C, 2.16 kg, ISO 1133) and the use of component (B) in said composition to increase the flexural modulus and reduce the VOC and FOG content of said composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high melt flow polypropylene composition having an improved balance of properties with respect to mechanical and impact properties, a process for the manufacture of said polypropylene composition, an article comprising said polypropylene composition and the use of said polypropylene composition in the manufacture of an article. [Background technology]

[0002] Heterophasic propylene copolymers are widely used in the packaging industry due to their excellent combination of stiffness and impact behavior. Heterophasic propylene copolymers find application in many aspects of daily life. One of the main application areas of polypropylene is found in the injection molding of thin-walled articles. Typical examples include plastic cups, pails and small containers, mainly intended for food packaging. To be suitable for thin-walled injection molding applications, polypropylene must exhibit excellent processability / flowability, usually represented by a high melt flow rate (MFR), i.e., a low average molecular weight. Nevertheless, the polymer and packaging industry desires to improve usable heterophasic polypropylene compositions with high melt flow rates (MFR) in terms of mechanical properties, especially the amount of impurities.

[0003] One of the fundamental challenges in the polymer business is recycling. At present, the market for recycled materials, especially those from household waste, commonly called post-consumer recyclates (PCR), is somewhat limited. Starting from household waste, the sorting and separation processes used do not allow the preparation of pure polymers; that is, there is always some contaminant present, or the process may result in a blend of different polymers. As for polyolefins, which make up the majority of the polymer fraction of collected household waste, it is very difficult and costly to completely separate polypropylene and polyethylene. Recycled polyolefin materials, especially post-consumer resins, are traditionally cross-contaminated by non-polyolefin materials such as polyethylene terephthalate, polyamide, polystyrene, or non-polymeric substances such as wood, paper, glass, aluminum, etc. To make matters worse, these post-consumer recycled polyolefin materials, although readily available on a multi-ton scale, unfortunately have limited mechanical properties and often suffer from severe odor and / or emission problems. Packaging industry applications require materials that combine good flowability, low impurities, and balanced mechanical properties between stiffness and impact strength. Recently, market demand has expanded towards the use of recycled polyolefins in blends with virgin polymers to meet specific requirements. However, there is a strong felt need to be able to upcycle and reuse post-consumer polyolefin recycles into end products without posing a risk to health and safety.

[0004] The unpublished patent applications EP 21178566.2 and EP 21178547.2 relate to polypropylene compositions for automotive exterior and interior applications, comprising mixed plastic polypropylene-based blends derived from post-consumer recycled polyolefin streams and inorganic fillers such as talc. These compositions exhibit a beneficial balance of mechanical properties and good flowability. However, these compositions require a fairly large amount of virgin polymer, limiting the amount of post-consumer recycled material.

[0005] The present invention is based on the surprising discovery that by carefully selecting the heterophasic propylene copolymer-based virgin components in polypropylene-based compositions comprising mixed plastic polypropylene / polyethylene blends derived from post-consumer recycled polyolefin streams, polypropylene-based compositions are obtained that exhibit an excellent balance of properties in terms of impact properties, mechanical properties such as flexural modulus, flow properties as indicated by high melt flow rates, and low impurity amounts as exemplified by low amounts of VOCs and FOGs. These compositions comprise a significant amount of mixed plastic polypropylene / polyethylene blends derived from post-consumer recycled polyolefin streams. Thus, the compositions of the present invention comprising mixed plastic polypropylene / polyethylene blends derived from post-consumer recycled polyolefin streams are suitable for injection molding applications, particularly packaging applications such as thin-wall packaging applications, and can replace complex heterophasic polypropylene copolymers. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] European Patent Application No. 21178566.2 [Patent Document 2] European Patent Application No. 21178547.2 Summary of the Invention [Means for solving the problem]

[0007] The present invention relates to a composition obtained by blending component (A) and component (B), said component (A) being 50-95% by weight, preferably 55-90% by weight, more preferably 60-88% by weight of a mixed plastic polypropylene / polyethylene blend; said component (B) being from 5 to 50 wt.%, preferably from 10 to 45 wt.%, more preferably from 12 to 40 wt.%, of a heterophasic propylene copolymer, all percentages being based on the total composition; The mixed plastic polypropylene / polyethylene blend (A) is a crystalline fraction (CF) content determined according to a CRYSTEX QC analysis in the range of 85.0-96.0 wt.%, preferably in the range of 86.5-95.5 wt.%, a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 4.0-15.0 wt.%, preferably in the range of 4.5-13.5 wt.%; having The crystalline fraction (CF) is quantitatively in the range of 11.0 to 55.0% by weight, preferably in the range of 20.0 to 49.5% by weight. 13 having an ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; the soluble fraction (SF) has an intrinsic viscosity (iV(SF)) in the range of 0.9 to 2.1 dl / g, preferably in the range of 1.0 to 2.0 dl / g, The heterophasic propylene copolymer (B) comprises a matrix phase and an elastomeric phase dispersed therein, A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min; a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0-35.0 wt.%, preferably in the range of 11.0-32.5 wt.%, more preferably in the range of 12.0-30.0 wt.%, an intrinsic viscosity (iV(SF)) of said soluble fraction measured in decalin at 135° C. according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; having The composition comprises: ·Has a melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of at least 9.0 g / 10 min, preferably 9.5 to 100 g / 10 min, more preferably 10.0 to 75 g / 10 min.

[0008] The present invention also relates to a process for the preparation of the above or below mentioned composition, said process comprising the steps of: a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in the presence of the single-site catalyst system in the second polymerization reactor to produce a second propylene polymer fraction; d) transferring a polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction, and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in the presence of a single-site catalyst system in said third polymerization reactor to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining said heterophasic propylene copolymer (B) comprising said first propylene polymer fraction, said second propylene polymer fraction and said third propylene-ethylene copolymer fraction; h) blending 5-50 wt.%, preferably 10-45 wt.%, more preferably 12-40 wt.% of said heterophasic propylene copolymer (B) with 50-95 wt.%, preferably 55-90 wt.%, more preferably 60-88 wt.% of said mixed plastic polypropylene / polyethylene blend (A); Includes.

[0009] The present invention further relates to an article comprising the above or below described composition.

[0010] Additionally, the present invention relates to the use of the above or below described composition in the manufacture of an article.

[0011] Finally, the present invention relates to the use of a heterophasic propylene copolymer in a composition as described above or below, said heterophasic propylene copolymer being A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min; a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0-35.0 wt.%, preferably in the range of 11.0-32.5 wt.%, more preferably in the range of 12.0-30.0 wt.%, an intrinsic viscosity (iV(SF)) of said soluble fraction measured in decalin at 135° C. according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; said use increases the melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) and flexural modulus, and reduces the VOC and FOG content of said composition.

[0012] definition All technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs, unless otherwise defined. Although any methods and materials similar or equivalent to those described herein can be used in the practice of testing the present invention, the preferred materials and methods are described herein. In describing and claiming the present invention, the following terms are used according to the definitions set forth below. Unless otherwise clearly indicated, the use of terms such as "a", "an" refers to one or more.

[0013] Mixed plastics are defined as the presence of small amounts of compounds not normally found in virgin polypropylene compositions, such as polystyrene, polyamides, polyesters, wood, paper, limonene, aldehydes, ketones, fatty acids, metals, and / or long-term degradation products of stabilizers. Virgin polypropylene blends refer to blends that originate directly from the manufacturing process without intermediate uses. As a matter of definition, a "mixed plastic" can be equated with detectable amounts of polystyrene and / or polyamide-6 and / or limonene and / or fatty acids. Thereby, mixed plastics, in contrast to virgin polymers, can come from both post-consumer and post-industrial sources. Post-consumer waste refers to objects that have completed at least their first use cycle (or life cycle), i.e. that have already fulfilled their initial purpose. In contrast, post-industrial waste refers to manufacturing or processing scrap that usually does not reach the consumer.

[0014] It will be appreciated by those skilled in the art that a soluble fraction (SF) having an intrinsic viscosity (iV(SF)) in the range of 0.9-2.1 dl / g as determined by CRYSTEX QC analysis is typically found in materials from recycle streams. In a preferred embodiment of the invention, the soluble fraction (SF) has an intrinsic viscosity (iV(SF)) in the range of 1.0-2.0 dl / g as determined by CRYSTEX QC analysis.

[0015] A polymer blend is a mixture of two or more polymer components. In general, the blend can be prepared by mixing two or more polymer components. A suitable mixing procedure known in the art is post-polymerization blending. The post-polymerization blend can be a dry blend of the polymer components, such as polymer powder and / or polymer pellets after compounding, or a melt blend by melt mixing the polymer components.

[0016] Propylene homopolymer is a polymer consisting essentially of propylene monomer units. Due to impurities, especially in commercial polymerization processes, propylene homopolymer may contain up to 0.1 mol% of comonomer units, preferably up to 0.05 mol% of comonomer units, and most preferably up to 0.01 mol% of comonomer units.

