High-strength cold-rolled steel sheet for double-sided enameled inner lining and its manufacturing method

A high-strength cold-rolled steel sheet with controlled chemical compositions and manufacturing processes addresses the challenges of double-sided enamel coating, achieving superior strength, scale explosion prevention, and adhesion for electric water heaters.

JP2024543159AInactive Publication Date: 2024-11-19BAOSHAN IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024531310
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-11-24
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high-strength steel plates for single-sided enamel coating do not meet the requirements for double-sided enamel, particularly in terms of strength, scale explosion prevention, and enamel adhesion, which are crucial for applications like electric water heaters with double-sided enameled inner and outer surfaces.

Method used

A high-strength cold-rolled steel sheet for double-sided enamel is developed, comprising specific chemical compositions and manufacturing processes that include controlled amounts of elements like C, Mn, P, Ti, B, and others, forming fine TiC and TiN particles to enhance strength, prevent scale explosion, and improve adhesion.

Benefits of technology

The steel sheet achieves yield strengths of ≥360 MPa, elongation at break of ≥28.0%, and hydrogen permeation values ≥7.5 min/mm², ensuring excellent scale explosion prevention and enamel adhesion, suitable for double-sided enamel applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543159000001_ABST
    Figure 2024543159000001_ABST
Patent Text Reader

Abstract

The present invention discloses a high-strength cold-rolled steel sheet for double-sided enamel inner liners containing Fe and inevitable impurities, and further containing, by mass percentage, chemical elements C: 0.06 - 0.12%, 0 < Si ≤ 0.08%, Mn: 0.5 - 1.2%, P: 0.01 - 0.05%, S: 0.005 - 0.05%, Al: 0.008 - 0.06%, N ≤ 0.006%, Ti: 0.03 - 0.1%, B: 0.0002 - 0.0035%, Cr: 0.01 - 0.06%, Cu: 0.01 - 0.06%, Mg: 0.0005 - 0.03%. Correspondingly, the present invention further discloses a manufacturing method of the above high-strength cold-rolled steel sheet for double-sided enamel inner liners, comprising the following steps: (1) steelmaking, refining and continuous casting; (2) heating of the casting blank; (3) hot rolling and coiling: controlling the final rolling temperature of hot rolling to be 810 - 880°C and the coiling temperature to be 620 - 680°C; (4) scale removal; (5) cold rolling: controlling the reduction ratio of cold rolling to be 60 - 70%; (6) continuous annealing: the soaking temperature is 780 - 850°C, the soaking time is 120 - 200 s, the overaging temperature is 165 - 450°C, and the overaging time is 250 - 350 s; (7) flattening.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metallic material and a manufacturing method thereof, and more particularly to a high-strength cold-rolled steel for double-sided enameled inner lining and a manufacturing method thereof. [Background technology]

[0002] In the conventional method for manufacturing enamel linings, steel sheets are punched and rolled to obtain end caps and barrel bodies, which are then welded to form lining slabs. These are then pretreated to remove impurities such as residual oil and oxide scale from the surface to obtain a surface suitable for enamel painting. Finally, wet enamel painting and high-temperature firing are performed to obtain the finished enamel lining.

[0003] Steel plate is one of the important materials for making enamel liner, which not only determines the compressive strength of the entire liner, but also greatly determines the enamel quality and service life of the entire liner. Therefore, the market requirements for the performance of steel for enamel liner are usually high, and it is required to have high yield strength, excellent formability, excellent weldability and enamel coating performance.

[0004] In the prior art, some researchers have already conducted research on high-strength steel plates for producing enamel galls. For example, the patent documents with publication numbers CN103510011A, CN10139684A, CN10125530A, CN202199726A, and CN103643118A all design high-strength steel plates for producing enamel galls. The characteristics of these components are based on low carbon steel, and the content of manganese and titanium is increased, and niobium or rare earth elements are added as auxiliary elements to achieve the purpose of increasing the strength and anti-scale explosion performance of the steel plate.

[0005] These patent documents mainly focus on the strength problem of the steel plate. In the examples given, the yield strength of the steel plate is all 350 MPa or more, but there are still some deficiencies: these steel plates are mainly applied to one-sided enamel painting technology and cannot meet the requirements for no scale explosion of double-sided enamel.

[0006] When the enamel liner is in use, a large amount of heat is lost as the hot water is discharged from the drain pipe; at present, electric heating companies adopt the method of filling a foam layer between the liner and the shell to achieve the effect of heat retention. In order to improve the working efficiency of electric water heaters, avoid heat loss and reduce energy consumption, many manufacturers have tried to develop new heat exchange liner structures, but in order to do so, it is necessary to apply enamel coating not only to the inner wall of the enamel liner that comes into contact with water, but also to the outer surface that comes into contact with residual heat to prevent the occurrence of steam corrosion.

[0007] However, up to now, there has been no data or application practice provided for the development of high-strength cold-rolled steel sheets for double-sided enameled piping in China. Based on this, the present invention is desirably provided with a new high-strength cold-rolled steel sheet for double-sided enameled piping and its manufacturing method to meet market demand. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a high strength cold rolled steel sheet for double sided enameled inner lining which not only has high strength, good plasticity and excellent enamel performance but also meets the requirements for double sided enameling. [Means for solving the problem]

[0009] This high-strength cold-rolled steel plate for double-sided enameled liner has good comprehensive performance in terms of forming, enamel painting, welding, pressure resistance, etc., and in particular has excellent welding performance, excellent anti-scale explosion performance, adhesion performance and pinhole / bubble defect resistance performance, and high strength after high-temperature enamel baking, and is especially suitable for the manufacture of double-sided enameled liner.

[0010] In order to achieve the above object, the present invention provides a high-strength cold-rolled steel sheet for double-sided enamel inner liners containing Fe and inevitable impurities, and further containing, by mass percentage, chemical elements C: 0.06 to 0.12%, 0 < Si ≤ 0.08%, Mn: 0.5 to 1.2%, P: 0.01 to 0.05%, S: 0.005 to 0.05%, Al: 0.008 to 0.06%, N ≤ 0.006%, Ti: 0.03 to 0.1%, B: 0.0002 to 0.0035%, Cr: 0.01 to 0.06%, Cu: 0.01 to 0.06%, Mg: 0.0005 to 0.03%, a high-strength cold-rolled steel sheet for double-sided enamel inner liners.

[0011] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enamel inner liners described in the present invention, the mass percentages of each chemical element are C: 0.06 to 0.12%, 0 < Si ≤ 0.08%, Mn: 0.5 to 1.2%, P: 0.01 to 0.05%, S: 0.005 to 0.05%, Al: 0.008 to 0.06%, N ≤ 0.006%, Ti: 0.03 to 0.1%, B: 0.0002 to 0.0035%, Cr: 0.01 to 0.06%, Cu: 0.01 to 0.06%, Mg: 0.0005 to 0.03%, and the balance is Fe and inevitable impurities.

