High Melt Flow Polypropylene Composition
A polypropylene composition with optimized crystalline and soluble fractions, produced via a single-site catalyst system, addresses the limitations of high MFR heterophasic polypropylenes by enhancing mechanical and impact properties, ensuring high processability and purity for injection molding applications.
Patent Information
- Application Number
- JP2024531255
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing heterophasic polypropylene compositions with high melt flow rates (MFR) face limitations in mechanical properties, particularly stiffness and impact strength, due to poor reactor solubility of ethylene and increased oligomer amounts, leading to issues like loss of additives and impurities.
A polypropylene composition with a specific balance of crystalline and soluble fractions, produced using a single-site catalyst system in multiple polymerization reactors, achieving a high MFR of 105 to 320 g/10 min, and optimized for high flexural modulus and impact strength, with low volatile organic compounds (VOC) and foul odor gases (FOG) content.
The composition exhibits excellent mechanical and impact properties, suitable for injection molding, with improved processability and purity, meeting the demands of thin-walled articles.
Smart Images

Figure 2024542566000001 
Figure 2024542566000002 
Figure 2024542566000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a high melt flow polypropylene composition having an improved balance of properties with respect to mechanical and impact properties, a process for the manufacture of said polypropylene composition, an article comprising said polypropylene composition, and the use of said polypropylene composition for the manufacture of an article. [Background technology]
[0002] Heterophasic propylene copolymers are widely used in the packaging industry due to their excellent combination of stiffness and impact behavior. Heterophasic propylene copolymers are applied in various aspects of daily life. One of the main application areas of polypropylene is the injection molding of thin-walled articles. Typical examples include plastic cups, pails and small containers mainly used for food packaging. To be suitable for thin-walled injection molding applications, polypropylene needs to show good processability / flowability, usually represented by a high melt flow rate (MFR), i.e. a low average molecular weight. Nevertheless, the polymer and packaging industry is desirous of improving usable heterophasic polypropylene compositions with high melt flow rate (MFR) in terms of mechanical properties, especially the amount of impurities. However, existing technologies have some limitations. For example, heterophasic polypropylene compositions with high melt flow rates (MFR) produced in the presence of Ziegler-Natta catalysts have inherent limitations for two reasons: First, the H2 response characteristics are poor, and at a given temperature / pressure ratio in the reactor, the solubility of H2 and therefore the MFR is limited, especially when producing copolymers with ethylene. Second, the amount of oligomers increases with the MFR. Although there are some techniques for removing oligomers from high melt flow heterophasic polypropylene compositions, they can cause other problems, such as additive loss, and are largely ineffective for long chain oligomers under normal conditions.
[0003] WO 2017 / 148970 A1 discloses heterophasic polypropylene compositions with good mechanical and impact properties. However, the melt flow rate MFR2 of these compositions is too low for some applications. Also, these compositions were prepared in the presence of Ziegler-Natta catalysts, which shows the limitations and impurities mentioned above. EP 3812404 A1 discloses heterophasic polypropylene compositions with good mechanical and impact properties and low extractables. However, the melt flow rate MFR2 of these compositions is too low for some applications. EP 2075284 A1 discloses heterophasic polypropylene compositions with high melt flow rate MFR2. However, these compositions lack mechanical properties, especially stiffness.
[0004] Therefore, what is needed in the art is a polypropylene composition suitable for injection molding and production of thin walled articles, having a high melt flow rate MFR2 of greater than 100 g / 10 min, and exhibiting an improved balance of properties in terms of mechanical and impact properties exemplified by high flexural modulus and high impact strength, high processability exemplified by high melt flow rate, and low levels of impurities exemplified by low levels of VOC and FOG. Surprisingly, it has been found that by carefully selecting the polymerization conditions for the polypropylene composition to optimize the properties of the elastomeric phase, identified as the soluble phase (SF) in the CRYSTEX measurements, polypropylene compositions exhibiting such an improved balance of properties can be obtained. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 148970A1 Brochure [Patent Document 2] European Patent Application Publication No. 3812404A1 [Patent Document 3] European Patent Application Publication No. 2075284A1 Summary of the Invention [Means for solving the problem]
[0006] The present invention relates to a polypropylene composition comprising a crystalline fraction (CF) and a soluble fraction (SF), both determined according to CRYSTEX QC analysis, The soluble fraction (SF) is is present in the polypropylene composition in an amount in the range of 10.0 to 35.0% by weight, preferably in the range of 11.0 to 32.5% by weight, more preferably in the range of 12.0 to 30.0% by weight, relative to the total weight of the polypropylene composition; having an intrinsic viscosity (iV(SF)) of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; quantitative 13 having an ethylene content (C2(SF)) in the range of 14.0 to 29.0% by weight, preferably in the range of 17.0 to 26.0% by weight, more preferably in the range of 19.0 to 24.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; the ratio of the intrinsic viscosity of the soluble fraction to the intrinsic viscosity of the crystalline fraction (iV(SF) / (iV(CF)) is in the range of 2.5 to 5.0, preferably in the range of 2.6 to 4.8; The polypropylene composition has a melt flow rate MFR2 (230° C., 2.16 kg, ISO 1133) in the range of 105 to 320 g / 10 min, preferably in the range of 107 to 300 g / 10 min, more preferably in the range of 110 to 280 g / 10 min.
[0007] The present invention also relates to a process for producing the polypropylene composition described above or below, said process comprising the steps of: a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in the presence of the single-site catalyst system in the second polymerization reactor to produce a second propylene polymer fraction; d) transferring a polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction, and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in the presence of a single-site catalyst system in said third polymerization reactor to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining a polymer composition comprising the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; Includes.
[0008] Furthermore, the present invention relates to an article comprising the above or below described polypropylene composition.
[0009] Finally, the present invention relates to the use of the polypropylene composition described above or below in the manufacture of an article.
[0010] definition Propylene homopolymer is a polymer consisting essentially of propylene monomer units. Due to impurities, particularly in commercial polymerization processes, propylene homopolymer may contain at most 0.1 mol% of comonomer units, preferably at most 0.05 mol% of comonomer units, and most preferably at most 0.01 mol% of comonomer units.
[0011] Propylene random copolymers are composed of propylene monomer units and preferably ethylene and C4-C 10 A copolymer with comonomer units selected from alpha olefins, the comonomer units being randomly distributed on the polymer chain. Propylene random copolymers may contain comonomer units from one or more comonomers with different amounts of carbon atoms.
[0012] Heterophasic polypropylenes are propylene-based copolymers having a semi-crystalline matrix phase, which may be a propylene homopolymer or a random copolymer of propylene and at least one alpha-olefin comonomer, and an elastomeric phase dispersed therein. In the case of random heterophasic propylene copolymers, said semi-crystalline matrix phase is a random copolymer of propylene and at least one alpha-olefin comonomer. The elastomeric phase may be a propylene copolymer containing a large amount of comonomer, not randomly distributed in the polymer chain, but distributed in comonomer-rich and propylene-rich block structures. Heterophasic polypropylenes differ from single-phase propylene copolymers in that they typically exhibit two different glass transition temperatures, Tg, which are assigned to the matrix and elastomeric phases.
[0013] Below, amounts are in weight percent unless otherwise stated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Polypropylene Composition In one aspect, the present invention relates to a polypropylene composition having a high melt flow rate that exhibits high flowability and good processability, making the polypropylene composition suitable for injection molding and thin wall applications.