[0017] "Polypropylene-polyethylene blend" refers to a composition containing both polypropylene and polyethylene, including polypropylene and polyethylene copolymers. Since it is not possible to directly determine the polypropylene and polyethylene content, the weight ratio of polypropylene to polyethylene ranging from 20 / 80 to 80 / 20 indicates the equivalence ratio determined from calibration with iPP and HDPE and determination by IR spectroscopy.

[0018] By polypropylene is meant a polymer composed of more than 50 mol % units derived from propylene. By polyethylene is meant a polymer composed of more than 50 mol % units derived from ethylene.

[0019] The presence of heterogeneous properties can be easily determined by glass transition numbers, such as the glass transition point in dynamic mechanical analysis (DMA), and / or high resolution microscopy, such as scanning electron microscopy (SEM), transmission electron microscopy (TEM) or atomic force microscopy (AFM).

[0020] The term "XCS" refers to the cold xylene soluble fraction (XCS, wt%) determined at 25°C according to ISO 16152. The term "XCI" refers to the cold xylene insoluble fraction (XCI, wt%) determined at 25°C according to ISO 16152.

[0021] A reactor blend is a blend resulting from production in two or more reactors connected in series, or in a reactor having two or more reaction zones. Alternatively, a reactor blend may be obtained by blending in solution. A reactor blend is in contrast to a compound produced by melt extrusion.

[0022] Unless otherwise indicated, "%" refers to % by weight. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] composition In a first aspect, the present invention relates to a composition obtained by blending component (A) with component (B), Component (A) is 50-95% by weight, preferably 55-90% by weight, more preferably 60-88% by weight of a mixed plastic polypropylene / polyethylene blend; Component (B) is from 5 to 50 wt.%, preferably from 10 to 45 wt.%, more preferably from 12 to 40 wt.%, of a heterophasic propylene copolymer, where all percentages are based on the total composition; The mixed plastic polypropylene / polyethylene blend (A) is a crystalline fraction (CF) content determined according to CRYSTEX QC analysis in the range of 85.0-96.0 wt.%, preferably in the range of 86.5-95.5 wt.%, a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 4.0-15.0 wt.%, preferably in the range of 4.5-13.5 wt.%; having The crystalline fraction (CF) is a quantitative fraction in the range of 11.0 to 55.0% by weight, preferably in the range of 20.0 to 49.5% by weight. 13having an ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; the soluble fraction (SF) has an intrinsic viscosity (iV(SF)) in the range of 0.9 to 2.1 dl / g, preferably in the range of 1.0 to 2.0 dl / g, The heterophasic propylene copolymer (B) comprises a matrix phase and an elastomeric phase dispersed therein, A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min; a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0-35.0 wt.%, preferably in the range of 11.0-32.5 wt.%, more preferably in the range of 12.0-30.0 wt.%, an intrinsic viscosity (iV(SF)) of the soluble fraction measured in decalin at 135°C according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; having The composition is It has a melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of at least 9.0 g / 10 min, preferably 9.5 to 100 g / 10 min, and more preferably 10.0 to 75 g / 10 min.

[0024] The compositions of the present invention have one or more of the following properties:

[0025] The composition has a melt flow rate MFR2 (230° C., 2.16 kg, ISO 1133) of at least 9.0 g / 10 min, preferably from 9.5 to 100 g / 10 min, more preferably from 10.0 to 75 g / 10 min.

[0026] The compositions according to the present invention preferably exhibit a good balance of properties with respect to mechanical properties such as flexural modulus, impact properties, flow properties as indicated by the melt flow rates mentioned above, and especially with respect to VOC and FOG content and minor amounts of impurities as indicated by fogging.

[0027] The compositions were prepared in injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2. 3 It is preferable that the material has a flexural modulus (FM) determined in accordance with ISO 178 for a material having a bending modulus (FM) in the range of 800 to 1300 MPa, preferably in the range of 850 to 1200 MPa, and more preferably in the range of 865 to 1050 MPa.

[0028] The compositions were also tested on injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2. 3 ) determined according to ISO179 / eA, 5.0-25.0 kJ / m 2 in the range of 5.5 to 20.0 kJ / m 2 It is preferred that the Charpy notched impact strength at 23° C. (CNIS, 23° C.) is in the range of

[0029] The composition preferably has a Charpy notched impact strength at 23° C. that satisfies the following inequality with respect to the melt flow rate MFR2 (230° C., 2.16 kg, ISO 1133): CNIS, 23℃ [kJ / m 2 ]>7.8[kJ / m 2 ]-0.17[kJ / m 2 / g / 10min]·MFR2[g / 10min] During the ceremony, CNIS, 23°C, injection molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO1873-2 3 ) is the Charpy notched impact strength of the composition at 23°C, determined in accordance with ISO 179 / eA; MFR2 is the melt flow rate MFR2 of the composition (230°C, 2.16 kg, ISO 1133).

[0030] Furthermore, the compositions were subjected to injection molding test specimens (80 x 10 x 4 mm) produced according to EN ISO 1873-2. 3 ) determined according to ISO179 / eA, 1.7-5.0 kJ / m 2 in the range of 1.9 to 4.0 kJ / m 2 It is preferred that the Charpy notched impact strength at -20°C (CNIS, -20°C) is in the range of

[0031] Additionally, the composition comprises: a volatile organic compounds (VOC) content, determined according to VDA 278, of less than or equal to 100 μg / g, preferably in the range from 5 to 95 μg / g, more preferably in the range from 10 to 90 μg / g, and / or a semi-volatile organic compounds (FOG) content, determined according to VDA 278, of less than or equal to 1100 μg / g, preferably in the range from 50 to 1050 μg / g, more preferably in the range from 80 to 1000 μg / g, and / or Fogging amount less than or equal to 5.0 mg, preferably in the range of 0.5-4.5 mg, determined according to DIN 75201, method B, for a compression-molded plaque of 2 mm thickness It is preferred that the composition has one or more, preferably all, of the following characteristics:

[0032] The composition of the present invention must contain the above or below-mentioned component (A) and component (B) in the amounts correspondingly described.

[0033] The composition may optionally include an additional polymer component. When a further polymeric component is present, the amount of that polymeric component in the composition is usually not more than 5% by weight, preferably not more than 2% by weight, based on the total weight of the composition. If a further polymer component is present, its lower limit is usually at least 0.1% by weight, preferably 0.2% by weight, based on the total weight of the composition. However, it is preferred that the composition does not comprise any further polymeric components, ie the amount of further polymeric components in the composition is 0 wt%.

[0034] In one embodiment, the composition is preferably free of inorganic fillers such as talc, mica, wollastonite, or glass fibers. In another embodiment, the composition preferably contains an inorganic filler, such as talc, mica, wollastonite or glass fiber, preferably in an amount of 5 to 40% by weight, based on the total weight of the composition.

[0035] Mixed Plastic Polypropylene / Polyethylene Blend (A) The mixed plastic polypropylene / polyethylene blend (A) is well characterized by CRYSTEX QC analysis, which provides the crystalline fraction (CF) and soluble fraction (SF) that can be quantified and analyzed for monomer and comonomer content, and intrinsic viscosity (iV). The mixed plastic polypropylene / polyethylene blend (A) was analyzed by CRYSTEX QC. a crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 85.0 to 96.0% by weight, preferably in the range of 86.5 to 95.5% by weight, and Soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 4.0-15.0 wt.%, preferably in the range of 4.5-13.5 wt.%. This shows the following characteristics.

[0036] The crystalline fraction (CF) is Quantitative in the range of 11.0 to 55.0% by weight, preferably in the range of 20.0 to 49.5% by weight 13 ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, and / or Intrinsic viscosity (iV(CF)) measured in decalin at 135 °C according to DIN ISO 1628 / 1, preferably in the range of 1.0 to less than 2.6 dl / g, more preferably in the range of 1.2 to 2.5 dl / g It has one or more, preferably all, of the following characteristics:

[0037] The soluble fraction (SF) is Quantitative, preferably in the range of 20.0 to 55.0% by weight, preferably in the range of 22.0 to 50.0% by weight 13 the ethylene content (C2(SF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, and / or Intrinsic viscosity (iV(SF)) measured in decalin at 135 °C according to DIN ISO 1628 / 1 in the range of 0.9 to 2.1 dl / g, preferably in the range of 1.0 to 2.0 dl / g It has one or more, preferably all, of the following characteristics:

[0038] Preferably, the mixed plastic polypropylene / polyethylene blend (A) comprises polypropylene and polyethylene in a weight ratio of 20 / 80 to 80 / 20, preferably 25 / 75 to 75 / 25.

[0039] The mixed plastic polypropylene / polyethylene blend (A) preferably contains propylene-derived units in an amount of 50.0 to 95.0% by weight, more preferably 51.5 to 90.0% by weight, and even more preferably 53.0 to 75.0% by weight.

