Method for producing catalytic membranes, catalytic membranes obtained thereby, and their uses

The spark ablation-based method for producing catalyst nanoparticles directly on membranes addresses the inefficiencies of existing electrocatalyst synthesis, achieving cost-effective, scalable, and high-performance catalyst layers with reduced noble metal usage.

JP2024543151APending Publication Date: 2024-11-19フェーエスパーティクル·ホールディング·ベー·フェー
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024531286
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-18
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing methods for producing electrocatalysts, particularly for proton exchange membrane (PEM) water electrolyzers, are complex, costly, and inefficient, with high reliance on noble metals like Pt and Ir, necessitating a simpler, scalable, and cost-effective method for synthesizing single/bi-metal/multi-metal electrocatalysts.

Method used

A method involving spark ablation to generate an aerosol of catalyst nanoparticles, which are then deposited directly onto a membrane without a binder, using vapor-phase nanoparticle aerosol printing to form a catalyst layer with low nanoparticle loading, achieving uniform and reproducible thin layers.

Benefits of technology

This method reduces the capital cost of PEM water electrolysis by minimizing noble metal usage, ensuring high catalytic activity and stability with reduced series resistance, enabling the production of high-quality, thin catalyst layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543151000001_ABST
    Figure 2024543151000001_ABST
Patent Text Reader

Abstract

1. A method for making a catalytic film, comprising: providing a film; generating an aerosol of catalytic nanoparticles by spark ablation; and directing the aerosol of catalytic nanoparticles toward a first side of the film such that the catalytic nanoparticles are deposited on the film, thereby forming a catalytic film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a catalytic membrane by generating an aerosol of catalytic nanoparticles. The present invention further relates to a catalytic membrane produced through said method, the membrane comprising catalytic nanoparticles attached to the membrane, a membrane electrode assembly comprising the catalytic membrane, and uses of the catalytic membrane. [Background technology]

[0002] Hydrogen will play a pivotal role in the transition to a low-carbon economy. Water electrolysis is expected to be important in establishing a global hydrogen market. Among various water electrolysis technologies, proton exchange membrane (PEM) electrolysis is promising due to its efficiency, compact design, and promise of dynamic operation. However, PEM electrolyzers rely on the use of rare and expensive precious metal catalysts (Pt-based catalysts at the cathode and Ir-based catalysts at the anode), which imposes limitations on market penetration.

[0003] Electrocatalysis has become an interesting and fast-growing field of catalysis in recent years, as researchers investigate new methods and materials to catalyze reactions related to energy storage and chemical synthesis. Significant progress has been made in the development of proton exchange membrane (PEM) water electrolysis devices, with Ir-based electrodes among the most active and stable electrocatalysts to promote the slow oxygen evolution reaction (OER). Currently, noble metal-based materials (Pt, Ir, Ru, Rh) are the most active for both the hydrogen evolution reaction (HER) and the oxygen evolution reaction (OER). To make these electrochemical processes scalable and commercially viable, their noble metal content must be reduced or replaced by cheaper alternatives such as Ni, Fe, Co, and Mn (among others). Methods for rapid and reproducible synthesis of a wide variety of single / bi- / multi-metal electrocatalysts are therefore not only highly desirable, but also crucial for today's researchers to create and compare novel electrocatalysts to address modern energy and chemical challenges.

[0004] Furthermore, Ir-based electrodes are currently synthesized through various multi-step approaches. These steps may include the preparation of a "catalyst ink" from pre-synthesized Ir nanoparticles and the subsequent application of this dispersion to the desired substrate (e.g., Ti felt, carbon). The latter step is typically achieved by air-assisted spray deposition onto a diffuse substrate or directly onto a membrane, or by a decal transfer technique. Reactive spray deposition and magnetron sputtering of Ir layers have been reported as alternatives to conventional techniques for the preparation of catalyst coated membranes (CCMs). Ideally and to minimize Ir loading, the deposition should result in a uniform catalyst layer with reduced Ir packing density. In addition, colloidal Ir nanoparticles can also be prepared and deposited onto substrates. Such methods require many well-thought-out steps to obtain an active electrocatalyst. Furthermore, using colloidal nanoparticles requires the removal of corrodible ligands to expose the Ir-based nanoparticle surface. It is therefore highly desirable to simplify the electrode synthesis process in order to reproducibly obtain active Ir-based electrocatalysts.