[0012] In the chemical composition design of the present invention, it is mainly strengthened by C, Mn and P elements, and an appropriate amount of Ti and B elements are compounded and added, the content of S element is appropriately increased, and alloy elements such as Cu, Cr and Mg are added as supplements. Here, by adding an appropriate amount of Ti element, increasing the content of S element, and controlling the content of N element, it is possible to generate fine and dispersed second-phase particles of Ti with C, S and N, which not only contributes to improving the scale explosion prevention performance, but also controls the growth of ferrite crystal grains during enamel firing and can improve the high-temperature softening resistance of the steel sheet. In addition, an appropriate amount of B element can reduce the secondary brittleness problem caused by P, and at the same time further improve the scale explosion prevention performance and increase the high-temperature strength of the steel sheet.

[0013] In the present invention, by rationally adjusting the chemical elements and their added amounts, particularly limiting the relationship between Ti, C, S and N which affect the anti-scale explosion performance, anti-pinhole defect performance and strength, and controlling the processing process, a high-strength cold-rolled steel plate for double-sided enamel inner lining is developed, which ensures that the steel plate has high strength and good plasticity, while at the same time ensuring that the double-sided enamel does not explode on scale and meets the good requirements for the bubble structure of the enamel layer.

[0014] In the high-strength cold-rolled steel sheet for double-sided enameled inner hull according to the present invention, the design principles of each chemical element are as follows: C: In the high-strength cold-rolled steel plate for double-sided enamel lining according to the present invention, C is the most basic strengthening element. With the increase of C element content in steel, the strength of the steel plate also increases, but the plasticity and toughness decrease accordingly. By adding an appropriate amount of C element to steel, it can not only guarantee the basic strength of the steel plate, but also combine with Ti element in steel to form TiC particles, so that C can exist in the form of pearlite and TiC particles; accordingly, through process control, the formed TiC particles can be uniformly dispersed on the ferrite matrix, which not only increases the strength of the steel plate by precipitation strengthening, but also improves the anti-scale explosion performance of the steel plate as an effective hydrogen trap, and can control the coarsening of austenite grains and the growth of ferrite grains during high-temperature enamel firing, effectively preventing the softening of the steel plate after enamel firing. If the content of C element in steel is too high, a large amount of pearlite will be generated in the steel, which will not only impair the formability of the steel sheet, but also generate a large amount of CO gas during enamel baking, resulting in the formation of bubbles and pinholes on the enamel surface, so the content of C element in steel should not be too high. Therefore, in the high-strength cold-rolled steel sheet for double-sided enamel inner lining according to the present invention, the mass percentage of C element is controlled to 0.06-0.12%.

[0015] Si: In the high-strength cold-rolled steel sheet for double-sided enamel inner liner according to the present invention, the Si element can dissolve in ferrite and austenite, and can increase the hardness and strength of the steel. However, if the content is too high, the plasticity and toughness of the steel will be significantly reduced. Generally, adding an appropriate amount of Si to the steel does not affect the adhesion performance of the steel sheet. However, if the Si element content in the steel is too high, a SiO 2 film will be formed on the surface during heating of the steel sheet, inhibiting the infiltration of enamel into the steel sheet and the chemical reaction between the two, and reducing the adhesion strength between the steel sheet and the enamel. In addition, Si accelerates the hydrogen adsorption of the steel sheet during the pickling process and increases the possibility of scale explosion. Therefore, considering comprehensively the beneficial effects and adverse effects of the Si element on the performance of the steel sheet, in the high-strength cold-rolled steel sheet for double-sided enamel inner liner according to the present invention, the mass percentage of Si is controlled to satisfy 0 < Si ≦ 0.08%. In some embodiments, the mass percentage of Si is 0.005 - 0.08%.

[0016] Mn: In the high-strength cold-rolled steel sheet for double-sided enamel inner liner according to the present invention, Mn is a normal strengthening element, exists in a solid solution state, and can play a role in strengthening the ferrite matrix. At the same time, the Mn element can react with the S element to generate MnS, not only overcoming the hot brittleness caused by sulfur, but also playing an important role in the scale explosion prevention performance as an effective hydrogen trap. However, since MnS is an elongated inclusion and is disadvantageous to the transverse performance of the steel sheet, in the design of the steel material, the elongated MnS is gradually replaced by spherical Ti 4 C 2 S 2 and an appropriate amount of Ti element is added to improve the plasticity and toughness in the transverse direction of the steel sheet. In addition, if the content of the Mn element in the steel is too high, the Mn element will lower the transformation temperature of ferrite to austenite, making the steel sheet prone to deflection and deformation during high-temperature enamel firing, not only reducing the plasticity and adhesion of the material, but also affecting the deflection performance of the steel sheet. Therefore, the content of the Mn element in the steel should not be too high either. Therefore, in order to ensure the performance of the steel sheet, in the high-strength cold-rolled steel sheet for double-sided enamel inner liner according to the present invention, the mass percentage of Mn is controlled to be 0.5 - 1.2%.

[0017] P: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, adding an appropriate amount of P element to steel can effectively improve the anti-scale explosion ability of the steel sheet; in addition, the solid solution of P in ferrite can increase the strength and hardness of the steel sheet; however, P has serious segregation, which not only increases the cold brittleness of the steel but also significantly reduces the plasticity and toughness. Therefore, in the present invention, in order to mitigate the secondary processing brittleness caused by the segregation of P, alloy elements such as boron and molybdenum can be added in an appropriate amount. Therefore, in the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, the mass percentage of P element is controlled to 0.01-0.05%.

[0018] S: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, if the content of S element is appropriately increased, it can form composite inclusions with titanium and manganese, which can play a beneficial role in preventing scale explosion during enamel coating; in the present invention, by rationally controlling the compounding amount and process, the size of these composite inclusions can be further prevented from being too large, which would otherwise affect the anti-scale explosion performance and forming performance of the steel sheet. Therefore, in the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, in order to realize the beneficial effect of S element in steel, the mass percentage of S is controlled to 0.005-0.05%.

[0019] Al: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, Al element not only plays a role in deoxidizing and refining crystal grains, but also fixes nitrogen in the steel, reduces the aging tendency of the steel, and improves the low-temperature toughness of the steel. However, if the content of Al element in the steel is too high, it will cause difficulties in smelting, casting, etc., so the content of Al element in the steel should not be too high. Based on this, in the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, the mass percent of Al element is controlled to 0.008-0.06%.

[0020] N: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, nitrogen, like carbon, is worse in formability of the steel sheet and causes aging as the content of N element in the steel increases, so the upper limit of the N element content should be limited; in the present invention, N element can combine with Ti to form corresponding nitrides, which can improve the scale explosion prevention performance of the steel sheet. If the content of N element in the steel is too high, the size of the formed nitrides will be large, which will have very limited effect on improving the scale explosion prevention performance and will impair the plasticity of the steel, so the N element content in the steel should not be too high. Therefore, in the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, the mass percentage of N element is controlled to N≦0.006%.