[0040] The mixed plastic polypropylene / polyethylene blend (A) preferably contains units derived from ethylene in an amount of 5.0 to 50.0% by weight, more preferably 10.0 to 48.5% by weight, and even more preferably 25.0 to 47.0% by weight.

[0041] In addition, the mixed plastic polypropylene / polyethylene blend (A) is A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 5.0 to 50 g / 10 min, preferably 5.2 to 45 g / 10 min, more preferably 5.4 to 40 g / 10 min, and / or Limonene content between 0.1 and 50 ppm, determined using solid phase microextraction (HS-SPME-GC-MS), and / or a tensile modulus of 800 to 1400 MPa, preferably 850 to 1200 MPa, and / or 4.0~8.5kJ / m 2 , preferably 5.0 to 8.0 kJ / m 2 Charpy notched impact strength at 23°C (CNIS, 23°C), and / or 1.0~4.5kJ / m 2 , preferably 1.5 to 4.0 kJ / m 2 Charpy notched impact strength at -20℃ (CNIS, -20℃) It is preferred that the composition has one or more, preferably all, of the following characteristics:

[0042] The mixed plastic polypropylene / polyethylene blend (A) according to the invention is preferably in the form of pellets, which reduces the amount of volatile substances.

[0043] Heterophasic propylene copolymer (B) The heterophasic polypropylene copolymer (B) comprises a matrix phase and an elastomeric phase dispersed therein.

[0044] The heterophasic propylene copolymer (B) is A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min; a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0% to 35.0% by weight, preferably in the range of 11.0 to 32.5% by weight, more preferably in the range of 12.0 to 30.0% by weight, and an intrinsic viscosity of the soluble fraction (iV(SF)) measured in decalin at 135°C according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; It has the following characteristics:

[0045] The heterophasic propylene copolymer (B) is a crystalline fraction (CF) determined according to CRYSTEX QC analysis in an amount ranging from 65.0 to 90.0% by weight, preferably ranging from 67.5 to 89.0% by weight, more preferably ranging from 70.0 to 88.0% by weight, and / or an intrinsic viscosity of the crystalline fraction (iV(CF)) of less than or equal to 1.2 dl / g, preferably in the range of 0.4 to 1.1 dl / g, and / or ·Quantitative 13 an ethylene content of the crystalline fraction (C2(CF)) of less than or equal to 1.0% by weight, preferably in the range of 0 to 0.9% by weight, based on the total weight of the crystalline fraction (CF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; and / or ·Quantitative 13 an ethylene content of the soluble fraction (C2(SF)) in the range of 14.0 to 29.0% by weight, preferably in the range of 17.0 to 26.0% by weight, more preferably in the range of 19.0 to 24.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; and / or Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO1873-2 3 ) in the range of 800 to 1500 MPa, preferably in the range of 850 to 1450 MPa, determined according to ISO 178; and / or ·Quantitative 13 a total ethylene content in the range of 2.0 to 5.5% by weight, preferably in the range of 2.5 to 5.0% by weight, based on the total weight of the heterophasic propylene copolymer (B), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, and / or a melting temperature in the range of 150 to 162°C, preferably in the range of 152 to 160°C, determined by DSC according to ISO 3146 (Part 3, Method C2), and / or a crystallization temperature in the range of 110 to 130°C, preferably in the range of 115 to 125°C, determined by DSC according to ISO 3146 (Part 3, Method C2), and / or Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO1873-2 3) determined according to ISO179 / eA, 2.5 to 15.0 kJ / m 2 in the range of 3.0 to 12.0 kJ / m 2 Charpy notched impact strength at 23°C in the range a volatile organic compounds (VOC) content, determined according to VDA 278, of less than or equal to 50 μg / g, preferably less than or equal to 40 μg / g, more preferably less than or equal to 35 μg / g, and usually at least 2 μg / g, preferably at least 4 μg / g, and / or A FOG content, determined according to VDA 278, of less than or equal to 300 μg / g, preferably less than or equal to 250 μg / g, more preferably less than or equal to 225 μg / g, and usually at least 20 μg / g, preferably at least 40 μg / g It is preferred that the composition has one or more, preferably all, of the following characteristics:

[0046] The heterophasic propylene copolymer (B) preferably has a flexural modulus (FM) with respect to the amount of soluble fraction (SF) that satisfies the following inequality: FM[MPa]>1550[MPa]-33.4[MPa / weight%] · Quantity (SF)[weight%] Preferably, FM[MPa]>1575[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%], More preferably, FM[MPa]>1600[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%], Most preferably, FM[MPa]>1625[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%], During the ceremony, F [MPa] is the flexural modulus of the heterophasic propylene copolymer (B), in MPa; The amount (SF) [wt. %] is the amount of soluble fraction (SF) in the heterophasic propylene copolymer (B), the unit being % by weight.

[0047] The polypropylene composition preferably has a Charpy notched impact strength at 23° C. (CNIS, 23° C.) that satisfies the following inequality with respect to the melt flow rate (MFR2): CNIS, 23℃ [kg / m 2 ]>10.0[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min] Preferably, CNIS, 23℃ [kg / m 2 ]>10.5[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min], More preferably, CNIS, 23℃ [kg / m 2 ]>11.0[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min], Most preferably, CNIS, 23℃ [kg / m 2 ]>11.5[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min].

[0048] The heterophasic propylene copolymer (B) preferably consists of propylene and ethylene units. Although not measured, it is preferred that the content of units derived from propylene (C3) in the soluble fraction (SF) and the content of units derived from ethylene (C2) in the soluble fraction (SF) sum to 100% by weight.

[0049] The content of units derived from propylene (C3) in the soluble fraction (SF) is preferably 71.0 to 86.0% by weight, more preferably 74.0 to 83.0% by weight, and even more preferably 76.0 to 81.0% by weight. Although not measured, it is preferred that the content of units derived from propylene (C3) in the crystalline fraction (CF) and the content of units derived from ethylene (C2) in the crystalline fraction (CF) sum to 100% by weight. The content of units derived from propylene (C3) in the crystalline fraction (CF) is preferably at least 99.0% by weight, more preferably 99.1 to 100% by weight. The total content of units derived from propylene (C3) in the heterophasic propylene copolymer (B) is preferably from 94.5 to 98.0% by weight, more preferably from 95.0 to 97.5% by weight.

[0050] Such heterophasic propylene copolymers are preferably prepared according to the above or below described process of the present invention in the presence of a single-site catalyst system.

[0051] Additives Additives are conventionally used in the compositions according to the invention. Preferably, the additives are selected from one or more of antioxidants, UV stabilizers, slip agents, nucleating agents, pigments, lubricants, masterbatch polymers and / or anti-fog agents. The additives are usually present in the composition in an amount of 0.01 to 5.0% by weight, preferably 0.05 to 3.5% by weight, based on the total composition.

[0052] process In a further aspect, the present invention relates to a process for the preparation of any of the above or below described compositions, said process comprising the steps of: a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in a second polymerization reactor in the presence of the single-site catalyst system to produce a second propylene polymer fraction; d) transferring the polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in a third polymerization reactor in the presence of a single-site catalyst system to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining a heterophasic propylene copolymer (B) comprising a first propylene polymer fraction, a second propylene polymer fraction and a third propylene-ethylene copolymer fraction; h) blending 5-50 wt.%, preferably 10-45 wt.%, more preferably 12-40 wt.% of the heterophasic propylene copolymer (B) with 50-95 wt.%, preferably 55-90 wt.%, more preferably 60-88 wt.% of the mixed plastic polypropylene / polyethylene blend (A); Includes.

[0053] The first polymerization reactor is preferably a slurry phase reactor, such as a loop reactor.

[0054] The operating temperature in the first polymerization reactor, preferably the loop reactor, is preferably in the range of 62 to 85°C, more preferably in the range of 65 to 82°C, and even more preferably in the range of 67 to 80°C.

[0055] Typically, the pressure in the first polymerization reactor, preferably the loop reactor, is in the range from 20 to 80 bar, preferably from 30 to 70 bar, for example from 35 to 65 bar.

[0056] It is preferred to produce a propylene homopolymer in a first polymerization reactor, preferably a loop reactor, and therefore the first propylene polymer fraction is preferably a propylene homopolymer fraction.

[0057] Preferably, hydrogen is added into the first polymerization reactor to control the molecular weight, ie the melt flow rate MFR2. Preferably, the hydrogen to propylene ratio (H2 / C3 ratio) in the first polypropylene reactor, preferably the loop reactor, is in the range of 0.70 to 2.5 mol / kmol, more preferably 0.75 to 2.0 mol / kmol.

[0058] Due to the strong hydrogen response of the catalyst and the relatively large amount of hydrogen, the melt flow rate of the first propylene polymer fraction is very high. The first propylene polymer fraction preferably has a melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) in the range of 1000 to 15000 g / 10 min, preferably in the range of 1100 to 13500 g / 10 min, more preferably in the range of 1250 to 11500 g / 10 min.

