Process for preparing polybutene compositions having elevated crystallization temperatures

By blending polybutene-1 with alkanoylhydrazines, the crystallization temperature is elevated, achieving faster crystallization and improved mechanical properties, suitable for high-speed extrusion molding and water pipe manufacturing.

JP2024542582AActive Publication Date: 2024-11-15BASELL POLIOLEFINE ITALIA SRL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024531353
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-21
Filing Date
2022-12-12
Publication Date
2024-11-15
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing methods struggle to significantly increase the crystallization temperature of polybutene-1 compositions, which is crucial for improving mechanical properties and processing speed in applications like water pipe manufacturing.

Method used

Incorporating specific alkanoylhydrazines into polybutene-1 compositions at precise weight percentages during the blending process, achieving a crystallization temperature above 60°C and a short crystallization time, while maintaining the polymer in a molten state.

Benefits of technology

The method results in polybutene-1 compositions with enhanced crystallization temperatures, reduced crystallization times, and improved mechanical properties, making them suitable for high-speed extrusion molding and applications such as water pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542582000001
    Figure 2024542582000001
  • Figure 2024542582000002
    Figure 2024542582000002
  • Figure 2024542582000003
    Figure 2024542582000003
Patent Text Reader

Abstract

A method for preparing a polybutene-1 composition with an elevated crystallization temperature, comprising blending as components A) 99.5-99.9% by weight, relative to the total weight of A)+B), of a butene-1 homopolymer, said butene-1 polymer being brought into or maintained in the molten state during the blending step, with B) 0.1-0.5% by weight, relative to the total weight of A)+B), of one or more alkanoyl hydrazines of specific formulas, the polybutene-1 composition thus obtained having a crystallization temperature T satisfying the following relationship: c C has. [0010] JPEG2024542582000029.jpg4092 Here, T c A is the crystallization temperature of butene-1 polymer A).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to methods for preparing polybutene-1 compositions having elevated crystallization temperatures and to methods for preparing the resulting compositions. [Background technology]

[0002] It is generally known that the crystallization temperature of polyolefins can be increased by adding nucleating agents. These nucleating agents are usually foreign bodies (heterogeneous nucleation) that promote the crystallization of the polymer from the melt. As a result of the nucleation effect, in addition to the increase in the crystallization temperature, other valuable properties are improved, especially the optical and mechanical properties.

[0003] Therefore, there is a continuing effort in the art to discover nucleating agents that can significantly increase the crystallization temperature of polyolefins.

[0004] Most valuable nucleating agents for polybutene-1 are capable of further increasing the crystallization temperature of already highly crystalline polybutene-1 materials, so that even in the absence of crystallization, relatively high crystallization temperatures should be obtainable, and the resulting improved mechanical properties are highly desirable for use in the water pipe sector.

[0005] Furthermore, in the pipe forming step, which is generally performed by extrusion molding, a sufficiently short crystallization time is necessary in order to increase the speed of extrusion molding.

[0006] More generally, in many polymer processing processes, short crystallization times are advantageous in order to achieve high throughput rates.

[0007] Applicants have discovered that the above effects can be successfully achieved by nucleating polybutene-1 with a specific class of alkanoyl hydrazines. Summary of the Invention

[0008] Thus, the present disclosure provides a process for the preparation of a polybutene-1 composition with increased crystallization temperature Tc, comprising: A) 99.5 to 99.9% by weight, preferably 99.6 to 99.85% by weight, based on the total weight of A)+B), of a butene-1 polymer chosen from butene-1 homopolymers, butene-1 copolymers and mixtures thereof, said butene-1 polymer being brought to or maintained in the molten state during the blending step; B) blending 0.1-0.5% by weight, preferably 0.15-0.4% by weight, based on the total weight of A)+B), of one or more alkanoyl hydrazines of formula (I), The polybutene-1 composition thus obtained has a crystallization temperature T c C having

number

[0009] The use of said hydrazine derivative compounds as stabilizers in polyolefins, including butene-1 polymers, is known, for example, from US Pat. No. 3,773,722 and US Pat. No. 4,812,500.

[0010] However, it has not been previously known that such compounds have a nucleating effect in crystalline butene-1 polymers, the crystallization temperature of which is sufficiently high.

[0011] The process of the invention therefore also involves the additional use of alkanoyl hydrazine B) in the abovementioned proportions in order to increase the crystallization temperature of component A).

[0012] The present disclosure also provides A) 99.5 to 99.9% by weight, preferably 99.6 to 99.85% by weight, based on the total weight of A)+B), of a butene-1 polymer chosen from butene-1 homopolymers, butene-1 copolymers and mixtures thereof, said butene-1 polymer having said crystallization temperature TcA greater than or equal to 60° C., preferably greater than or equal to 65° C.; B) 0.1 to 0.5% by weight, preferably 0.15 to 0.4% by weight, based on the total weight of A)+B), of one or more alkanoyl hydrazines of formula (I) above, Said composition provides a polybutene-1 composition having said crystallization temperature TcC satisfying the following relationship:

number

[0013] The polybutene-1 composition of the present invention preferably has a crystallization temperature TcC that satisfies the following relationship:

number

number

[0014] A further advantage of component B) is the short crystallization time of the polybutene-1 compositions of the invention.