[0005] Significant developments have been made in recent years with respect to cathode electrocatalysis, particularly with respect to reducing the platinum group metal (PGM) dependency on cathode electrocatalysis for PEM water electrolysis. Studies have shown that by introducing electrocatalysts that do not contain precious metals (e.g., MoS2, CoP, FeP, NiP2 catalysts) or by reducing the Pt loading by a factor of 10, the performance of PEM water electrolyzers can still be sufficiently high. However, enabling a similar success with anode electrocatalysis remains a major challenge for PEM water electrolyzers. To reduce the Ir loading and thereby the specific power density of Ir, literature studies have been primarily focused on maximizing Ir dispersion through the use of high surface area supports (TiO2, TiC, TaC). Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above, there is a need in the art for improved methods for rapid, scalable, and cost-effective production of mono / bi / multi-metallic electrocatalysts. Additionally, there is a need in the art for reproducible, affordable, high quality, uniform, thin, mono / bi / multi-metallic electrocatalysts. [Means for solving the problem]

[0007] It is an object of the present invention, among other objects, to address the above-mentioned needs in the art, which objects are met by the present invention as outlined in the appended claims.

[0008] In particular, the above objects, among others, are achieved by the present invention according to a first aspect by a method for producing a catalytic membrane or an electrolytic membrane with a catalytic layer, the method comprising the steps of: - providing a membrane: - generating an aerosol of catalytic nanoparticles by spark ablation; - directing an aerosol of catalytic nanoparticles onto a first side of the membrane such that the catalytic nanoparticles are deposited on the membrane, thereby forming a catalytic membrane or a catalytically layered electrolytic membrane.

[0009] In contrast to conventional methods for the development of catalytically layered electrochemical membranes (CCMs), which are based on a process involving catalyst synthesis by generating an aerosol of catalytic nanoparticles and applying the catalytic nanoparticles to a membrane, the method of the present invention provides low nanoparticle (e.g., metal nanoparticles such as Ir nanoparticles) loading by introducing an alternative catalyst layer manufacturing technique. The method of the present invention uses nanoparticle deposition techniques, including gas-phase nanoparticle aerosol printing, to generate CCMs under low nanoparticle loading compared to the current state of the art, thereby lowering the capital cost of PEM water electrolysis without compromising activity or stability, whereby no binder is required to attach the nanoparticles to the membrane. Thus, transport of the generated ions from the catalyst towards the membrane does not require transport through or along the binder, which may cause reduced transport quality for ions such as hydrogen ions, hydronium or hydroxide, and / or reduced electrical conductivity (electron transport). The generated nanoparticles are also surfactant-free, preferably surfactant-free Ir nanoparticles. Using the method of the present invention, Ir was deposited onto a Nafion 115 polymer exchange membrane and the final CCM was representative of an industrial electrolyzer.

[0010] According to a preferred embodiment, the present invention relates to a method for producing a catalyst film, wherein the spark ablation is performed by at least one spark generator. The method of the present invention comprises a gas phase process, in other words spark ablation (or spark discharge), to produce nanoparticles with a particle size of less than 10 nm, free of impurities, free of surfactants and / or ligands. Optionally, at least one spark generator can be used in series and / or parallel, e.g. as a co-catalyst, to allow higher throughput of the printer and / or the mixing of nanoparticles of different compositions.

[0011] According to another preferred embodiment, the present invention relates to a method for producing a catalytic membrane, the membrane being an ion-conducting polymer, preferably the membrane is adapted to conduct hydrogen ions, hydroxide or hydronium ions. Preferably, the ion-conducting membrane is a proton exchange membrane selected from the group consisting of polysulfonic acid polymers, perfluorocarbon sulfonic acid polymers, polyacrylic acid polymers, preferably perfluorocarbon sulfonic acid polymers and polysulfonic acid polymers. The ion-conducting polymer may for example be a sulfonated tetrafluoroethylene-based fluoropolymer-copolymer, such as the polymer commonly known under the trade name Nafion.

[0012] According to another embodiment, the ion conducting membrane is an anion exchange membrane. According to yet another preferred embodiment, the present invention relates to a method for producing a catalytic membrane, further comprising the step of allowing the aerosol of catalytic nanoparticles to pass through a nozzle after creating the aerosol of catalytic nanoparticles, and directing the aerosol of catalytic nanoparticles towards the membrane comprises directing the aerosol of catalytic nanoparticles through the nozzle and towards the membrane.