[0059] The second polymerization reactor is preferably a first gas phase reactor, such as a first fluidized bed gas phase reactor.

[0060] The operating temperature in the second polymerization reactor, preferably the first gas phase reactor, is preferably in the range of 75-95°C, more preferably in the range of 78-92°C.

[0061] Typically, the pressure in the second polymerization reactor, preferably the first gas phase reactor, is in the range of from 5 to 50 bar, preferably from 15 to 40 bar.

[0062] It is preferred to produce a propylene homopolymer in a second polymerization reactor, preferably in the first gas phase reactor, and therefore the second propylene polymer fraction is preferably a propylene homopolymer fraction.

[0063] Preferably, hydrogen is added into the second polymerization reactor to control the molecular weight, ie the melt flow rate MFR2. Preferably, the hydrogen to propylene ratio (H2 / C3 ratio) in the second polypropylene reactor, preferably the first gas phase reactor, is in the range of 2.0 to 6.5 mol / kmol, more preferably in the range of 2.8 to 5.5 mol / kmol.

[0064] Due to the strong hydrogen response of the catalyst and the relatively large amount of hydrogen, the melt flow rate of the combined first and second propylene polymer fractions is very high. The combined first and second propylene polymer fractions preferably have a melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) of at least 1000 g / 10 min, preferably in the range of 1200 to 9000 g / 10 min, more preferably in the range of 1500 to 8000 g / 10 min.

[0065] It is further preferred that the combined first and second propylene polymer fractions have a xylene cold soluble (XCS) fraction at 25° C. in an amount of less than or equal to 2.0 wt %, preferably in the range of 0.1 to 1.5 wt %, based on the total weight of the combined first and second propylene polymer fractions.

[0066] The third polymerization reactor is preferably a second gas phase reactor, such as a second fluidized bed gas phase reactor.

[0067] The operating temperature in the third polymerization reactor, preferably the second gas phase reactor, is preferably in the range of 65 to 85° C., more preferably in the range of 68 to 82° C. Typically, the operating temperature in the third polymerization reactor is lower than the operating temperature in the second polymerization reactor.

[0068] Typically, the pressure in the third polymerization reactor, preferably the second gas phase reactor, is in the range of from 5 to 50 bar, preferably from 15 to 40 bar.

[0069] It is preferred to produce a propylene ethylene copolymer in a third polymerization reactor, preferably a second gas phase reactor, and the third propylene polymer fraction is therefore a propylene ethylene copolymer fraction.

[0070] The ethylene to propylene ratio (C2 / C3 ratio) in the third polymerization reactor, preferably the second gas phase reactor, is in the range of 700 to 1000 mol / kmol, more preferably in the range of 800 to 950 mol / kmol. Due to its high ethylene to propylene ratio (C2 / C3 ratio), the third propylene copolymer fraction is preferably an elastomeric block copolymer having a propylene-rich portion and an ethylene-rich portion.

[0071] Preferably, hydrogen is added into the second polymerization reactor to control the molecular weight, ie the melt flow rate MFR2.

[0072] Preferably, the hydrogen to ethylene ratio (H2 / C2 ratio) in the third polymerization reactor, preferably the second gas phase reactor, is in the range of 0.5 to 3.5 mol / kmol, more preferably 1.0 to 2.5 mol / kmol.

[0073] The first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined preferably have a melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) of at least 150 g / 10 min, preferably in the range of 165 to 500 g / 10 min, more preferably in the range of 175 to 400 g / 10 min.

[0074] It is further preferred that the combined first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction have a xylene cold soluble (XCS) fraction at 25° C. in an amount ranging from 8.0 to 32.0 wt.%, preferably ranging from 9.0 to 30.0 wt.%, more preferably ranging from 10.0 to 28.0 wt.%, based on the total weight of the heterophasic propylene copolymer (B). The XCS fraction is an intrinsic viscosity (iV(XCS)) of at least 2.2 dl / g, preferably in the range of 2.3 to 4.6 dl / g, more preferably in the range of 2.5 to 4.4 dl / g, and ·Quantitative 13 An ethylene content (C2(XCS)) in the range of 15.0-30.0% by weight, preferably in the range of 18.0-27.0% by weight, more preferably in the range of 20.0-25.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy. It is preferable that the material has the following characteristics.

[0075] Also, the combined first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction are quantitatively 13 It is preferred to have a total comonomer content, preferably an ethylene (C2) content, in the range of 2.0 to 5.5 wt.%, preferably in the range of 2.5 to 5.0 wt.%, based on the total weight of the polypropylene composition, determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy.

[0076] Preferably, the combined first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction form a heterophasic propylene copolymer.

[0077] The preparation of the first, second and third propylene polymer fractions may comprise, in addition to the (main) polymerization stage in at least three polymerizations, a prepolymerization step prior thereto in a preliminary (pre)polymerization reactor upstream of the first polymerization reactor.

[0078] In the prepolymerization reactor, polypropylene is produced. Prepolymerization is preferably carried out in the presence of a single-site polymerization catalyst system. According to this embodiment, the single-site polymerization catalyst system is introduced in the prepolymerization step. However, this does not exclude the option of adding further cocatalysts in the polymerization process, for example in a later stage, for example in the first reactor. In one embodiment, when applying prepolymerization, all components of the single-site catalyst are added only in the prepolymerization reactor.

[0079] The prepolymerization reaction is typically carried out at a temperature of 0 to 60°C, preferably 15 to 50°C, and more preferably 20 to 45°C.

[0080] The pressure in the prepolymerization reactor is not particularly limited, but must be high enough to maintain the reaction mixture in the liquid phase. Thus, the pressure may be 20 to 100 bar, for example 30 to 70 bar.

[0081] In a preferred embodiment, the prepolymerization is carried out as a bulk slurry polymerization in liquid propylene, ie, the liquid phase comprises mainly propylene, optionally with inert components dissolved therein.

[0082] It is also possible to add other ingredients to the prepolymerization stage. Thus, hydrogen may be added to the prepolymerization stage to control the molecular weight of the polypropylene, as is well known in the art. Antistatic agents may also be used to prevent particles from adhering to each other and to the walls of the reactor.

[0083] The precise control of prepolymerization conditions and reaction parameters is within the skill of one of ordinary skill in the art.

[0084] The above-specified process conditions in the prepolymerization preferably result in a mixture of the single-site catalyst system and the polypropylene produced in the prepolymerization reactor. Preferably, the single-site catalyst system is (finely) dispersed in the polypropylene. In other words, the single-site catalyst particles introduced in the prepolymerization reactor are divided into small fragments that are homogeneously distributed in the growing polypropylene. The size of the introduced single-site catalyst particles and the size of the resulting fragments are not of essential relevance to the present invention and are within the knowledge of the person skilled in the art.

[0085] As mentioned above, when prepolymerization is used, following said prepolymerization, the mixture of single-site catalyst and polypropylene produced in the prepolymerization reactor is transferred to the first polymerization reactor. Typically, the total amount of polypropylene produced in the prepolymerization reactor in the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction is fairly small, typically not more than 5.0 wt%, more preferably not more than 4.0 wt%, even more preferably in the range of 0.5 to 4.0 wt%, for example in the range of 1.0 to 3.0 wt%.

[0086] When prepolymerization is not used, propylene and other components, such as the single-site catalyst system, are introduced directly into the first polymerization reactor.

[0087] The residence times of the polymerization mixture in the different polymerization stages are adjusted to obtain respective amounts of the first polymer fraction, the second polymer fraction and the third polymer fraction within the combined first polymer fraction, the second polymer fraction and the third polymer fraction.

[0088] Preferably, the first propylene polymer fraction is present in an amount of 40 to 60 wt%, more preferably 45 to 55 wt%, based on the total weight of the first, second and third propylene polymer fractions combined. If a prepolymerization reactor is present, the amount of polypropylene produced therein is generally added to the amount of the first propylene polymer fraction.

[0089] Preferably, the second propylene polymer fraction is present in an amount of from 25 to 45% by weight, more preferably from 30 to 40% by weight, based on the total weight of the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined.

[0090] Preferably, the third propylene polymer fraction is present in an amount of from 10 to 30% by weight, more preferably from 15 to 25% by weight, based on the total weight of the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined.

[0091] Catalyst system The single-site catalyst system according to the present invention may be any supported metallocene catalyst system suitable for the production of isotactic polypropylene.

[0092] The single-site catalyst system preferably comprises a metallocene complex, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst, and a silica support.

