Adhesive
An adhesive with a crosslinked acrylic copolymer provides flexibility and structural integrity by adjusting modulus based on temperature, ensuring effective deformation and recovery in flexible devices.
Patent Information
- Application Number
- JP2024532333
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-05-27
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Existing adhesives for flexible devices face challenges in balancing low modulus at low temperatures for flexibility with high modulus at high temperatures for structural integrity, while maintaining adequate adhesion and workability.
Development of an adhesive with a crosslinked acrylic copolymer that exhibits a low storage modulus at low temperatures and a high storage modulus at high temperatures, along with appropriate peel strength and optical clarity, achieved through a specific composition and crosslinking process.
The adhesive effectively follows repeated deformations, maintains structural integrity, and ensures good workability and cuttability without defects like peeling or bubble formation, suitable for flexible devices.
Smart Images

Figure 2024542670000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0065231, filed May 27, 2022, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.
[0002] The present application relates to a pressure sensitive adhesive and its uses. [Background technology]
[0003] A flexible device is a new concept of device, and examples thereof include so-called foldable devices and rollable devices.
[0004] The adhesive layer applied to the foldable device is stretched after repeated folding or unraveled after rolling.
[0005] Therefore, the layers applied to the foldable device are required to effectively follow the repeated deformation and further to recover to their original shape when the force applied during deformation is removed.
[0006] It is generally known that the lower the elastic modulus of a pressure-sensitive adhesive, particularly the elastic modulus at low temperatures, the more effectively it can accommodate the above-mentioned repeated deformation.
[0007] However, if the elastic modulus of the pressure-sensitive adhesive layer is too low, the recovery property when the force applied for deformation is removed decreases, resulting in problems of decreased cuttability and workability.
[0008] Therefore, taking into consideration cuttability and workability, it is preferable for the adhesive layer to have a certain level or higher of elasticity modulus; however, it is not easy to obtain an adhesive layer that can effectively follow deformation while ensuring desired levels of recovery, cuttability, workability, etc.
[0009] Furthermore, when the elastic modulus is increased in consideration of cuttability and workability, there is a problem that the peel strength that is fundamentally required for the pressure-sensitive adhesive layer decreases.
[0010] Therefore, it is not an easy task to provide a pressure-sensitive adhesive layer having physical properties suitable for flexible devices. Summary of the Invention [Problem to be solved by the invention]
[0011] The present application relates to an adhesive. One of the objects of the present application is to provide an adhesive suitable for flexible devices. In one example, one of the objects of the present application is to provide an adhesive capable of forming an adhesive layer that exhibits a low elastic modulus at low temperatures, a relatively high elastic modulus at high temperatures, and at the same time an appropriate level of adhesive strength (peeling strength).
[0012] It is a further object of the present application to provide an adhesive film or flexible device comprising the adhesive. [Means for solving the problem]
[0013] In the present specification, when a physical property is affected by the measurement temperature, the physical property is measured at room temperature, unless otherwise specified.
[0014] The term "room temperature" as used herein refers to a temperature in a state in which the temperature is not particularly increased or decreased, and may mean any one temperature within a range of about 10° C. to 30° C., for example, a temperature of about 15° C. or higher, 18° C. or higher, 20° C. or higher, or about 23° C. or higher, and about 27° C. or lower. Furthermore, unless otherwise specified, the unit of temperature referred to in this specification is ° C.
[0015] In the present specification, when the measurement pressure affects a physical property, the physical property is measured at normal pressure, unless otherwise specified.
[0016] In this specification, the term "normal pressure" refers to pressure in a state where there is no particular increase or decrease in pressure, and generally refers to a pressure of approximately 740 mmHg to 780 mmHg, which is the atmospheric pressure level.
[0017] In the present specification, when the humidity at which the property is measured affects the property, the property is measured at the natural humidity at room temperature and pressure, unless otherwise specified.
[0018] The present application relates to a pressure sensitive adhesive. The pressure sensitive adhesive of the present application may include an acrylic copolymer.
[0019] As used herein, the term copolymer refers to the result of a polymerization reaction of a monomer mixture, and the term monomer unit refers to the state of the monomer after the polymerization reaction.
[0020] In the present specification, the term "acrylic copolymer" refers to a copolymer containing acrylic monomer units as a main component. The lower limit of the ratio of the acrylic monomer units in the acrylic copolymer may be about 50% by weight, 55% by weight, 60% by weight, 65% by weight, 70% by weight, 75% by weight, 80% by weight, 85% by weight, 90% by weight, or 95% by weight, and the upper limit may be about 100% by weight, 99% by weight, 98% by weight, 97% by weight, 96% by weight, or 95% by weight. The ratio may be in a range of equal to or greater than any one of the lower limits mentioned above; equal to or less than any one of the upper limits mentioned above; or equal to or greater than any one of the lower limits mentioned above and equal to or less than any one of the upper limits mentioned above.
[0021] As used herein, the term acrylic monomer refers to acrylic acid or methacrylic acid or derivatives of said acrylic acid or methacrylic acid (eg, acrylate or methacrylate esters).
[0022] As used herein, the term (meth)acrylic means acrylic or methacrylic.
[0023] When the acrylic copolymer in the pressure-sensitive adhesive of the present application is crosslinkable, the acrylic copolymer in the pressure-sensitive adhesive may be in a pre-crosslinked state or a crosslinked state, and may preferably be in a crosslinked state. Thus, the pressure-sensitive adhesive may contain the crosslinked acrylic copolymer.
[0024] As a result, the present application can relate to a pressure-sensitive adhesive that contains a crosslinked acrylic copolymer and has the storage modulus at low temperature (−20° C.), peel strength to glass, and haze described below.
[0025] The present application also relates to a pressure-sensitive adhesive that includes a crosslinked acrylic copolymer, exhibits a temperature-dependent change in storage modulus as described below, and has haze as described below.
[0026] The present application may also relate to a pressure sensitive adhesive comprising a crosslinked acrylic copolymer and a compound of Formula 1 described below.
[0027] The adhesive may include the acrylic copolymer as a main component. For example, the lower limit of the ratio of the acrylic copolymer based on the total weight of the adhesive may be about 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, 97 wt%, or 99 wt%, and the upper limit may be about 100 wt%, 99 wt%, 98 wt%, 97 wt%, 96 wt%, or 95 wt%. The ratio may be in a range equal to or greater than any one of the lower limits; equal to or less than any one of the upper limits; or equal to or greater than any one of the lower limits and equal to or less than any one of the upper limits. When the adhesive includes a component that is not included in the final adhesive layer, such as a solvent or a solvent, the content of the acrylic copolymer is the content in the adhesive excluding the component that is not included in the final adhesive layer.
[0028] The storage modulus and peel strength of the adhesive referred to in this specification are the storage modulus and peel strength when the adhesive composition is in a crosslinked state (i.e., when the acrylic copolymer contained in the adhesive composition is crosslinked), and therefore may be the storage modulus and peel strength of the adhesive or the adhesive layer.
[0029] The pressure sensitive adhesive of the present application can exhibit a low storage modulus at low temperatures.
[0030] In this specification, the storage modulus is a result measured by the method presented in the following examples.
[0031] For example, the pressure-sensitive adhesive may have an upper limit of storage modulus at -20°C of about 100,000 Pa, 98,000 Pa, 96,000 Pa, 95,000 Pa, 94,000 Pa, 93,000 Pa, 92,000 Pa, 90,000 Pa, 88,000 Pa, 86,000 Pa, 85,000 Pa, or 84,000 Pa, and the lower limit may be, for example, 30,000 Pa, 40,000 Pa, 42,000 Pa, 44,000 Pa, 45,000 Pa, 46,000 Pa, 48,000 Pa, 50,000 Pa, 52,000 Pa, The pressure may be approximately 54,000 Pa, 55,000 Pa, 56,000 Pa, 58,000 Pa, 60,000 Pa, 62,000 Pa, 64,000 Pa, 65,000 Pa, 66,000 Pa, 68,000 Pa, 70,000 Pa, 72,000 Pa, 74,000 Pa, 75,000 Pa, 76,000 Pa, 78,000 Pa, 80,000 Pa, 82,000 Pa, 84,000 Pa, 86,000 Pa, 88,000 Pa, 90,000 Pa, 92,000 Pa, 94,000 Pa or 96,000 Pa. The storage modulus at -20°C may be in a range of less than or equal to any one of the upper limits mentioned above; or in a range of more than or equal to any one of the lower limits mentioned above and less than or equal to any one of the upper limits mentioned above.