[0021] Ti: In the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, Ti is a highly active metal element and can form stable compounds with carbon, nitrogen, and sulfur. Through process control, these compounds are uniformly dispersed in the ferrite matrix, which plays a role in preventing scale explosion and strengthening the matrix. In addition, Ti element has a certain advantage in adhesion, and Ti element oxidized to form Ti m O n The Ti concentrates on the steel sheet surface and significantly widens the width of the adhesive layer between the steel sheet and the enamel. m O n If the number of Ti is too large, it will inhibit the physical and chemical reaction between the steel sheet and the enamel. Therefore, in order to exert the beneficial effect of Ti element, the mass percent content of Ti element in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention is controlled to be 0.03-0.1%.

[0022] B: In the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, the B element can effectively reduce the secondary embrittlement problem caused by P segregation; B can also form boron carbide in the steel, partially exist in solid solution form, and further improve the anti-scale explosion performance of the material; However, if the B content is too high, it can also cause transverse cracks at the corners of the continuous casting blank. In addition, the B element can segregate at the austenite grain boundaries, which can prevent the diffusion of elements and the movement of grain boundaries during high-temperature enamel sintering, and increase the high-temperature strength of the steel sheet. Therefore, in order to exert the beneficial effect of the B element, the mass percentage of the B element is controlled to 0.0002-0.0035% in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention. In some embodiments, the mass percentage of the B element is 0.0005-0.0035%.

[0023] Cr: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, the Cr element can effectively strengthen the strength of the steel material and reduce the toughness of the steel material; an appropriate amount of Cr is advantageous for increasing the adhesion of the steel material; however, if the content of the Cr element in the steel is too high, it will cause scale explosion, so the content of the Cr element in the steel should not be too high. Therefore, in the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, the mass percentage of the Cr element is controlled to 0.01-0.06%. In some embodiments, the mass percentage of the Cr element is 0.01-0.05%.

[0024] Cu: In the high-strength cold-rolled steel sheet for double-sided enamel coating according to the present invention, in the pretreatment process including pickling, a trace amount of Cu has a certain advantage in the enamel adhesion performance; Cu element mainly exists in the form of solid solution in steel, and Cu dissolved in the acid solution during pickling 2+ The Cu or Cu alloy is then reappeared on the steel sheet surface by a substitution reaction. 2 S compounds are formed, and Cu or Cu, which is a residue after pickling, 2S is a porous film, which generates galvanic corrosion as a cathode during high-temperature enamel firing, increases the roughness of the steel sheet surface, and improves the adhesion performance of the enamel. However, in the places where copper is locally concentrated, a large amount of bubbles are generated in the enamel layer. Based on this, in order to exert the beneficial effect of Cu element, the mass percentage of Cu element is controlled to 0.01-0.06% in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention. In some embodiments, the mass percentage of Cu element is 0.01-0.05%.

[0025] Mg: In the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, adding an appropriate amount of Mg element can effectively improve the morphology of inclusions in the steel and enhance the plasticity and toughness of the steel. Therefore, in the present invention, the mass percentage of Mg element is controlled to 0.0005-0.03%.

[0026] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention, the unavoidable impurities are O≦0.008%, Ni≦0.1%, and Mo≦0.1%.

[0027] In the technical solution of the present invention, O, Ni, and Mo are all unavoidable impurity elements in steel, and the contents of these impurity elements in steel should be controlled as low as possible within the limits of technical conditions and production costs.

[0028] O: In the present invention, the O element affects the processing performance and enamel performance of the steel plate. On the one hand, if the content of the O element is too high, the steel will contain too many oxides, which will deteriorate the plasticity and toughness of the steel plate; on the other hand, if the content of the O element is too high, it will consume a large amount of Ti, resulting in excessive Ti. m O n The formation of TiN and TiN particles is detrimental to adhesion and beneficial to scale explosion prevention. 4 C 2 S 2Therefore, in the high-strength cold-rolled steel sheet for double-sided enameled lining according to the present invention, the content of the impurity element O must be strictly controlled so that the mass percentage of O element satisfies 0≦0.008%.

[0029] Ni and Mo: In the present invention, Ni and Mo elements are advantageous in improving the adhesion of enamel, because during high-temperature enamel firing, Ni and Mo elements can promote the infiltration and penetration of enamel into the steel sheet, and can promote the mutual dissolution and diffusion of ions and iron ions in the enamel. Ni also has the effect of blocking hydrogen diffusion in steel, and can improve the anti-scale explosion performance of the steel sheet. However, Ni and Mo elements are both valuable alloys, and if the content of Ni and Mo elements is too high, not only will the cost increase, but the adhesion performance will also decrease. In general, the adverse effects of the impurity elements Ni and Mo are greater than the beneficial effects they bring. Therefore, in the high-strength cold-rolled steel sheet for double-sided enamel inner lining according to the present invention, the content of the impurity elements Ni and Mo should be strictly controlled so that the mass percentages of Ni and Mo elements satisfy Ni≦0.1% and Mo≦0.1%. In some embodiments, the mass percentages of Ni and Mo elements are controlled to satisfy Ni≦0.02%, Mo≦0.04%.

[0030] In addition, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention, each chemical element further satisfies at least one of the following formulae: 0.05%≦C-(Ti-3.43N-1.5S) / 4≦0.1%; 0.08%≦Ti+0.875C≦0.25%; 0.65≦2.5Ti / (1.2C+8.57N+3.75S)≦1.35; The element symbols in the formulas represent the mass percentage of the corresponding element.

[0031] Prior art documents do not mention the limitation of the relationship between Ti, C, N, and S. Based on the formation free energy and solid solubility of titanium compounds, Ti first fixes N and S in steel, and when Ti remains, it combines with C to form TiC. If excess titanium = Ti-(4C+3.43N+1.5S)>0, it indicates that all carbon is fixed to titanium; if excess titanium≦0, it indicates that titanium is only combined with some carbon or not combined with carbon, and carbon exists in the form of pearlite. The control of pearlite components has a great impact on the coating performance of steel sheets, especially the pinhole defect resistance performance. Pearlite decomposes during the firing process to generate CO gas. Generally, the higher the pearlite content, the higher the firing temperature or the longer the firing time, the more gas is generated, which is easy to generate too many and too large bubbles in the enamel layer, resulting in surface bubbles, pinhole defects, and impairing the quality of the enamel layer.

[0032] In the above-mentioned embodiment, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention, the content of each single element is controlled, and the mass percentages of C, Ti, N and S are further controlled to satisfy 0.05%≦C-(Ti-3.43N-1.5S) / 4≦0.1%.