[0015] The polypropylene composition has a melt flow rate MFR2 (230° C., 2.16 kg, ISO 1133) in the range of 105 to 320 g / 10 min, preferably in the range of 107 to 300 g / 10 min, more preferably in the range of 110 to 280 g / 10 min.
[0016] The polypropylene composition can be characterized by CRYSTEX QC analysis, which provides a crystalline fraction (CF) and a soluble fraction (SF) that can be quantified and analyzed for monomer and comonomer content, and intrinsic viscosity (iV). The polypropylene composition was analyzed by CRYSTEX QC. A crystalline fraction (CF) content, determined according to CRYSTEX QC analysis, in the range of 65.0 to 90.0 wt.%, preferably in the range of 67.5 to 89.0 wt.%, more preferably in the range of 70.0 to 88.0 wt.%, based on the total weight of the polypropylene composition; and A soluble fraction (SF) content, determined according to CRYSTEX QC analysis, in the range of 10.0-35.0 wt.%, preferably in the range of 11.0-32.5 wt.%, more preferably in the range of 12.0-30.0 wt.%, based on the total weight of the polypropylene composition. It is preferred that the material exhibit one or all of the following characteristics:
[0017] The crystalline fraction (CF) is A quantitative amount of 1.0% by weight or less, preferably in the range of 0 to 0.9% by weight, based on the total weight of the crystalline fraction (CF) 13 ethylene content (C2(CF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, and / or Intrinsic viscosity (iV(CF)) measured in decalin according to DIN ISO 1628 / 1 at 135°C of less than 1.2 dl / g, preferably in the range of 0.4 to 1.1 dl / g It is preferred that the composition has one or more, preferably all, of the following characteristics:
[0018] The soluble fraction (SF) is A quantitative amount of 14.0 to 29.0% by weight, preferably 17.0 to 26.0% by weight, more preferably 19.0 to 24.0% by weight, based on the total weight of the soluble fraction (SF). 13 the ethylene content (C2(SF)) determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy, and / or An intrinsic viscosity (iV(SF)) measured in decalin according to DIN ISO 1628 / 1 at 135° C. of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g. It has the following characteristics.
[0019] The ratio of the intrinsic viscosity of the soluble fraction to the intrinsic viscosity of the crystalline fraction (iV(SF) / (iV(CF)) is in the range of 2.5 to 5.0, and preferably in the range of 2.6 to 4.8.
[0020] The polypropylene composition is quantitatively 13 It is preferred that the polypropylene composition comprises a total ethylene (C2) content in the range of 2.0 to 5.5 wt.%, preferably in the range of 2.5 to 5.0 wt.%, based on the total weight of the polypropylene composition, as determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy.
[0021] It is also preferred that the polypropylene composition has an intrinsic viscosity (iV), measured in decalin according to DIN ISO 1628 / 1 at 135° C., in the range of 0.8 to 1.8 dl / g, more preferably in the range of 1.0 to 1.4 dl / g.
[0022] Preferably, the polypropylene composition comprises a xylene cold soluble (XCS) fraction at 25°C in an amount in the range of 8.0 to 32.0 wt%, preferably in the range of 9.0 to 30.0 wt%, more preferably in the range of 10.0 to 28.0 wt%, based on the total weight of the polypropylene composition. The above XCS fraction is an intrinsic viscosity (iV(XCS)) of at least 2.2 dl / g, preferably in the range of 2.3 to 4.6 dl / g, more preferably in the range of 2.5 to 4.4 dl / g, and / or quantitative 13 An ethylene content (C2(XCS)) in the range of 15.0-30.0% by weight, preferably in the range of 18.0-27.0% by weight, more preferably in the range of 20.0-25.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy. It is preferable for the material to have one or both of the following characteristics:
[0023] The polypropylene composition preferably has a melting temperature (Tm) in the range of 150-162°C, more preferably in the range of 152-160°C, determined by DSC according to ISO 3146 (Part 3, Method C2).
[0024] It is also preferred that the polypropylene composition has a crystallization temperature (Tc) in the range of 110 to 130° C., more preferably in the range of 115 to 125° C., determined by DSC according to ISO 3146 (Part 3, Method C2).
[0025] Furthermore, it is preferred that the polypropylene composition has an enthalpy of fusion (Hm) in the range of 80 to 100 J / g, more preferably in the range of 85 to 95 J / g, determined by DSC according to ISO 3146 (part 3, method C2).
[0026] The polypropylene composition according to the present invention preferably exhibits an excellent balance of properties in terms of mechanical properties such as high flexural modulus and impact properties such as high Charpy notched impact strength. In this regard, the flexural modulus and Charpy notched impact strength depend on the amount of soluble fraction (SF) in the polypropylene composition and the melt flow rate MFR2, which reflects the elastomer content of the polypropylene composition. It has been found that the polypropylene composition exhibits a high flexural modulus depending on the soluble fraction (SF) and a high Charpy notched impact strength depending on the melt flow rate MFR2.
[0027] The compositions were prepared in injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2. 3 It is preferred that the material has a flexural modulus, determined in accordance with ISO 178 for tensile strength (MPa) in the range of 800 MPa to 1500 MPa, preferably in the range of 850 MPa to 1450 MPa.
[0028] The polypropylene composition preferably has a flexural modulus (FM) with respect to the amount of soluble fraction (SF) that satisfies the following inequality: FM[MPa]>1550[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%] Preferably FM[MPa]>1575[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%], More preferably FM[MPa]>1600[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%], Most preferably FM[MPa]>1625[MPa]-33.4[MPa / weight%]・Amount (SF)[weight%] During the ceremony, F [MPa] is the flexural modulus of the polypropylene composition, in MPa; The amount (SF) [wt %] is the amount of the soluble fraction (SF) in the polypropylene composition, and the unit is weight %.
[0029] The compositions were also tested on injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2. 3 ) determined according to ISO 179 / eA, 2.5 to 15.0 kJ / m 2 in the range of 3.0 to 12.0 kJ / m 2 It is preferred that the Charpy notched impact strength at 23° C. is in the range of
[0030] The polypropylene composition preferably has a Charpy notched impact strength at 23° C. (CNIS, 23° C.) that satisfies the following inequality with respect to the melt flow rate (MFR2): CNIS, 23℃ [kg / m 2 ]>10.0[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min] Preferably CNIS, 23℃ [kg / m 2 ]>10.5[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min], More preferably CNIS, 23℃ [kg / m 2 ]>11.0[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min], Most preferably CNIS, 23℃ [kg / m 2 ]>11.5[kg / m 2 ]-0.05[kg / m 2 / g / 10min]·MFR2[g / 10min].
[0031] In addition to a good balance of mechanical and impact properties, the polypropylene compositions also exhibit high purity with low levels of VOCs and FOGs.
[0032] The polypropylene composition preferably has a content of volatile organic compounds (VOC), determined according to VDA 278, of less than or equal to 50 μg / g, preferably less than or equal to 40 μg / g, more preferably less than or equal to 35 μg / g. The lower limit for the VOC content is usually at least 2 μg / g, preferably at least 4 μg / g.
[0033] It is also preferred that the polypropylene composition has a FOG content, determined according to VDA 278, of less than or equal to 300 μg / g, preferably less than or equal to 250 μg / g, more preferably less than or equal to 225 μg / g. The lower limit of the FOG content is usually at least 20 μg / g, preferably at least 40 μg / g.