[0015] Preferably, it has a crystallization half-life at 95° C. of 50 to 150 seconds, in particular 65 to 130 seconds.

[0016] This determination is made by DSC, which first melts the sample, then rapidly cools it to the desired temperature (in this case 95°C), and measures the heat flow due to the release of heat from crystallization. The integral of the heat transfer is recorded as a function of time until crystallization is complete, i.e., when heat transfer stops.

[0017] The crystallization half time is the time for the heat transfer integral to reach half of its final value. Furthermore, the polybutene-1 composition of the present invention preferably has at least one of the following additional characteristics: -T c C The value must be 85℃ or higher, especially 85℃~98℃. The tensile modulus, measured at 23 °C by DMTA analysis according to ISO 6721-4:2019 for a compression molded plaque of 1 mm thickness, is 500 to 800 MPa, more preferably 550 to 750 MPa - Charpy impact resistance values ​​between 3 and 20 kJ / m at 23°C, measured according to ISO 179-1:2010 1eA 2 , especially 5 to 15 kJ / m 2 To be - Charpy impact resistance values ​​at 0°C, measured according to ISO 179-1:2010 1eA, are between 1 and 10 kJ / m 2, especially 1 to 5 kJ / m 2 To be

[0018] - Charpy impact resistance values ​​at -23°C, measured according to ISO 179-1:2010 1eA, are between 1 and 8 kJ / m 2 , especially 1 to 3 kJ / m 2 To be

[0019] Butene-1 polymers When component A) consists of or comprises one or more butene-1 copolymers, such copolymers may comprise one or more comonomers, preferably selected from ethylene, propylene and CH2=CHR alpha-olefins, Wherein R is a C3-C8 alkyl radical, in particular pentene-1,4-methyl-pentene-1, hexene-1 and octene-1.

[0020] Ethylene, propylene and hexene-1 are preferred.

[0021] From the above definition, it is apparent that the term "copolymer" includes polymers containing more than one comonomer.

[0022] The butene-1 polymers component A) are known in the art and commercially available, as shown in the examples.

[0023] The butene-1 polymer component A) is preferably a linear polymer with high isotacticity.

[0024] In particular, the butene-1 polymer component A) operates at 150.91 MHz 13 It has an isotacticity of 90-99%, more preferably 93-99%, and most preferably 95-99%, as measured by C-NMR as mmmm pentads / total pentads, or as the amount by weight of xylene insolubles at 0° C.

[0025] The butene-1 polymer component A) preferably has an MI2 value of 0.05 to 50 g / 10 min, more preferably 0.1 to 10 g / 10 min, the melt flow index MI being measured according to ISO 1133-1:2011 at 190° C. under a load of 2.16 kg.

[0026] Butene-1 polymer component A) MI 10 The value is preferably 1 to 100 g / 10 min, more preferably 2 to 50 g / 10 min, where MI 10 is the melt flow index MI at 190° C. under a load of 10 kg, measured according to ISO 1133-1:2011.

[0027] Butene-1 polymer component A) MI 10 The / MI2 ratio is preferably 20-40, and more preferably 25-35.

[0028] In one embodiment, the butene-1 polymer component A) may be selected from homopolymers.

[0029] In a further embodiment, the butene-1 polymer A) may be chosen from copolymers having a comonomer content, in particular a copolymerized ethylene content, of 0.5 to 10 mol %, preferably 0.7 to 9 mol %.

[0030] In a further embodiment, the butene-1 polymer component A) may be a butene-1 copolymer composition comprising: A1) butene-1 homopolymers or copolymers of butene-1 with at least one comonomer selected from ethylene, propylene, the CH2=CHR olefins defined above and mixtures thereof, with a copolymerized comonomer content of up to 2 mol %. A2) Copolymers of butene-1 with at least one comonomer selected from ethylene, propylene, the CH2=CHR olefins defined above and mixtures thereof, having a copolymerized comonomer content of 3 to 25 mol %.

[0031] Said composition has a total copolymerizable comonomer content of 0.5 to 18 mol %, preferably 0.7 to 15 mol %, relative to the sum of A1)+A2).

[0032] The relative amounts of A1) and A2) range from 10% to 40% by weight, in particular 15% to 35% by weight of A1) and 90% to 60% by weight, in particular 85% to 65% by weight of A2), based on the sum of A1)+A2).

[0033] In one embodiment, the butene-1 polymer component A) may have at least one of the following additional features: -The upper limit of crystallization temperature is 80℃ The flexural modulus value, measured 10 days after molding according to the standard ISO 178:2010, is between 100 and 800 MPa, more preferably between 250 and 600 MPa, most preferably between 300 and 600 MPa. the molecular weight distribution Mw / Mn is greater than or equal to 4, preferably greater than or equal to 5, the upper limit being in all cases preferably 10, Mw being the weight-average molar mass as measured by gel permeation chromatography and Mn being the number-average molar mass as measured by gel permeation chromatography; The melting point TmII, measured by DSC (differential scanning calorimetry) in the second heating run at a scanning rate of -10°C / min, is not more than 125°C, preferably not more than 120°C, the lower limit being preferably 75°C in all cases. - the content of fractions soluble in xylene at 0° C., based on the total weight of A), is not more than 15% by weight, more preferably not more than 10% by weight, the lower limit being preferably 0.5% by weight in all cases; -X-ray crystallinity is 25-65%

