Method for fabricating 3D circuits with shared recrystallization and dopant activation steps - Patents.com

By forming semiconductor structures with alternating amorphous and crystalline sublayers and using lower-temperature recrystallization, the method addresses material degradation and defects in 3D integrated circuits, improving transistor performance and reliability.

JP2024543230APending Publication Date: 2024-11-19COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024533881
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-12-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing methods for producing 3D integrated circuits face issues such as material degradation, unwanted dopant diffusion, and crystallization defects due to high-temperature thermal treatments, which affect transistor performance and device reliability.

Method used

A method involving the formation of a semiconductor structure with alternating amorphous and crystalline sublayers, where the amorphous sublayer is recrystallized using the crystalline sublayer as a starting region, and heat treatments are conducted at lower temperatures to minimize defects and dopant activation.

Benefits of technology

This approach reduces crystal defects and dopant diffusion, maintaining device integrity and performance by limiting thermal exposure, thereby enhancing the quality of 3D integrated circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543230000001_ABST
    Figure 2024543230000001_ABST
Patent Text Reader

Abstract

(a) producing a structure comprising a support (100) comprising a semiconductor layer (12) of a first level (N1), said support (100) comprising another semiconductor layer (120) of a second level (N2), said another semiconductor layer (120) comprising a lower sublayer (121) in contact with an insulating layer and an upper sublayer (122) disposed on the lower sublayer, a first of said lower and upper sublayers being made from a crystalline semiconductor material (C) while a second of said lower and upper sublayers being made from an amorphous semiconductor material (A); (b) forming at least one transistor gate block (132) on the semiconductor layer (120); (c) implanting dopants into said semiconductor layer (120) on either side of a gate block (132) to form doped regions (125) on either side of a semiconductor region positioned facing said gate block (132) and intended to accommodate a channel of said transistor; (d) performing at least one low temperature thermal treatment to perform recrystallization of the second semiconductor sublayer while using the first semiconductor sublayer as a starting region of the crystallization plane during activation of the dopants; Fabrication of microelectronic devices, including:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application relates to the field of microelectronic devices, and in particular to devices with components distributed across multiple levels. Such devices are commonly referred to as three-dimensional or "3D" integrated circuits. [Background technology]

[0002] Generally, in the field of integrated circuits, there is a continuing demand for increasing transistor density.

[0003] To this end, one solution consists in distributing the transistors over several levels of semiconductor layers arranged one on top of the other: such a circuit therefore generally comprises at least two superimposed semiconductor layers, between which an insulating layer is inserted.

[0004] For example, Brunet et al., "First demonstration of a CMOS over CMOS 3D VLSI CoolCube TM The document “integration on 300 mm wafer”, 2016 Symposium on VLSI Technology Digest of Technical Papers, for example, presents the use of such types of devices.

[0005] Creating transistors in an upper level may include performing one or more thermal processing steps, particularly when dopant activation is performed.

[0006] However, high temperature thermal processing can cause degradation of one or more low levels, in particular damage to the material of the low level contacts or the material of the mid-level connecting elements, or even unwanted diffusion of dopants within the low levels.

[0007] Once the first level of transistors has been produced, it is generally desirable to limit the thermal budget of the fabrication of one or more upper levels accordingly, in particular to avoid performing thermal processes above 600°C.

[0008] The activation of dopants or even the diffusion of dopants to create extension regions is one of the most important issues when it is desired to create transistors in the upper levels of 3D circuits. Such steps generally require high temperatures, which can be higher than 1000° C.

[0009] The method illustrated in Figures 9A-9B, which is used in 2D devices and therefore includes single level transistors, consists of making amorphous and doping by implantation of semiconductor regions 925 on either side of a gate block 932 on which spacers 932 are placed.

[0010] During the recrystallization period, horizontal F H and vertical F V This makes it easier to create a recrystallized surface of surface F. H and F V This can cause the creation of crystallization defects where they meet.

[0011] Such a method is typically carried out on an SOI substrate (SOI stands for "silicon on insulator") and involves the formation of a region 925, i.e., an undoped layer 926 of thickness e below the region that is to be made amorphous, doped, and then recrystallized. nd Controlling the doping poses problems since this undoped layer 926 tends to contribute to increasing the resistance to access and affecting the performance of the device.