[0034] The polypropylene composition preferably comprises a heterophasic propylene copolymer comprising a semi-crystalline matrix phase and an elastomeric phase dispersed in said matrix phase.
[0035] The polypropylene composition preferably comprises the heterophasic propylene copolymer in an amount in the range of 93.0-100 wt.%, preferably in the range of 95.0-99.9 wt.%, more preferably in the range of 96.5-99.8 wt.%, based on the total weight of the polypropylene composition.
[0036] The polypropylene composition may comprise additional polymeric components. However, it is preferred that the polypropylene composition comprises the heterophasic propylene copolymer as the sole polymeric component.
[0037] The polypropylene composition may further contain an additive in an amount of 0.01 to 7.0% by weight, preferably 0.1 to 5.0% by weight, more preferably 0.2 to 3.5% by weight, based on the total weight of the polypropylene composition. Typically, the additives are selected from antioxidants, anti-slip agents, nucleating agents, anti-scratch agents, anti-scorch agents, metal deactivators, UV stabilizers, acid scavengers, lubricants, antistatic agents, pigments, and the like, and combinations thereof. These additives are well known in the polymer industry, and those skilled in the art are familiar with their use. Any additives present can be added as isolated raw materials or as a mixture with a carrier polymer, i.e., as a so-called masterbatch.
[0038] process In a further aspect, the present invention relates to a process for the manufacture of a polypropylene composition as described above or below, the process comprising the steps of: a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in a second polymerization reactor in the presence of a single-site catalyst system to produce a second propylene polymer fraction; d) transferring the polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction, and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in a third polymerization reactor in the presence of a single-site catalyst system to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining a polymer composition comprising a first propylene polymer fraction, a second propylene polymer fraction, and a third propylene-ethylene copolymer fraction; Includes.
[0039] The first polymerization reactor is preferably a slurry phase reactor, such as a loop reactor.
[0040] The operating temperature in the first polymerization reactor, preferably the loop reactor, is preferably in the range of 62 to 85°C, more preferably in the range of 65 to 82°C, and even more preferably in the range of 67 to 80°C.
[0041] Typically the pressure in the first polymerization reactor, preferably the loop reactor, is in the range from 20 to 80 bar, preferably from 30 to 70 bar, for example from 35 to 65 bar.
[0042] It is preferred to produce a propylene homopolymer in a first polymerization reactor, preferably a loop reactor, and therefore the first propylene polymer fraction is preferably a propylene homopolymer fraction.
[0043] Preferably, hydrogen is added into the first polymerization reactor to control the molecular weight, ie the melt flow rate MFR2. Preferably, the hydrogen to propylene ratio (H2 / C3 ratio) in the first polypropylene reactor, preferably the loop reactor, is in the range of 0.70 to 2.5 mol / kmol, more preferably 0.75 to 2.0 mol / kmol.
[0044] Due to the strong hydrogen response of the catalyst and the relatively large amount of hydrogen, the melt flow rate of the first propylene polymer fraction is very high. The first propylene polymer fraction preferably has a melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) in the range of 1000 to 15000 g / 10 min, preferably in the range of 1100 to 13500 g / 10 min, more preferably in the range of 1250 to 11500 g / 10 min.
[0045] The second polymerization reactor is preferably a first gas phase reactor, such as a first fluidized bed gas phase reactor.
[0046] The operating temperature in the second polymerization reactor, preferably the first gas phase reactor, is preferably in the range of 75-95°C, more preferably in the range of 78-92°C.
[0047] Typically, the pressure in the second polymerization reactor, preferably the first gas phase reactor, is in the range of from 5 to 50 bar, preferably from 15 to 40 bar.
[0048] It is preferred to produce a propylene homopolymer in a second polymerization reactor, preferably in the first gas phase reactor, and therefore the second propylene polymer fraction is preferably a propylene homopolymer fraction.
[0049] Preferably, hydrogen is added into the second polymerization reactor to control the molecular weight, ie the melt flow rate MFR2. Preferably, the hydrogen to propylene ratio (H2 / C3 ratio) in the second polypropylene reactor, preferably the first gas phase reactor, is in the range of 2.0 to 6.5 mol / kmol, more preferably 2.8 to 5.5 mol / kmol.
[0050] Due to the strong hydrogen response of the catalyst and the relatively large amount of hydrogen, the melt flow rate of the combined first and second propylene polymer fractions is very high. The combined first and second propylene polymer fractions preferably have a melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) of at least 1000 g / 10 min, preferably in the range of 1200 to 9000 g / 10 min, more preferably in the range of 1500 to 8000 g / 10 min.
[0051] It is further preferred that the combined first and second propylene polymer fractions have a xylene cold soluble (XCS) fraction at 25° C. in an amount of less than or equal to 2.0 wt %, preferably in the range of 0.1 to 1.5 wt %, based on the total weight of the combined first and second propylene polymer fractions.
[0052] The third polymerization reactor is preferably a second gas phase reactor, such as a second fluidized bed gas phase reactor.
[0053] The operating temperature in the third polymerization reactor, preferably the second gas phase reactor, is preferably in the range of 65 to 85° C., more preferably in the range of 68 to 82° C. Typically, the operating temperature in the third polymerization reactor is lower than the operating temperature in the second polymerization reactor.
[0054] Typically, the pressure in the third polymerization reactor, preferably the second gas phase reactor, is in the range of from 5 to 50 bar, preferably from 15 to 40 bar.
[0055] In a third polymerization reactor, preferably a second gas phase reactor, a propylene ethylene copolymer is produced. The third propylene polymer fraction is therefore a propylene ethylene copolymer fraction.
[0056] The ethylene to propylene ratio (C2 / C3 ratio) in the third polymerization reactor, preferably the second gas phase reactor, is in the range of 700 to 1000 mol / kmol, more preferably 800 to 950 mol / kmol. Due to its high ethylene to propylene ratio (C2 / C3 ratio), the third propylene copolymer fraction is preferably an elastomeric block copolymer having a propylene-rich portion and an ethylene-rich portion.
[0057] Preferably, hydrogen is added into the second polymerization reactor to control the molecular weight, ie the melt flow rate MFR2. Preferably, the hydrogen to ethylene ratio (H2 / C2 ratio) in the third polymerization reactor, preferably the second gas phase reactor, is in the range of 0.5 to 3.5 mol / kmol, more preferably in the range of 1.0 to 2.5 mol / kmol.
[0058] The first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined preferably have a melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) of at least 150 g / 10 min, preferably in the range of 165 to 500 g / 10 min, more preferably in the range of 175 to 400 g / 10 min.
[0059] It is further preferred that the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined have a xylene cold soluble (XCS) fraction at 25° C. in an amount in the range of 8.0 to 32.0 wt %, preferably in the range of 9.0 to 30.0 wt %, more preferably in the range of 10.0 to 28.0 wt %, based on the total weight of the polypropylene composition. The XCS fraction is an intrinsic viscosity (iV(XCS)) of at least 2.2 dl / g, preferably in the range of 2.3 to 4.6 dl / g, more preferably in the range of 2.5 to 4.4 dl / g; and quantitative 13 An ethylene content (C2(XCS)) in the range of 15.0-30.0% by weight, preferably in the range of 18.0-27.0% by weight, more preferably in the range of 20.0-25.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy. It is preferable that the material has the following characteristics.