[0013] According to a preferred embodiment, the present invention relates to a method for producing a catalyst film, where an aerosol of catalyst nanoparticles is accelerated through a nozzle into a vacuum downstream of the nozzle. The nanoparticle aerosol produced by spark ablation can be deposited directly onto a substrate (e.g. Nafion 115 polymer) using inertial impaction. This is achieved by accelerating the nanoparticle aerosol through a nozzle aimed at the substrate. The pressure difference introduced by holding the substrate under a rough vacuum (approximately 1 mbar) is the driving force for accelerating the nanoparticle aerosol through the nozzle. The inertial impaction results in the adhesion of the nanoparticles to the substrate without the need for a binder, preserving the purity / cleanliness of the particles. Surprisingly and advantageously, this adhesion is strong enough to prevent the catalyst nanoparticles from being washed away under typical operating conditions. By securing the substrate on an XY(Z)-stage, the nanoparticles are efficiently patterned on the substrate. This approach allows for the production of reproducible CCMs in a single step (as opposed to conventional methods) and also leads to the production of high quality and uniform thin catalyst layers.

[0014] According to yet another preferred embodiment, the present invention relates to a method for producing a catalytic film, wherein the gas pressure upstream of the nozzle is in the range of 0.8 bar to 1.4 bar, preferably 0.9 bar to 1.3 bar, more preferably 1 bar to 1.2 bar. Operating the spark generator at higher pressures tends to increase the mass output and particle size, which is beneficial for the throughput of the printer. The indicated pressure ranges have the benefit of increased mass output, while films are produced with good performance.

[0015] According to another preferred embodiment, the present invention relates to a method for producing a catalytic membrane, in which the pressure of the vacuum downstream of the nozzle ranges from 0.1 mbar to 4 mbar, preferably from 0.5 mbar to 2.5 mbar, more preferably from 1 mbar to 2 mbar. The pressure of the vacuum downstream of the nozzle determines the kinetic energy of the nanoparticles depositing on the membrane, the preferred pressure being high enough to prevent damage during membrane production and low enough to allow sufficient adhesion of the catalytic nanoparticles, to avoid said nanoparticles being washed away during operation.

[0016] According to yet another preferred embodiment, the present invention relates to a method for producing a catalytic membrane, wherein the pressure at the nozzle inlet is less than 900 mbar, preferably less than 800 mbar, more preferably less than 700 mbar.

[0017] In the method, a virtual impactor (large particle filter / low pass filter) can be used to remove micron-sized debris that may be present in the aerosol. The virtual impactor can be placed upstream of the nozzle and / or next to the nozzle inlet. Reducing the pressure in the virtual impactor to the pressures mentioned above will promote separation between large and small particles.

[0018] According to a preferred embodiment, the present invention relates to a method for producing a catalytic membrane, where catalytic nanoparticles are directly attached to the membrane in a binder-free manner.

[0019] According to another preferred embodiment, the present invention relates to a method for producing a catalytic film, whereby catalytic nanoparticles are deposited by inertial impaction onto the film.

[0020] When producing films, it is preferred to keep the substrate under a rough vacuum (approximately 1 mbar): the nanoparticle aerosol is accelerated through a nozzle, and inertial impaction results in the nanoparticles adhering to the substrate without the need for a binder, preserving particle purity / cleanliness.

[0021] According to yet another preferred embodiment, the present invention relates to a method for producing a catalytic film, wherein the catalytic nanoparticles are composed of one or more elements selected from the group consisting of Ir, Pt, Ru, Rh, Au, Ag, Ni, Fe, Co, Ti, C, Mo and Mn and / or their oxides, which may include combinations of the listed metal elements and metal oxides of the listed elements.

[0022] According to another preferred embodiment, the invention relates to a method for producing a catalytic film, wherein the catalytic nanoparticles consist of iridium or iridium oxide.

[0023] According to a preferred embodiment, the present invention relates to a method for producing a catalyst film, wherein the catalyst nanoparticles are amorphous nanoparticles and have an average particle size in the range of 0.5 nm to 10 nm, preferably 1 nm to 7 nm, more preferably 1.5 nm to 3 nm, and most preferably 2 nm to 2.5 nm. The particle size and size distribution were confirmed by transmission electron microscopy (TEM) of Ir nanoparticles prepared through spark ablation according to the method of the present invention.