[0012] Furthermore, in very thin semiconductor layers, for example intended for FDSOI type (meaning fully depleted silicon on insulator) applications, it can be difficult to preserve the thickness of the crystalline nuclei for recrystallization if an excessively deep amorphization implant is performed. This is even more particularly difficult and important if the amorphization is performed after the epitaxial growth of the source and drain regions, since in this case the semiconductor thickness varies along the support of this layer. [Prior art documents] [Non-patent literature]

[0013] [Non-Patent Document 1] Brunet et al., "First demonstration of a CMOS over CMOS 3D VLSI CoolCubeTM integration on 300 mm wafer," 2016 Symposium on VLSI Technology Digest of Technical Papers. Summary of the Invention [Problem to be solved by the invention]

[0014] The problem posed is to find a new method for manufacturing 3D microelectronic devices which improves with respect to at least one of the above mentioned drawbacks. [Means for solving the problem]

[0015] According to one aspect, the present invention relates to a method for producing a microelectronic device comprising multiple superimposed levels of electronic components, the method comprising: (a) First level N 1 producing a structure comprising a support comprising at least one of the components of said support covered by an insulating layer, itself covered by a second level semiconductor layer; the semiconductor layer includes at least one lower sublayer and an upper sublayer disposed on the lower sublayer, a first one of the lower and upper sublayers being made of a crystalline semiconductor material while a second one of the lower and upper sublayers being made of an amorphous semiconductor material; (b) forming at least one transistor gate block on the semiconductor layer; (c) forming doped regions on either side of a semiconductor region positioned facing a gate block and adapted to accommodate a channel of the transistor by implanting dopants into the semiconductor layer on either side of the gate block; (d) performing at least one heat treatment to perform a recrystallization of the second amorphous sublayer while using the first crystalline sublayer as a starting area of ​​a crystallization plane during the activation of the dopants; The method includes the steps of:

[0016] Step (a) includes forming a second level N so as to form the second sublayer made of an amorphous semiconductor material. 2 may include an amorphization implant to a thickness of said semiconductor layer of

[0017] Advantageously, said second sublayer made of amorphous semiconductor material extends over the entire surface, such that the support is totally covered by the second sublayer.

[0018] According to a first implementation possibility, in step (a), the first sublayer made from an amorphous material is the upper sublayer and said second sublayer made from a crystalline material is the lower sublayer.

[0019] In a variant, according to a second implementation possibility, in step (a), the first sublayer, which is amorphous, is the bottom sublayer and said second sublayer, which is crystalline, is the surface sublayer.

[0020] Advantageously, the formation of the structure in step (a) comprises - providing a first substrate, said first level N 1 wherein the at least one component of the components is generated; - bonding a second substrate on the first substrate, the second substrate comprising the semiconductor layer of the second level; - removing a portion of the second substrate while preserving the second semiconductor layer bonded to the first substrate; The method may include the sub-steps of:

[0021] When the removal of said parts is carried out by fracture and / or Smart cut™ type methods, the heat treatment step (d) can make it possible to carry out the repair of defects liable to be generated by this fracture.

[0022] According to a particular embodiment, step (a) may further comprise, prior to said bonding, a step of amorphization of said semiconductor layer of a second level so as to form a second semiconductor sublayer.

[0023] The amorphization of the semiconductor layer can, in a variant, be carried out after said creation of the weakened zone.

[0024] Performing this step prior to bonding allows for the best control over the thickness of the first sublayer and the thickness of each of the second sublayers.

[0025] Advantageously, when an implantation of the first substrate is carried out prior to said bonding so as to create a weak zone, amorphization of said semiconductor layer can be carried out after said creation of said weak zone.

[0026] Advantageously, an etch stop layer is arranged on the second substrate facing said semiconductor layer, and removing the portion of the second substrate further comprises selective etching of the etch stop layer relative to said semiconductor layer.

[0027] The method may further include forming insulating spacers on either side of the gate block.

[0028] In this case, the step (c) of forming the doped region may then comprise implanting a dopant prior to said formation of the insulating spacers. The step (c) of forming the doped region may comprise an implantation of dopants carried out after said formation of insulating spacers, advantageously said implantation of dopants being carried out in an inclined manner with respect to a normal to the main plane of the semiconductor layer.

[0029] Advantageously, the method may further comprise at least one auxiliary dopant implantation after the thermal treatment step (d).