[0093] In particular, single-site catalyst systems (i) a metallocene complex of the following general formula (I): [ka] (In the formula, each X is independently a sigma donor ligand; L is a divalent bridge selected from -R'2C-, -R'2C-CR'2-, -R'2Si-, -R'2Si-SiR'2-, -R'2Ge-, where each R' is independently a hydrogen atom or a C1-C6 heteroatom optionally containing one or more heteroatoms or fluorine atoms from Groups 14-16 of the Periodic Table of the Elements. 20 is a hydrocarbyl group, or optionally two R′ groups can be taken together to form a ring; Each R 1 may be independently the same or different, and are hydrogen, a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group, and optionally two adjacent R 1 The groups may be part of a ring that includes the phenyl carbon to which they are attached; Each R 2 may be independently the same or different, CH-R 8 group, where R 8 is H or linear or branched C 1~6 Alkyl group, C 3~8 Cycloalkyl groups, C 6~10 is an aryl group, R 3 is a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C6-C 20 is an aryl group, R 4 is C(R 9 ) groups, where R 9 is a linear or branched C1 to C6 alkyl group, R 5 is hydrogen or an aliphatic C1-C optionally containing one or more heteroatoms from groups 14-16 of the periodic table 20 is a hydrocarbyl group, R 6 is hydrogen or an aliphatic C1-C optionally containing one or more heteroatoms from groups 14-16 of the periodic table 20 is a hydrocarbyl group, or R 5 and R 6 Together, n (n is 0 to 4) R 10 can form a 5-membered saturated carbocyclic ring optionally substituted with a group, Each R 10 are the same or different, C1 to C 20 Hydrocarbyl groups or C1-C groups optionally containing one or more heteroatoms belonging to groups 14-16 of the Periodic Table 20 may be a hydrocarbyl group, R 7 is H, or a linear or branched C1-C6 alkyl group, or one to three R 11 an aryl group or heteroaryl group having 6 to 20 carbon atoms optionally substituted with a group; Each R 11 may be independently the same or different, and are hydrogen, a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group. (ii) a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst; (iii) a silica support; It is preferred that the compound contains

[0094] The term "sigma donor ligand" is well understood by those of skill in the art, i.e., refers to a group that bonds to a metal via a sigma bond. Thus, the anionic ligand "X" may be independently halogen or selected from the group consisting of R', OR', SiR'3, OSiR'3, OSO2CF3, OCOR', SR', NR'2, and PR'2 groups, where R' is independently hydrogen, linear or branched, cyclic or acyclic, C1-C 20 Alkyl, C2-C 20 Alkenyl, C2-C 20 Alkynyl, C3-C 12 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Aryl alkyl, C7-C 20 Alkylaryl, C8-C 20 Arylalkenyl, where the R' group may optionally contain one or more heteroatoms belonging to groups 14 to 16. In a preferred embodiment, the anionic ligands "X" are the same and are halogens such as Cl, or methyl, or benzyl.

[0095] Preferred monovalent anionic ligands are the halogens, especially chlorine (Cl).

[0096] Preferred metallocene complexes include: rac-Dimethylsilanediylbis[2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-(4'-tert-butylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-phenyl-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(3',5'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-Dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-5-di-tert-butyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride.

[0097] Particularly preferred is rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride.

[0098] The ligands required to form the complexes of the present invention, and thus the catalytic system, can be synthesized by any process, and an organic chemist skilled in the art will be able to devise various synthetic protocols to produce the required ligand materials. For example, WO 2007 / 116034 discloses the necessary chemicals. Synthetic protocols can also be found generally in WO 2002 / 002576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790 and WO 2018 / 122134. In particular, reference is made to WO 2019 / 179959, in which the most preferred catalysts of the present invention are described.

[0099] Cocatalyst To form the active catalytic species, it is usually necessary to use a cocatalyst, as is well known in the art.

[0100] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with the metallocene catalyst complex defined above.

[0101] The aluminoxane cocatalyst may be of the formula (II):

[0102] [ka] In the formula, n is usually 6 to 20, and R has the following meaning.

[0103] Aluminoxanes are produced by partial hydrolysis of organoaluminum compounds, for example of the formula AlR3, AlR2Y, Al2R3Y3, where R is, for example, C1-C 10 Alkyl, preferably C1 to C5 alkyl, or C3 to C 10 Cycloalkyl, C7-C 12 Y may be arylalkyl or alkylaryl, and / or phenyl or naphthyl, and Y is hydrogen, halogen, preferably chlorine or bromine, or C1-C 10 It may be alkoxy, preferably methoxy or ethoxy.The oxygen-containing aluminoxanes obtained are generally not pure compounds but are mixtures of oligomers of formula (II).

[0104] A preferred aluminoxane is methylaluminoxane (MAO). Because the aluminoxanes used as cocatalysts in the present invention are not pure compounds due to their mode of preparation, the molarity of the aluminoxane solutions below is based on their aluminum content.

[0105] According to the present invention, a boron-containing cocatalyst can be used in place of the aluminoxane cocatalyst, or the aluminoxane cocatalyst can be used in combination with the boron-containing cocatalyst.

[0106] Those skilled in the art will appreciate that when using boron-based cocatalysts, it is common to pre-alkylate the complex by reacting it with an aluminum alkyl compound such as TIBA. This procedure is well known and any suitable aluminum alkyl can be used, such as Al(C1-C6 alkyl)3. Preferred aluminum alkyl compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum and triisooctylaluminum.

[0107] Alternatively, when a borate cocatalyst is used, the metallocene catalyst complex may be an alkylated version thereof, ie, for example, a dimethyl or dibenzyl metallocene catalyst complex may be used.

[0108] Boron-based cocatalysts of interest include those of formula (III): BY3(III) In the formula, Y is the same or different and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkylaryl, an arylalkyl, a haloalkyl or a haloaryl, each having 1 to 10 carbon atoms in the alkyl radical and 6 to 20 carbon atoms in the aryl radical, or a fluorine, chlorine, bromine or iodine. Preferred choices are trifluoroborane, triphenylborane, tris(4-fluorophenyl)borane, tris(3,5-difluorophenyl)borane, tris(4-fluoromethylphenyl)borane, tris(2,4,6-trifluorophenyl)borane, tris(pentafluorophenyl)borane, tris(tolyl)borane, tris(3,5-dimethylphenyl)borane, tris(3,5-difluorophenyl)borane and / or tris(3,4,5-trifluorophenyl)borane.

[0109] Particularly preferred is tris(pentafluorophenyl)borane.

[0110] However, it is preferred to use borate, i.e. compounds containing borate 3+ ions. Such ionic cocatalysts preferably contain non-coordinating anions, such as tetrakis(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amine or aniline derivatives, such as methylammonium, anilinium, dimethylammonium, diethylammonium, N-methylanilinium, diphenylammonium, N,N-dimethylanilinium, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridinium, p-bromo-N,N-dimethylanilinium or p-nitro-N,N-dimethylanilinium.

[0111] Surprisingly, it has been discovered that certain boron cocatalysts are particularly preferred. Thus, the preferred borates for use in the present invention contain a trityl ion. Thus, the use of N,N-dimethylammonium-tetrakispentafluorophenylborate and Ph3CB(PhF5)4 and analogs thereof is particularly preferred.

[0112] Preferred cocatalysts are aluminoxanes, more preferably methylaluminoxane, combinations of aluminoxanes with Al-alkyls, boron or borate cocatalysts, and combinations of aluminoxanes with boron-based cocatalysts.

[0113] The catalyst system of the present invention is used in supported form. The particulate support material used is silica or a mixed oxide such as silica-alumina, in particular silica. The use of a silica support is preferred. The skilled person is aware of the procedures required to support metallocene catalysts.

[0114] In a preferred embodiment, the catalyst system corresponds to ICS3 of WO 2020 / 239598 A1.

[0115] The process further comprises a post-reactor treatment step of separating a polymer fraction from the polymerization mixture, preferably obtained from the last polymerization stage, and blending the heterophasic propylene copolymer (B) in an amount of 5-50 wt.%, preferably 10-45 wt.%, more preferably 12-40 wt.%, with the mixed plastic polypropylene blend (A) in an amount of 50-95 wt.%, preferably 55-90 wt.%, more preferably 60-88 wt.%, optionally in the presence of other components and / or additives, such as further polymeric components as described herein, to obtain a composition.

[0116] This blending step is preferably carried out by compounding the components in an extruder, such as a twin screw extruder, using typical compounding conditions. Post reactor processing steps are already well established in the art.

[0117] In one embodiment, the present invention relates to said composition obtainable, more preferably obtained, through the process described herein. All preferred embodiments and alternatives given for the compositions above and below apply mutatis mutandis to the process of the present invention.

[0118] Goods In another aspect, the present invention relates to an article comprising the above or below described composition. The article is preferably a molded article, such as an injection molded article, a fiber or mineral reinforced composite. The article may be an automotive article comprising the above or below described composition. The article may for example be a packaging article intended for food packaging, preferably a thin-walled packaging article, such as plastic cups, pails, small containers including lids, comprising a composition as described above or below.