[0032] When the pressure-sensitive adhesive exhibits a storage modulus in the above range at a low temperature of -20°C, it can be applied to a flexible device and can effectively respond to repeated deformation and recovery.
[0033] The adhesive of the present application can exhibit the low storage modulus at low temperatures, and at the same time, can exhibit a high storage modulus above a certain level at relatively high temperatures. The storage modulus of an adhesive is a function that depends on temperature, and is usually. As the temperature increases, the storage modulus decreases. Thus, the storage modulus of an adhesive at high temperatures is usually lower than the storage modulus at low temperatures. However, when an adhesive has a low storage modulus at low temperatures, the storage modulus at high temperatures also decreases relatively, so that the storage modulus of an adhesive with a low storage modulus at low temperatures at high temperatures is lower than the storage modulus of an adhesive with a high storage modulus at low temperatures at high temperatures.
[0034] However, the pressure-sensitive adhesive of the present application may exhibit a relatively high storage modulus at a high temperature in addition to the low storage modulus at a low temperature, i.e., the pressure-sensitive adhesive of the present application may exhibit a relatively gentle slope in a graph of storage modulus versus temperature.
[0035] For example, the pressure-sensitive adhesive of the present application may have a rate of change in elastic modulus according to the following mathematical formula 1 within a predetermined range. [Formula 1] Elastic modulus change rate = (M20-M25) / 45
[0036] In Equation 1, M20 is the storage modulus (unit: Pa) of the pressure-sensitive adhesive at -20°C, and M25 is the storage modulus (unit: Pa) of the pressure-sensitive adhesive at 25°C.
[0037] The upper limit of the elastic modulus change rate may be about 2500, 2400, 2300, 2200, 2100, 2000, 1900, 1800, 1700, 1600, 1500, 1400, 1300, 1200 or 1100, and the lower limit may be about 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100 or 1200. The elastic modulus change rate may be in a range of less than or equal to any one of the upper limits mentioned above; or in a range of more than or equal to any one of the lower limits mentioned above and less than or equal to any one of the upper limits mentioned above.
[0038] The adhesive layer exhibiting the above-mentioned elastic modulus change rate can effectively follow the repeated deformation and recovery in a foldable device, and can maintain good workability and cuttability. However, as described above, an adhesive having a low elastic modulus at low temperatures exhibits a relatively low elastic modulus at high temperatures, so that it is not an easy task to satisfy the elastic modulus change rate. In the present application, the above-mentioned elastic modulus change rate can be satisfied by applying a specific acrylic copolymer described later as the acrylic copolymer.
[0039] The lower limit of the storage modulus of the pressure-sensitive adhesive at 25° C. may be about 10,000 Pa, 12,000 Pa, 13,000 Pa, 14,000 Pa, 15,000 Pa, 16,000 Pa, 17,000 Pa, 18,000 Pa, 20,000 Pa, 21,000 Pa, 22,000 Pa, 23,000 Pa, 24,000 Pa, 26,000 Pa, 28,000 Pa, 30,000 Pa, 32,000 Pa, 34,000 Pa, 36,000 Pa, or 38,000 Pa, and the upper limit thereof may be, for example, about 100,000 Pa, 98,000 Pa, 96,000 Pa, 94,000 Pa, 92,000 Pa, or 96,000 Pa. Pa, 90,000 Pa, 88,000 Pa, 86,000 Pa, 84,000 Pa, 82,000 Pa, 80,000 Pa, 78,000 Pa, 76,000 Pa, 74,000 Pa, 72,000 Pa, 70,000 Pa, 68,000 Pa, 66,000 Pa, 64,000 Pa, 62,000 Pa, 60,000 Pa, 58,000 Pa, 56,000 Pa, 54,000 Pa, 52,000 Pa, 50,000 Pa, 48,000 Pa, 46,000 Pa, 44,000 Pa, 42,000 Pa, 40,000 Pa, 38,000 Pa or 36,000 Pa. The storage modulus at 25°C may be in a range greater than or equal to any one of the lower limits mentioned above; or in a range greater than or equal to any one of the lower limits mentioned above and less than or equal to any one of the upper limits mentioned above.
[0040] The pressure-sensitive adhesive of the present application can exhibit a relatively high high-temperature modulus as described above, and at the same time, can exhibit a high peel strength. For example, the pressure-sensitive adhesive may have a room-temperature peel strength from glass within a predetermined range.
[0041] The room temperature peel strength is a peel strength measured at about 25° C., and the method for measuring this peel strength is described in the Examples.
[0042] The lower limit of the peel force may be, for example, about 1,700 gf / inch, 1,800 gf / inch, 1,900 gf / inch, 2,000 gf / inch, 2,100 gf / inch, 2,200 gf / inch, 2,300 gf / inch, or 2,400 gf / inch, and the upper limit may be about 5,000 gf / inch, 4,500 gf / inch, 4,000 gf / inch, 3,500 gf / inch, 3,000 gf / inch, 2,800 gf / inch, 2,600 gf / inch, 2,500 gf / inch, or 2,400 gf / inch. The peel force may be in a range of equal to or greater than any one of the lower limits mentioned above; or in a range of equal to or greater than any one of the lower limits mentioned above and equal to or less than any one of the upper limits mentioned above.
[0043] Such adhesives with a sufficient storage modulus and peel strength can effectively handle the repeated deformation and recovery that occurs in flexible devices, and do not cause defects before or after deformation (e.g., visible deformation marks), have excellent cuttability and workability, and do not induce lifting, peeling, and / or air bubble formation.
[0044] The pressure sensitive adhesive can exhibit excellent optical transparency. For example, the upper limit of the haze of the pressure sensitive adhesive may be about 0.5%, 0.45%, 0.4%, 0.35%, 0.3%, 0.25% or 0.2%, and the lower limit may be about 0.1%, 0.15%, 0.2%, 0.25%, 0.3% or 0.35%. The haze may be in a range of less than or equal to any one of the upper limits; or in a range of more than or equal to any one of the lower limits and less than or equal to any one of the upper limits.
[0045] In the present application, a specific acrylic copolymer is used to form a pressure sensitive adhesive having the above-mentioned specific physical properties.
[0046] The acrylic copolymer may contain at least an alkyl (meth)acrylate unit, a unit of the following chemical formula 3, and a polar functional group-containing unit. The copolymer may further contain a unit of the following chemical formula 4 as an optional monomer unit, if necessary.
[0047] The above unit means a monomer unit.
[0048] [Chemical formula 3] [ka] In Chemical Formula 3, R1 represents hydrogen or an alkyl group, and R2 represents an alkyl group having 11 to 13 carbon atoms.
[0049] [Chemical formula 4] [ka] In Chemical Formula 4, R1 represents hydrogen or an alkyl group, and R3 represents an aromatic ketone group or a (meth)acryloyl group.
[0050] An acrylic copolymer containing the above monomer units is effective in forming the desired adhesive.
[0051] The acrylic copolymer is a so-called crystalline copolymer formed with a predetermined ratio of the unit of Formula 3 and / or the polar functional group-containing unit, or has properties similar to those of a crystalline copolymer. In the present specification, the term crystalline copolymer refers to a copolymer whose melting point is confirmed to be within a predetermined range by a DSC (Differential Scanning Calorimeter) measurement method described in the examples of the present specification.
[0052] Acrylic copolymers are known as non-crystalline copolymers. However, when the units of formula 3 are present in a certain ratio, and when the units of formula 3 interact with polar functional groups present in a certain ratio, such copolymers can exhibit crystallinity or at least properties similar to crystallinity. When a copolymer having crystallinity or properties similar to crystallinity is applied, a pressure-sensitive adhesive having the above-mentioned characteristics can be efficiently formed. Therefore, a pressure-sensitive adhesive layer having the above-mentioned elastic modulus and peel force characteristics can be effectively formed through a pressure-sensitive adhesive to which such a copolymer is applied.