[0024] According to another preferred embodiment, the present invention relates to a method for producing a catalytic membrane having a catalytic activity of 0.2 mgIr / cm 2 More than 1.8mgIr / cm 2 Less than 0.4 mgIr / cm, preferably 0.4 mgIr / cm 2 More than 1.2mgIr / cm 2 Less than 0.4 mgIr / cm, most preferably 0.4 mgIr / cm 2 More than 0.8mgIr / cm 2The iridium is deposited to form a catalyst layer with a mass per unit area in the following ranges: 1. The results show that high performance catalyst membranes are obtained within the claimed ranges. A higher mass per unit area would result in a more expensive membrane and also a membrane of lower quality. A lower mass per unit area would result in a membrane of lower quality in terms of current CCMs on the market. Considering the demands of practical application and the demands of operation at a certain current density, the applied voltage, the specific electrical consumption and the Ir-specific power density should be as low as possible while the energy efficiency should be high. Based on these criteria, an Ir loading of 0.4 mg / cm2 was selected. 2 More than 0.8mg / cm 2 The following CCMs produced through the method of the present invention were identified as the most promising:

[0025] According to yet another preferred embodiment, the present invention relates to a method for producing a catalytic film, wherein the aerosol of catalytic nanoparticles is passed through a filter before passing through a nozzle. Preferably, the produced aerosol of catalytic nanoparticles is passed through a filter, preferably a low pass filter, to remove particles larger than a threshold size from the aerosol. The threshold size preferably ranges from 0.1 μm to 10 μm, more preferably the threshold size is 0.1 μm.

[0026] According to a preferred embodiment, the present invention relates to a method for producing a catalytic membrane, further comprising attaching a porous transport layer to a first side of the catalytic membrane, the porous transport layer being electrically conductive, thereby forming a membrane electrode assembly. The porous transport layer enhances the mobility of electrons and gaseous species across the membrane surface.

[0027] According to one embodiment, the deposited iridium catalyst or iridium oxide nanoparticles have a layer thickness in the range of 1 μm to 3 μm and / or a layer thickness density of 3.9 gIr / cm 3 More than 3.9 gIr / cm, preferably 3.9 gIr / cm 3 More than 10gIr / cm 3 More preferably, the range is 3.9 gIr / cm 3More than 8.0gIr / cm 3 These high Ir densities allow the use of thinner catalyst films, reducing transport limitations perpendicular to the plane of the membrane.

[0028] In general, the deposited layers of catalytic nanoparticles according to the present invention are relatively small while having surprisingly high availability of catalytically active sites, which allows the use of thinner catalytic nanoparticle layers, which in turn reduces the series resistance of the membrane.

[0029] In this patent disclosure, the term "catalyst membrane" may be substituted with "catalyst coated membrane."

[0030] According to a second aspect, the present invention relates to a catalytic membrane produced according to the inventive method as disclosed above.

[0031] According to another preferred embodiment, the present invention relates to a catalytic membrane, comprising a membrane and catalytic nanoparticles directly attached to the membrane in a binder-free manner.

[0032] According to yet another preferred embodiment, the present invention relates to a catalytic membrane, the membrane being an ion-conducting membrane, preferably a proton-conducting membrane.Preferably, the ion-conducting membrane is a proton exchange membrane selected from the group consisting of polysulfonic acid polymers, perfluorocarbon sulfonic acid polymers, polyacrylic acid polymers, preferably perfluorocarbon sulfonic acid polymers and polysulfonic acid polymers.The ion-conducting polymer may be, for example, a sulfonated tetrafluoroethylene-based fluoropolymer-copolymer, such as the polymer commonly known under the trade name Nafion.

[0033] According to another embodiment, the ion-conducting membrane is an anion exchange membrane.

[0034] According to another preferred embodiment, the present invention relates to a catalytic membrane, wherein the catalytic nanoparticles are metal nanoparticles or metal oxide nanoparticles. Preferably, the catalytic nanoparticles are composed of one or more elements selected from the group consisting of Ir, Pt, Ru, Rh, Au, Ag, Ni, Fe, Co, Ti, C, Mo and Mn and / or oxides thereof. This may include combinations of the listed metal elements and metal oxides of the listed elements. Most preferred catalytic nanoparticles are composed of iridium, iridium oxide, or combinations thereof.

[0035] According to a preferred embodiment, the present invention relates to a catalytic membrane, the catalytic layer having a mass per unit area of ​​0.2 mgIr / cm 2 More than 1.8 mgIr / cm 2 Less than 0.4 mgIr / cm, preferably 0.4 mgIr / cm 2 More than 1.2mgIr / cm 2 Less than 0.4 mgIr / cm, most preferably 0.4 mgIr / cm 2 More than 0.8mgIr / cm 2 Including iridium having the following ranges:

[0036] According to another preferred embodiment, the present invention relates to a catalyst membrane, in which the catalyst nanoparticles have an average particle size in the range of 0.5 nm to 10 nm, preferably 1 nm to 7 nm, more preferably 1.5 nm to 3 nm, most preferably 2 nm to 2.5 nm. The smaller the particle, the higher the specific surface area. The reduced particle size with respect to the particle size of catalyst nanoparticles in the prior art further allows the formation of a catalyst layer with a higher density of catalyst nanoparticles and increased porosity, allowing the use of thinner catalyst layers to prevent mass transport limitations of the catalyst membrane.