[0033] The reason is that in the present invention, carbon mainly exists in the form of TiC particles, which are low-temperature precipitates of titanium, and pearlite. This relationship limits the content of free carbon that forms pearlite structure; on the one hand, it ensures that pearlite is formed with more than 0.05% C in the steel to ensure the strength and anti-scale explosion performance of the steel plate; on the other hand, it limits that the pearlite content must not be too high, otherwise a large amount of CO gas will be generated during high-temperature enamel firing, resulting in poor bubble structure of the enamel layer and surface pinhole defects, and may also impair the plasticity of the steel plate.

[0034] In addition, in order to ensure that a sufficient amount of second phase particles are formed in the steel sheet, it is also preferable to control the mass percentages of Ti and C to satisfy 0.08%≦Ti+0.875C≦0.25%.

[0035] In addition, the type, size and shape of precipitates have a great impact on the performance of steel sheet, so in order to control precipitates, the present invention controls the content of each single element and also controls the mass percentage of Ti, C, N and S elements to be 0.65≦2.5Ti / (1.2C+8.57N+3.75S)≦1.35, the purpose of which is to ensure that the titanium carbon, nitrogen and sulfide particles are finely and uniformly distributed in the ferrite matrix, and further improve the scale explosion resistance of the steel sheet, as well as play the role of precipitation strengthening and inhibit the growth of ferrite grains during high-temperature enamel firing, thereby increasing the strength of the steel sheet and the strength after enamel firing. If this relationship is not satisfied, the size of the second phase particles formed in the steel sheet will be large, which will reduce the forming performance and scale explosion prevention performance of the steel sheet.

[0036] Furthermore, the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention further contains Nb: 0.005 to 0.04%.

[0037] In the above-mentioned embodiment of the present invention, Nb element may be further added to the steel. Nb is a strong carbon / nitride forming element like Ti, and a part of Nb exists in a solid solution state.

[0038] In the present invention, Nb element can increase the recrystallization temperature of steel, inhibit the recrystallization of austenite, and effectively maintain the deformation effect of austenite, thereby refining ferrite grains; the effect of refining grains of Nb makes the steel sheet soften after enamel firing, and can prevent the grains in the heat-affected area from becoming coarse during welding. In addition, Nb carbon / nitride precipitates also contribute to the hydrogen storage capacity of the steel sheet. Therefore, considering the beneficial effect of Nb element, in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, it is preferable to add an appropriate amount of Nb element, and the mass percentage of Nb element may be controlled to 0.005-0.04%.

[0039] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enameled steel according to the present invention, the matrix of the microstructure is uniform and fine ferrite + pearlite, and the pearlite phase fraction by volume is <8%, where the pearlite is located at the ferrite trifurcation grain boundary. In some embodiments, the pearlite phase fraction by volume is 2.0-6.5%.

[0040] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enameled lining according to the present invention, the microstructure contains second phase particles including fine, dispersedly distributed second phase particles of Ti.

[0041] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, the second phase particles of Ti are TiN, Ti 4 C 2 S 2 and TiC, the diameter of the TiN precipitates being 50 to 300 nm, 4 C 2 S 2 The diameter of the precipitates is 30 to 200 nm, and the diameter of the TiC precipitates is 1 to 15 nm.

[0042] Furthermore, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention, the crystal grain size of ferrite is 10-11 grade.

[0043] Furthermore, the high-strength cold-rolled steel sheet for double-sided enameled inner pipes according to the present invention satisfies at least one of the following performances: yield strength ≥ 360 MPa, elongation at break at a gauge distance of 80 mm ≥ 28.0%, yield strength after high-temperature enamel baking at 850°C for 12 minutes ≥ 330 MPa. Furthermore, the high-strength cold-rolled steel sheet for double-sided enameled inner pipes according to the present invention has a tensile strength ≥ 440 MPa.

[0044] In some embodiments, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention, the yield strength is 360 to 415 MPa, the tensile strength is 440 to 510 MPa, and the breaking elongation A 80 The yield strength after high-temperature enamel firing at 850° C. for 12 minutes is 330 to 370 MPa.

[0045] In some embodiments, the present invention provides a double-sided enameled steel having a substrate and an enamel layer on both sides of the substrate, the substrate having the same elemental composition as the double-sided enameled high-strength cold-rolled steel sheet for inner hull construction described in any of the embodiments of the present invention. In some embodiments, the enameled steel has a yield strength of ≥ 330 MPa (preferably 330 to 370 MPa), a tensile strength of ≥ 400 MPa (preferably 400 to 460 MPa), and a hydrogen permeation value of ≥ 7.5 min / mm 2 。 In some embodiments, the hydrogen permeation value of the enameled steel is between 7.5 and 16.0 min / mm 2 In some embodiments, the matrix of the substrate microstructure is a uniform and fine ferrite+pearlite, where the volumetric phase fraction of pearlite is <8% (preferably 1.5-6.5%) and the pearlite is located at the ferrite trifurcation grain boundaries. In some embodiments, the substrate microstructure comprises fine and dispersedly distributed second phase particles including Ti second phase particles. Furthermore, the Ti second phase particles can be TiN, Ti 4 C 2 S 2 and TiC, the diameter of TiN precipitates is 50 to 300 nm, and Ti 4 C 2 S 2 The diameter of the precipitate is 30-200 nm, and the diameter of the TiC precipitate is 3-25 nm. The material used for the enamel layer may be an enamel glaze well known in the art. A typical material is Fukuroku EMP 6515 type high temperature glaze.

[0046] Accordingly, another object of the present invention is to provide a method for manufacturing a high-strength cold-rolled steel sheet for double-sided enameled piping, which is simple and easy to carry out, and the high-strength cold-rolled steel sheet for double-sided enameled piping has a yield strength of ≥ 360 MPa, a breaking elongation at a gauge distance of 80 mm of ≥ 28.0%, and a hydrogen permeation value of ≥ 7.5 min / mm 2 The yield strength after high temperature enamel baking at least 850℃ for at least 12 minutes is ≧330MPa, which can meet the requirements of double-sided enamel coating.

[0047] In order to achieve the above object, the present invention provides a method for producing the high-strength cold-rolled steel sheet for double-sided enameled welding, comprising the following steps: (1) Smelting, refining and continuous casting; (2) heating of the casting blank; (3) Hot rolling and coiling: the final rolling temperature of hot rolling is controlled at 810-880°C, and the coiling temperature is controlled at 620-680°C; (4) Descaling; (5) Cold rolling: The reduction ratio of cold rolling is controlled to 60-70%; (6) Continuous annealing: the soaking temperature is 780-850°C, the soaking time is 120-200s, the overaging temperature is 165-450°C, and the overaging time is 250-350s; (7) Flattening.