[0053] As the alkyl(meth)acrylate unit contained in the copolymer, for example, a unit derived from an alkyl(meth)acrylate having an alkyl group having 1 to 10 carbon atoms can be used. In other examples, the alkyl group may be an alkyl group having 2 to 20 carbon atoms, 3 to 10 carbon atoms, 4 to 10 carbon atoms, 4 to 9 carbon atoms, or 4 to 8 carbon atoms. The alkyl group may be linear or branched, and may be substituted or unsubstituted. In one example, the unit can be formed using an alkyl(meth)acrylate having an unsubstituted alkyl group that is linear or branched as the alkyl group.
[0054] Examples of the alkyl (meth)acrylate include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, isononyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate.
[0055] In the acrylic copolymer, the lower limit of the weight ratio of the alkyl (meth)acrylate unit may be about 10% by weight, 15% by weight, 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, or 55% by weight, and the upper limit may be about 80% by weight, 75% by weight, 70% by weight, or 65% by weight. The ratio may be in a range equal to or greater than any one of the lower limits mentioned above; equal to or less than any one of the upper limits mentioned above; or equal to or greater than any one of the lower limits mentioned above and equal to or less than any one of the upper limits mentioned above. Within such a range, the desired adhesive can be effectively formed.
[0056] The polar functional group-containing unit is a unit formed by a monomer having a polar functional group. Such a monomer usually contains both a polymerizable group (e.g., a carbon-carbon double bond) and a polar functional group.
[0057] Examples of the monomer having a polar functional group include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and a nitrogen-containing monomer. In the present application, it is particularly advantageous to apply a hydroxyl group-containing monomer, but the present invention is not limited thereto.
[0058] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 2-hydroxypolyethylene glycol (meth)acrylate, or 2-hydroxypolypropylene glycol (meth)acrylate, and examples of carboxyl group-containing monomers include (meth)acrylic acid, 2-(meth)acryloyloxyacetic acid, 3-(meth)acryloyloxypropyl acid, 4-(meth)acryloyloxybutyric acid, acrylic acid dimer, itaconic acid, maleic acid, and maleic anhydride, and examples of nitrogen-containing monomers include (meth)acrylamide, N-vinylpyrrolidone, or N-vinylcaprolactam, but are not limited thereto. One or a mixture of two or more of the above may be used.
[0059] The weight ratio of the polar functional group-containing unit to 100 parts by weight of the alkyl (meth)acrylate unit may be adjusted within a range that can stably maintain the durability, adhesion, and peel strength of the adhesive layer. For example, the lower limit of the weight ratio of the polar functional group-containing unit to 100 parts by weight of the alkyl (meth)acrylate unit may be about 1 part by weight, 5 parts by weight, 10 parts by weight, or 15 parts by weight, and the upper limit may be about 100 parts by weight, 95 parts by weight, 90 parts by weight, 85 parts by weight, 80 parts by weight, 75 parts by weight, 70 parts by weight, 65 parts by weight, 60 parts by weight, 55 parts by weight, 50 parts by weight, 45 parts by weight, 40 parts by weight, 35 parts by weight, 30 parts by weight, 25 parts by weight, or 20 parts by weight.
[0060] The unit of Chemical Formula 3 is a unit containing a long-chain alkyl group, and such a unit is contained in the copolymer at a certain ratio or more, and can interact with a polar functional group as necessary to impart crystallinity or crystal-like properties to the copolymer.
[0061] In the unit of Chemical Formula 3, R1 may be hydrogen or an alkyl group having 1 to 4 carbon atoms, specifically, hydrogen, a methyl group, or an ethyl group.
[0062] In Chemical Formula 3, R2 is an alkyl group having 11 to 13 carbon atoms, and such an alkyl group may be linear or branched, and may be substituted or unsubstituted. In one example, R2 may be a linear and unsubstituted alkyl group. For example, the unit of Chemical Formula 3 may be formed using lauryl (meth)acrylate and / or tetradecyl (meth)acrylate.
[0063] The lower limit of the weight ratio of the units of Chemical Formula 3 relative to 100 parts by weight of the alkyl (meth)acrylate units may be about 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, or 50 parts by weight, and the upper limit thereof may be about 300 parts by weight, 280 parts by weight, 260 parts by weight, 240 parts by weight, 220 parts by weight, 200 parts by weight, 180 parts by weight, 160 parts by weight, 140 parts by weight, 120 parts by weight, 100 parts by weight, 90 parts by weight, 80 parts by weight, 70 parts by weight, 65 parts by weight, 60 parts by weight, 55 parts by weight, or 50 parts by weight. The ratio may be greater than or equal to, or in excess of, any one of the lower limits discussed above; less than or equal to, or below any one of the upper limits discussed above; or greater than or equal to, or above, any one of the lower limits discussed above and less than or equal to, or below any one of the upper limits discussed above.
[0064] The unit of Chemical Formula 4 that may be contained as an arbitrary monomer unit in the acrylic copolymer is a unit containing an aromatic ketone group or a (meth)acryloyl group in the side chain.
[0065] In the pressure sensitive adhesive, the aromatic ketone group or (meth)acryloyl group may exist as it is, or may exist after undergoing a hydrogen abstraction reaction or a radical reaction, which will be described later.
[0066] The aromatic ketone group in the unit of Chemical Formula 4 means an aromatic ketone group that induces hydrogen abstraction from a polymer chain when exposed to electromagnetic waves, or a substituent containing such an aromatic ketone group.
[0067] When exposed to electromagnetic waves, the aromatic ketone groups can remove hydrogen atoms from other polymer chains or from other portions of the polymer chain. Such removal leads to the formation of radicals that can form cross-links between polymer chains or within the same polymer chain. The category of such aromatic ketone groups includes, for example, aromatic ketone groups such as derivatives of benzophenone, acetophenone, or anthraquinone.
[0068] Monomers from which the unit of Chemical Formula 4 having an aromatic ketone group can be derived include, but are not limited to, 4-benzoylphenyl (meth)acrylate, 4-(meth)acryloyloxyethoxybenzophenone, 4-(meth)acryloyloxy-4'-methoxybenzophenone, 4-(meth)acryloyloxyethoxy-4'-methoxybenzophenone, 4-(meth)acryloyloxy-4'-bromobenzophenone and / or 4-acryloyloxyethoxy-4'-bromobenzophenone.
[0069] In the unit of Chemical Formula 4, the (meth)acryloyl group means a (meth)acryloyl group or a substituent containing the same that induces free radical polymerization when exposed to electromagnetic waves in the presence of a suitable radical initiator. Such a (meth)acryloyl group can act similarly to the aromatic ketone group when irradiated with electromagnetic waves.
[0070] The unit of formula 4, in which R3 is a (meth)acryloyl group, can be formed, for example, by preparing a precursor copolymer and then further reacting with an unsaturated reagent compound to introduce a (meth)acryloyl group. Typically, the introduction of the (meth)acryloyl group involves (1) a reaction between a nucleophilic group on the precursor copolymer and an electrophilic group on the unsaturated reagent compound (i.e., the unsaturated reagent compound contains both an electrophilic group and a (meth)acryloyl group), or (2) a reaction between an electrophilic group on the precursor copolymer and a nucleophilic group on the unsaturated reagent compound (i.e., the unsaturated reagent compound contains both a nucleophilic group and a (meth)acryloyl group). These reactions between nucleophilic groups and electrophilic groups are typically ring-opening reactions, addition reactions, or condensation reactions.
[0071] In such cases, the precursor copolymer has hydroxy, carboxylic acid (-COOH), or anhydride (-O-(CO)-O-) groups. When the precursor copolymer has hydroxy groups, the unsaturated reagent compound often has carboxylic acid (-COOH), isocyanato (-NCO), epoxy (i.e., oxiranyl), or anhydride groups in addition to (meth)acryloyl groups. When the precursor copolymer has carboxylic acid groups, the unsaturated reagent compound often has hydroxy, amino, epoxy, isocyanato, aziridinyl, azetidinyl, or oxazolinyl groups in addition to (meth)acryloyl groups. When the precursor (meth)acrylate copolymer has anhydride groups, the unsaturated reagent compound often has hydroxy or amine groups in addition to (meth)acryloyl groups.