[0030] According to one possible implementation, the method may further include, after step (d), growing semiconductor blocks on both sides of the gate block on the semiconductor layer.

[0031] According to one possible implementation of the method in which in step (a) the first sublayer that is amorphous is a bottom sublayer and the second sublayer that is crystalline is a surface sublayer, the method may further include removal of an undoped surface region after step (d) and before growth of the semiconductor block.

[0032] Advantageously, the recrystallization is a solid phase recrystallization and the heat treatment is carried out at a temperature below 550°C, advantageously below 500°C, typically between 450°C and 500°C.

[0033] Advantageously, the first component level is fabricated, at least in part, in a layer of semiconductor material.

[0034] The invention will be best understood from reading the description of exemplary embodiments, given purely by way of indication and without limitation, and from referring to the accompanying drawings, in which: [Brief description of the drawings]

[0035] [Figure 1A] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 1B] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 1C] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 1D] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 1E] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 1F] FIG. 1 shows a first example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Diagram 2] FIG. 2 illustrates an example structure comprising at least one level of components upon which upper level transistors may be formed. [Diagram 3] 5A-5C show examples of doping steps by angled implantation that can be carried out during the method according to the invention; [Figure 4] 5A-5C show examples of doping steps by implantation that can be carried out during the method according to the invention before forming the spacers; [Figure 5A] 5A-5C show examples of doping steps by implantation that can be carried out during the method according to the invention, before forming the spacers and after forming the regions protecting the gate; [Figure 5B] 5A-5C show examples of doping steps by implantation that can be carried out during the method according to the invention, before forming the spacers and after forming the regions protecting the gate; [Figure 6A] FIG. 2 illustrates a second example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 6B] FIG. 2 illustrates a second example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 6C] FIG. 2 illustrates a second example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 6D] FIG. 2 illustrates a second example of a method according to the invention for producing a 3D integrated circuit whose upper levels comprise transistors. [Figure 6E] FIG. 2 illustrates a second example of a method according to the present invention for producing a 3D integrated circuit in which the upper levels comprise transistors. [Figure 7A] 2A-2C illustrate a first sequence of steps of a method for assembling a semiconductor layer of a first level component and a semiconductor layer of a second level component. [Figure 7B] 2A-2C illustrate a first sequence of steps of a method for assembling a semiconductor layer of a first level component and a semiconductor layer of a second level component. [Figure 7C] 2A-2C illustrate a first sequence of steps of a method for assembling a semiconductor layer of a first level component and a semiconductor layer of a second level component. [Figure 7D] 2A-2C illustrate a first sequence of steps of a method for assembling a semiconductor layer of a first level component and a semiconductor layer of a second level component. [Figure 7E] 2A-2C illustrate a first sequence of steps of a method for assembling a semiconductor layer of a first level component and a semiconductor layer of a second level component. [Figure 8A] FIG. 2 shows a step of a second sequence in which the semiconductor layers of the first level components and the semiconductor layers of the second set of components are assembled, and amorphization of the second level semiconductor layers is performed prior to this assembly. [Figure 8B]FIG. 2 shows a step of a second sequence in which the semiconductor layers of the first level components and the semiconductor layers of the second set of components are assembled, and amorphization of the second level semiconductor layers is performed prior to this assembly. [Figure 8C] FIG. 2 shows a step of a second sequence in which the semiconductor layers of the first level components and the semiconductor layers of the second set of components are assembled, and amorphization of the second level semiconductor layers is performed prior to this assembly. [Figure 9A] FIG. 1 shows an example of a prior art method performed on a device having a single level of transistors. [Figure 9B] FIG. 1 shows an example of a prior art method performed on a device having a single level of transistors. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Identical, similar or equivalent parts of the various figures bear the same reference numbers to facilitate transition from one figure to another.

[0037] The various parts shown in the figures are not necessarily shown to uniform scale in order to make the figures more legible.

[0038] Additionally, in the following description, terms that depend on the orientation of a structure, such as "top," "surface," "side," etc., are applied by considering the structure as oriented as shown in the figures.

[0039] A first example of a method according to the invention for producing a microelectronic device comprising one or more transistors will now be described with reference to Figures 1A to 1F.