[0048] In the manufacturing method of the high-strength cold-rolled steel sheet for double-sided enameled piping according to the present invention, in step (1), a steel liquor composition that satisfies basic requirements may be obtained through iron water pre-desulfurization, combined top-bottom blowing of a converter, and tapping alloying, and then a steel liquor having a uniform and stable temperature and composition may be obtained through a CAS refining process, and finally a continuous casting blank of the above composition may be formed through continuous casting.

[0049] In the hot rolling and coiling process in step (3), the hot rolling is all performed in the austenite single phase region, and the purpose is to accumulate a sufficient amount of deformation in the austenite unrecrystallized region, and to obtain a fine ferrite structure in the hot rolled sheet by using both the austenite grain boundaries and the "deformation bands" inside the crystal grains as ferrite nuclei. The final rolling temperature is set to Ar 3 The temperature is set to be equal to or higher than the phase transformation temperature (the transition temperature of austenite to ferrite during cooling) and close to this temperature, so that in the present invention the final rolling temperature is controlled to 810-880°C; accordingly, in the coiling process, the effect of the coiling temperature on the structural performance of the steel sheet is very significant, so in order to ensure that the steel sheet has high strength and at the same time fully analyze the pearlite and TiC particles, in the present invention the coiling temperature is controlled to 620-680°C; if the coiling temperature is too low, the bending strength ratio of the material will increase, which is detrimental to the forming performance.

[0050] In the manufacturing method according to the present invention, in the step (4), the descaling can effectively remove iron oxide scale on the surface of the hot rolled steel strip, making the subsequent operations easier.

[0051] In the cold rolling operation of step (5), the reduction ratio of cold rolling affects the mechanical properties and scale explosion prevention performance of the steel sheet. First, the reduction ratio affects the strength of the steel sheet. The larger the reduction ratio of cold rolling, the greater the degree of elongation of the structure along the rolling direction, which increases the nucleation rate of the recrystallization process, and the finer the ferrite grains are when the recrystallization is completed, thereby further improving the yield strength of the steel sheet. Second, in the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, the room temperature structure contains hard phases such as carburized body and titanium carbon / nitrogen / sulfide, and these particles are not deformed during cold rolling and are not in harmony with the deformation of the matrix, so a large number of voids are formed around the particles, which increases the hydrogen storage capacity of the steel sheet. The larger the reduction ratio of cold rolling and the greater the number of voids, the stronger the scale explosion prevention performance of the steel sheet. In consideration of the strength of the steel sheet, the prevention of scale explosion, and the load capacity of the rolling mill, the reduction rate of the cold rolling is controlled to 60 to 70% in step (5) of the production method according to the present invention.

[0052] Accordingly, in the above step (6), a high-temperature and high-speed continuous annealing process is adopted, specifically, the soaking temperature is controlled to 780-850°C, the soaking time is controlled to 120-200s, the overaging temperature is controlled to 165-450°C, and the overaging time is controlled to 250-350s. In this manner, the recrystallization process can be completed at high temperature in a short time, the coarsening of ferrite grains can be avoided, and a high-strength cold-rolled steel sheet with excellent strength and plasticity can be obtained; the short-time overaging treatment sufficiently precipitates the carburized body and TiC particles, which are low-temperature precipitates of titanium, and effectively improves the anti-scale explosion performance of the steel sheet.

[0053] Furthermore, in the production method according to the present invention, in step (2), the heating temperature is 1100 to 1230° C. and the furnace time is ≧360 min.

[0054] In the manufacturing method of the high-strength cold-rolled steel sheet for double-sided enameled steel according to the present invention, in step (2), it is preferable to control the heating temperature to 1100-1230°C and the furnace time to ≧360min, since the following two beneficial effects can be obtained: 1. Increase the plasticity of the steel material, reduce the deformation resistance, and obtain a large reduction during rolling; 2. Ensure sufficient dissolution of alloy elements, and obtain a uniform austenitic structure of the components. In some embodiments, in step (2), the heating temperature is 1130-1230°C, and the furnace time is 370-420min.

[0055] In the heating of the casting blank in step (2), if the heating temperature or time is lower than the set value, the above two objectives cannot be achieved; on the other hand, if the heating temperature is high or the heating time is long, the casting blank will be oxidized and decarbonized, and the burning damage of the casting blank will be serious, which will affect the material forming rate.

[0056] Furthermore, in the manufacturing method according to the present invention, in step (7), the flat rolling reduction is controlled to 0.6 to 1.2%.

[0057] According to the above embodiment, in the above step (7), the cold rolled strip steel after annealing is subjected to secondary cold rolling with a small reduction ratio, and the flatness reduction ratio is controlled to 0.6-1.2%, since it can obtain the following two beneficial effects: 1, reducing or eliminating the "yield platform" in the stress-strain curve and avoiding the "Luders band" during pressing; 2, improving the flatness of the steel plate and the finish of the plate surface.

[0058] In some embodiments, the present invention also provides a method for producing a double-sided enameled steel sheet, comprising the steps of producing a high-strength cold-rolled steel sheet for double-sided enameled inner lining according to the present invention by the above method, and enameling the produced high-strength cold-rolled steel sheet for double-sided enameled inner lining. In some embodiments, the enamel firing step is performed at 840-900°C for 8-15 minutes. In some embodiments, the enamel firing is performed by a one-coat and one-fire process, or a two-coat and two-fire process. The glaze used for the enamel layer may be any glaze known in the art.

[0059] Compared with the prior art, the high strength cold rolled steel sheet for double sided enameled inner tube and its manufacturing method according to the present invention have the following advantages and beneficial effects: (1) The present invention is based on the design concept of low alloy cost and low processing cost. In terms of component design, carbon, manganese and phosphorus strengthening is the basis, and relatively low-cost titanium and boron elements are added, and alloying elements such as copper, chromium and magnesium are added as auxiliary elements. In terms of processing technology, the heating temperature of the continuous casting blank, the final rolling temperature of hot rolling, the coiling temperature and the reduction rate of cold rolling are controlled, and a highly efficient high-temperature and high-speed continuous annealing process is adopted to ensure the excellent surface quality, mechanical properties and enamel coating performance of the steel sheet.

[0060] (2) In the high-strength cold-rolled steel sheet for double-sided enamel piping according to the present invention, the microstructure matrix is ​​uniform and fine ferrite+pearlite, the pearlite phase ratio is <8%, and the ferrite grain size is 10-11 grades. In the present invention, the strength of the steel sheet is mainly enhanced by solid solution strengthening, precipitation strengthening and fine grain strengthening, and the yield strength of the steel sheet is ≥360MPa and the breaking elongation at a gauge distance of 80mm is ≥28.0%; after high-temperature enamel sintering at 850℃ for 12 minutes, the fine and dispersed titanium second phase particles can effectively control the growth of ferrite grains, and the boron element can enhance the high-temperature strength of the steel, ensuring that the yield strength of the steel sheet after enamel sintering remains above 330MPa, which better meets the pressure resistance requirements of electric heating piping.