[0060] Also, the combined first propylene polymer fraction, the second propylene polymer fraction, and the third propylene polymer fraction are quantitatively 13 It is preferred to have a total comonomer content, preferably an ethylene (C2) content, in the range of 2.0 to 5.5 wt.%, preferably in the range of 2.5 to 5.0 wt.%, based on the total weight of the polypropylene composition, determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy.
[0061] The combined first propylene polymer fraction, the second propylene polymer fraction, and the third propylene polymer fraction preferably form a heterophasic propylene copolymer.
[0062] The preparation of the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction may comprise, in addition to the (main) polymerization stage in at least three polymerizations, a preliminary (pre)polymerization step prior thereto in a preliminary (pre)polymerization reactor upstream of the first polymerization reactor.
[0063] In the prepolymerization reactor, polypropylene is produced. The prepolymerization is preferably carried out in the presence of a single-site polymerization catalyst system. According to this embodiment, the single-site polymerization catalyst system is introduced in the prepolymerization step. However, this does not exclude the option of adding further cocatalysts in the polymerization process, for example in a later stage, for example in the first reactor. In one embodiment, when applying prepolymerization, all components of the single-site catalyst are added only in the prepolymerization reactor.
[0064] The prepolymerization reaction is typically carried out at a temperature of 0 to 60°C, preferably 15 to 50°C, and more preferably 20 to 45°C.
[0065] The pressure in the prepolymerization reactor is not particularly limited, but must be high enough to maintain the reaction mixture in the liquid phase. Thus, the pressure may be 20 to 100 bar, for example 30 to 70 bar.
[0066] In a preferred embodiment, the prepolymerization is carried out as a bulk slurry polymerization in liquid propylene, ie, the liquid phase comprises mainly propylene, optionally with inert components dissolved therein.
[0067] It is also possible to add other ingredients to the prepolymerization stage. Thus, hydrogen may be added to the prepolymerization stage to control the molecular weight of the polypropylene, as is well known in the art. Antistatic agents may also be used to prevent particles from adhering to each other and to the walls of the reactor.
[0068] The precise control of prepolymerization conditions and reaction parameters is within the skill of one in the art.
[0069] The above-specified process conditions in the prepolymerization preferably result in a mixture of the single-site catalyst system and the polypropylene produced in the prepolymerization reactor. Preferably, the single-site catalyst system is (finely) dispersed in the polypropylene. In other words, the single-site catalyst particles introduced in the prepolymerization reactor are divided into small fragments that are homogeneously distributed in the growing polypropylene. The size of the introduced single-site catalyst particles and the size of the resulting fragments are not of essential relevance to the present invention and are within the knowledge of the person skilled in the art.
[0070] As mentioned above, when prepolymerization is used, following said prepolymerization, the mixture of single-site catalyst and polypropylene produced in the prepolymerization reactor is transferred to the first polymerization reactor. Typically, the total amount of polypropylene produced in the prepolymerization reactor in the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene polymer fraction is fairly small, typically 5.0 wt% or less, more preferably 4.0 wt% or less, even more preferably in the range of 0.5 to 4.0 wt%, for example 1.0 to 3.0 wt%.
[0071] When prepolymerization is not used, propylene and other components, such as the single-site catalyst system, are introduced directly into the first polymerization reactor.
[0072] The residence times of the polymerization mixture in the different polymerization stages are adjusted to obtain respective amounts of the first polymer fraction, the second polymer fraction, and the third polymer fraction within the combined first polymer fraction, the second polymer fraction, and the third polymer fraction.
[0073] Preferably, the first propylene polymer fraction is present in an amount of 40 to 60 wt%, more preferably 45 to 55 wt%, based on the total weight of the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene polymer fraction combined. If a prepolymerization reactor is present, the amount of polypropylene produced therein will generally be added to the amount of the first propylene polymer fraction.
[0074] Preferably, the second propylene polymer fraction is present in an amount of from 25 to 45% by weight, more preferably from 30 to 40% by weight, based on the total weight of the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined.
[0075] Preferably, the third propylene polymer fraction is present in an amount of from 10 to 30% by weight, more preferably from 15 to 25% by weight, based on the total weight of the first propylene polymer fraction, the second propylene polymer fraction and the third propylene polymer fraction combined.
[0076] Catalyst system The single-site catalyst system according to the present invention may be any supported metallocene catalyst system suitable for the production of isotactic polypropylene.
[0077] The single-site catalyst system preferably comprises a metallocene complex, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst, and a silica support.
[0078] In particular, single-site catalyst systems (i) a metallocene complex of the following general formula (I): [ka] (In the formula, each X is independently a sigma donor ligand; L is a divalent bridge selected from -R'2C-, -R'2C-CR'2-, -R'2Si-, -R'2Si-SiR'2-, -R'2Ge-, where each R' is independently a hydrogen atom or a C1-C6 heteroatom optionally containing one or more heteroatoms or fluorine atoms from Groups 14-16 of the Periodic Table of the Elements. 20 is a hydrocarbyl group, or optionally two R′ groups can be taken together to form a ring; Each R 1 may be independently the same or different, and are hydrogen, a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group, and optionally two adjacent R 1 The groups may be part of a ring that includes the phenyl carbon to which they are attached; Each R 2 may be independently the same or different, CH-R 8 group, where R 8 is H or linear or branched C 1~6 Alkyl group, C 3~8 Cycloalkyl groups, C 6~10 is an aryl group, R 3 is a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C6-C 20 is an aryl group, R 4 is C(R 9 ) groups, where R 9 is a linear or branched C1 to C6 alkyl group, R 5is hydrogen or an aliphatic C1-C optionally containing one or more heteroatoms from groups 14-16 of the periodic table 20 is a hydrocarbyl group, R 6 is hydrogen or an aliphatic C1-C optionally containing one or more heteroatoms from groups 14-16 of the periodic table 20 is a hydrocarbyl group, or R 5 and R 6 Together, n (n is 0 to 4) R 10 can form a 5-membered saturated carbocyclic ring optionally substituted with a group, Each R 10 are the same or different, C1 to C 20 Hydrocarbyl groups or C1-C groups optionally containing one or more heteroatoms belonging to groups 14-16 of the Periodic Table 20 may be a hydrocarbyl group, R 7 is H, or a linear or branched C1-C6 alkyl group, or one to three R 11 an aryl group or heteroaryl group having 6 to 20 carbon atoms optionally substituted with a group; Each R 11 may be independently the same or different, and are hydrogen, a linear or branched C1 to C6 alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group. (ii) a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst; (iii) a silica support; It is preferred that the compound contains
[0079] The term "sigma donor ligand" is well understood by those of skill in the art, i.e., refers to a group that bonds to a metal via a sigma bond. Thus, the anionic ligand "X" may be independently halogen or selected from the group consisting of R', OR', SiR'3, OSiR'3, OSO2CF3, OCOR', SR', NR'2, and PR'2 groups, where R' is independently hydrogen, linear or branched, cyclic or acyclic, C1-C 20 Alkyl, C2-C 20 Alkenyl, C2-C 20 Alkynyl, C3-C 12 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Aryl alkyl, C7-C 20 Alkylaryl, C8-C 20 Arylalkenyl, where the R' group may optionally contain one or more heteroatoms belonging to groups 14 to 16. In a preferred embodiment, the anionic ligands "X" are the same and are halogens such as Cl, or methyl, or benzyl.