[0034] Optionally, the butene-1 polymer component A) may have at least one of the following further additional features: Intrinsic viscosity (IV), measured in tetrahydronaphthalene (THN) at -135°C, not more than 5 dl / g, preferably not more than 3 dl / g, the lower limit being preferably 0.4 dl / g in all cases. Mw is 100,000 g / mol or more, in particular 100,000 to 650,000 g / mol -The melting point TmI measured by DSC with a scanning rate of 10℃ / min is 95℃~135℃ -Density is 885-925kg / m 3 , preferably 900 to 920 kg / m 3 , especially 912-920kg / m 3 To be

[0035] Said homopolymers and copolymers can be obtained by low pressure Ziegler-Natta polymerization of butene-1 (with any comonomer) using a catalyst based on halogenated compounds of titanium (especially TiCl4) supported on TiCl3 or magnesium chloride and a cocatalyst (especially alkyl compounds of aluminum). Electron donor compounds can be added to said catalyst components to adjust the polymer properties such as molecular weight and isotropic regularity. Examples of said electron donor compounds are esters of carboxylic acids and alkylalkoxysilanes.

[0036] In particular, the butene-1 polymer component A) can be prepared by polymerizing the monomers in the presence of a stereospecific catalyst comprising a solid component comprising (i) a Ti compound supported on MgCl2 and an internal electron donor compound, (ii) an alkylaluminum compound, and, optionally, (iii) an external electron donor compound.

[0037] As a support, magnesium dichloride in active form is preferably used. It is widely known from the patent literature that magnesium dichloride in active form is particularly suitable as a support for Ziegler-Natta catalysts. In particular, US Pat. No. 4,298,718 and US Pat. No. 4,495,338 were the first to describe the use of these compounds in Ziegler-Natta catalysis. From these patents it is known that magnesium dihalides in active form, used as supports or co-supports in components of catalysts for the polymerization of olefins, are characterized by their X-ray spectrum. In this X-ray spectrum, the intensity of the non-active halides is reduced and replaced by a halo, the maximum intensity of which is shifted to lower angles compared to the intensity of the more intense lines.

[0038] The titanium compounds used in the catalyst component (i) are preferably TiCl4 and TiCl3 and have the formula Ti(OR) n-y X y Titanohaloalkoxides represented by the formula (wherein n is the valence of titanium, X is a halogen, preferably chlorine, and y is a number ranging from 1 to n) can also be used.

[0039] The internal electron donor compound is preferably selected from esters, more preferably from alkyl, cycloalkyl or aryl esters of monocarboxylic acids (e.g., benzoic acid) or polycarboxylic acids (e.g., phthalic acid, succinic acid, glutaric acid), the alkyl, cycloalkyl or aryl having 1 to 18 carbon atoms. Examples of the electron donor compound include diisobutyl phthalate, diethyl phthalate, dihexyl phthalate, diethyl or diisobutyl 3,3-dimethylglutarate. Usually, the molar ratio of the internal electron donor compound to MgCl2 is 0.01 to 1, preferably 0.05 to 0.5.

[0040] The alkyl-Al compound (ii) is preferably selected from among the trialkylaluminum compounds, such as, for example, triethylaluminum, triisobutylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, etc. It is also possible to use mixtures of the trialkylaluminum compounds with alkylaluminum halides, alkylaluminum hydrides or alkylaluminum sesquichlorides, such as AlEt2Cl and Al2Et3Cl3.

[0041] The external electron donor compound (iii) is R a 1 R b 2 Si(OR 3 ) c (In the formula, a and b are integers of 0 to 2, c is an integer of 1 to 3, (a+b+c) is 4, and R 1 , R 2 and R 3 is an alkyl, cycloalkyl or aryl having 1 to 18 carbon atoms which may contain a heteroatom.) is preferably selected from silicon compounds represented by the formula: 2 is a branched alkyl or cycloalkyl group which may contain heteroatoms; R 3 is methyl. Examples of such preferred silicon compounds are cyclohexyltrimethoxysilane, t-butyltrimethoxysilane, diisopropyltrimethoxysilane and thexyltrimethoxysilane. Particularly preferably, hexyltrimethoxysilane is used.

[0042] The external electron donor compound (iii) is used in such an amount that the molar ratio of the organoaluminum compound to the external electron donor compound (iii) is 0.1 to 500, preferably 1 to 300, and more preferably 3.

[0043] To make the catalyst particularly suitable for the polymerization step, the catalyst can be prepolymerized in a prepolymerization step. The prepolymerization may be carried out in liquid (slurry or solution) or gas phase, usually at a temperature below 100° C., preferably 20-70° C. The prepolymerization step is carried out with a small amount of monomer, in an amount of 0.5-2000 g, preferably 5-500 g, more preferably 10-100 g per gram of solid catalyst component, for the time required to obtain a polymer.

[0044] Alternatively, the butene-1 polymer component A) can be obtained by polymerizing the monomers in the presence of a metallocene catalyst system obtained by contacting them with: - stereorigid metallocene compounds, a compound capable of forming an aluminoxane or an alkylmetallocene cation, and optionally -Organoaluminum compounds.