[0072] In one example, the precursor copolymer has a carboxylic acid group and the unsaturated reagent compound may have an epoxy group. Exemplary unsaturated reagent compounds include, for example, glycidyl (meth)acrylate and 4-hydroxybutyl acrylate glycidyl ether. In another example, the precursor copolymer has an anhydride group that reacts with an unsaturated reagent compound such as a hydroxy-substituted alkyl (meth)acrylate, for example, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate. In yet another example, the precursor copolymer has a hydroxy group and the unsaturated reagent compound has an isocyanato group and a (meth)acryloyl group. Such unsaturated reagent compounds include, but are not limited to, isocyanatoalkyl (meth)acrylate, for example, isocyanatoethyl (meth)acrylate.
[0073] In one embodiment, the (meth)acryloyl group may be represented by the formula CH2=CHR1-(CO)-QL- (wherein L is a linking group and Q is oxy (-O-) or -NH-), where L includes alkylene, arylene, or a combination thereof, and may further include -O-, -O-(CO)-, -NH-(CO)-, -NH-, or a combination thereof depending on the precursor copolymer and the specific unsaturated reagent compound reacting to form a (meth)acryloyl group. In some specific examples, the (meth)acryloyl group is H2C=CHR1-(CO)-O-R6-NH-(CO)-O-R5-O-(CO)- formed by reacting a hydroxy-containing group of the precursor copolymer represented by the formula -(CO)-O-R5-OH with an unsaturated reagent compound represented by the formula H2C=CHR1-(CO)-O-R6-NCO, which is an isocyanatoalkyl (meth)acrylate. In the above, R5 and R6 are each independently an alkylene group, for example, an alkylene having 1 to 10 carbon atoms, 1 to 6 carbon atoms, or 1 to 4 carbon atoms. In addition, in the above, R1 is methyl or hydrogen.
[0074] In the unit of Chemical Formula 4, R1 may be hydrogen or an alkyl group having 1 to 4 carbon atoms, specifically, hydrogen, a methyl group, or an ethyl group.
[0075] When the unit of Chemical Formula 4 is included, the lower limit of the weight ratio of the unit of Chemical Formula 4 to 100 parts by weight of the alkyl (meth)acrylate unit is 0 parts by weight, 0.001 parts by weight, 0.003 parts by weight, 0.005 parts by weight, 0.007 parts by weight, 0.009 parts by weight, 0.01 parts by weight, 0.015 parts by weight, 0.02 parts by weight, 0.025 parts by weight, 0.03 parts by weight, 0.035 parts by weight, 0.04 parts by weight, 0.045 parts by weight, 0.05 parts by weight, 0.055 parts by weight, 0.0 It may be about 6 parts by weight, 0.065 parts by weight, 0.07 parts by weight, 0.075 parts by weight, 0.08 parts by weight, 0.085 parts by weight, 0.09 parts by weight or 0.1 parts by weight, and its upper limit may be about 5 parts by weight, 4.5 parts by weight, 4 parts by weight, 3.5 parts by weight, 3 parts by weight, 2.5 parts by weight, 2 parts by weight, 2 parts by weight, 1.5 parts by weight, 1 part by weight, 0.5 parts by weight, 0.3 parts by weight, 0.1 parts by weight, 0.08 parts by weight, 0.06 parts by weight, 0.04 parts by weight or 0.02 parts by weight. The ratio may be in a range of not less than or exceeding any one of the lower limits mentioned above; not more than or less than any one of the upper limits mentioned above; or not less than or exceeding any one of the lower limits mentioned above and not more than or less than any one of the upper limits mentioned above. At such a ratio, the desired adhesive layer can be effectively formed by irradiation with electromagnetic waves.
[0076] The acrylic copolymer may suitably contain other monomer units in addition to the monomer units mentioned above, so long as the other monomer units do not impair the purpose (eg, do not impair the crystallinity of the copolymer).
[0077] In one example, the acrylic copolymer contained in the pressure-sensitive adhesive may be a crystalline acrylic copolymer. As described above, the term crystalline copolymer refers to a copolymer whose melting point is confirmed to be within a predetermined range by a DSC (Differential Scanning Calorimeter) measurement method described in the Examples of this specification.
[0078] In one example, the upper limit of the melting point of the acrylic copolymer confirmed by the above method may be about -20°C, -25°C, -30°C, -35°C or -40°C, and the lower limit may be about -100°C, -95°C, -90°C, -85°C, -80°C, -75°C, -70°C, -65°C, -60°C, -55°C, -50°C or -45°C. The melting point may be in a range equal to or greater than any one of the lower limits mentioned above; in a range equal to or less than any one of the upper limits mentioned above; or in a range equal to or greater than any one of the lower limits mentioned above and less than or less than any one of the upper limits mentioned above. An acrylic copolymer having such a melting point can effectively form a desired adhesive.
[0079] The specific composition of the crystalline acrylic copolymer is not particularly limited. In one example, the crystalline acrylic copolymer may be a copolymer containing at least the above-mentioned three types of units (alkyl (meth)acrylate unit, unit of formula 3, and polar functional group-containing unit). However, not all of the above-mentioned acrylic copolymers are crystalline. In order for the acrylic copolymer to exhibit crystallinity, it is necessary that the above-mentioned units of formula 3 are contained at a certain level or more. In the crystalline acrylic copolymer, the lower limit of the weight ratio of the unit of formula 3 to 100 parts by weight of the alkyl (meth)acrylate unit may be about 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, or 60 parts by weight, and the upper limit may be about 300 parts by weight, 250 parts by weight, 200 parts by weight, 150 parts by weight, 100 parts by weight, 90 parts by weight, 80 parts by weight, 70 parts by weight, 60 parts by weight, or 50 parts by weight. The ratio may be in the range greater than or equal to any one of the lower limits stated above; or greater than or equal to any one of the lower limits stated above and less than or equal to any one of the upper limits stated above.
[0080] In the crystalline acrylic copolymer, the lower limit of the ratio (A / B) of the weight (A) of the unit of formula 3 to the weight (B) of the polar functional group-containing unit may be about 1.5, 2, 2.5 or 3, and the upper limit may be about 10, 9, 8, 7, 6, 5, 4 or 3. The ratio may be in a range equal to or greater than any one of the lower limits mentioned above; equal to or less than any one of the upper limits mentioned above; or equal to or greater than any one of the lower limits mentioned above and equal to or less than any one of the upper limits mentioned above.
[0081] In the crystalline acrylic copolymer, the polar functional group-containing unit may be a hydroxy group-containing unit. In one example, a hydroxyalkyl (meth)acrylate having a hydroxyalkyl group with a carbon number in a certain range can appropriately form the crystalline acrylic copolymer. Although the reason is not clear, it is considered that the interaction between the alkyl group (R2) of the unit of chemical formula 3 and the hydroxyalkyl group contributes to the expression of crystallinity of the acrylic copolymer. The lower limit of the carbon number in the hydroxyalkyl group may be about 3 or 4, and the upper limit may be about 10, 9, 8, 7, 6, 5 or 4. The carbon number may be in a range of equal to or more than any one of the lower limits described above; equal to or less than any one of the upper limits described above; or equal to or more than any one of the lower limits described above and equal to or less than any one of the upper limits described above.
[0082] In the crystalline acrylic copolymer, the lower limit of the proportion of the alkyl (meth)acrylate unit may be about 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, 55% by weight or 60% by weight, and the upper limit may be about 70% by weight, 65% by weight or 60% by weight. The proportion may be in a range equal to or greater than any one of the lower limits mentioned above; equal to or less than any one of the upper limits mentioned above; or equal to or greater than any one of the lower limits mentioned above and equal to or less than any one of the upper limits mentioned above. Within such a range, the desired adhesive layer can be effectively formed.
[0083] Although the reason is not clear, it is believed that the interaction and regularity of the monomer units contained in the above ratio imparts crystallinity to the acrylic copolymer, thereby enabling the melting point to be confirmed.
[0084] The acrylic copolymer may have a weight average molecular weight of at least a certain level. In this specification, the weight average molecular weight means a polystyrene equivalent value measured by GPC (gel permeation chromatography). In addition, unless otherwise specified, the unit of the weight average molecular weight is g / mol. The lower limit of the weight average molecular weight of the copolymer may be about 1 million, 1.1 million, 1.2 million, 1.3 million, 1.4 million, 1.5 million, 1.6 million, 1.7 million, 1.8 million, 1.9 million or 2 million, and the upper limit may be about 5 million, 4 million, 3 million, 2.5 million or 2 million. The weight average molecular weight may be in a range of at least or more than any one of the lower limits described above; in a range of at most or less than any one of the upper limits described above; or in a range of at least or more than any one of the lower limits described above and at most or less than any one of the upper limits described above.