[0080] Preferred monovalent anionic ligands are the halogens, especially chlorine (Cl).
[0081] Preferred metallocene complexes include the following: rac-Dimethylsilanediylbis[2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-(4'-tert-butylphenyl)- 5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-phenyl-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4-(3',5'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-Dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-5-di-tert-butyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride.
[0082] Particularly preferred is rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride.
[0083] The ligands required to form the complexes of the present invention, and thus the catalytic system, can be synthesized by any process, and an organic chemist skilled in the art will be able to devise various synthetic protocols to produce the required ligand materials. For example, WO 2007 / 116034 discloses the necessary chemicals. Synthetic protocols can also be found generally in WO 2002 / 002576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790, and WO 2018 / 122134. In particular, reference is made to WO 2019 / 179959, in which the most preferred catalysts of the present invention are described.
[0084] Cocatalyst To form the active catalytic species, it is usually necessary to use a cocatalyst, as is well known in the art.
[0085] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with the metallocene catalyst complex defined above.
[0086] The aluminoxane cocatalyst may be of formula (II): [ka] In the formula, n is usually 6 to 20, and R has the following meaning.
[0087] Aluminoxanes are produced by partial hydrolysis of organoaluminum compounds, for example compounds of formula AlR3, AlR2Y, Al2R3Y3, where R is, for example, C1-C 10 Alkyl, preferably C1 to C5 alkyl, or C3 to C 10 Cycloalkyl, C7-C 12 Y may be arylalkyl or alkylaryl, and / or phenyl or naphthyl, and Y is hydrogen, halogen, preferably chlorine or bromine, or C1-C10 It may be alkoxy, preferably methoxy or ethoxy.The oxygen-containing aluminoxanes obtained are generally not pure compounds but are mixtures of oligomers of formula (II).
[0088] A preferred aluminoxane is methylaluminoxane (MAO). Because the aluminoxanes used as cocatalysts in the present invention are not pure compounds due to their mode of preparation, the molarity of the aluminoxane solutions below is based on their aluminum content.
[0089] According to the present invention, a boron-containing cocatalyst can be used in place of the aluminoxane cocatalyst, or the aluminoxane cocatalyst can be used in combination with the boron-containing cocatalyst.
[0090] Those skilled in the art will appreciate that when using boron-based cocatalysts, it is common to pre-alkylate the complex by reacting it with an aluminum alkyl compound such as TIBA. This procedure is well known and any suitable aluminum alkyl can be used, for example Al(C1-C6 alkyl)3. Preferred aluminum alkyl compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum and triisooctylaluminum.
[0091] Alternatively, when a borate cocatalyst is used, the metallocene catalyst complex may be an alkylated version thereof, ie, for example, a dimethyl or dibenzyl metallocene catalyst complex may be used.
[0092] Boron-based cocatalysts of interest include those of formula (III): BY3(III) In the formula, Y is the same or different and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkylaryl, arylalkyl, haloalkyl or haloaryl, each having 1 to 10 carbon atoms in the alkyl radical and 6 to 20 carbon atoms in the aryl radical, or fluorine, chlorine, bromine or iodine. Preferred choices are trifluoroborane, triphenylborane, tris(4-fluorophenyl)borane, tris(3,5-difluorophenyl)borane, tris(4-fluoromethylphenyl)borane, tris(2,4,6-trifluorophenyl)borane, tris(pentafluorophenyl)borane, tris(tolyl)borane, tris(3,5-dimethylphenyl)borane, tris(3,5-difluorophenyl)borane, and / or tris(3,4,5-trifluorophenyl)borane.
[0093] Particularly preferred is tris(pentafluorophenyl)borane.
[0094] However, it is preferred to use borate, i.e. compounds containing borate 3+ ions. Such ionic cocatalysts preferably contain non-coordinating anions, such as tetrakis(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amine or aniline derivatives, such as methylammonium, anilinium, dimethylammonium, diethylammonium, N-methylanilinium, diphenylammonium, N,N-dimethylanilinium, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridinium, p-bromo-N,N-dimethylanilinium or p-nitro-N,N-dimethylanilinium.
[0095] Surprisingly, it has been found that certain boron cocatalysts are particularly preferred. Thus, the preferred borates used in the present invention contain trityl ions. Thus, the use of N,N-dimethylammonium-tetrakispentafluorophenylborate and Ph3CB(PhF5)4 and its analogs is particularly preferred.
[0096] Preferred cocatalysts are aluminoxanes, more preferably methylaluminoxane, combinations of aluminoxanes with Al-alkyls, boron or borate cocatalysts, and combinations of aluminoxanes with boron-based cocatalysts.
[0097] The catalyst system of the present invention is used in supported form. The particulate support material used is silica or a mixed oxide such as silica-alumina, in particular silica. The use of a silica support is preferred. The skilled person is aware of the procedures required to support metallocene catalysts.
[0098] In a preferred embodiment, the catalyst system corresponds to ICS3 of WO 2020 / 239598 A1.
[0099] The process preferably further comprises a post-reactor processing step, in which a polymer fraction is separated from the polymerization mixture obtained from the last polymerization stage and blended, optionally in the presence of other components and / or additives, such as further polymeric components as described herein, to obtain a polypropylene composition. The post-reactor processing step is already well established in the art.
[0100] In one embodiment, the present invention relates to said polypropylene composition obtainable, and more preferably obtained, through the process described herein. All preferred embodiments and alternatives given for the polypropylene composition above and below apply mutatis mutandis to the process of the present invention.
[0101] Goods and Use In a third aspect, the present invention relates to an article comprising the polypropylene composition as described above or below, and to the use of the polypropylene composition as described above or below in the manufacture of an article.
[0102] The article is preferably a molded article, such as an injection molded article, or a fiber reinforced composite material. The article may be an automotive article comprising the polypropylene composition described above or below. The article may also be a packaging article, preferably a thin-walled packaging article, such as a plastic cup, pail, small container including lid, for example intended for food packaging, comprising a polypropylene composition as described above or below.
[0103] In one embodiment, the article composition may include fibers, such as glass or carbon fibers, and when fibers are present in the article composition, the amount of fibers ranges from 5 to 40 weight percent of the article composition.
[0104] In another embodiment, the composition of the article may include a mineral filler, such as talc or mica. When a mineral filler is present in the composition of the article, the amount of the filler ranges from 5 to 40% by weight of the composition of the article. EXAMPLES
[0105] The following examples are included to demonstrate certain aspects and embodiments of the claimed invention. However, it should be understood by those of ordinary skill in the art that the following descriptions are merely illustrative and should not be construed as limiting the invention in any way.
[0106] 1. Determination method MFR2 (230°C) was measured according to ISO 1133 at 230°C and a load of 2.16 kg.