[0045] The polymerization process can be carried out with said catalysts by operating in the liquid phase, optionally in the presence of an inert hydrocarbon solvent, or in the gas phase using fluidized bed or mechanically agitated gas phase reactors.

[0046] The hydrocarbon solvent may be aromatic (eg, toluene) or aliphatic (eg, propane, hexane, heptane, isobutane, cyclohexane, and 2,2,4-trimethylpentane, isododecane, and the like).

[0047] Preferably, the polymerization process is carried out by using liquid butene-1 as the polymerization medium.

[0048] The polymerization temperature may be between 20°C and 150°C, particularly between 50°C and 90°C, for example 65°C to 82°C.

[0049] To control the molecular weight, molecular weight regulators, in particular hydrogen, are provided to the polymerization environment.

[0050] Mw / Mn values ​​of 4 or greater and MI as previously defined10 The value of the / MI2 ratio is generally considered to result in a broad molecular weight distribution (MWD).

[0051] Broad molecular weight butene-1 polymers can be obtained in several ways. One of the ways consists in using a catalyst that is capable of producing inherently broad MWD polymers when (co)polymerizing butene-1. Another possible way is to mechanically blend butene-1 polymers with sufficiently different molecular weights using conventional mixing equipment.

[0052] It is also possible to operate according to a multi-stage polymerization method in which butene-1 polymers of different molecular weights are prepared successively in two or more reactors with different reaction conditions, such as the concentration of molecular weight regulator fed to each reactor.

[0053] It is also possible to feed different amounts of monomer to each reactor.

[0054] In particular, when the butene-1 polymer component A) of the invention comprises the two aforementioned components A1) and A2), the polymerization process can be carried out in two or more reactors connected in series, in which components B1) and B2) are prepared in separate subsequent stages, operated in each stage except the first stage, in the presence of the formed polymer and of the catalyst used in the previous stage.

[0055] The catalyst may be added only to the first reactor, or it may be added to multiple reactors.

[0056] High MI values ​​can be achieved directly during polymerization, or by subsequent chemical treatment (chemical visbreaking).

[0057] Chemical visbreaking of polymers is carried out in the presence of a free radical initiator such as a peroxide.

[0058] The decomposition temperature of the peroxide most suitably used in the polymer visbreak step is preferably 150° C. to 250° C. As the peroxide, for example, di-tert-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, etc. are commercially available.

[0059] The amount of peroxide required for the visbreaking process is preferably in the range of 0.001-0.5% by weight of the polymer, more preferably 0.001-0.2%.

[0060] Examples of alkyl R1 and R2 in the alkanoyl hydrazines A) of formula (I) are particularly preferably methyl, ethyl, propyl, isopropyl, butyl, t-butyl, pentyl, hexyl, t-butyl.

[0061] The alkanoyl hydrazine A) preferably has the following formula (II): [ka] (In formula (I), R1 and R2 have the same meanings as described above in formula (I).)

[0062] A particularly preferred alkanoyl hydrazine A) is the compound N,N'-bis-β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionyl-hydrazine, also called 2',3-bis[[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide, having the formula (III).

[0063] [ka]

[0064] The alkanoyl hydrazines A) can be prepared by reaction of hydrazine with an ester of an alkylhydroxyphenylalkanoic acid, followed by further acylation, as exemplified in US Pat. No. 3,773,722.

[0065] Alkanoyl hydrazines of formula (III) are sold under the trade name Irganox 1024 by BASF. The polybutene-1 composition of the present invention may also contain talc as optional component C). The preferred amount of component C) is 0.15-2.5% by weight, more preferably 0.2-2% by weight, most preferably 0.2-1.5% by weight, based on the total weight of A)+B)+C). Particularly preferred is talc in the form of particles having a volume-based (volume) particle size distribution Dv(0.95) of less than or equal to 45 μm, preferably less than or equal to 35 μm, more preferably less than or equal to 25 μm and in particular less than or equal to 20 μm, the volume-based (volume) particle size distribution Dv being determined by laser light diffraction, the lower limit being in all cases preferably 5 μm. In addition to said Dv(0.95) value, component C) preferably has at least one of the following volumetric particle size distribution characteristics: -Dv(0.99) is 100 μm or less, or 50 μm or less, or 30 μm or less, with the lower limit preferably being 10 μm in all cases. -Dv(0.90) is 20μm or less, or 15μm or less, with the lower limit being 3μm in all cases -Dv(0.50) is 10μm or less, or 8μm or less, with the lower limit being 2μm -Dv(0.10) is 5 μm or less, or 4 μm or less, with the lower limit preferably being 1 μm. The volumetric particle size refers to the diameter of an equivalent sphere having the same volume as the target particle. Therefore, the volume-based particle size distribution value means that particles having a specified volume fraction (eg, 95% by volume for Dv(0.95)) have an equivalent diameter smaller than a predetermined value. Such determination is made by laser diffraction. The analytical device used is preferably a Malvern Mastersizer instrument. Talc is known to be a magnesium silicate hydrate. Its formula is usually reported to be Mg3Si4O10(OH)2. In essence, it is a mineral that consists primarily or substantially of said hydrated magnesium silicate, optionally in association with other mineral materials such as chlorite (hydrated magnesium aluminum silicate) and dolomite. To achieve the above values ​​of particle size distribution, the talc can be milled using known techniques, such as air classifying mills, compressed air, steam and impact milling. The polybutene-1 compositions of the present invention can be obtained by blending components A), B), and, optionally, C), using blending techniques and equipment well known in the art.