[0037] According to yet another preferred embodiment, the present invention relates to a catalytic film, wherein the catalytic nanoparticles are amorphous nanoparticles. The catalytic nanoparticles used in the prior art are generally crystalline nanoparticles, in contrast to the amorphous nanoparticles of the present invention, which provide an improved catalytic surface / activity. The use of spark ablation to create iridium (oxide) nanoparticles as in the preferred embodiment of the present invention is advantageous since amorphous nanoparticles are formed.

[0038] It will be appreciated that any features and / or advantages of the second aspect described above can be readily implemented and / or applied in the method of the first aspect, and vice versa, as well as the further aspects below.

[0039] According to a further aspect, the present invention relates to a membrane electrode assembly (MEA) comprising the catalytic membrane of the invention as described above and / or below. Preferably, the membrane electrode assembly is configured for water electrolysis.

[0040] According to a further aspect, the present invention relates to the use of a catalytic membrane or a membrane electrode assembly as disclosed herein for water electrolysis.

[0041] The invention will be further detailed in the following examples and figures. [Brief description of the drawings]

[0042] [Figure 1] Figure 1 shows polarization curves recorded at room temperature for a catalyst membrane of the invention and a commercial CCM. The labeled loadings correspond to Ir loadings (0.2 mg / cm2 to 2.4 mg / cm2). The commercial CCM contains a 2 mg cm-2 IrRuOx anode. [Diagram 2] Figure 2 shows the effect of Ir loading on the catalyst membrane of the present invention; (a) the cell potential required to pass a current density of 200 mA cm-2; (b) the current density obtained under a constant cell polarization of 1.8 V. [Diagram 3]Figure 1 shows the effect of Ir loading on the Ir specific power density of the catalyst membrane of the present invention when operated under the following conditions: (a) constant current density of 200 mA cm-2, (b) constant cell polarization of 1.8 V. The total amount of PGM metals (Ir+Ru) was considered in the calculation for the commercial CCM. [Figure 4] Scanning electron microscope images of the thickness and density of the Ir layer of the catalyst membrane of the present invention (left, 0.8 mg / cm2) and a commercial sample (right, 2 mg / cm2) are shown. [Diagram 5] Polarization curves recorded at 60° C. for the catalyst membrane of the present invention and a commercial sample are shown. The labeled loadings correspond to Ir loadings of 0.4 mg / cm2 and 0.8 mg / cm2. The commercial CCM contains an IrRuOx anode of 2 mg / cm2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] [Example] Example 1 - Fabrication of an Ir-based membrane electrode assembly (MEA) via spark ablation and vapor deposition onto a Nafion membrane.

[0044] Five different catalytic films (CCMs) (samples 1 to 5) were fabricated according to the method of the present invention, with different thicknesses (and therefore Ir loadings) of spark ablation-produced Ir-based materials. A square deposition area of ​​2.0 x 2.0 cm was achieved by depositing a constant flow of nanoparticles (i.e., fixed voltage, current, and gas flow rate) directly onto the film through the nozzle and moving the nozzle relative to the substrate using a scripted deposition procedure at a constant printing speed. Different metal loadings were obtained by varying the printing speed while maintaining the same Ir power settings on the nanoparticle generator, with faster printing speeds yielding shorter printing times and therefore lower metal loadings.

[0045] [Sample 1] A polymer membrane (Nafion 115 membrane (4.0 cm x 4.0 cm x 0.125 mm, FuelCellEtc.) was fixed to the substrate container in a vacuum chamber, which was evacuated to a pressure of 1 mbar. Ir nanoparticles were generated using a spark ablation nanoparticle generator (VSP-G1, Nanoparticles were fabricated using a VSP particle ion exchanger (VSP-G1) and deposited on a Nafion-115 film by inertial impaction. The VSP-G1 employed 13 W (1.3 kV, 10 mA) with an Ar flow rate of 2.0 L / min. The nanoparticle stream was delivered into the vacuum chamber through a nozzle (d=0.35 mm) while maintaining the pressure at 1 mbar. By moving the substrate under the nozzle in the XY plane, a deposition area of ​​2.0 × 2.0 cm was achieved, thus depositing nanoparticles in 100 parallel lines at a constant printing speed. Each line was 20 mm long, yielding a total printing length of 2000 mm. 0.4 mg / cm 2 A printing speed of 200 μm / s was employed to achieve an Ir loading of .