[0107] CRYSTEX Determination of the crystalline and soluble fractions and their respective characteristics (IV and ethylene content) The crystalline fraction (CF) and soluble fraction (SF) of the polypropylene (PP) compositions, as well as the comonomer content and intrinsic viscosity of each fraction, were analyzed using a CRYSTEX instrument from Polymer Char (Valencia, Spain). Details of the technique and method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer and Markus Gahleitner (2020), Rapid characterization of high-impact ethylene-propylene copolymer composition by crystallization extraction separation: comparability to standard separation methods, International Journal of Polymer Analysis and Characterization, 25:8, 581-596). Crystalline and amorphous fractions are separated by temperature cycling of dissolution at 160° C., crystallization at 40° C., and redissolution in 1,2,4-trichlorobenzene at 160° C. Quantification of SF and CF as well as determination of ethylene content (C2) are performed by an integrated infrared detector (IR4), and determination of intrinsic viscosity (iV) is performed using an on-line two-capillary viscometer. The IR4 detector detects two distinct bands (CH stretching vibration (approximately 2960 cm)) that are useful for determining the concentration of ethylene-propylene copolymers and the ethylene content in ethylene-propylene copolymers. -1 ) and CH stretching vibration (2700-3000cm -1 The IR4 detector is a multi-wavelength detector that measures the IR absorbance of ethylene in the range of known ethylene content from 2% to 69% by weight ( 13 A series of eight EP copolymers with different concentrations ranging from 2 to 13 mg / ml are used for calibration, each with a different ethylene content (determined by C-NMR). In order to simultaneously encounter both the concentration and ethylene content features for the various polymer concentrations expected during the Crystex analysis, the following calibration equation was applied: Conc=a+b×Abs(CH)+c×(Abs(CH)) 2 +d×Abs(CH3)+e×(Abs(CH3) 2 +f×Abs(CH)×Abs(CH3) (Formula 1) CH3 / 1000C=a+b×Abs(CH)+c×Abs(CH3)+d×(Abs(CH3) / Abs(CH))+e×(Abs(CH3) / Abs(CH)) 2 (Formula 2)
[0108] Constants a through e in Equation 1 and constants a through f in Equation 2 were determined using least squares regression analysis. CH3 / 1000C is converted to ethylene content (wt%) using the following relationship: Weight % (ethylene in EP copolymer) = 100-CH3 / 1000TC x 0.3 (Equation 3)
[0109] The amounts of soluble fraction (SF) and crystalline fraction (CF) are related by XS calibration to the amount of "cold xylene soluble" (XCS) and the respective cold xylene insoluble (XCI) fractions, determined according to standard gravimetric methods according to ISO 16152. The XS calibration is achieved by testing various EP copolymers with XS contents ranging from 2 to 31 wt. %. The determined XS calibration is linear. Weight%XS=1.01×weight% (Formula 4) The intrinsic viscosity (iV) of the parent EP copolymer and its soluble and crystalline fractions are determined using an online two-capillary viscometer and related to the corresponding iV determined in decalin by standard method according to ISO 1628-3. Calibration is achieved using various EP PP copolymers with iV=2-4 dL / g. The determined calibration curve is linear. iV(dL / g)=a×Vsp / c (Formula 5)
[0110] The samples to be analyzed are weighed out at a concentration of 10 mg / ml to 20 mg / ml. To avoid possible gels and / or the injection of polymers that are not soluble in TCB at 160° C., such as PET and PA, the weighed samples are packed into a stainless steel mesh of MW 0.077 / D 0.05 mm. After autofilling the vials with 1,2,4-TCB containing 250 mg / l 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the samples are dissolved at 160° C. with constant stirring at 400 rpm until completely dissolved, typically 60 min. The polymer solution is covered with a N2 atmosphere during dissolution to avoid sample degradation. A defined volume of sample solution is injected into a column filled with an inert carrier, where the sample undergoes crystallization and separation of the soluble fraction from the crystalline portion. This process is repeated twice. During the first injection, the entire sample is measured at high temperature to determine the iV [dl / g] and C2 [wt%] of the PP composition. During the second injection, a crystallization cycle is used to measure the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) (wt% SF, wt% C2, iV).
[0111] The cold xylene soluble fraction (XCS, wt%) was determined at 25 °C according to ISO 16152 (1st edition, 2005-07-01).
[0112] The intrinsic viscosity was determined according to DIN ISO 1628 / 1 (October 1999) (in Decalin at 135° C.).
[0113] Determination of Microstructure by NMR Spectroscopy - Ethylene Content in HECO Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers. 13 C{ 1 H}NMR spectrum. 1 H and 13 All spectra were recorded in solution using a Bruker Advance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz for C, respectively. 13A C optimized 10 mm extended temperature probe head was used and all air pressures were recorded using nitrogen gas. Approximately 200 mg of material was dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) along with chromium-(III)-acetylacetonate (Cr(acac)3) to obtain a 65 mM solution of the relaxant in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475). After initial sample preparation in a heat block to ensure a homogenous solution, the NMR tube was further heated in a rotating oven for at least 1 hour. Once inserted in the magnet, the tube was spun at 10 Hz. This setup was chosen primarily due to the high resolution and quantitativeness required for accurate ethylene content quantification. Standard single-pulse excitation was used without NOE using an optimized tip angle, 1 second recycle delay, and a bilevel WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D., Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transients were acquired per spectrum. quantitative 13 C{ 1 H}NMR spectra were processed, integrated, and relevant quantitative properties were determined from the integrals using a dedicated computer program. All chemical shifts were indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This approach allowed for equal reference even when this structural unit was not present. Characteristic signals corresponding to the incorporation of ethylene were observed (Cheng, HN, Macromolecules 17 (1984), 1950). Characteristic signals corresponding to 2,1erythro regio-defects were observed (as described in L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100(4), 1253; Cheng, HN, Macromolecules 1984, 17, 1950; and WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157), necessitating correction for the influence of regio-defects on the determined properties. No characteristic signals corresponding to other types of regio-defects were observed. Using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157), 13 C{ 1 The comonomer fraction was quantified by integration of multiple signals over the entire spectral region of the {H} spectrum. This method was chosen for its robust nature and ability to take into account the presence of regio-defects, if necessary. The integration region was slightly adjusted to increase applicability over the full range of comonomer contents encountered. For systems where only isolated ethylene in the PPEPP sequence was observed, we modified the method of Wang et al. to reduce the influence of nonzero integrals of sites known to be absent. This approach reduces the overestimation of ethylene content in such systems and reduces the number of sites used to determine absolute ethylene content. E=0.5(Sββ+Sβγ+Sβδ+0.5(Sαβ+Sαγ)) This was achieved by reducing With this set of sites, the corresponding integral equation is given by, using the same notation as used in Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157): E = 0.5(I H +I G +0.5(I C +I D )) The formula used for absolute propylene content was not modified. The mole percent of comonomer incorporation was calculated from the mole fractions. E[mol%]=100×fE The weight percent of comonomer incorporation was calculated from the mole fraction. E[weight%]=100×(fE×28.06) / ((fE×28.06)+((1-fE)×42.08)) Comonomer sequence distributions at the triad level were determined using the analytical method of Kakugo et al. (Kakugo, M., Naito, Y., Mizunuma, K., Miyatake, T. Macromolecules 15 (1982) 1150.) This method was chosen because of its robust nature and the integral region that was slightly adjusted to enhance applicability to a wider range of comonomer contents.
[0114] Flexural modulus is measured according to EN ISO 1873-2 for injection molded 80 x 10 x 4 mm 3 The deformation was determined by the three-point bending method according to ISO 178 on injection-molded test specimens.
[0115] Charpy notched impact strength according to EN ISO 1873-2 for injection molded 80 x 10 x 4 mm 3 The thermal expansion coefficient was determined according to ISO 179 / 1eA at 23°C on injection moulded specimens.