[0066] Thus, extruders commonly known in the art can be used, including single screw extruders, conventional and CoKneader (such as Buss), twin co-rotating screw extruders or mixers (continuous and batch). Such blending equipment can be equipped with separate feed systems for components A), B) and optionally C), respectively. Component B) and optional component C) can be added to the polymer mass inside the blending equipment, particularly the extruder, either at the same feed port or downstream from the point where A) is fed into the blending equipment, allowing A) to reach the form of a molten homogenous mass.

[0067] Components B) and C) may be provided in the form of a masterbatch in a polymeric carrier, more preferably a polyolefin carrier, especially a polybutene carrier of the same type as the butene-1 polymer component A).

[0068] The processing temperature during the blending step must be sufficient to bring (and maintain) component A) in a molten state, or, if component A) is already molten when B) and optionally C) are added, to maintain component A) in a molten state. Such temperatures preferably range from 100°C to 220°C, more preferably from 150°C to 220°C, and most preferably from 180°C to 220°C.

[0069] In addition to the main components A) and B) and any other polymeric components, additives commonly used in the art such as stabilizers (heat, light, UV), plasticizers, antacids, antistatic and water repellents, pigments, etc. may be introduced during the preparation of the polymer composition.

[0070] As mentioned above, the preferred application of the polybutene-1 compositions of the present invention is the manufacture of pipes, especially pipes for conveying water and thermal fluids, and pipe joints. In general, they can be advantageously used in any application requiring improved mechanical and processing properties. EXAMPLES

[0071] Examples and advantages of the various embodiments, compositions and methods provided herein are disclosed in the following examples, which are merely illustrative and are not intended to limit the scope of the appended claims in any manner.

[0072] The following analytical methods are used to characterize the polymer compositions:

[0073] Crystallization and Melting Temperatures

[0074] Crystallization temperature (T c ) and melting temperature values ​​were determined using the following procedure.

[0075] Differential scanning calorimetry (DSC) data were obtained using a Perkin Elmer DSC-7 instrument. Weighed samples (5–10 mg) were enclosed in aluminum disks and heated to 200 °C at a scan rate equivalent to 10 °C / min. The samples were held at 200 °C for 5 min to completely melt all crystallites and clear the thermal history of the samples. They were then cooled to -20 °C at a scan rate of 10 °C / min and the peak temperature was taken as the crystallization temperature (T c ) and the area was taken as the crystallization enthalpy. After standing at -20 °C for 5 min, the sample was heated a second time to 200 °C at a scan rate corresponding to 10 °C / min. In this second heating run, the peak temperature was taken as the melting temperature of polybutene-1 crystalline form II (TmII) and the area was taken as the melting enthalpy (ΔHfII).

[0076] To determine the melting temperature (TmI) of polybutene-1 crystalline form I, a sample was melted and held at 200°C for 5 min, then cooled to 20°C at a cooling rate of 10°C / min. The sample was then stored at room temperature for 10 days. After 10 days, the sample was subjected to DSC, cooled to -20°C, and then heated at 200°C at a scanning rate corresponding to 10°C / min. In this heating run, the first peak temperature from the low temperature side of the thermogram was taken as the melting temperature (Tml).

[0077] Crystallization half time at 95℃

[0078] Differential scanning calorimetry (DSC) data were obtained using a Perkin Elmer DSC-7 instrument. Weighed samples (5–10 mg) were enclosed in aluminum discs and heated from room temperature to 180 °C at a scan rate equivalent to 10 °C / min.

[0079] The thermal history of the sample was eliminated by holding the sample at 180° C. for 5 min to ensure complete melting of all crystallites.

[0080] It was then cooled to 95° C. at a scan rate corresponding to 60° C. / min, and the heat flow due to the crystallization exotherm at 95° C. was measured. The integral of the heat transfer was recorded as a function of time until crystallization was complete, i.e., until heat transfer stopped.

[0081] The crystallization half time is the time for the heat transfer integral to reach half of its final value.

[0082] Particle size distribution

[0083] Particle size distribution (PSD) was measured by laser diffraction according to ISO 13320:2009.

[0084] The instrument used is a Mastersizer® 2000 equipped with a sample dispersion unit manufactured by Malvern, UK.

[0085] The detection system has the following features: -Red light: forward scatter, side scatter, back scatter; - Blue light: wide-angle back-and-forth scattering; -Light source: red light He-Ne laser; blue light solid light source; -Optical alignment system: automatic high-speed alignment system with dark field optical reticle; -Laser system: Class 1 laser product.

[0086] PSD determination is based on the principle of optical diffraction, where a laser monochromatic light is scattered through a dispersed particulate sample. The signal is received by a computer connected to the instrument, which processes the received signal and converts it into a 3-dimensional physical quantity.

[0087] The results are presented by a PSD report consisting of 106 class diameters (virtual sieves) and associated cumulative percentages for volume and additional derived parameters.