[0085] The lower the weight average molecular weight of the copolymer is set, the greater the change in physical properties after crosslinking, but if the weight average molecular weight is too low, it is disadvantageous in terms of durability under high temperature and / or high humidity conditions. However, in the case of the present application, by using the above-mentioned specific copolymer, the desired pressure-sensitive adhesive layer can be effectively formed even when the weight average molecular weight is maintained at an appropriate level.
[0086] The acrylic copolymer may have a molecular weight distribution within a predetermined range. The acrylic copolymer may be crosslinked with an appropriate crosslinking agent according to the molecular weight distribution and included in the adhesive. The molecular weight distribution is a value (Mw / Mn) obtained by dividing the number average molecular weight (Mn) by the weight average molecular weight (Mw). In general, it is recognized that the smaller the molecular weight distribution, the smaller the proportion of components with relatively low molecular weights and components with relatively high molecular weights based on the average molecular weight in the copolymer, the more uniform the composition of the copolymer, and the more stable the rheological properties such as elastic modulus. However, physical properties suitable for flexible devices include mutually contradictory physical properties such as conformability and recovery to deformation, conformability, cuttability, and reliability, and therefore, in order to stably ensure such physical properties, it may be necessary to adjust the molecular weight distribution depending on the type of crosslinking agent applied.
[0087] In one example, when the acrylic copolymer is crosslinked with a thermal crosslinking agent described later, the lower limit of the molecular weight distribution may be about 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9 or 5.0, and the upper limit may be about 10, 9.5, 9, 8.5, 8, 7.5, 7, 6.5, 6 or 5.5. The molecular weight distribution may be less than or equal to any one of the upper limits described above, or greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above and greater than or equal to any one of the lower limits described above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a thermal crosslinking agent described later. It is preferable that such a type of acrylic copolymer is crosslinked only by the thermal crosslinking agent. For example, even if the acrylic copolymer is crosslinked only by the thermal crosslinking agent or crosslinked by simultaneously applying the thermal crosslinking agent and the radical crosslinking agent, the ratio (A / B) of the weight (A) of the thermal crosslinking agent to the weight (B) of the radical crosslinking agent used is below a certain level. For example, the upper limit of the weight ratio A / B may be about 0.5, 0.4, 0.3, 0.2, 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003, 0.0002 or 0.0001, and the lower limit may be about 0. The ratio A / B may be equal to or less than any one of the upper limits described above, or equal to or less than any one of the upper limits described above and equal to or more than any one of the lower limits described above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a radical crosslinking agent described later.
[0088] In one example, when the acrylic copolymer is crosslinked by a so-called radical crosslinking agent, the lower limit of the molecular weight distribution may be about 0.5, 1, 1.5 or 2, and the upper limit may be about 3, 2.8, 2.6 or 2.4. The molecular weight distribution may be less than or equal to any one of the upper limits, or more than or equal to any one of the lower limits, or less than or equal to any one of the upper limits and more than or equal to any one of the lower limits. An acrylic copolymer having such a molecular weight distribution is suitable for forming a type of adhesive intended to be crosslinked by a so-called radical crosslinking agent. It is preferable that such a type of acrylic copolymer is crosslinked only by the radical crosslinking agent. For example, when the acrylic copolymer is crosslinked only by the radical crosslinking agent, or when the acrylic copolymer is crosslinked by simultaneously applying the thermal crosslinking agent and the radical crosslinking agent, the ratio (C / D) of the weight of the thermal crosslinking agent (C) to the weight of the radical crosslinking agent (D) used is preferably at a certain level or less. For example, the upper limit of the weight ratio C / D may be about 0.5, 0.4, 0.3, 0.2, 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003, 0.0002 or 0.0001, and the lower limit may be about 0. The ratio C / D may be equal to or less than any one of the upper limits mentioned above, or equal to or less than any one of the upper limits mentioned above and equal to or more than any one of the lower limits mentioned above. The acrylic copolymer having such a molecular weight distribution is suitable for forming a desired type of adhesive when crosslinked with a radical crosslinking agent described later.
[0089] The method for adjusting the molecular weight distribution of the acrylic copolymer is known per se. For example, the molecular weight distribution can be controlled by one or more methods selected from the following: use of a molecular weight regulator, adjustment of the ratio of an initiator, and / or adjustment of a polymerization time.
[0090] The adhesive may include a compound represented by the following Chemical Formula 1. An adhesive including such a compound can effectively achieve the desired properties.
[0091] [Chemical formula 1] [ka] In Chemical Formula 1, X is carbon or nitrogen, R1 to R3 are each independently hydrogen, an alkyl group or a hydroxyl group, and when X is nitrogen, R4 does not exist and at least one of R1 to R3 is a hydroxyl group. In Chemical Formula 1, R4, when present, may be a substituent of Chemical Formula 2 below.
[0092] [Chemical formula 2] [ka] In Chemical Formula 2, R5 is a single bond, an oxygen atom, -L1-C(=O)-L2-, -L1-C(=O)-O-L2-, or -L1-OC(=O)-L2-; R6 is an alkylidene group or an alkylene group; R7 is a single bond, -OC(=O)-, -C(=O)-, or -C(=O)-O-; R8 and R9 are each independently a hydrogen atom or an alkyl group; and n is a number in the range of 0 to 10.
[0093] In Chemical Formula 2, when R7 is a single bond or -C(=O)-O-, R9 does not exist. In addition, in Chemical Formula 2, L1 and L2 are each independently a single bond, an alkylidene group, or an alkylene group.
[0094] In the case where X in Chemical Formula 1 is carbon, R1 to R3 may each independently be hydrogen or an alkyl group. The alkyl group may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkyl group may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0095] In Chemical Formula 2, R5 may be, in one example, an oxygen atom, -C(=O)-, -C(=O)-O-, or -OC(=O)-.
[0096] The term alkylidene group refers to a divalent residue formed by removing two hydrogen atoms from one carbon atom in an alkane, and alkylene group refers to a divalent residue formed by removing hydrogen atoms from two different carbon atoms in an alkane.
[0097] In Chemical Formula 2, the alkylidene group of R6 may be an alkylidene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkylidene group may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0098] In Chemical Formula 2, the alkylene group of R6 may be an alkylene group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms. Such an alkylene group may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0099] In Chemical Formula 2, R8 may be hydrogen or an alkyl group, and the alkyl group may be an alkyl group having 1 to 20 carbon atoms, 4 to 20 carbon atoms, 6 to 20 carbon atoms, 6 to 16 carbon atoms, 6 to 12 carbon atoms, or 6 to 8 carbon atoms. Such an alkyl group may have a linear or branched chain structure, and may be optionally substituted with one or more substituents (e.g., alkyl groups).
[0100] In Chemical Formula 1, when X is nitrogen, R1 and R2 may each independently be hydrogen or an alkyl group, and the alkyl group may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkyl group may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0101] When X in formula 1 is nitrogen, R3 may be a hydroxy group.
[0102] When X in Chemical Formula 1 is carbon, n in Chemical Formula 2 may be 0 or not 0. When n is not 0, the lower limit of n may be 1, 2 or 3, and the upper limit may be 10, 9, 8, 7, 6, 5, 4 or 3. When n is not 0, n may be less than or equal to any one of the upper limits mentioned above, or may be greater than or equal to any one of the lower limits mentioned above, or may be less than or equal to any one of the upper limits and greater than or equal to any one of the lower limits mentioned above.
[0103] In the formula 1, when X is carbon, R1 to R3 may each independently be hydrogen or an alkyl group. In this case, any one of R1 to R3 may be hydrogen and the remaining two may be alkyl groups. In this case, the alkyl group may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkyl group may have a linear or branched chain structure and may be optionally substituted with one or more substituents. In addition, when any one of R1 to R3 is hydrogen and the remaining two are alkyl groups, the carbon numbers of the two alkyl groups may be different from each other or may be the same.