[0040] A possible starting structure for carrying out this method is given in FIG. 1A. This structure can be, for example, SiO 2It comprises a support 100 coated with an insulating layer 110 made from silicon, which is itself intended to be coated with a surface semiconducting layer 120 to form one or more transistors. The surface semiconducting layer 120, for example made from silicon, has a thickness e of, for example, between 5 nm and 60 nm. 0 may have the following structure:

[0041] Here, a semiconductor layer 120 is defined in a lower sublayer 121 in contact with the insulating layer 110 and an upper sublayer 122 on the outer surface and positioned above the lower sublayer.

[0042] One of the sublayers 121, 122, here the upper sublayer 122, is made from an amorphous semiconductor material A, while the other of the sublayers 121, 122 is made from a crystalline semiconductor material C. In this case, the upper sublayer 122 made from the amorphous material A has a thickness e of, for example, between 3 nm and 50 nm. 2 The sublayer 121 made of the crystalline material C for that part may have a thickness e of, for example, between 2 nm and 30 nm, for example, about 2 nm or 3 nm. 1 It can be provided with:

[0043] Advantageously, the upper sublayer 122 made from amorphous material A is produced over the entire surface, the insulating layer 110 and the support 100, thus making it possible to face the upper sublayer 122 over its entire extent (taken parallel to the plane [O;x;y] of the Cartesian reference coordinate system [O;x;y;z]). The upper sublayer 122 made from amorphous material A is typically formed by one or more amorphizing implants.

[0044] By carrying out an amorphization of a thickness of the semiconductor layer 120 covering the entire surface even before the formation of the transistor (and in particular the production of its gate), when this thickness is then recrystallized, it is possible to limit the appearance of crystal defects resulting from recrystallization planes of different orientations.

[0045] The implant dose and energy are designed to achieve amorphization while preserving the sublayer 121 in crystalline form. For example, implantation of Ge+ ions at dose and energy conditions determined by simulation and experimental verification by TEM (Transmission Electron Microscopy) imaging can be performed to create a given thickness of a silicon amorphous layer.

[0046] The simulation tool is based on Monte Carlo methods, in particular of the TRIM type (TRIM stands for "Transport of Ions in Matter") and / or KMC (for "Kinetic Monte Carlo").

[0047] The species used to perform this amorphization may be a neutral species, such as, for example, Si or Ge.

[0048] For example, 2*10 at 1keV energy 15 Ions*cm -2 The implantation of Ge+ ions may make it possible to obtain an amorphous thickness between 4 nm and 5 nm, while the implantation of 2*10 15 The implantation of Ge+ ions may make it possible to obtain an amorphous thickness between 7 nm and 10 nm. 15 The implantation of Ge+ ions may make it possible to obtain an amorphous thickness between 10 nm and 12 nm.

[0049] In this particular exemplary embodiment, the support 100 on which the semiconductor layer 120 is arranged can be formed from a structure comprising a first substrate 10 and a semiconductor layer 12, in which one or more components, in particular electronic components, have already been formed. The first substrate 10 can be a solid substrate ("bulk" according to the English term) or a substrate of the semiconductor-on-insulator type, in particular SOI, on which the semiconductor layer 12 rests. In the particular exemplary embodiment shown in FIG. 2, the first level N1 One or more transistors T 1 are implemented in this semiconductor layer 12, in particular their channel regions being provided on this layer. 1 Here, for example, SiO 2 , which is covered with one or more insulating layers, typically one or more stages of metal interconnects 25 formed in a stack of insulating layers.

[0050] 2 and a stack or another substrate comprising the semiconductor layer 120. By achieving amorphization of the semiconductor layer 120 before assembly, it becomes possible in particular to more easily adjust the respective thicknesses of the crystalline material C and the amorphous material A.

[0051] From the structure of FIG. 1A, then Level N 2 One or more transistors of the component are formed at least partially in the semiconductor layer 120. It is therefore the case to produce devices of the type commonly referred to as "3D" and including the superposition of multiple semiconductor layers in each of which the superposition of component levels of components is formed.

[0052] Thus, in a step subsequent to amorphization of the thickness of the semiconductor layer 120 and optional assembly of this semiconductor layer 120 on the substrate 10 comprising the semiconductor layer 12, a gate stack is formed on the semiconductor layer 120.

[0053] This stack is made of e.g. SiO 2 or HfO 2 and one or more layers of a gate material, for example based on polysilicon or TiN or W, or a stack of at least a plurality of these materials. Then (FIG. 1B), in this stack, a gate dielectric region 131 is defined, covered by a gate block 132.