[0061] (3) In the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, the anti-scale explosion performance of the steel sheet is improved mainly by relying on pearlite at the trifurcation grain boundaries of ferrite and the fine and dispersedly distributed second phase particles of titanium; boron can also further improve the anti-scale explosion performance, and the fine ferrite grains also play a role in storing hydrogen at the grain boundaries, and the finer the grains and the larger the grain boundary area, the higher the hydrogen storage capacity, so that the anti-scale explosion performance can be improved. In the high-strength cold-rolled steel sheet for double-sided enamel lining according to the present invention, the hydrogen permeation value is ≧7.5 min / mm 2 In addition, the high-strength cold-rolled steel sheet for double-sided enamel inner lining according to the present invention limits the content of free carbon that forms pearlite, thereby suppressing the occurrence of bubble defects and pinhole defects during the enamel baking process. [Brief description of the drawings]

[0062] [Figure 1] FIG. 1 shows the metallographic microstructure of the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1. [Diagram 2] 2 and 3 show the distribution state of second phase particles in the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1, observed under a transmission electron microscope. [Diagram 3] 2 and 3 show the distribution state of second phase particles in the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1, observed under a transmission electron microscope. [Figure 4] FIG. 4 shows the metallurgical microstructure of the high strength cold rolled steel sheet for double sided enameled inner lining of Example 1 after simulated high temperature enamel firing. [Diagram 5] 5 and 6 show the distribution state of second phase particles observed under a transmission electron microscope after the simulated high-temperature enamel firing of the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1. [Figure 6] 5 and 6 show the distribution state of second phase particles observed under a transmission electron microscope after the simulated high-temperature enamel firing of the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1. [Figure 7]FIG. 7 shows the bubble structure of the enamel layer of the double-sided enameled high-strength cold-rolled steel sheet for inner lining of Example 1 after double-sided enameling and high-temperature firing. [Figure 8] FIG. 8 shows the bubble structure of the enamel layer after double-sided enamel coating and high-temperature firing of the comparative steel plate of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0063] The high-strength cold-rolled steel sheet for double-sided enameled inner lining and the manufacturing method thereof according to the present invention will be further interpreted and explained below in conjunction with specific examples and drawings of the specification, but these interpretations and explanations are not intended to unduly limit the configuration of the embodiments of the present invention.

[0064] Examples 1 to 6 and Comparative Examples 1 to 2 Tables 1-1 and 1-2 show the mass percentages of the chemical elements in the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6 and the comparative steel sheets of Comparative Examples 1 and 2.

[0065] [Table 1-1]

[0066] [Table 1-2]

[0067] The high strength cold rolled steel sheets for double sided enameled inner lining of the present invention in the above Examples 1 to 6 and the comparative steel sheets in Comparative Examples 1 and 2 were all manufactured by the following process: (1) Smelting, refining and continuous casting were carried out according to the compounding ratios of the chemical components shown in Tables 1-1 and 1-2. After the iron water pre-desulfurization, combined blowing at the top and bottom of the converter, and alloying at the tapping steel, a steel liquor composition that satisfied the basic requirements was obtained. Then, through the CAS refining process, a steel liquor with a uniform temperature and stable composition was obtained. Finally, through continuous casting, a continuous casting blank with the chemical composition shown in Tables 1-1 and 1-2 was formed.

[0068] (2) Heating of the casting blank: The heating temperature was controlled to 1100-1230°C, and the heating furnace time was controlled to ≧360min, so that the plate slab casting blank was sufficiently austenitized, an austenitic structure with a uniform composition was obtained, and the deformation resistance of the steel was reduced.

[0069] (3) Hot rolling and coiling: The final rolling temperature of the hot rolling was controlled to 810 to 880°C. After rolling, the steel sheet was cooled to the coiling temperature by laminar flow, and then the coiling temperature was controlled to 620 to 680°C for coiling.

[0070] (4) Scale removal: The iron oxide scale on the roll surface of the hot-rolled plate was thoroughly removed. (5) Cold rolling: The reduction ratio of cold rolling was controlled to 60-70%.

[0071] (6) Continuous annealing: the soaking temperature was 780 to 850°C, the soaking time was 120 to 200s, the overaging temperature was 165 to 450°C, and the overaging time was 250 to 350s.

[0072] (7) Flattening: The flattening reduction rate was controlled to 0.6 to 1.2%. In the present invention, the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6 are all manufactured by the above-mentioned process, and their chemical compositions and related process parameters all meet the design rule control requirements of the present invention. The comparative steel sheets of Comparative Examples 1 and 2 were also manufactured by the above-mentioned process, but their chemical compositions have parameters that do not meet the design rule control requirements of the present invention.

[0073] Tables 2-1 and 2-2 show specific process parameters for the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6 and the comparative steel materials of Comparative Examples 1 and 2.

[0074] [Table 2-1]

[0075] [Table 2-2]

[0076] During actual operation, the overaging temperature changes and does not stabilize at a constant value, but the temperature gradually decreases during the overaging period. Therefore, the overaging temperature in step (6) of Table 2-2 is shown as a constant range value rather than a point value in each embodiment and comparative example.

[0077] Performance tests were carried out on the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6 and the comparative steel materials of Comparative Examples 1 and 2, which were manufactured by the above manufacturing process. The test results are listed in Tables 3-1 and 3-2 below. The specific test methods are as follows: (1) The special feature of enamel steel is that it is used after high-temperature firing. In order to verify the change in yield strength of the steel sheets of each Example and Comparative Example before and after high-temperature enamel firing, in the present invention, tensile tests are directly performed on the continuously annealed steel sheets of Examples 1 to 6 and Comparative Examples 1 to 2, and the annealed steel sheets are sampled along the rolling direction and processed into tensile samples at a gauge distance of 80 mm according to the JIS 13A standard. Then, the usual mechanical properties of the tensile samples of each Example and Comparative Example are measured to determine the yield strength, tensile strength, and fracture elongation A at a gauge distance of 80 mm. 80 obtained.

[0078] Accordingly, a simulated high-temperature enamel firing test was conducted on the manufactured steel plates of Examples 1 to 6 and Comparative Examples 1 and 2, in which the enamel firing temperature was controlled to 850°C and the furnace time was controlled to 12 min; thereafter, samples were taken along the rolling direction of the steel plates after the high-temperature enamel firing, and a tensile test was performed to obtain the yield strength after enamel firing (850°C x 12 min) of the steel plates of each Example and Comparative Example.