[0119] In one embodiment, the article composition may include fibers, such as glass fibers or carbon fibers, and when fibers are present in the article composition, the amount of fibers ranges from 5 to 40 weight percent of the article composition.

[0120] In another embodiment, the composition of the article may include a mineral filler such as talc, mica, wollastonite, etc. When a mineral filler is present in the composition of the article, the amount of the filler is in the range of 5 to 40 weight percent of the composition of the article.

[0121] use In yet another aspect, the present invention relates to the use of the above or below described composition in the manufacture of an article.

[0122] The present invention also relates to the use of a heterophasic propylene copolymer in the above or below mentioned compositions, which heterophasic propylene copolymer comprises A melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min; a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0-35.0 wt.%, preferably in the range of 11.0-32.5 wt.%, more preferably in the range of 12.0-30.0 wt.%, an intrinsic viscosity (iV(SF)) of the soluble fraction, measured in decalin at 135°C according to DIN ISO 1628 / 1, of at least 2.0 dl / g, preferably in the range of 2.4 to 4.8 dl / g, more preferably in the range of 2.5 to 4.5 dl / g; The use of this increases the melt flow rate MFR2 (230°C, 2.16 kg, ISO1133) and flexural modulus, and reduces the VOC and FOG content of the composition.

[0123] All preferred embodiments and alternatives given above and below with regard to the heterophasic propylene copolymer (B), compositions and / or articles apply mutatis mutandis to the uses of the present invention. EXAMPLES

[0124] Experimental Department The following examples are included to demonstrate certain aspects and embodiments of the claimed invention. However, it should be understood by those of ordinary skill in the art that the following descriptions are merely illustrative and should not be construed as limiting the invention in any way.

[0125] 1. Determination method MFR2 (230°C) was measured at 230°C and a load of 2.16 kg in accordance with ISO1133.

[0126] CRYSTEX Determination of the crystalline and soluble fractions and their respective characteristics (IV and ethylene content) The crystalline fraction (CF) and soluble fraction (SF) of the polypropylene (PP) compositions, as well as the comonomer content and intrinsic viscosity of each fraction, were analyzed using a CRYSTEX instrument from Polymer Char (Valencia, Spain). Details of the technique and method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer and Markus Gahleitner (2020), Rapid characterization of high-impact ethylene-propylene copolymer composition by crystallization extraction separation: comparability to standard separation methods, International Journal of Polymer Analysis and Characterization, 25:8, 581-596). Crystalline and amorphous fractions are separated by temperature cycling: dissolution at 160° C., crystallization at 40° C. and redissolution in 1,2,4-trichlorobenzene at 160° C. Quantification of SF and CF as well as determination of ethylene content (C2) are performed by an integrated infrared detector (IR4) and determination of intrinsic viscosity (iV) is performed using an on-line two-capillary viscometer. The IR4 detector detects two distinct bands (CH stretching vibration (approximately 2960 cm)) that are useful for determining the concentration of ethylene-propylene copolymers and the ethylene content in ethylene-propylene copolymers. -1 ) and CH stretching vibration (2700-3000cm -1 The IR4 detector is a multi-wavelength detector that measures the IR absorbance of ethylene oxides of known ethylene content ( 13 The ethylene content of the copolymers is determined by C-NMR and is calibrated using a series of eight EP copolymers, each with various concentrations ranging from 2 to 13 mg / ml. For the various polymer concentrations expected during the Crystex analysis, the following calibration formula was applied to simultaneously encounter both the concentration and ethylene content characteristics: Conc=a+b×Abs(CH)+c×(Abs(CH)) 2 +d×Abs(CH3)+e×(Abs(CH3) 2 +f×Abs(CH)×Abs(CH3) (Formula 1) CH3 / 1000C=a+b×Abs(CH)+c×Abs(CH3)+d×(Abs(CH3) / Abs(CH))+e×(Abs(CH3) / Abs(CH)) 2 (Formula 2)

[0127] Constants a through e in Equation 1 and constants a through f in Equation 2 were determined using least squares regression analysis. CH3 / 1000C is converted to ethylene content (wt%) using the following relationship: Weight % (ethylene in EP copolymer) = 100-CH3 / 1000TC x 0.3 (Equation 3)

[0128] The amounts of soluble fraction (SF) and crystalline fraction (CF) are correlated by XS calibration with the "cold xylene soluble" (XCS) quantity and the individual cold xylene insoluble (XCI) fractions, determined according to standard gravimetric methods according to ISO 16152. The XS calibration is achieved by testing various EP copolymers with XS contents ranging from 2 to 31 wt. %. The determined XS calibration is linear. Weight%XS=1.01×Weight%SF (Formula 4) The intrinsic viscosity (iV) of the parent EP copolymer and its soluble and crystalline fractions are determined using an online two-capillary viscometer and correlated with the corresponding iV determined by standard methods in decalin according to ISO 1628-3. Calibration is achieved using various EP PP copolymers with iV = 2-4 dL / g. The determined calibration curve is linear. iV(dL / g)=a×Vsp / c (Formula 5)

[0129] The samples to be analyzed are weighed out at a concentration of 10 mg / ml to 20 mg / ml. To avoid the injection of possible gels and / or polymers that are not soluble in TCB at 160°C, such as PET and PA, the weighed samples are packed into a stainless steel mesh of MW 0.077 / D 0.05 mm.

[0130] After autofilling the vials with 1,2,4-TCB containing 250 mg / l 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the samples are dissolved at 160° C. with constant stirring at 400 rpm until completely dissolved, typically 60 min. The polymer solution is covered with a N2 atmosphere during dissolution to avoid sample degradation. A defined volume of sample solution is injected into a column filled with an inert carrier, where the sample undergoes crystallization and separation of the soluble fraction from the crystalline portion. This process is repeated twice. During the first injection, the entire sample is measured at high temperature to determine the iV [dl / g] and C2 [wt%] of the PP composition. During the second injection, the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) are measured using a crystallization cycle (wt% SF, wt% C2, iV).

[0131] The cold xylene soluble (XCS, wt%) fraction was determined at 25 °C according to ISO 16152 (1st edition, 2005-07-01).

[0132] The intrinsic viscosity was determined according to DIN ISO 1628 / 1 (October 1999) (in decalin at 135° C.).

[0133] Determination of Microstructure by NMR Spectroscopy - Ethylene Content in HECO Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers. 13 C{ 1 H}NMR spectrum. 1 H and 13 All spectra were recorded in solution using a Bruker Advance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz for C, respectively. 13 A C optimized 10 mm extended temperature probe head was used and all air pressures were recorded using nitrogen gas. Approximately 200 mg of material was dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) along with chromium-(III)-acetylacetonate (Cr(acac)3) to obtain a 65 mM solution of the relaxant in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475). After initial sample preparation in a heat block to ensure a homogenous solution, the NMR tube was further heated in a rotating oven for at least 1 hour. Once inserted in the magnet, the tube was spun at 10 Hz. This setup was chosen primarily due to the high resolution and quantitativeness required for accurate ethylene content quantification. Standard single pulse excitation was used without NOE, using an optimized tip angle, 1 second recycle delay and a bilevel WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transients were acquired per spectrum. quantitative 13 C{ 1H}NMR spectra were processed, integrated, and relevant quantitative properties were determined from the integrals using a dedicated computer program. All chemical shifts were indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This approach allowed for equal reference even when this structural unit was not present. Characteristic signals corresponding to the incorporation of ethylene were observed (Cheng, HN, Macromolecules 17 (1984), 1950). Characteristic signals corresponding to 2,1erythro regio-defects were observed (as described in L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100(4), 1253; Cheng, HN, Macromolecules 1984, 17, 1950; and WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157), necessitating correction for the influence of regio-defects on the determined properties. No characteristic signals corresponding to other types of regio-defects were observed. Using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157), 13 C{ 1 The comonomer fraction was quantified by integration of multiple signals over the entire spectral region of the {H} spectrum. This method was chosen for its robust nature and ability to take into account the presence of regio-defects, if necessary. The integration region was slightly adjusted to increase applicability over the full range of comonomer contents encountered. For systems in which only isolated ethylene was observed in the PPEPP sequence, the method of Wang et al. was modified to reduce the influence of nonzero integrals for sites known to be absent. This approach reduced the overestimation of ethylene content in such systems, achieved by reducing the number of sites used to determine absolute ethylene content to E = 0.5(Sββ + Sβγ + Sβδ + 0.5(Sαβ + Sαγ)). With this set of sites, the corresponding integral equation is E = 0.5(I H +I G +0.5(I C +I D ) The formula used for absolute propylene content was not modified. The mole percent of comonomer incorporation was calculated from the mole fractions. E[mol%]=100×fE The weight percent of comonomer incorporation was calculated from the mole fraction. E[weight%]=100×(fE×28.06) / ((fE×28.06)+((1-fE)×42.08)) Comonomer sequence distributions at the triad level were determined using the analytical method of Kakugo et al. (Kakugo, M., Naito, Y., Mizunuma, K., Miyatake, T. Macromolecules 15 (1982) 1150.) This method was chosen because of its robust nature and the integral region that was slightly adjusted to enhance applicability to a wider range of comonomer contents.