[0046] [Sample 2] 0.8 mg / cm 2 In order to achieve this Ir loading, the same method as in Sample 1 was adopted, except that the printing speed was 80 μm / s.

[0047] [Sample 3] 1.2 mg / cm 2 In order to achieve this Ir loading, the same method as in Sample 1 was adopted, except that the printing speed was 60 μm / s.

[0048] [Sample 4] 1.8 mg / cm 2 In order to achieve this Ir loading, the same method as in Sample 1 was adopted, except that the printing speed was 40 μm / s.

[0049] [Sample 5] 2.4 mg / cm 2 In order to achieve this Ir loading, the same method as in Sample 1 was adopted, except that the printing speed was 30 μm / s.

[0050] [Table 1]

[0051] Samples 1 to 5 (Pt-C on carbon cloth, 4 mg Pt cm 2 The membrane electrode assemblies (including samples 1 to 5) were completed by connecting a Pt cathode to the other side of the Nafion membrane of a 1000-kV Nafion ... 2 PEM was added to the electrolyzer. The operating temperature was monitored using a K-type thermocouple and controlled with an Omega CN16DPT-144-EIP temperature controller. Deionized water was delivered to the anode and cathode compartments at a flow rate of 10 ml / min using a dual channel peristaltic pump (Masterflex C / L). Electrochemical data were collected using a Vertex potentiostat / galvanostat (Ivium Technologies). Polarization curves were obtained by holding a constant potential step for 3 min.

[0052] [Example 2] Performance test of various CCMs with different Ir addition amounts The performance tests were carried out on various CCMs with different Ir doping amounts obtained in Example 1. The performance tests were carried out by electrolysis at room temperature, and the Ir doping amount was 0.4 mg / cm. 2 More than 2.4mg / cm 2 Similar experiments were performed using a commercial prior art CCM equipped with an IrRuOx anode at 2 mg / cm 2 The experiment was carried out with an addition amount of 1000 ml.

[0053] Polarization curves were recorded at room temperature using the various prepared CCMs (see Figure 1). The current density (representative of the hydrogen evolution rate) at a given potential was 0.2 mg cm−1 for Ir doping in the CCM. -2 to 1.2 mg cm -2However, it decreased again with further increase in Ir doping (1.8 mg cm -2 and 2.4 mg cm -2 Considering that the active sites of the reaction are located at the catalyst / membrane / water interface, the observed decrease in activity may be due to the blocking of the active sites when higher amounts of Ir are deposited. For comparison, a commercial membrane electrode assembly (2 mg cm) -2 The polarization curves obtained for IrRuOx are also shown in Figure 1. It is clearly shown that the VSP-CCM outperforms the commercial CCM with a lower Ir content.

[0054] To allow for improved comparison, Figures 2a and 2b were constructed based on the polarization data of Figure 1. Figure 2a shows the polarization at 200 mA / cm 2 Figure 2b shows the potential (indicative of the energy required) required to perform electrolysis at a constant rate of 1.8 V. Figure 2c shows the current density (indicative of the hydrogen production rate) obtained when the cell is polarized at a constant potential of 1.8 V. These figures demonstrate the great potential of the method of the present invention to produce highly active CCM with reduced Ir loading compared to known commercial CCM.

[0055] To quantify the Ir utilization in CCM, the Ir specific power density was used as a descriptor. A lower value of this parameter indicates a lower amount of Ir required to perform electrolysis at a certain specific power density. The value of Ir specific power density is expressed as the ratio of Ir to Ir at a particular current density (200 mA cm -2 , Fig. 3a) and the cell operation at a specific applied potential (1.8 V, Fig. 3b). -2 More than 1.8 mg cm -2 FIG. 3a, b suggests that the method of the invention can produce CCMs with improved Ir utilization, since the Ir specific power density using Ir-based CCMs (see below) can be reduced by up to an order of magnitude compared to known commercial CCMs.

[0056] To evaluate the activity of the CCM, two further performance indicators were used based on the EU harmonized protocols for testing of low temperature water electrolysers [Tsotridis, G. and Pilenga, A., “EU harmonised protocols for testing of low temperature water electrolysers”, DOI:10.2760 / 58880]. The energy efficiency (ε) is defined as the ratio between the total amount of energy required to split 1 mol of water under reversible conditions and the actual amount of energy (electrical and thermal) used in the process, including the energy required to overcome irreversibilities. The energy efficiency of a single cell, ε cell can be expressed as:

[0057]

number

[0058] Here, U cell is the measured cell voltage, Q input is the amount of heat supplied to the cell by an external heat source. Thermodynamics tells us that the thermoneutral potential (U tn ) is equal to 1.48V in standard conditions, and the cell is tn When operating at a higher potential, Q input is equal to zero.