[0079] (2) The steel sheets of Examples 1 to 6 and Comparative Examples 1 to 2 were subjected to double-sided wet enamel coating and sintered at 850°C for 12 minutes, and then the steel sheets were left for 72 hours to observe the scale explosion phenomenon; and the micro-morphology of the cross section of the enamel sheet was observed by an optical microscope to inspect the bubble structure of the enamel layer. Accordingly, in order to further quantify the scale explosion prevention performance of the steel sheets, the TH of the unpainted steel sheets was measured by the electrochemical hydrogen permeation method specified in the European standard EN 10209-2013. 2 The values ​​were measured.

[0080] Tables 3-1 and 3-2 show the performance test results of the double-sided enameled high-strength cold-rolled steel sheets for inner casings of Examples 1 to 6 and the enameled steels of Comparative Examples 1 and 2.

[0081] [Table 3-1]

[0082] [Table 3-2]

[0083] As shown in Table 3, in the present invention, the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6 have a high yield strength of 363 to 409 MPa, a high tensile strength of 447 to 502 MPa, and a high breaking elongation A at a gauge distance of 80 mm. 80 The viscosity is 28.5-32.5%, which can meet the forming requirements of three-stage inner body rolling or embossing press.

[0084] Accordingly, in the high-strength cold-rolled steel sheets for double-sided enameled inner linings of Examples 1 to 6, the pearlite phase ratio was 2.17 to 6.03%, and the ferrite grain size was all class 10.5.

[0085] After the simulated high-temperature enamel baking (850°C x 12 min), the high-strength cold-rolled steel sheets for double-sided enamel liner of Examples 1 to 6 still maintained high yield strength, the yield strength was all over 330 MPa, ranging from 332 to 368 MPa, and the tensile strength was also over 400 MPa, ranging from 400 to 460 MPa. This shows that the cold-rolled steel sheets for enamel liner of Examples 1 to 6 according to the present invention have good high-temperature softening resistance, can effectively improve the striking ability of the enamel liner, and can extend the service life of the liner.

[0086] Based on the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6, the enamel sheets obtained after double-sided enameling have a good bubble structure in the enamel layer, and the bubbles are fine and uniformly distributed; the hydrogen permeation times of the steel sheets are all within the threshold value of 6.7 min / mm 2 specified in the European standard EN 10209-2013. 2 It meets the requirement of preventing scale explosion during double-sided enamel coating.

[0087] However, in Comparative Example 1, although the Ti element is within the control range designed in the present invention, the calculation results are Ti-3.43N-1.5S<0, which indicates that all Ti is consumed by bonding with N and S, and there is no remaining Ti to bond with C. Also, in Comparative Example 1, the content of C element exceeds the control range, that is, all C is used for forming pearlite, and the content of pearlite structure exceeds the limited range of the present invention, so that a large amount of gas is generated during enamel firing, gas is not sufficiently released when the enamel layer is fused, and bubbles are densely packed in the enamel layer and have different sizes, resulting in a poor bubble structure.

[0088] In Comparative Example 2, the C and Ti contents were both lower than the control range of the present invention, and sufficient pearlite and titanium carbon / sulfur / nitrides could not be formed, which reduced the strength and hydrogen absorption capacity of the steel plate. The comparative steel plate in Comparative Example 2 had a further decrease in strength after double-sided enamel coating and high-temperature firing, which did not meet the requirements for high-pressure water circulation pressurization, and the double-sided enamel coating could not meet the requirements for preventing scale explosion.

[0089] FIG. 1 shows the metallographic microstructure of the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1. 2 and 3 show the distribution state of second phase particles in the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1, observed under a transmission electron microscope.

[0090] As shown in FIG. 1, in this embodiment, in the high-strength cold-rolled steel sheet for double-sided enameled steel of Example 1, the matrix of the microstructure is uniform and fine ferrite + pearlite with an average grain size of ferrite of 8.14 μm.

[0091] As shown in FIG. 2 and FIG. 3, in this embodiment, in the high-strength cold-rolled steel sheet for double-sided enameled lining of Example 1, TiN and Ti are contained in the ferrite matrix. 4 C 2 S 2 The TiC particles are dispersed, the diameter of the TiN precipitate is 76 nm, and the Ti 4 C 2 S 2 The diameter of the precipitate is 41 nm, and the size of the TiC precipitate is mainly 1 to 7 nm.

[0092] Figure 4 shows the metallographic microstructure of the high-strength cold-rolled steel sheet for double-sided enameled piping of Example 1 after the simulated high-temperature enamel firing. Figures 5 and 6 show the distribution of second phase particles observed under a transmission electron microscope after the simulated high-temperature enamel firing of the high-strength cold-rolled steel sheet for double-sided enameled piping of Example 1.

[0093] As shown in FIG. 4, in this embodiment, in the high-strength cold-rolled steel sheet for double-sided enamel annealing of Example 1, the microstructure after the simulated high-temperature enamel firing is uniform and fine ferrite + pearlite, that is, the same as the structure state after cold rolling annealing, the average grain diameter of ferrite is 9.52 μm, and no obvious change was observed in the grain size of ferrite after the high-temperature enamel firing.

[0094] In the high-strength cold-rolled steel sheets for double-sided enameled inner lining of Examples 1 to 6, the volume fraction of pearlite in the microstructure after simulated high-temperature enamel firing was still less than 8%, and was 1.5 to 6.5%.

[0095] As shown in Figs. 5 and 6, in this embodiment, in the high-strength cold-rolled steel sheet for double-sided enamel lining of Example 1, TiN, Ti 4 C 2 S 2 The TiC particles are dispersed, the diameter of the TiN precipitate is 82 nm, and the Ti 4 C 2 S 2 The diameter of the precipitate is 73 nm, and the size of the TiC precipitate is mainly 3-25 nm, which indicates that the precipitate tends to aggregate and grow during the high-temperature sintering process.

[0096] FIG. 7 shows the bubble structure of the enamel layer of the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1 after double-sided enameling and high-temperature enamel baking.

[0097] As shown in FIG. 7, in this embodiment, in the high-strength cold-rolled steel sheet for double-sided enameled inner lining of Example 1, bubbles are finely and uniformly dispersed in the enamel layer after double-sided enameling and high-temperature enamel baking, and the bubble structure is good.

[0098] FIG. 8 shows the bubble structure of the enamel layer of the comparative steel plate of Comparative Example 1 after both sides were enameled and then baked at a high temperature.

[0099] As shown in FIG. 8, in the comparative steel plate of Comparative Example 1, the pearlite content is too high, which causes a large amount of gases such as CO to be generated during enamel firing. These gases are not sufficiently released before the enamel layer is fused, resulting in the formation of a large number of bubbles of non-uniform size in the enamel layer. The diameter of each large bubble reaches 300 μm and almost penetrates the entire enamel layer. Pinhole defects are easily formed, which affects the use performance of the enamel product.

[0100] In addition, the combination methods of each technical feature in this application are not limited to the combination methods described in the claims of this application or the combination methods described in the specific examples, and all technical features described in this application may be freely combined or combined in any manner as long as there are no contradictions between them.