[0104] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is 0, R5 in Chemical Formula 2 may be -L1-C(=O)-L2-, -L1-C(=O)-O-L2-, or -L1-OC(=O)-L2-, in which case L1 and L2 may each independently be an alkylene group or an alkylidene group. The alkylidene group may be an alkylidene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, and the alkylene group may be an alkylene group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms. Such an alkylene group or alkylidene group may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0105] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is 0, R7 in Chemical Formula 2 may be -OC(=O)-, -C(=O)- or -C(=O)-O-.
[0106] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is 0, R8 and R9 in Chemical Formula 2 may each independently be hydrogen or an alkyl group, or may each independently be an alkyl group. In such a case, the alkyl group may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkyl group may have a linear or branched chain structure, and may be optionally substituted with one or more substituents. In addition, when R8 and R9 are each independently an alkyl group, their carbon numbers may be the same or different from each other.
[0107] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is not 0, R5 in Chemical Formula 2 may be -L1-C(=O)-L2-, -L1-C(=O)-O-L2- or -L1-OC(=O)-L2-, in which case L1 and L2 may each be a single bond.
[0108] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is not 0, the alkylidene group of R6 in Chemical Formula 2 may be an alkylidene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, and the alkylene group may be an alkylene group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms. Such alkylene groups or alkylidene groups may have a linear or branched chain structure and may be optionally substituted with one or more substituents.
[0109] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is not 0, R7 in Chemical Formula 2 may be -OC(=O)-, -C(=O)- or -C(=O)-O-.
[0110] When X in Chemical Formula 1 is carbon and n in Chemical Formula 2 is not 0, R8 and R9 in Chemical Formula 2 may each independently be hydrogen or an alkyl group, or may each independently be an alkyl group. In such a case, the alkyl group may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. Such an alkyl group may have a linear or branched chain structure, and may be optionally substituted with one or more substituents. In addition, when R8 and R9 are each independently an alkyl group, their carbon numbers may be the same or different from each other.
[0111] In the adhesive, the compound of formula 1 may be included in an amount of 0.1 to 50 parts by weight based on 100 parts by weight of the acrylic copolymer. In this range, the adhesive layer can exhibit the desired properties such as storage modulus and peel strength. In other examples, the ratio may be about 0.2 parts by weight or more, about 0.3 parts by weight or more, about 0.4 parts by weight or more, about 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, 9 parts by weight or more, or 10 parts by weight or more, or about 45 parts by weight or less, 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, about 15 parts by weight or less, or 10 parts by weight or less.
[0112] The pressure-sensitive adhesive may further include a crosslinking agent, which may react with the acrylic copolymer to form a crosslinked structure.
[0113] The type of crosslinking agent is not particularly limited, and general crosslinking agents such as isocyanate-based compounds, epoxy-based compounds, aziridine-based compounds, and metal chelate-based compounds can be used. Such crosslinking agents are so-called thermal crosslinking agents that realize a crosslinked structure by application of heat, and are different from radical crosslinking agents described below. Specific examples of the isocyanate-based compounds include at least one selected from the group consisting of tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, tetramethylxylene diisocyanate, naphthalene diisocyanate, and a reaction product of any one of the above with a polyol (e.g., trimethylolpropane); specific examples of the epoxy-based compounds include ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, and the like. ether, N,N,N',N'-tetraglycidylethylenediamine, and glycerin diglycidyl ether; specific examples of the aziridine-based compound include, but are not limited to, one or more selected from the group consisting of N,N'-toluene-2,4-bis(1-aziridinecarboxamide), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), and tri-1-aziridinylphosphine oxide. Specific examples of the metal chelate-based compound include, but are not limited to, compounds in which a polyvalent metal such as aluminum, iron, zinc, tin, titanium, antimony, magnesium, and / or vanadium is coordinated with acetylacetone or ethyl acetoacetate.
[0114] In the pressure-sensitive adhesive layer, the lower limit of the weight ratio of the crosslinking agent relative to 100 parts by weight of the acrylic copolymer may be about 0.01 parts by weight, 0.02 parts by weight, about 0.03 parts by weight, about 0.04 parts by weight, about 0.05 parts by weight, 0.06 parts by weight, 0.07 parts by weight, 0.08 parts by weight, or 0.09 parts by weight, and the upper limit may be about 10 parts by weight, 9 parts by weight, 8 parts by weight, 7 parts by weight, 6 parts by weight, 5 parts by weight, 4 parts by weight, about 3 parts by weight, about 2 parts by weight, about 1 part by weight, about 0.8 parts by weight, about 0.6 parts by weight, about 0.4 parts by weight, about 0.2 parts by weight, about 0.15 parts by weight, about 0.1 parts by weight, 0.09 parts by weight, 0.08 parts by weight, or 0.07 parts by weight. The ratio may be in a range equal to or greater than any one of the lower limits mentioned above; equal to or less than any one of the upper limits mentioned above; or equal to or greater than any one of the lower limits mentioned above and equal to or greater than any one of the upper limits mentioned above. By selecting the content of the crosslinking agent so as to crosslink the acrylic copolymer at an appropriate level within the above content range, the desired pressure sensitive adhesive can be effectively formed.
[0115] The pressure-sensitive adhesive layer may contain, as the crosslinking agent, a so-called radical crosslinking agent, which is a type of crosslinking agent different from the thermal crosslinking agent. Such a crosslinking agent realizes a crosslinked structure by a radical reaction. Examples of such radical crosslinking agents include so-called multifunctional acrylates, such as 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentylglycol adipate di(meth)acrylate, hydroxypivalic acid, etc. acid) neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone modified dicyclopentenyl di(meth)acrylate, ethylene oxide modified di(meth)acrylate, di(meth)acryloxyethyl isocyanurate, allyl cyclohexyl di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, ethylene oxide modified hexahydrophthalic acid di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, neopentyl glycol modified trimethylpropane di(meth)acrylate, adamantane di (meth)acrylate or difunctional acrylates such as 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorine; trifunctional acrylates such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, trifunctional urethane (meth)acrylate or tris(meth)acryloxyethyl isocyanurate; tetrafunctional acrylates such as diglycerin tetra(meth)acrylate or pentaerythritol tetra(meth)acrylate;Pentafunctional acrylates such as propionic acid modified dipentaerythritol penta(meth)acrylate; and hexafunctional acrylates such as dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, or urethane(meth)acrylate (e.g., a reaction product of an isocyanate monomer and trimethylolpropane tri(meth)acrylate), but are not limited thereto.
[0116] The radical crosslinking agent may also be present in the pressure-sensitive adhesive layer in an appropriate ratio depending on the purpose, and may be contained in an amount of, for example, 0.01 to 10 parts by weight or 0.01 to 5 parts by weight per 100 parts by weight of the acrylic copolymer.
[0117] The radical crosslinking agent is not an essential component.
[0118] In addition to the above components, the adhesive may contain appropriate additive components as necessary, and may further contain components such as a radical initiator, an ultraviolet absorber, a light stabilizer, a plasticizer and / or a crosslinking catalyst.
[0119] In the present application, the method of forming the pressure-sensitive adhesive is not particularly limited. For example, the pressure-sensitive adhesive can be formed by applying an appropriate crosslinking method to a pressure-sensitive adhesive composition containing each component (copolymer, crosslinker, etc.) that forms the pressure-sensitive adhesive, taking into consideration the type of acrylic copolymer and / or crosslinker applied to the composition. For example, if the acrylic copolymer and / or crosslinker are of a type that can be crosslinked by application of heat, a crosslinked product can be formed by applying appropriate heat, if they are of a type that can be crosslinked by irradiation of electromagnetic waves, a crosslinked product can be formed by irradiating appropriate electromagnetic waves, and other crosslinking methods can also be applied.
[0120] Such adhesives can exhibit the modulus and / or peel force properties described above.
[0121] The thickness of the adhesive of the present application is not particularly limited, and may have a normal adhesive thickness taking into consideration the intended use.
[0122] For example, the adhesive may have an appropriate thickness within the range of approximately 5 μm to 100 μm.
[0123] The present application also relates to a pressure-sensitive adhesive film or optical laminate comprising a base film and a pressure-sensitive adhesive layer formed on one or both sides of the base film. In the case of an optical laminate, the base film may be an optical film. The pressure-sensitive adhesive layer may include the pressure-sensitive adhesive described above.
[0124] The pressure-sensitive adhesive layer of the present application can be formed on one or both sides of a base film to form a pressure-sensitive adhesive film, or can be formed on one or both sides of the base film, which is an optical film, to form an optical laminate.