[0088] In addition to background electrical noise, the measurement data will also be contaminated by scattered data from dust on the optics or contaminants suspended in the dispersion, so it is important to ensure that the sample dispersion unit is clean and free of all traces of impurities and residual material.

[0089] Therefore, background measurements with pure dispersant (solvent) and electrical background measurements were performed. The resulting total background values ​​were subtracted from the sample measurements to obtain the true sample data.

[0090] For background measurements, anhydrous n-heptane solvent containing 2 g / 1 SPAN 80 Pure as an antistatic agent was introduced into the sample dispersion unit. Before each measurement, residual air in the solvent was removed by ultrasonic treatment (60 s).

[0091] The solvent was then pumped into the measurement cell with the stirrer and circulation pump operating in the power range of 2205 rpm.

[0092] measurement

[0093] The sample, suspended in anhydrous n-heptane by stirring, was added directly to the sample unit.

[0094] Circulation of the sample suspension was required for 2 min to facilitate the breakup of aggregates (if present).

[0095] The obscuration bar can be seen on the monitor, allowing the optimal volume concentration of the sample to be reached. The concentration of the sample must correspond to an obscuration value in the range of 10% to 30%. This range ensures representativeness and stable results.

[0096] The refractive index (RI) was set as follows: Particle RI:1.596; Dispersant RI: 1.390.

[0097] The measurement time is 4 seconds.

[0098] The signal received from the laser device was processed and then the PSD was calculated using software provided with the Mastersizer device.

[0099] Melt Flow Index MI

[0100] Determined at 190°C and a specified load according to ISO 1133-12012-03.

[0101] intrinsic viscosity

[0102] Determined in tetrahydronaphthalene at 135° C. according to standard ASTM D 2857-16.

[0103] Tensile modulus (MET-DMTA)

[0104] Determined on 1 mm thick compression molded plaques by dynamic mechanical thermal analysis (DMTA) at 23 °C according to ISO 6721-4:2019.

[0105] Flexural modulus

[0106] Measurements were performed after 10 days of molding according to standard ISO 178:2019.

[0107] Izod impact resistance at 23°C and 0°C

[0108] Measured according to ISO 179-1:2010 1eA 10 days after molding.

[0109] Comonomer Content

[0110] The comonomer content of the butene-1 polymers was determined by FT-IR.

[0111] The spectra of pressed polymer films are expressed as absorbance vs. wavenumber (cm -1 The ethylene content was calculated from the following measurements: a) 4482-3950 cm, used for spectroscopic normalization of film thickness -1 The area of ​​the combined absorption band (A t ). b) The subtraction coefficient (FCR) of the digital subtraction between the spectrum of the polymer sample and the absorption bands due to the methylene group sequences BEE and BEB (B: butene unit, E: ethylene unit). C2 )(CH2 Shake Vibration). c) The area of ​​the remaining band after subtracting the C2PB spectrum (A C2,block ) It is derived from the methylene group sequence EEE (CH2 shake vibration).

[0112] Device

[0113] A Fourier transform infrared spectrophotometer (FTIR) capable of providing the above-mentioned spectral measurements was used.

[0114] A hydraulic press (Carver or equivalent) with platens heatable to 200° C. was used.

[0115] method

[0116] Calibration of (BEB+BEE) sequence

[0117] %(BEB+BEE)wt vs. FCR C2 / A t A calibration line was obtained by plotting the slope r and intercept I r was calculated by linear regression.

[0118] Calibrating the EEE sequence

[0119] %(EEE)wt vs A C2,block / A t A calibration straight line was obtained by plotting the slope G H and intercept I H was calculated by linear regression.

[0120] Sample preparation

[0121] A thick sheet was obtained by pressing approximately 1.5 g of sample between two pieces of aluminum foil using a hydraulic press. If there are problems with uniformity, it is suggested to perform a minimum of two pressing operations. A small portion was cut from this sheet to form a membrane. The recommended membrane thickness is 0.1-0.3 mm.

[0122] The press temperature is 140(10°C.

[0123] Because changes in crystalline phase occur over time, we suggest collecting IR spectra of sample films immediately after casting.

[0124] procedure

[0125] The instrument data acquisition parameters are as follows: Purge time: 30 seconds minimum Collection time: Minimum 3 minutes Apodization: Happ-Genzel Resolution: 2cm -1 IR spectra of the samples against an air background were collected.

[0126] calculation The weight concentration of the BEE+BEB sequence of ethylene units was calculated.

number

number

number

[0127] Determination of isotactic pentad content 13 C NMR spectra were acquired at 120 °C on polymer solutions (8–12 wt %) in deuterated 1,1,2,2-tetrachloroethane. 13 C NMR spectra were obtained on a Bruker AV-600 spectrometer equipped with a cryoprobe, operating in Fourier transform mode at 120 °C and 150.91 MHz. 1 H- 13 A 90° pulse with a 15 second delay between the pulse and the CPD (WALTZ 16) was used to remove C bonds. Approximately 512 transients were stored in 32K data points using a spectral window of 60 ppm (0-60 ppm). The mmmm pentad peak (27.73 ppm) was used as the reference. The assignment was performed as described in the literature (Macromolecules 1991, 24, 2334-2340, by Asakura T.). The percentage value of pentad tacticity (mmmm%) of butene-1 polymer is the percentage of stereoregular pentads (isotactic pentads) calculated from the relevant pentad signals (peak areas) in the NMR region of the branched methylene carbons, as follows:

number

[0128] Fractions soluble and insoluble in xylene at 0℃ (XS-0℃)