[0116] DSC analysis, melting temperature (Tm) and crystallization temperature (Tc) were measured on 5-7 mg samples by TA Instrument Q2000 Differential Scanning Calorimetry (DSC). DSC is performed according to ISO 11357 / Part 3 / Method C2 in a heat / cool / heat cycle at a scan rate of 10°C / min over a temperature range of -30°C to +225°C. Crystallization temperature (Tc) and crystallization enthalpy (Hc) are determined from the cooling step, and melting temperature (Tm) and melting enthalpy (Hm) are determined from the second heating step.
[0117] The VOC and FOG values were determined according to VDA 278 (Thermal Desorption Analysis of Organic Emissions for the Characterization of Non-Metallic Materials for Automobiles, October 2011, VDA Verband der Automobilindustrie) after sample preparation of injection-molded plaques according to EN ISO 19069-2:2016. The plaques were packed into aluminum composite foils immediately after production and the foils were sealed. According to VDA 278 (October 2011), the VOC value is defined as the "sum of readily and moderately volatile substances". It is calculated as the toluene equivalent. The method described in this recommendation allows the determination of n-pentacosane (C 25 ) allows the determination and analysis of substances with a boiling / elution range up to 1000 nm. The FOG value is defined as the sum of the less volatile substances eluted from the retention time of n-tetradecane (including this). It is calculated as the hexadecane equivalent. 14 " ~ "C 32 " boiling point range substances are determined and analyzed.
[0118] 2. Example The catalyst used in the polymerization process of all examples was anti-dimethylsilanediyl[2-methyl-4,8-di(3,5-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, disclosed as MC-2 in WO 2019 / 179959A1. The supported metallocene catalyst was prepared similarly to IE2 in WO 2019 / 179959A1.
[0119] The heterophasic propylene copolymers of inventive examples IE1, IE2 and IE3, as well as comparative example CE1, were prepared in a Borstar PP pilot plant with a continuous process including one prepolymerization reactor, one loop reactor and two gas phase reactors. The reaction conditions are summarized in Table 1.
[0120] [Table 1]
[0121] To prepare the polypropylene compositions of inventive examples IE1, IE2 and IE3, and comparative example CE1, the heterophasic propylene copolymers listed in Table 1 above were compounded with 1500 ppm of Irganox B215 (a synergistic 2:1 blend of antioxidants Irgafos 168 (tris(2,4-di-tert-butylphenyl)phosphite, CAS number: 31570-04-4) and Irganox 1010 (pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate], CAS number: 6683-19-8), commercially available from BASF SE), and 500 ppm of calcium stearate (CAS number: 1592-23-0, commercially available from Baerlocher under the trade name CEASIT-1). Comparative Example CE2 is the heterophasic polypropylene composition BJ400HP (commercially available from Borealis AG). The properties of the polypropylene compositions of inventive examples IE1 and IE2, and comparative examples CE1 and CE2 are listed in Table 2 below.
[0122] [Table 2] nm = not measured (VOG+FOG for CE1 is estimated to be within the range of IE1 / IE2)
[0123] The polypropylene compositions of the invention examples IE1, IE2 and IE3 exhibit higher MFR2 and a better balance of flexural modulus and Charpy NIS compared to the comparative example CE1, as shown in the formula in the last two rows of Table 2. The polypropylene composition of Comparative Example CE2 shows the problems of high melt flow heterophasic propylene copolymers with Ziegler-Natta catalysts. The high MFR2 of CE2 is accompanied by high VOC and FOG values. CE2 shows a higher flexural modulus but a poorer balance of Charpy NIS and melt flow rate MFR2 compared to IE1 and IE2, as shown in the formulas in the last two rows of Table 2.
Claims
1. A polypropylene composition comprising a crystalline fraction (CF) and a soluble fraction (SF), both determined according to CRYSTEX QC analysis, The soluble fraction (SF) is present in the polypropylene composition in an amount in the range of 10.0 to 35.0 wt%, preferably in the range of 11.0 to 32.5 wt%, more preferably in the range of 12.0 to 30.0 wt%, based on the total weight of the polypropylene composition; having an intrinsic viscosity (iV(SF)) of at least 2.0 dl / g, preferably in the range of 2.3 to 4.5 dl / g, more preferably in the range of 2.5 to 4.3 dl / g; quantitative 13 having an ethylene content (C2(SF)) in the range of 14.0 to 29.0% by weight, preferably in the range of 17.0 to 26.0% by weight, more preferably in the range of 19.0 to 24.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; the ratio of the intrinsic viscosity of the soluble fraction to the intrinsic viscosity of the crystalline fraction (iV(SF) / (iV(CF)) is in the range of 2.5 to 5.0, preferably in the range of 2.6 to 4.8; The polypropylene composition has a melt flow rate MFR in the range of 105 to 320 g / 10 min, preferably in the range of 107 to 300 g / 10 min, more preferably in the range of 110 to 280 g / 10 min. 2 (230° C., 2.16 kg, ISO 1133).
2. The crystalline fraction (CF) is present in the polypropylene composition in an amount in the range of 65.0 to 90.0 wt%, preferably in the range of 67.5 to 89.0 wt%, more preferably in the range of 70.0 to 88.0 wt%, based on the total weight of the polypropylene composition; having an intrinsic viscosity (iV(CF)) of 1.2 dl / g or less, preferably in the range of 0.4 to 1.1 dl / g; quantitative 13 2. The polypropylene composition according to claim 1, having an ethylene content (C2(CF)) less than or equal to 1.0 wt.-%, preferably in the range of 0 to 0.9 wt.-%, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy.
3. 3. The polypropylene composition according to claim 1 or 2, wherein said polypropylene composition comprises a heterophasic propylene copolymer comprising a semi-crystalline matrix phase and an elastomeric phase dispersed in said matrix phase, said polypropylene composition preferably comprising said heterophasic propylene copolymer in an amount in the range of 93.0 wt.% to 100 wt.%, preferably in the range of 95.0 wt.% to 99.9 wt.%, more preferably in the range of 96.5 wt.% to 99.8 wt.%.
4. The polypropylene composition comprises a xylene cold soluble (XCS) fraction at 25° C. in an amount ranging from 8.0 to 32.0 wt.%, preferably ranging from 9.0 to 30.0 wt.%, more preferably ranging from 10.0 to 28.0 wt.%, based on the total weight of the polypropylene composition, the XCS fraction preferably comprising: an intrinsic viscosity (iV(XCS)) of at least 2.2 dl / g, preferably in the range of 2.3 to 4.6 dl / g, more preferably in the range of 2.5 to 4.4 dl / g; and quantitative 13 an ethylene content (C2(XCS)) in the range of 15.0 to 30.0% by weight, preferably in the range of 18.0 to 27.0% by weight, more preferably in the range of 20.0 to 25.0% by weight, relative to the total weight of the soluble fraction (SF), determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; The polypropylene composition according to any one of claims 1 to 3, having the following characteristics:
5. Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 5. The polypropylene composition according to any one of claims 1 to 4, having a flexural modulus (FM), determined according to ISO 178 for tensile strength (Tg) of 1000 to 1500 MPa in the range of 800 MPa to 1500 MPa, preferably in the range of 850 MPa to 1450 MPa.