[0125] In this case, the type of the applicable base film is not particularly limited, and as the base film, a base film that is generally applicable to the formation of a pressure-sensitive adhesive film can be used.
[0126] For example, the substrate film may be, but is not limited to, a PET (poly(ethylene terephthalate)) film, a PTFE (poly(tetrafluoroethylene)) film, a PP (polypropylene) film, a PE (polyethylene) film, a polyimide film, a polyamide film, a COP (cyclic olefin polymer) film, a polybutene film, a polybutadiene film, a vinyl chloride copolymer film, a polyurethane film, an ethylene-vinyl acetate film, an ethylene-propylene copolymer film, an ethylene-ethyl acrylate copolymer film, an ethylene-methyl acrylate copolymer film, and / or a polyimide film.
[0127] The thickness of the base film is not particularly limited, and may be any appropriate thickness within a range suitable for the purpose.
[0128] When an optical film is used as the base film, the type of the optical film is not particularly limited. In one example, the optical film may be a polarizing film, a polarizing plate, or a retardation film. In such a case, the optical film may have a thickness in an appropriate range depending on the purpose.
[0129] The pressure-sensitive adhesive film or optical laminate may further include a release film or a protective film for protecting the pressure-sensitive adhesive layer before use, as necessary.
[0130] The present application also relates to a flexible device including an adhesive layer, an adhesive film, or an optical laminate containing the adhesive. There is no particular limitation on the application form of the adhesive layer, the adhesive film, or the optical laminate containing the adhesive in the device. For example, the adhesive layer can be used in the device for so-called OCA (Optically Clear Adhesive) or OCR (Optically Clear Resin), and therefore the application form of the adhesive layer, the adhesive film, or the optical laminate may be the same as the application form of a normal OCA or OCR.
[0131] In this case, in one example, the flexible device may include a display panel and the adhesive layer, adhesive film, or optical laminate present on one or both sides of the display panel. In this case, the display panel may be configured to be folded or rolled through one or more folding or rolling axes.
[0132] Other elements constituting the flexible device as described above are not particularly limited, and known components of a flexible device can be adopted without any limitations. Effect of the Invention
[0133] The present application can provide an adhesive that can be applied to flexible devices to effectively handle repeated deformation and recovery, does not cause defects before and after deformation (e.g., observation of deformation marks), has excellent cuttability and workability, and does not induce lifting, peeling, and / or bubble generation.
[0134] The present application also provides an adhesive layer including the adhesive, an adhesive film or optical film including the adhesive, and a flexible device such as a foldable device or a rollable device. [Brief description of the drawings]
[0135] [Figure 1] FIG. 1 shows the structure of a test specimen applied in a dynamic folding test. [Diagram 2] 1 is a diagram showing a process of performing a dynamic folding test. [Diagram 3] FIG. 1 is a diagram showing the contents of evaluation of the cuttability of a pressure-sensitive adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0136] The present application will be described in detail below based on examples and comparative examples, but the scope of the present application is not limited to the following examples.
[0137] 1. Evaluation of storage modulus The storage modulus was evaluated using ARES G2 (Advanced Rheometric Expansion System G2) (TA). A test specimen was prepared by cutting an adhesive layer having a thickness of about 0.8 mm into a circle having a diameter of about 8 mm. The adhesive layer was prepared by overlapping adhesive layers having a thickness of about 25 μm to a thickness of about 0.8 mm. The storage modulus of the test specimen at the measurement temperature was evaluated using a parallel plate fixture having a diameter of about 8 mm. The evaluation conditions during the evaluation were a frequency of 1 Hz and a strain of 5%, and the temperature was increased from -40°C to 90°C at a rate of about 10°C / min.
[0138] 2. Evaluation of peel strength The adhesive film (structure of release film / adhesive layer / base film) to be measured was cut into a rectangle with a width of about 25 mm and a length of about 100 mm to prepare a test piece. Next, the release film was peeled off, and the adhesive layer was attached to soda lime glass using a 2 kg roller according to the JIS Z 0237 standard, and left at room temperature for one day. After that, the peel force was measured by peeling the adhesive layer at a peel angle of 180 degrees and a peel speed of 0.3 m / min at room temperature using a TA (Texture Analyzer) device (Stable Micro System).
[0139] 3. Haze measurement Haze was measured after applying an adhesive having a thickness of about 25 μm to a soda lime glass having a thickness of 0.5 mm using a 2 kg roller according to the JIS Z 0237 standard, and leaving it at room temperature for one day. The measurement equipment used was a COH-400 device (Nippon Denshoku Co., Ltd.), and the evaluation was performed using a D65 standard light source.
[0140] 4. Evaluation of weight-average molecular weight The weight-average molecular weight (Mw) and molecular weight distribution were measured using GPC (Gel Permeation Chromatograph), and the measurement conditions were as follows. When measuring the weight-average molecular weight, the measurement results were converted using standard polystyrene (manufactured by Aglient system) for the preparation of the calibration curve. The molecular weight distribution was the value (Mw / Mn) obtained by dividing the weight-average molecular weight (Mw) by the number-average molecular weight (Mn) determined by the above method.
[0141] <GPC Measurement Conditions> Measuring instrument: Aglient GPC (Aglient 1200 series, U.S.) Columns: Two PL Mixed B columns connected in series Column temperature: 40 °C Eluent: THF (Tetrahydrofuran) Flow rate: 1.0 μL / min Concentration: ~1 mg / mL (100 μl injection)
[0142] 5. Dynamic Folding Test The dynamic folding test was performed by manufacturing a test piece as shown in Fig. 1. A laminate was manufactured by sequentially laminating a polyimide film 200 with a thickness of about 50 μm having a hard coating layer 100 formed on both sides, an adhesive layer 300, a polarizing plate 400, an adhesive layer 300, and a display panel 500 as shown in Fig. 1, and then cutting it into a rectangular shape with a horizontal length of about 7.8 cm and a vertical length of about 17 cm to manufacture a test piece. Next, as shown in Fig. 2, the test piece was sandwiched between parallel plates at 5 mm intervals and folded back and forth 200,000 times at -20 °C. After collecting the samples, defects such as the generation of bubbles, floating / lifting / peeling, and cracks in the hard coating layer in the samples were visually observed. If any of the above defects occurred, it was evaluated as NG, and if none of the defects occurred, it was evaluated as PASS.
[0143] 6. Cutability Test Cuttability was evaluated using test piece 400 produced by cutting a laminate having an adhesive layer 300 between two release films (light liner, heavy liner) 100, 200 to a horizontal and vertical length of 10 cm each, as shown in Figure 3. As shown in Figure 3, the length L of the protruding part of the adhesive generated during the cutting was measured, and if the length was 100 μm or more, it was evaluated as NG, and if it was less than 100 μm, it was evaluated as PASS.
[0144] 7. Evaluation of melting point and glass transition temperature The melting point was measured by a measurement method using a DSC (Differential Scanning Calorimeter). The equipment used was a DSC2500 (TA). Approximately 10 mg of the sample (copolymer) was sealed in a dedicated pan, and the endothermic and exothermic amounts were confirmed by temperature in a N2 atmosphere with a heating condition of 10°C / min and a cooling condition of -10°C / min, to measure the melting point and glass transition temperature. The measurement temperature range was -120°C to 200°C. The conditions were first cooled from room temperature (about 30°C) to -120°C at a rate of about -10°C / min, and then heated to 200°C at a heating rate of 10°C / min (first heating). Then, the sample was further cooled to -120°C at a rate of about -10°C / min, and then heated to 200°C at a heating rate of 10°C / min (second heating). The melting point was evaluated during the second heating.
[0145] Production Example 1. Production of Copolymer (A) The monomer mixture was introduced into a 1L reactor in which nitrogen gas was refluxed and a cooling device was installed for easy temperature control. The monomer mixture was a mixture of n-butyl acrylate (BA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) in a weight ratio of 6:3:1 (BA:LA:HBA). After introducing the monomer mixture and adding an appropriate amount of ethyl acetate, the reactor was purged with nitrogen gas for 1 hour to remove oxygen and the temperature of the reactor was maintained at about 62°C. The mixture was homogenized, and a reaction initiator (AIBN: azobisisobutyronitrile) was introduced at about 400 ppm, and n-dodecyl mercaptan was also introduced at about 400 ppm to initiate the reaction. The reaction was continued for about 6 to 7 hours to produce a polymer (copolymer (A)). The copolymer (polymer) (A) had a weight average molecular weight of about 2 million and a molecular weight distribution of about 4.5, and the melting point of the copolymer (polymer) (A) was about -43°C.