[0129] 2.5 g of polymer sample was stirred at 135 °C and dissolved in 250 ml of xylene. After 30 min, the solution was cooled to 100 °C while stirring, then cooled to 0 °C in an ice-water bath. The solution was then left to stand in the ice-water bath for 1 h. The precipitate was filtered with filter paper. During filtration, the flask was left in the ice-water bath to keep the temperature inside the flask as close to 0 °C as possible. After the filtration was completed, the filtrate temperature was kept at 25 °C, and the volumetric flask was immersed in a water flow bath for about 30 min, after which two 50 ml aliquots were taken. The solution aliquots were evaporated in a nitrogen gas flow, and the residue was dried in a vacuum at 80 °C until a constant weight was reached. The weight difference between both residues should be less than 3%. Otherwise, the test should be repeated. The weight percentage of polymer solubles (xylene solubles at 0 °C = XS0 °C) was then calculated from the average weight of the residue. The insoluble fraction in o-xylene at 0° C. (xylene insolubles at 0° C.=XI% 0° C.) is as follows:

number

[0130] X-ray crystallinity determination

[0131] X-ray crystallinity was measured using an X-ray diffraction powder diffractometer using Cu-Kα1 radiation with a fixed slit, collecting spectra between diffraction angles 2θ = 5° and 2θ = 35° with a step of 0.1° every 6 s.

[0132] The measurements were carried out on disk-shaped compression-molded test pieces with a thickness of about 1.5 to 2.5 mm and a diameter of about 2.5 to 4.0 cm. These test pieces were compressed at a temperature of 200°C ± 5°C for 10 minutes without applying any significant pressure, and then compressed under a pressure of about 10 kg / cm. 2 Pressure was applied for several seconds, and the last operation was repeated three times.

[0133] The diffraction pattern was used to define an appropriate linear baseline throughout the spectrum and all components required for crystallinity were derived by calculating the total area (Ta) (expressed in counts / sec·2θ) between the spectral profile and the baseline. Then, along the entire spectrum, we defined an appropriate amorphous profile that separates the amorphous and crystalline regions according to a two-phase model. Thus, the amorphous area (Aa), expressed in counts / s·2θ, may be calculated as the area between the amorphous profile and the baseline, and the crystalline area (Ca), expressed in counts / s·2θ, as Ca = Ta - Aa.

[0134] The crystallinity of the samples was then calculated based on the following formula:

number

[0135] Determination of Mw / Mn by GPC

[0136] The determination of the average Mn and Mw, and the derived Mw / Mn, was carried out using a Waters GPCV 2000 instrument equipped with a column set of four PLgel Olexis mixed gels (Polymer Laboratories) and an IR4 infrared detector (PolymerChar). The column dimensions are 300 × 7.5 mm, with a particle size of 13 μm. 1-2-4-Trichlorobenzene (TCB) was used as the mobile phase, and its flow rate was kept at 1.0 ml / min. All measurements were performed at 150 °C. The solution concentration in TCB was 0.1 g / dL, and 0.1 g / l of 2,6-dibutyl-p-cresol was added to prevent decomposition. For GPC calculations, a universal calibration curve was obtained using 10 polystyrene (PS) standard samples (peak molecular weights ranging from 580 to 8.5 million) supplied by Polymer Laboratories. A third-order polynomial fit was used to interpolate the experimental data and obtain the relevant calibration curve. Data acquisition and processing were performed using Empower (Waters). The Mark-Houwink relationship was used to determine the molecular weight distribution and the associated average molecular weight. The K values ​​of PS and polybutene (PB) were calculated using K PS =1.21×10 -4 dL / g and K PB=1.78×10 -4 dL / g, and the Mark-Hwink index α = 0.706 for PS and the Mark-Hwink index α = 0.725 for PB are used in combination.

[0137] For butene-1 / ethylene copolymers, the composition was assumed to be constant over all molecular weights for data evaluation, and the K value of the Mark-Houwink relationship was calculated using the linear combination:

number

[0138] density

[0139] Determined at 23°C according to standard ISO 1183-1:2019.

[0140] Examples 1 and 2, and Comparative Examples 1 and 2

[0141] To prepare the polybutene-1 composition, the following materials were used:

[0142] Butene-1 Polymer A)

[0143] Prepared by polymerization of liquid monomer using Ziegler-Natta catalyst, flexural modulus 450MPa, MI 10 12g / 10min, MI 20.4g / 10min, content of fraction soluble in xylene at 0°C of 2% by weight, density 914kg / cm 3 butene-1 homopolymer.

[0144] It is commercially available under the trademark Toppyl PB 0110M and is sold by LyondellBasell.

[0145] Alkanoyl hydrazine component B)

[0146] Alkanoyl hydrazine having the above formula (III) is sold by BASF under the trademark Irganox 1024.

[0147] Talc C)

[0148] Talc having a volumetric particle size distribution as set forth in Table 1, without additives, sold by Imifabi under the trademark HM05.