[0054] Preferably, methods at temperatures below 500° C. are suitable for producing the gate. In this case, according to a particular example of implementation, the gate dielectric region 131 may be a region of silicon oxide obtained by oxidation of silicon by plasma at a temperature of the order of 450° C. As for the gate material, it may be TiN deposited at 350° C. or doped Si deposited at a temperature of the order of 475° C., which is subsequently recrystallized by a laser annealing process.

[0055] Then (FIG. 1C), spacers 137 are formed on both sides of the gate block 132. These spacers 137 may be based on, for example, SiN or SiBCN or SiOCN. Preferably, also methods for implementation at temperatures below 500° C. are suitable. To this end, it is possible to form the spacers 137, for example, by depositing SiCO at a temperature of the order of 400° C.

[0056] Subsequent doped regions 125 are formed in this layer 120 on either side of a region 120C of the semiconductor layer 120 that is positioned opposite the gate block 132 and is designed to accommodate the transistor channel. These doped regions 125 are typically created by implanting dopants into the second semiconductor layer 120.

[0057] 1D, the doped region 125 extends into the amorphous upper sublayer 122 and into the crystalline lower sublayer 121. The implant conditions can be designed by one skilled in the art with a CTRIM or KMC type implant simulation tool as described above.

[0058] Preferably, methods are suitable for implantation at temperatures below 500° C. The implantation methods here are carried out mainly at ambient temperature.

[0059] Once the dopant implantation has been performed, at least one heat treatment is performed to perform a recrystallization anneal of the upper sublayer 122 (FIG. 1E), where the use of the lower sublayer 121 as the starting area of ​​the recrystallization plane, which in this example is an ascending plane, i.e., away from the insulating layer 110, is performed.

[0060] The method of solid phase epitaxial regrowth (SPER) of an amorphous semiconductor material in contact with a crystalline semiconductor material is in particular carried out at temperatures typically below 600° C., preferably below 500° C., which may be between 450° C. and 500° C. Concomitantly, a heat treatment carried out makes it possible to carry out the activation of the dopants. The speed of the SPER recrystallization method varies according to the temperature, the material, the concentration of the dopants and the type of dopant (implanted species). The person skilled in the art will be able to establish the recrystallization conditions by measuring the recrystallized thickness according to the annealing time. The thickness is measured, for example, by ellipsometry. Here, the doped region 125 is made of a crystalline semiconductor material C. In this way, the recrystallization and the activation of the dopants are made reciprocal using a limited thermal budget.

[0061] When the formation of the support 100 is carried out by transferring and assembling the semiconductor 120 onto a structure comprising another semiconductor layer 12, in particular when carrying out a method for the Smart cut™ type having a crushing step, the thermal annealing carried out by the above-mentioned SPER technique may optionally make it possible to repair crystalline defects that are likely to be caused in the semiconductor layer 120 during this crushing period.

[0062] Upper Level N 2 The method for producing one or more transistors of may then continue with a step of carrying out the growth of semiconductor blocks 145 positioned on either side of the gate block 132 of the semiconductor layer 120, on the doped regions 125. Such growth may be carried out by epitaxy with an in situ doping step, during which the growth of the semiconductor material and the doping of this material are reciprocal.

[0063] The formation of the source and drain regions of the transistor is then completed (Figure 1F).

[0064] It is then possible to complete the formation of one or more transistors by other steps, in particular by forming regions of a metal-semiconductor alloy, in particular by performing a silicidation of the semiconductor regions 145. Such regions allow the formation of contacts, which are typically produced by depositing a material, for example tungsten or copper, followed by annealing.

[0065] In a variant of the method example just described, it is possible to prepare for doping so-called extension regions 126 arranged under the spacers 137, in addition to doping the regions 125 of the semiconductor layer 120 positioned on either side of the gate 132.

[0066] In this case, if the spacers 137 are formed before carrying out the doping of the semiconductor layer 120, it is possible to make preparations to carry out an implantation that is inclined with respect to the normal n to the main plane of the semiconductor layer 120, as in Figure 3. In this way it is possible to reach and dope these extension regions 126.