[0059] Specific power consumption (SEC) is kWh Nm 3 H2 and is expressed as 1Nm 3 (or equivalently 1 kg) of hydrogen. In our case, the SEC is 200 mA cm -2 The SEC was calculated by considering the cell operating at a current density of 1000 s. The SEC is given by:

[0060]

number

[0061] P cellis the input power to the cell. Assuming a faradaic efficiency of 100% (no current loss), this is 200 mA cm -2 The H2 production rate at is 3.6x10 -4 Nm 3 h -1 Table 2 shows the four performance indicators we used to evaluate the activity of the VSP-CCM, including key physical properties. The Ir layer thickness of the electrocatalyzed membranes of the present invention and commercial samples was measured by scanning electron microscopy (SEM) (see also Figure 4).

[0062] [Table 2]

[0063] Considering the requirements for practical application, the energy efficiency must be high, while the specific power consumption and Ir specific power density must be as low as possible for operation at a specific current density and applied potential. Based on these criteria, the Ir loading of 0.4 mg cm -2 and 0.8 mg cm -2 The following CCMs of the present invention were identified as the most promising ones for follow-up investigation. Figure 4 shows the polarization curves obtained for the two most promising CCMs of the present invention during water electrolysis at 60 °C. The Ir specific power density is significantly reduced (0.4 mg cm) compared to the commercial one (5.88 g Ir / kW). -2 CCM: 1.19 gIr / kW, 0.8 mg cm -2 For CCM, it is 2.45gIr / kW).

[0064] Stability and durability testing of the samples showed acceptable stability and good durability.

[0065] Further embodiments The proton exchange membrane (PEM) used in this patent disclosure can be based on polysulfonic acid materials, such as those commercially available under the names Aquivion® and Nafion®. Other proton exchange membranes may be used. Proton exchange membrane materials that can be used to implement the present invention can be perfluorocarbon sulfonic acid or polysulfonic acid polymers (e.g., those commercially available under the names Nafion®, Aquivion®, Fumapem®-F, Fumapem® SX Pemion®), polybenzimidazole membranes (especially capable of use at high temperatures), such as those commercially available under the names Celtec®, Fumapem® AM, Fumapem® ST, polyacrylic acid, hydrocarbon membranes (e.g., those commercially available under the names Fumatech® ST, Fumatech® P, E). The preferred materials for the proton exchange membrane are perfluorocarbon sulfonic or polysulfonic acid polymers, or polyacrylic acid, most preferably perfluorocarbon sulfonic or polysulfonic acid polymers.

[0066] The present invention is also applicable in the field of anion exchange membranes (AEM). AEM materials containing quaternary ammonium groups (e.g., those sold under the trade names Fumasep® FAA, A201, Orion® TM1, Durion®, Selemion®) or low-density polyurethanes with quaternary ammonium groups; anion exchange membrane materials with imidazolium or polybenzimidazole groups (e.g., those sold under the trade names Aemion®, Sustainion®), or tri- or di-amine crosslinked quaternized polysulfone. Preferred anion exchange membrane materials are those with quaternary ammonium groups, low-density polyurethanes with quaternary ammonium groups, or anion exchange membranes with imidazolium or polybenzimidazole groups. A particularly preferred choice is the use of anion exchange membranes based on materials with vinylbenzyl chloride groups and imidazolium groups (e.g., those sold under the trade name Sustainion®). Low density polyethylene (LDPE), including grafted LDPE, is another preferred option.

Claims

1. A method for producing a catalyst film, comprising the steps of: Providing a membrane; generating an aerosol of catalytic nanoparticles by spark ablation; and Directing the aerosol of catalytic nanoparticles toward a first side of the membrane such that the catalytic nanoparticles are deposited on the membrane, thereby forming a catalytic membrane.

2. The method of claim 1 , wherein the spark ablation is performed by at least one spark generator.

3. 3. The method of claim 1 or 2, wherein the membrane is an ion-conducting polymer, preferably the membrane is configured to conduct hydrogen ions, hydroxide or hydronium ions.

4. 4. The method of claim 1, 2 or 3, further comprising, after generating the aerosol of catalytic nanoparticles, passing the aerosol of catalytic nanoparticles through a nozzle, and directing the aerosol of catalytic nanoparticles toward the membrane comprises directing the aerosol of catalytic nanoparticles that has passed through the nozzle toward the membrane.