[0101] It should be noted that the above are only specific examples of the present invention, and the present invention is not limited to the above examples, and it is obvious that there are many similar variations thereto. All modifications directly derived or conceived by those skilled in the art from the disclosure of the present invention are included in the protection scope of the present invention.

Claims

1. A high-strength cold-rolled steel sheet for double-sided enamel lining containing Fe and unavoidable impurities, Further, the high strength cold rolled steel plate for double sided enameled inner piping contains, in mass percent, the chemical elements C: 0.06-0.12%, 0<Si≦0.08%, Mn: 0.5-1.2%, P: 0.01-0.05%, S: 0.005-0.05%, Al: 0.008-0.06%, N≦0.006%, Ti: 0.03-0.1%, B: 0.0002-0.0035%, Cr: 0.01-0.06%, Cu: 0.01-0.06%, and Mg: 0.0005-0.03%.

2. The high strength cold rolled steel sheet for double sided enameled inner tubes according to claim 1, wherein the mass percentages of each chemical element are: C: 0.06-0.12%, 0<Si≦0.08%, Mn: 0.5-1.2%, P: 0.01-0.05%, S: 0.005-0.05%, Al: 0.008-0.06%, N≦0.006%, Ti: 0.03-0.1%, B: 0.0002-0.0035%, Cr: 0.01-0.06%, Cu: 0.01-0.06%, Mg: 0.0005-0.03%, and the balance is Fe and unavoidable impurities.

3. 3. The high-strength cold-rolled steel sheet for double-sided enamel inner lining according to claim 1, wherein the unavoidable impurities are 0≦0.008%, Ni≦0.1%, and Mo≦0.1%.

4. Each chemical element is further 0.05%≦C-(Ti-3.43N-1.5S) / 4≦0.1%; 0.08%≦Ti+0.875C≦0.25%; 0.65≦2.5Ti / (1.2C+8.57N+3.75S)≦1.35 3. The high-strength cold-rolled steel sheet for double-sided enameled inner lining according to claim 1 or 2, which satisfies at least one of the following conditions:

5. The high-strength cold-rolled steel sheet for double-sided enameled inner lining according to claim 1 or 2, further comprising Nb: 0.005 to 0.04%.

6. The high-strength cold-rolled steel sheet for double-sided enameled piping according to claim 1 or 2, wherein the microstructural matrix is ​​uniform and fine ferrite + pearlite, the pearlite phase proportion by volume is <8%, and the pearlite is located at the ferrite trifurcation grain boundaries.

7. 7. The high strength cold rolled steel sheet for double sided enamelled piping according to claim 6, wherein the microstructure comprises fine, dispersedly distributed second phase particles including Ti second phase particles.

8. The second phase particles of Ti are TiN, Ti 4 C 2 S 2 and TiC, the diameter of the TiN precipitates being 50 to 300 nm, Ti 4 C 2 S 2 8. The high-strength cold-rolled steel sheet for double-sided enamel lining according to claim 7, wherein the precipitates have a diameter of 30 to 200 nm, and the TiC precipitates have a diameter of 1 to 15 nm.

9. 7. The high-strength cold-rolled steel sheet for double-sided enameled inner lining according to claim 6, wherein the crystal grain size of ferrite is 10 to 11 grades.

10. Yield strength ≧360 MPa, breaking elongation at a gauge distance of 80 mm ≧28.0%, tensile strength ≧440 MPa, and yield strength after high-temperature enamel baking at 850 ° C for 12 minutes ≧330 MPa; preferably, the yield strength of the high-strength cold-rolled steel sheet for double-sided enameled inner lining is 360-415 MPa, the tensile strength is 440-510 MPa, and the breaking elongation A is ≧28.0%. 80 The yield strength after high temperature enamel firing at 850°C for 12 minutes is 330-370MPa.

3. The high-strength cold-rolled steel sheet for double-sided enameled inner lining according to claim 1, which satisfies at least one of the following properties:

11. The substrate and both surfaces are provided with an enamel layer; The elemental composition of the substrate is the same as that of the high-strength cold-rolled steel plate for double-sided enameled inner hull according to any one of claims 1 to 5; preferably, the yield strength of the enameled steel is ≧330 MPa, preferably 330-370 MPa, the tensile strength is ≧400 MPa, preferably 400-460 MPa, and the hydrogen permeation value is ≧7.5 min / mm 2 , preferably 7.5 to 16.0 min / mm 2 Preferably, the matrix of the microstructure of the substrate is a uniform and fine ferrite+pearlite, where the volumetric phase fraction of pearlite is <8%, preferably 1.5-6.5%, and the pearlite is located at the ferrite trifurcation boundaries; Preferably, the microstructure of the substrate contains fine and dispersedly distributed second phase particles including Ti second phase particles; Preferably, the Ti second phase particles are TiN, ... 4 C 2 S 2 and TiC, the diameter of the TiN precipitates is 50 to 300 nm, and Ti 4 C 2 S 2 The diameter of the precipitates is 30 to 200 nm, and the diameter of the TiC precipitates is 3 to 25 nm. Double-sided enamelled steel.

12. (1) Smelting, refining and continuous casting; (2) heating the casting blank; (3) Hot rolling and coiling: the final rolling temperature of hot rolling is controlled at 810-880°C, and the coiling temperature is controlled at 620-680°C; (4) Descaling; (5) Cold rolling: The reduction ratio of cold rolling is controlled to 60-70%; (6) Continuous annealing: the soaking temperature is 780-850°C, the soaking time is 120-200s, the overaging temperature is 165-450°C, and the overaging time is 250-350s; (7) Flattening; The method for producing a high-strength cold-rolled steel sheet for double-sided enameled inner lining according to any one of claims 1 to 10, comprising the steps of:

13. The method according to claim 12, wherein in step (2), the heating temperature is 1100 to 1230° C. and the furnace time is ≧360 min.

14. The method according to claim 12 or 13, wherein in the step (7), the rolling reduction rate of the flattening is controlled to 0.6 to 1.2%.

15. The method for producing double-sided enameled steel according to claim 11, further comprising the steps of: producing the high-strength cold-rolled steel sheet for double-sided enameled inner piping by the method according to any one of claims 12 to 14; and enameling the produced high-strength cold-rolled steel sheet for double-sided enameled inner piping; preferably, in the enamel-firing step, the enameling is performed at 840 to 900°C for 8 to 15 minutes.

Citation Information

Patent Citations

  • Cold rolled steel sheet with yield strength being greater than 500 MPa for enameling and production method thereof

    CN110343964A

  • A double window

    JP1984006196U

  • Electrical fixture mounting device

    JP1986026226U

  • Cold-rolled enameled steel for deep-drawing inner pot and its manufacturing method

    JP2023526409A

  • Cold-rolled enamel steel for deep drawing inner container and manufacturing method therefor

    WO2021233247A1