6. The polypropylene composition according to any one of claims 1 to 5, having a flexural modulus (FM) with respect to the amount of the soluble fraction (SF) that satisfies the following inequality: FM [MPa]>1550 [MPa]-33.4 [MPa / wt%]·amount (SF) [wt%], preferably FM [MPa]>1575 [MPa]-33.4 [MPa / wt%]·amount (SF) [wt%], more preferably FM [MPa]>1600 [MPa]-33.4 [MPa / wt%]·amount (SF) [wt%], most preferably FM [MPa]>1625 [MPa] - 33.4 [MPa / wt%]・Amount (SF) [wt%] (In the formula, F [MPa] is the flexural modulus of the polypropylene composition, and is expressed in MPa; The amount (SF) [wt%] is the amount of the soluble fraction (SF) in the polypropylene composition, and the unit is weight%.
7. quantitative 13 a total ethylene (C2) content in the range of 2.0 to 5.5 wt.%, preferably in the range of 2.5 to 5.0 wt.%, based on the total weight of the polypropylene composition, determined by FT-IR spectroscopy calibrated by C-NMR spectroscopy; A melting temperature (Tm) in the range of 150 to 162° C., preferably in the range of 152 to 160° C., determined by DSC according to ISO 3146 (Part 3, Method C2); A crystallization temperature (Tc) in the range of 110 to 130° C., preferably in the range of 115 to 125° C., determined by DSC according to ISO 3146 (Part 3, Method C2); Injection-molded test specimens (80 x 10 x 4 mm) manufactured according to EN ISO 1873-2 3 ) 2.5 to 15.0 kJ / m2, determined according to ISO 179 / eA 2 in the range of 3.0 to 12.0 kJ / m 2 Charpy notched impact strength at 23°C in the range of a content of volatile organic compounds (VOCs), determined according to VDA 278, of less than or equal to 50 μg / g, preferably less than or equal to 40 μg / g, more preferably less than or equal to 35 μg / g, and / or FOG content, determined according to VDA 278, of less than or equal to 300 μg / g, preferably less than or equal to 250 μg / g, more preferably less than or equal to 225 μg / g The polypropylene composition according to any one of claims 1 to 6, having one or more, preferably all, of the following characteristics:
8. a) polymerizing propylene in a first polymerization reactor in the presence of a single-site catalyst system to produce a first propylene polymer fraction; b) transferring a polymerization mixture comprising the single-site catalyst system and the first propylene polymer fraction from the first polymerization reactor to a second polymerization reactor; c) polymerizing propylene in the presence of the single-site catalyst system in the second polymerization reactor to produce a second propylene polymer fraction; d) transferring a polymerization mixture comprising the single-site catalyst system, the first propylene polymer fraction, and the second propylene polymer fraction from the second polymerization reactor to a third polymerization reactor; e) polymerizing propylene and ethylene in the presence of a single-site catalyst system in said third polymerization reactor to produce a third propylene-ethylene copolymer fraction; f) withdrawing a polymerization mixture from the third polymerization reactor comprising the single-site catalyst system, the first propylene polymer fraction, the second propylene polymer fraction, and the third propylene-ethylene copolymer fraction; g) obtaining a polymer composition comprising said first propylene polymer fraction, said second propylene polymer fraction, and said third propylene-ethylene copolymer fraction; A method for producing the polypropylene composition according to any one of claims 1 to 7, comprising:
9. The single-site catalyst system comprises: (i) a metallocene complex of the following general formula (I): 【Chemistry 1】 (In the formula, each X is independently a sigma donor ligand; L is -R' 2 C-, -R' 2 C-CR' 2 -, -R' 2 Si-, -R' 2 Si-SiR' 2 -, -R' 2 Ge-, where each R' is independently a hydrogen atom or a C optionally containing one or more heteroatoms or fluorine atoms from Groups 14-16 of the Periodic Table of the Elements. 1 ~C 20 is a hydrocarbyl group, or optionally two R′ groups can be taken together to form a ring; Each R 1 may be independently the same or different, and are hydrogen, linear or branched C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group, and optionally two adjacent R 1 The groups may be part of a ring that includes the phenyl carbon to which they are attached; Each R 2 may be independently the same or different, CH 2 -R 8 group, where R 8 is H or a linear or branched C 1~6 Alkyl group, C 3~8 Cycloalkyl group, C 6~10 is an aryl group, R 3 is a linear or branched chain C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6 ~C 20 is an aryl group, R 4 is C(R 9 ) 3 group, where R 9 is a linear or branched chain C 1 ~C 6 is an alkyl group, R 5 is hydrogen or an aliphatic C optionally containing one or more heteroatoms from groups 14 to 16 of the periodic table of the elements; 1 ~C 20 is a hydrocarbyl group, R 6 is hydrogen or an aliphatic C optionally containing one or more heteroatoms from groups 14 to 16 of the periodic table of the elements; 1 ~C 20 is a hydrocarbyl group, or R 5 and R 6 together, n (n is 0 to 4) R 10 can form a 5-membered saturated carbocyclic ring optionally substituted with a group, Each R 10 are the same or different, C 1 ~C 20 Hydrocarbyl groups or C optionally containing one or more heteroatoms belonging to groups 14 to 16 of the Periodic Table 1 ~C 20 may be a hydrocarbyl group, R 7 is H or linear or branched C 1 ~C 6 An alkyl group or one to three R 11 an aryl or heteroaryl group having 6 to 20 carbon atoms, optionally substituted with a group; Each R 11 may be independently the same or different, and are hydrogen, linear or branched C 1 ~C 6 Alkyl group, C 7~20 Aryl alkyl, C 7~20 Alkylaryl group or C 6~20 an aryl group or an OY group, where Y is C 1~10 is a hydrocarbyl group. (ii) a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst; and (iii) a silica support; The method of claim 8 , comprising:
10. 10. The process according to claim 8 or 9, wherein the first propylene polymer fraction and / or the second propylene polymer fraction is a propylene homopolymer fraction.
11. The first propylene polymer fraction has a melt flow rate MFR in the range of 1000 to 15000 g / 10 min, preferably in the range of 1100 to 13500 g / 10 min, more preferably in the range of 1250 to 11500 g / 10 min. 2 (230°C, 2.16 kg, ISO 1133).
12. The first propylene polymer fraction and the second propylene polymer fraction combined have a melt flow rate MFR of at least 1000 g / 10 min, preferably in the range of 1200 to 9000 g / 10 min, more preferably in the range of 1500 to 8000 g / 10 min. 2 (230°C, 2.16 kg, ISO 1133).
13. 13. The process according to any one of claims 8 to 12, wherein the first propylene polymer fraction and the second propylene polymer fraction combined have a xylene cold soluble (XCS) fraction at 25°C in an amount of not more than 2.0 wt%, preferably in the range of 0.1 to 1.5 wt%, based on the total weight of the first propylene polymer fraction and the second propylene polymer fraction combined.
14. An article comprising the polypropylene composition according to any one of claims 1 to 13.
15. Use of the polypropylene composition according to any one of claims 1 to 13 as a formulation base for increasing the melt flow rate of a polymer composition.
Citation Information
Patent Citations
Heterophasic polypropylene with high flowability and excellent low temperature impact properties
EP2075284A1
Propylene-based composition with improved appearance and excellent flow
JP2017502148A
Olefin polymerization catalysts
JP2021518462A
Heterophasic polypropylene composition having improved mechanical properties
EP3812404A1
High flow heterophasic polyolefin composition having improved stiffness / impact balance
WO2017148970A1