5. The method of claim 4 , wherein the aerosol of catalytic nanoparticles is accelerated through the nozzle and into a vacuum downstream of the nozzle.

6. 6. The method of claim 5, wherein the gas pressure upstream of the nozzle is in the range of 0.8 bar to 1.4 bar.

7. 7. The method according to claim 5 or 6, wherein the pressure of the vacuum downstream of the nozzle is in the range of 0.1 mbar to 4 mbar.

8. 7. The method according to claim 6, wherein the pressure at the inlet of the nozzle is less than 900 mbar, preferably less than 800 mbar, more preferably less than 700 mbar.

9. The method according to any one of claims 1 to 8, wherein the catalytic nanoparticles are directly attached to the membrane in a binder-free manner.

10. The method of any one of claims 1 to 9, wherein the catalyst nanoparticles are deposited by inertial impaction onto the membrane.

11. 11. The method of any one of claims 1 to 10, wherein the catalyst nanoparticles are composed of one or more elements selected from the group consisting of Ir, Pt, Ru, Rh, Au, Ag, Ni, Fe, Co, Ti, C, Mo and Mn and / or their oxides.

12. The method of any one of claims 1 to 11, wherein the catalytic nanoparticles are composed of iridium or iridium oxide.

13. 13. The method according to any one of claims 1 to 12, wherein the catalyst nanoparticles are amorphous nanoparticles having an average particle size in the range of 0.5 nm to 10 nm, preferably 1 nm to 7 nm, more preferably 1.5 nm to 3 nm, and most preferably 2 nm to 2.5 nm.

14. 0.2mgIr / cm 2 More than 1.8 mgIr / cm 2 Less than 0.4 mgIr / cm, preferably 0.4 mgIr / cm 2 1.2mgIr / cm or more 2 or less, most preferably 0.4 mgIr / cm 2 More than 0.8 mgIr / cm 2 13. The method of claim 10 or 12, wherein the iridium is deposited to form a catalyst layer having a mass per unit area in the following range:

15. A method according to any one of the preceding claims, wherein the aerosol of produced catalytic nanoparticles is passed through a filter, preferably a low pass filter.

16. 16. The method of claim 15, wherein the aerosol of catalytic nanoparticles passes through a filter before passing through a nozzle.

17. 17. The method of any one of claims 1 to 16, further comprising attaching a porous transport layer to the first side of the catalytic membrane, the porous transport layer being electrically conductive, thereby forming a membrane electrode assembly.

18. 18. A catalytic membrane produced according to the method of any one of claims 1 to 17.

19. A catalytic membrane comprising a membrane and catalytic nanoparticles directly attached to the membrane by a binderless method.

20. 20. The catalytic membrane of claim 18 or 19, wherein the membrane is an ion-conducting membrane.

21. 21. The catalytic membrane according to any one of claims 18 to 20, wherein the membrane is an ion-conducting polymer selected from the group consisting of polysulfonic acid polymers, perfluorocarbon sulfonic acid polymers, polyacrylic acid polymers, preferably an ion-conducting polymer selected from the group consisting of perfluorocarbon sulfonic acid polymers and polysulfonic acid polymers.

22. 20. The catalytic membrane of claim 19, wherein the catalytic nanoparticles are metal nanoparticles or metal oxide nanoparticles.

23. 23. The catalyst film of claim 19 or 22, wherein the catalyst nanoparticles are iridium or iridium oxide.

24. The catalyst layer is 0.2 mg Ir / cm 2 More than 1.8 mgIr / cm 2 Less than 0.4 mgIr / cm, preferably 0.4 mgIr / cm 2 1.2mgIr / cm or more 2 or less, most preferably 0.4 mgIr / cm 2 More than 0.8 mgIr / cm 2 24. The catalytic membrane of any one of claims 18 to 23, comprising iridium having a mass per unit area in the following ranges:

25. 25. The catalyst film according to any one of claims 18 to 24, wherein the catalyst nanoparticles have an average particle size in the range of 0.5 nm to 10 nm, preferably 1 nm to 7 nm, more preferably 1.5 nm to 3 nm, and most preferably 2 nm to 2.5 nm.

26. 26. The catalytic film of any one of claims 18 to 25, wherein the catalytic nanoparticles are amorphous nanoparticles.

27. A membrane electrode assembly comprising the catalyst membrane according to any one of claims 18 to 26.

28. 28. The membrane electrode assembly of claim 27, wherein the membrane electrode assembly is configured for water electrolysis.

29. 29. Use of a catalytic membrane or a membrane electrode assembly according to any one of claims 18 to 28 for water electrolysis.