[0146] Production Example 2. Production of Copolymer (B) A copolymer (polymer) (B) was produced in the same manner as in Production Example 1, except that a monomer mixture of ethylhexyl acrylate (EHA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) in a weight ratio of 4:4:2 (EHA:LA:HBA) was used. The weight average molecular weight of the copolymer (polymer) (B) was about 2 million, and the molecular weight distribution was about 3.5. The melting point of the copolymer (polymer) (B) was about -42°C.
[0147] Production Example 3. Production of Copolymer (C) A copolymer (polymer) (C) was produced in the same manner as in Production Example 1, except that a monomer mixture of n-butyl acrylate (BA), lauryl acrylate (LA) and 4-hydroxybutyl acrylate (HBA) in a weight ratio of 58:40:2 (BA:LA:HBA) was used. The weight average molecular weight of the copolymer (polymer) (C) was about 2 million, and the molecular weight distribution was about 3.5. The melting point of the copolymer (polymer) (C) was about -42°C.
[0148] Example 1. A pressure-sensitive adhesive composition was prepared by mixing about 0.07 parts by weight of an isocyanate crosslinker (TKA-100, Needfill Co.), about 10 parts by weight of TEG-EH (triethylene glycol bis(2-ethylhexanoate)), and a catalytic amount of a catalyst with 100 parts by weight of the copolymer (polymer) (A) of Preparation Example 1. The catalyst used was a catalyst that promotes the urethane reaction of a hydroxyl group and an isocyanate group. The pressure-sensitive adhesive composition was diluted with a solvent (ethyl acetate) to an appropriate viscosity and mixed with a mechanical stirrer for 15 minutes or more. The mixture was kept at room temperature to remove air bubbles, and then coated on a release film (release PET (poly(ethylene terephthalate)) with a comma coater, and then kept at 140°C for about 3 minutes to form a pressure-sensitive adhesive layer with a thickness of about 25 μm.
[0149] Example 2. An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that DEHA (diethylhexyl adipate) was used instead of TEG-EH (triethylene glycol bis(2-ethylhexanoate)).
[0150] Comparative Example 1 An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that TEG-EH (triethylene glycol bis(2-ethylhexanoate)) was not used.
[0151] Comparative Example 2 An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that IPMS (isopropyl myristate) was used instead of TEG-EH (triethylene glycol bis(2-ethylhexanoate)).
[0152] Comparative Example 3. An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that TEC (triethyl citrate) was used instead of TEG-EH (triethylene glycol bis(2-ethylhexanoate)).
[0153] Comparative Example 4. An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that ATBC (Acetyl Tributyl Citrate) was used instead of TEG-EH (Triethylene Glycol Bis(2-ethylhexanoate)).
[0154] Comparative Example 5. An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that copolymer (B) of Preparation Example 2 was used instead of copolymer (A) of Preparation Example 1, and TEG-EH (triethylene glycol bis(2-ethylhexanoate)) was not used.
[0155] Comparative Example 6. An adhesive layer having a thickness of about 25 μm was formed in the same manner as in Example 1, except that copolymer (C) of Preparation Example 3 was used instead of copolymer (A) of Preparation Example 1, and TEG-EH (triethylene glycol bis(2-ethylhexanoate)) was not used.
[0156] The evaluation results of the storage modulus, haze, peel strength, dynamic folding test and cuttability of the pressure-sensitive adhesive layers of the Examples and Comparative Examples are summarized in Table 1 below.
[0157] In Table 1 below, G'(-20) is the storage modulus at -20°C, G'(25) is the storage modulus at 25°C, ΔG is the change in modulus determined by Equation 1, and DF is the result of the folding test.
[0158] In Table 1, the units of storage modulus are Pa and the units of peel force are gf / inch.
[0159] [Table 1]
Claims
1. A crosslinked acrylic copolymer is included. The storage modulus at −20° C. is 100,000 Pa or less, The peel strength to glass is 1,700 gf / inch or more, An adhesive having a haze of 0.5% or less.
2. A crosslinked acrylic copolymer is included. The rate of change in elastic modulus according to the following formula 1 is 2500 or less, Adhesive having a haze of 0.5% or less: [Formula 1] Elastic modulus change rate=(M20-M25) / 45 In Equation 1, M20 is the storage modulus of the adhesive at -20°C, and M25 is the storage modulus of the adhesive at 25°C.
3. An adhesive comprising a crosslinked acrylic copolymer and a compound of the following formula 1: [Chemical formula 1] [Formula 1] In formula 1, X is carbon or nitrogen, and R 1 ~R 3 are each independently a hydrogen atom, an alkyl group, or a hydroxyl group; R 4 is a substituent of the following formula 2, and when X is nitrogen, R 4 does not exist, and R 1 ~R 3 At least one of the groups is a hydroxy group: [Chemical formula 2] [Case 2] In Chemical Formula 2, R 5 is a single bond, an oxygen atom, -L 1 -C(=O)-L 2 -, -L 1 -C(=O)-OL 2 - or -L 1 -OC(=O)-L 2 -, and said L 1 and L 2are each independently a single bond, an alkylene group, or an alkylidene group; R 6 is an alkylidene group or an alkylene group, R 7 is a single bond, —O—C(═O)—, —C(═O)—, or —C(═O)—O—, and R 8 and R 9 are each independently a hydrogen or an alkyl group, and n is a number in the range of 0 to 10.
4. The pressure-sensitive adhesive according to claim 2 or 3, having a storage modulus at -20°C of 100,000 Pa or less.
5. The pressure-sensitive adhesive according to claim 2 or 3, which has a peel strength from glass of 1,800 gf / inch or more.
6. The pressure-sensitive adhesive according to claim 1 , which has a storage modulus at 25° C. of 10,000 Pa or more.
7. The pressure-sensitive adhesive according to claim 1 , wherein the acrylic copolymer has a weight average molecular weight of 1,000,000 or more.
8. The pressure-sensitive adhesive according to any one of claims 1 to 3, wherein the acrylic copolymer comprises an alkyl (meth)acrylate unit, a unit of the following chemical formula 3, and a polar functional group-containing unit: [Chemical formula 3] [C3] In Chemical Formula 3, R 1 represents hydrogen or an alkyl group; R 2 represents an alkyl group having 11 to 13 carbon atoms.
9. The pressure-sensitive adhesive according to claim 8, wherein the alkyl (meth)acrylate unit has a linear or branched alkyl group having 1 to 10 carbon atoms.
10. The pressure-sensitive adhesive according to claim 8 , wherein the polar functional group-containing unit is a unit derived from a hydroxy group-containing monomer.
11. The pressure-sensitive adhesive according to claim 8, wherein the acrylic copolymer contains 10% by weight to 80% by weight of alkyl (meth)acrylate units.
12. The pressure-sensitive adhesive according to claim 8, wherein the acrylic copolymer contains 10 to 300 parts by weight of the unit of formula 3 per 100 parts by weight of the alkyl (meth)acrylate unit.
13. The pressure-sensitive adhesive according to claim 8, wherein the acrylic copolymer contains 1 to 100 parts by weight of the polar functional group-containing unit per 100 parts by weight of the alkyl (meth)acrylate unit.
14. A pressure-sensitive adhesive film comprising: a base film; and the pressure-sensitive adhesive according to claim 1 formed on one or both sides of the base film.
15. An optical laminate comprising: an optical film; and the pressure-sensitive adhesive according to claim 1 formed on one or both sides of the optical film.
16. A display panel configured to be folded or rolled about one or more folding or rolling axes; and A flexible device comprising the adhesive of claim 1 present on one or both sides of the display panel.
Citation Information
Patent Citations
Adhesive for optical film, adhesive layer for optical film, optical member and image display device
JP2017095653A
Adhesive sheet, repeated bending laminate member and repeated bending device
JP2020139035A
Surface protection film
JP2022548286A
Adhesive composition for foldable displays and adhesive film for foldable displays containing the cured product
JP2023541062A
Adhesive film, optical member including same, and optical display device including same