[0134] The flexural modulus was measured by the three-point bending method according to ISO178 on an injection-molded 80 x 10 x 4 mm 3 The results were determined for injection molded specimens.

[0135] Charpy notched impact strength is measured according to ISO179 / 1eA at 23°C and -20°C on injection moulded 80x10x4mm plates according to EN ISO1873-2 3 The results were determined for injection molded specimens.

[0136] DSC analysis, melting temperature (Tm) and crystallization temperature (Tc) were measured on 5-7 mg samples by TA Instrument Q2000 differential scanning calorimetry (DSC). DSC is performed according to ISO11357 / Part 3 / Method C2 in a heat / cool / heat cycle at a scan rate of 10°C / min in the temperature range of -30 to +225°C. Crystallization temperature and crystallization enthalpy (Hc) are determined from the cooling step and melting temperature and melting enthalpy (Hm) are determined from the second heating step.

[0137] The VOC and FOG values ​​were determined according to VDA 278 (Thermal Desorption Analysis of Organic Emissions for the Characterization of Non-Metallic Materials for Automobiles, October 2011, VDA Verband der Automobilindustrie) after sample preparation of injection molded plaques according to EN ISO19069-2:2016. The plaques were packed into aluminum composite foils immediately after production and the foils were sealed. According to VDA 278 (October 2011), the VOC value is defined as the "sum of readily and moderately volatile substances". It is calculated as the toluene equivalent. The method described in this recommendation allows the determination of n-pentacosane (C 25 ) allows the determination and analysis of substances with a boiling / elution range up to 10 ... The FOG value is defined as the sum of the less volatile substances eluted from the retention time of n-tetradecane (including this). It is calculated as the hexadecane equivalent. 14 " ~ "C 32 " boiling point range substances are determined and analyzed.

[0138] Fogging was measured on compression-molded plaques of 2 mm thickness according to DIN 75201, method B. Heat treatment was carried out at 100° C. for 16 h. Fogging is expressed as the difference in weight before and after treatment.

[0139] 1. Example Heterophasic Propylene Copolymers 1 and 2 (HECO1 and HECO2) The catalyst used in the polymerization process of heterophasic propylene copolymers 1 (HECO1) and 2 (HECO2) was anti-dimethylsilanediyl[2-methyl-4,8-di(3,5-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, disclosed as MC-2 in WO 2019 / 179959 A1. The supported metallocene catalyst was prepared similarly to IE2 in WO 2019 / 179959 A1.

[0140] HECO1 and HECO2 were prepared in a Borstar PP pilot plant with a continuous process including one prepolymerization reactor, one loop reactor and two gas phase reactors. The reaction conditions are summarized in Table 1.

[0141] [Table 1]

[0142] For stabilization, HECO1 and HECO2 were each blended with 1500 ppm of Irganox B215 (a synergistic 2:1 blend of the antioxidants Irgafos 168 (tris(2,4-di-tert-butylphenyl)phosphite, CAS number: 31570-04-4) and Irganox 1010 (pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate], CAS number: 6683-19-8), available from BASF SE) and 500 ppm of calcium stearate (CAS number: 1592-23-0, available from Baerlocher under the trade name CEASIT-1).

[0143] The HECO3 used in Comparative Example CE3 is a copolymer based on a Ziegler-Natta type catalyst, just like the HECO3 in WO2021144401A1.

[0144] [Table 2]

[0145] Propylene homopolymer 2 (PPH2) PPH2 is a propylene homopolymer commercially available as HL504FB from Borealis AG with a melt flow rate (230°C, 2.16 kg, ISO 1133) of 450 g / 10 min, a flexural modulus of 1519 MPa, a VOC content of 267 μg / g, and a FOG content of 629 μg / g.

[0146] Polypropylene / Polyethylene Blend The properties of the polypropylene / polyethylene blends (A) used in the evaluation are shown in Table 3. The properties are presented as ranges since these compositions are obtained from a mechanical recycling process.

[0147] ·Antioxidant masterbatch Irganox B215 (a synergistic 2:1 blend of antioxidants Irgafos 168 (tris(2,4-di-tert-butylphenyl)phosphite, CAS number: 31570-04-4) and Irganox 1010 (pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate], CAS number: 6683-19-8), commercially available from BASF SE) was blended with propylene homopolymer HC001, commercially available from Borealis AG, to form an antioxidant masterbatch. The amounts of Irganox B215 and HC001 separately are shown in Table 4.

[0148] [Table 3]

[0149] The polymers were used together with an antioxidant masterbatch to compound the final compositions in a Coperion ZSK40 twin screw extruder at 220° C. The compositions of the examples are shown in Table 4.

[0150] [Table 4]

[0151] The characteristics of the embodiment are shown in Table 5.

[0152] [Table 5]

[0153] It is seen that the composition according to the invention shows improved impact properties, sufficient mechanical properties even at low temperatures, and low amounts of impurities in the form of VOCs, FOG and fogging.The composition according to the invention is therefore suitable for moldings intended for packaging purposes, containing mixed plastic polypropylene blends obtained from post-consumer waste in amounts up to 84% by weight.

Claims

1. A composition obtained by blending component (A) and component (B), said component (A) being 50-95% by weight, preferably 55-90% by weight, more preferably 60-88% by weight, of a mixed plastic polypropylene / polyethylene blend; said component (B) being 5-50 wt.%, preferably 10-45 wt.%, more preferably 12-40 wt.% of a heterophasic propylene copolymer, where all percentages are based on the total composition; The mixed plastic polypropylene / polyethylene blend (A) is a crystalline fraction (CF) content determined according to CRYSTEX QC analysis in the range of 85.0 to 96.0 wt.%, preferably in the range of 86.5 to 95.5 wt.%; A soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 4.0 to 15.0 wt.%, preferably in the range of 4.5 to 13.5 wt.%. having The crystalline fraction (CF) is quantitatively in the range of 11.0 to 55.0% by weight, preferably in the range of 20.0 to 49.5% by weight. 13 having an ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; the soluble fraction (SF) has an intrinsic viscosity (iV(SF)) in the range of 0.9 to 2.1 dl / g, preferably in the range of 1.0 to 2.0 dl / g; The heterophasic propylene copolymer (B) comprises a matrix phase and an elastomeric phase dispersed therein, Melt flow rate (MFR) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min 2 (230°C, 2.16kg, ISO1133) a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0 to 35.0 wt.%, preferably in the range of 11.0 to 32.5 wt.%, more preferably in the range of 12.0 to 30.0 wt.%; an intrinsic viscosity (iV(SF)) of said soluble fraction measured in decalin at 135° C. according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; having The composition has a melt flow rate MFR of at least 9.0 g / 10 min, preferably from 9.5 to 100 g / 10 min, more preferably from 10.0 to 75 g / 10 min. 2 (230°C, 2.16 kg, ISO 1133).

2. Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 2. The composition of claim 1, having a flexural modulus (FM) determined according to ISO 178 for a tensile strength of 1000 g / m2 (1000 g / m2) in the range of 800 to 1300 MPa, preferably in the range of 850 to 1200 MPa, more preferably in the range of 865 to 1050 MPa.

3. Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 ) 5.0 to 25.0 kJ / m2, determined according to ISO 179 / eA 2 in the range of 5.5 to 20.0 kJ / m 2 3. The composition of claim 1 or 2, having a Charpy notched impact strength at 23° C. in the range of

4. Melt flow rate MFR 2 The composition according to any one of claims 1 to 3, having a Charpy notched impact strength at 23 ° C. that satisfies the following inequality with respect to (230 ° C., 2.16 kg, ISO 1133): CNIS, 23℃[kJ / m 2 ]>7.8[kJ / m 2 ]-0.17[kJ / m 2 / g / 10 minutes]・MFR 2 [g / 10 minutes] (In the formula, CNIS, 23°C, was measured using injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2. 3 ) is the Charpy notched impact strength of the composition at 23° C., determined according to ISO 179 / eA; MFR 2 is the melt flow rate MFR of the composition 2 (230°C, 2.16 kg, ISO 1133).

5. Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 ) 1.7 to 5.0 kJ / m2, determined according to ISO 179 / eA 2 in the range of 1.9 to 4.0 kJ / m 2 The composition according to any one of claims 1 to 4, having a Charpy notched impact strength at -20°C in the range of

6. a volatile organic compounds (VOC) content, determined according to VDA 278, of less than or equal to 100 μg / g, preferably in the range of 5 to 95 μg / g, more preferably in the range of 10 to 90 μg / g, and / or and / or a FOG content, determined according to VDA 278, of less than or equal to 1100 μg / g, preferably in the range of 50 to 1050 μg / g, more preferably in the range of 80 to 1000 μg / g; and / or Fogging amount less than or equal to 5.0 mg, preferably in the range of 0.5 to 4.5 mg, determined according to DIN 75201, method B, on a compression-molded plaque of 2 mm thickness A composition according to any one of claims 1 to 5, having one or more, preferably all, of the following properties:

7. The composition according to any one of claims 1 to 6, comprising an additional polymer component in an amount of up to 5 wt%, preferably up to 2 wt%, more preferably 0 wt%.