[0149] Irgafos 168 (registered trademark)

[0150] Tris(2,4-di-tert-butylphenyl)phosphite, sold by Ciba Geigy, heat stabilizer. [Table 1]

[0151] Preparation of Polybutene-1 Composition

[0152] The ingredients were melt blended in a Leistritz Micro27 extruder equipped with co-rotating twin screws, a split screw diameter of 27 mm, an L / D ratio of 40:1, and a maximum screw speed of 500 rpm.

[0153] Main extrusion parameters: Temperature: 200℃ Screw speed: 200 rpm Output: 15kg / h

[0154] The component amounts and properties of the final compositions thus obtained are shown in Table 3.

Table 2

Claims

1. A process for preparing a polybutene-1 composition comprising the following components: A) 99.5 to 99.9% by weight, preferably 99.6 to 99.85% by weight, based on the total weight of A)+B), of a butene-1 polymer chosen from butene-1 homopolymers, butene-1 copolymers and mixtures thereof, said butene-1 polymer being brought to or maintained in a molten state during the blending step; B) 0.1-0.5% by weight, preferably 0.15-0.4% by weight, based on the total weight of A)+B), of one or more alkanoyl hydrazines of formula (I), The polybutene-1 composition thus obtained has a crystallization temperature T c C having [0010] Preferably, [0025] More preferably, [0030] Here, T c A and T c C is expressed in ° C., T c A is the crystallization temperature of the butene-1 polymer A), preferably 60° C. or higher, more preferably 65° C. or higher, said crystallization temperature being determined by differential scanning calorimetry (DSC) at heating and cooling rates of 10° C. / min. 【number】 (In the formula, R 1 is an alkyl group having 1 to 6 carbon atoms; R 2 is hydrogen or alkyl having 1 to 6 carbon atoms, and n is an integer from 0 to 5.

2. 10. The method of claim 1, wherein talc C) is added in the blending step.

3. 3. The process according to claim 2, wherein the talc C) is in the form of particles having a volume-based particle size distribution Dv(0.95), determined by laser light diffraction, of ≦45 μm, preferably ≦35 μm, more preferably ≦25 μm, in particular ≦20 μm, the lower limit being in all cases preferably 5 μm.

4. The method of claim 1 or 2, wherein the blending step is carried out at a temperature of from 100°C to 220°C.

5. 3. The method of claim 1 or 2, wherein the alkanoyl hydrazine B) has the formula (II). [Case 2] (In the formula, R 1 is an alkyl group having 1 to 6 carbon atoms; R 2 is hydrogen or alkyl having 1 to 6 carbon atoms.

6. The process according to claim 5, wherein B) has the formula (III): [C3]

7. 1. A polybutene-1 composition comprising: A) from 99.5 to 99.9% by weight, preferably from 99.6 to 99.85% by weight, based on the total weight of A)+B), of a butene-1 polymer chosen from butene-1 homopolymers, butene-1 copolymers and mixtures thereof, said butene-1 polymer having a crystallization temperature TcA greater than or equal to 60° C., preferably greater than or equal to 65° C. B) 0.1 to 0.5% by weight, preferably 0.15 to 0.4% by weight, based on the total weight of A)+B), of one or more alkanoylhydrazines of formula (I), Said polybutene-1 composition has a crystallization temperature TcC that satisfies the following relationship: [0045] Preferably, [0050] More preferably, [006] Said crystallization temperature is determined by Differential Scanning Calorimetry (DSC) at a heating and cooling rate of 10° C. / min. of a polybutene-1 composition. 【number】 (In the formula, R1 is an alkyl group having 1 to 6 carbon atoms, R2 is hydrogen or an alkyl group having 1 to 6 carbon atoms, and n is an integer of 0 to 5.)

8. 8. The polybutene-1 composition of claim 7, further comprising talc C).

9. Polybutene-1 composition according to claim 8, wherein said talc C) is in the form of particles having a volume-based particle size distribution Dv(0.95) determined by laser light diffraction less than or equal to 45 μm, preferably less than or equal to 35 μm, more preferably less than or equal to 25 μm, in particular less than or equal to 20 μm, the lower limit being in all cases preferably 5 μm.

10. 10. Polybutene-1 composition according to claim 8 or 9, wherein said talc C) is present in an amount of 0.15 to 2.5% by weight, preferably 0.2 to 2% by weight, more preferably 0.2 to 1.5% by weight, based on the total weight of A)+B)+C).

11. 9. Polybutene-1 composition according to claim 7 or 8, wherein said alkanoyl hydrazine B) has formula (II). [C5] (In the formula, R 1 is an alkyl group having 1 to 6 carbon atoms; R 2 is hydrogen or alkyl having 1 to 6 carbon atoms.

12. 12. The polybutene-1 composition of claim 11, wherein said B) has formula (III): [C6]

13. T c C 9. Polybutene-1 composition according to claim 7 or 8, having a value of at least 85°C, in particular between 85°C and 98°C.

14. An article, preferably a pipe or a pipe fitting, containing the polybutene-1 composition according to any one of claims 6 to 13.

Citation Information

Patent Citations

  • Polybutylene material for pipes and preparation method of polybutylene material

    CN105504552A

  • Improved polyolefin composition for water pipe

    JP1989103638A

  • Production of crosslinked foamed material of polyolefin resin

    JP1999060773A