8. The mixed plastic polypropylene / polyethylene blend (A) is an intrinsic viscosity of the crystalline fraction (iV(CF)) measured in decalin at 135° C. according to DIN ISO 1628 / 1 in the range of from 1.0 to less than 2.6 dl / g, more preferably in the range of from 1.2 to 2.5 dl / g; Quantitatively in the range of 20.0 to 55.0% by weight, preferably in the range of 22.0 to 50.0% by weight. 13 the ethylene content of the soluble fraction (C2(SF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; Melt flow rate (MFR) of 5.0 to 50 g / 10 min, preferably 5.2 to 45 g / 10 min, more preferably 5.4 to 40 g / 10 min 2 (230℃, 2.16kg, ISO1133), units derived from ethylene in an amount of 5.0 to 50.0% by weight, more preferably 10.0 to 48.5% by weight, even more preferably 25.0 to 47.0% by weight, Propylene-derived units in an amount of 50.0 to 95.0% by weight, more preferably 51.5 to 90.0% by weight, and even more preferably 53.0 to 75.0% by weight; a limonene content of 0.1 to 50 ppm, determined using solid phase microextraction (HS-SPME-GC-MS); and / or a tensile modulus of 800 to 1400 MPa, preferably 850 to 1200 MPa, and / or 4.0~8.5kJ / m 2 , preferably 5.0 to 8.0 kJ / m 2 Charpy notched impact strength at 23°C (CNIS, 23°C), and / or 1.0~4.5kJ / m 2 , preferably 1.5 to 4.0 kJ / m 2 Charpy notched impact strength at -20°C (CNIS, -20°C) A composition according to any one of claims 1 to 7, having one or more, preferably all, of the following properties:

9. The heterophasic propylene copolymer (B) is a crystalline fraction (CF) determined according to CRYSTEX QC analysis in an amount ranging from 65.0 to 90.0 wt.%, preferably ranging from 67.5 to 89.0 wt.%, more preferably ranging from 70.0 to 88.0 wt.%, relative to the total weight of said heterophasic propylene copolymer (B); an intrinsic viscosity of the crystalline fraction (iV(CF)) of less than or equal to 1.2 dl / g, preferably in the range of 0.4 to 1.1 dl / g; quantitative 13 an ethylene content of the crystalline fraction (C2(CF)) of less than or equal to 1.0% by weight, preferably ranging from 0 to 0.9% by weight, based on the total weight of the crystalline fraction (CF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; quantitative 13 an ethylene content of the soluble fraction (C2(SF)) in the range of 14.0 to 29.0 wt.%, preferably in the range of 17.0 to 26.0 wt.%, more preferably in the range of 19.0 to 24.0 wt.%, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; and / or Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 Flexural modulus, determined according to ISO 178, in the range of 800 to 1500 MPa, preferably in the range of 850 to 1450 MPa; quantitative 13 a total ethylene content in the range of 2.0 to 5.5 wt.%, preferably in the range of 2.5 to 5.0 wt.%, based on the total weight of said heterophasic propylene copolymer (B), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; A melting temperature in the range of 150 to 162° C., preferably in the range of 152 to 160° C., determined by DSC according to ISO 3146 (Part 3, Method C2); a crystallization temperature in the range of 110 to 130° C., preferably in the range of 115 to 125° C., determined by DSC according to ISO 3146 (part 3, method C2); Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 ) 2.5 to 15.0 kJ / m2, determined according to ISO 179 / eA 2 in the range of 3.0 to 12.0 kJ / m 2 Charpy notched impact strength at 23°C in the range of a volatile organic compounds (VOC) content, determined according to VDA 278, of less than or equal to 50 μg / g, preferably less than or equal to 40 μg / g, more preferably less than or equal to 35 μg / g, and / or FOG content, determined according to VDA 278, of less than or equal to 300 μg / g, preferably less than or equal to 250 μg / g, more preferably less than or equal to 225 μg / g A composition according to any one of claims 1 to 8, having one or more, preferably all, of the following properties:

10. a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in the presence of the single-site catalyst system in the second polymerization reactor to produce a second propylene polymer fraction; d) transferring a polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction, and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in the presence of a single-site catalyst system in said third polymerization reactor to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining said heterophasic propylene copolymer (B) comprising said first propylene polymer fraction, said second propylene polymer fraction and said third propylene-ethylene copolymer fraction; h) blending 5-50 wt.%, preferably 10-45 wt.%, more preferably 12-40 wt.% of said heterophasic propylene copolymer (B) with 50-95 wt.%, preferably 55-90 wt.%, more preferably 60-88 wt.% of said mixed plastic polypropylene / polyethylene blend (A); A method for producing the composition according to any one of claims 1 to 9, comprising:

11. The single-site catalyst system comprises: (i) a metallocene complex of the following general formula (I): 【Chemistry 1】 (In the formula, each X is independently a sigma donor ligand; L is -R' 2 C-, -R' 2 C-CR' 2 -, -R' 2 Si-, -R' 2 Si-SiR' 2 -, -R' 2 Ge-, where each R' is independently a hydrogen atom or a C optionally containing one or more heteroatoms or fluorine atoms from Groups 14-16 of the Periodic Table of the Elements. 1 ~C 20 - a hydrocarbyl group, or optionally two R' groups can be taken together to form a ring; Each R 1 may be independently the same or different, and are hydrogen, linear or branched C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group, and optionally two adjacent R 1 The groups may be part of a ring that includes the phenyl carbon to which they are attached; Each R 2 may be independently the same or different, CH 2 -R 8 group, where R 8 is H or linear or branched C 1~6 Alkyl group, C 3~8 Cycloalkyl group, C 6~10 is an aryl group, R 3 is a linear or branched chain C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6 ~C 20 is an aryl group, R 4 is C(R 9 ) 3 group, where R 9 is a linear or branched chain C 1 ~C 6 is an alkyl group, R 5 is hydrogen or an aliphatic C optionally containing one or more heteroatoms from groups 14 to 16 of the periodic table of the elements; 1 ~C 20 is a hydrocarbyl group, R 6 is hydrogen or an aliphatic C optionally containing one or more heteroatoms from groups 14 to 16 of the periodic table of the elements; 1 ~C 20 is a hydrocarbyl group, or R 5 and R 6 together, n (n is 0 to 4) R 10 can form a 5-membered saturated carbocyclic ring optionally substituted with a group, Each R 10 are the same or different, C 1 ~C 20 Hydrocarbyl groups or C optionally containing one or more heteroatoms belonging to groups 14 to 16 of the Periodic Table 1 ~C 20 may be a hydrocarbyl group, R 7 is H or linear or branched C 1 ~C 6 An alkyl group or one to three R 11 an aryl or heteroaryl group having 6 to 20 carbon atoms, optionally substituted with a group; Each R 11 may be independently the same or different, and are hydrogen, linear or branched C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group. (ii) an aluminoxane cocatalyst; and (iii) a silica support; The method of claim 10, comprising:

12. An article comprising the composition of any one of claims 1 to 11.

13. 13. The article of claim 12 which is an automotive article or a packaging article.

14. Use of the polypropylene composition according to any one of claims 1 to 11 as a formulation base for the manufacture of articles.

15. Use of a heterophasic propylene copolymer in a composition according to any one of claims 1 to 11, said heterophasic propylene copolymer being Melt flow rate (MFR) of 105 to 320 g / 10 min, preferably 107 to 300 g / 10 min, more preferably 110 to 280 g / 10 min 2 (230°C, 2.16kg, ISO1133) a soluble fraction (SF) content determined according to CRYSTEX QC analysis in the range of 10.0 to 35.0 wt.%, preferably in the range of 11.0 to 32.5 wt.%, more preferably in the range of 12.0 to 30.0 wt.%; an intrinsic viscosity (iV(SF)) of said soluble fraction measured in decalin at 135° C. according to DIN ISO 1628 / 1 of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; and by the above use, the melt flow rate MFR 2 (230°C, 2.16 kg, ISO 1133) and flexural modulus and reduce the VOC and FOG content of the composition.

Citation Information

Patent Citations

  • Polypropylene-polyethylene composition with improved flowability

    JP2018532859A

  • Method for making heterophasic polymer compositions

    JP2020508388A

  • Olefin polymerization catalysts

    JP2021518462A

  • Polypropylene composition for interior automotive applications

    EP4101889B1

  • Polypropylene composition for exterior automotive applications

    EP4101890B1