[0067] Another possibility for producing these doped extension regions 126 consists in carrying out the doping by implantation, this time before forming the spacers 137, as shown in figure 4. In this case, the implantation conditions, especially in terms of the beam orientation, are designed to avoid doping under the gate 132.

[0068] To avoid any doping under the gate 132, it is also possible to first make preparations for coating the lateral sides of the gate block 132 with a fine protective layer 135 made of a dielectric material. For example, the fine protective layer 135 is based on a layer of nitride with a thickness of the order of 1 nm to 10 nm, which is anisotropically etched. Then, as in FIG. 5A, one or more implants are performed to perform the doping. Then (FIG. 5B), a spacer 137 is formed with a greater thickness relative to the fine protective layer 135. Now, if necessary, another implant can be performed.

[0069] According to another variant, it is possible to achieve a reverse order of amorphous and crystalline thicknesses in the semiconductor layer 120 in which one or more transistors are formed.

[0070] Thus, in the example method given in Figures 6A-6E, the semiconductor layer 120 now includes a lower sublayer 121 made from an amorphous semiconductor material A, for example amorphous silicon, while an upper sublayer 122 is made from a crystalline material C, for example crystalline silicon.

[0071] To obtain a structure as shown in FIG. 6A, typically the implementation of amorphization, in particular by implantation, is dispensed with before implementing the method for assembly between a structure including a semiconductor layer 12 having first level components and another structure or another substrate comprising a second semiconductor layer 120, as previously mentioned, for example as shown in FIG. 2.

[0072] In this way, once the semiconductor layer 120 and the insulating layer 110 are assembled and adhesively bonded together, it may be easier to obtain a completely amorphous sublayer 121, particularly adjacent to the insulating layer 110, rather than when it is desired to perform one or more amorphization implants.

[0073] The lower sublayer 121 made of amorphous material A has a thickness e' between 3 nm and 50 nm, for example.1 The upper sublayer 122, for its part made of crystalline material C, may have a thickness e' between 2 nm and 30 nm, for example. 2 It can be provided with:

[0074] Next, the gate block 132 is formed from the structure shown in Figure 6A.

[0075] In the exemplary embodiment shown in FIG. 6B, insulating spacers 137 on either side of the gate block 132 are formed before the doping of the source and drain regions and, optionally, before the doping of the extension regions.

[0076] In the exemplary embodiment shown in Figure 6C, doped regions 125 are then formed by implanting dopants into the second semiconductor layer 120 on both sides of the gate block 132 and the spacer 137. Optionally, this doping can also be performed by one or more angled implants, as previously described in relation to Figure 3. As a variant and previously described in relation to Figures 4 or 5A-5B, a reverse order of the steps for generating the spacer 137 and the steps of doping by implantation can also be realized.

[0077] Recrystallization is then performed by heat treating the lower sublayer 121 while performing activation of the dopants in the doped regions 125 (FIG. 6D). This heat treatment is again typically performed at a temperature preferably between 450° C. and 500° C. to obtain a SPER type recrystallization.

[0078] This time, use is made of the upper sublayer 122 as a starting region for the recrystallization plane. By having the amorphous sublayer 121 extending over the entire surface, it is possible to have a recrystallization plane that is essentially vertical and therefore more favorable for defect-free regeneration of crystalline structures.

[0079] Optionally, it is then possible to carry out a SPER type recrystallization with in situ doping, where doping and recrystallization are carried out in this same equipment.

[0080] Advantageously, where applicable, it is now possible to carry out the removal of any non-doped surface regions.

[0081] It is now possible to carry out the steps as described in the previous example, in particular the growth of semiconductor block 145 to form source and drain regions (FIG. 6E), and then silicidation to form contacts.

[0082] As previously indicated, to obtain a structure as shown in FIG. 1A or as shown in FIG. 6A, it is first possible to carry out a method of assembly between a substrate 10 comprising a first semiconductor layer 12 in which first level components are formed, and another substrate 1 comprising a semiconductor layer 120 in which one or more transistors of a higher level are provided.

[0083] Thus, in the exemplary embodiment shown in Fig. 7A, a semiconductor handle substrate 1 is provided on which a semiconductor layer 120, for example made of silicon, is arranged and an implantation is carried out in said substrate 1 in order to form a weakened region 3. The implantation is carried out, for example, by H+ or helium ions.

[0084] Assembly by molecular bonding of the structure and the handle substrate 1 as previously described in connection with Fig. 2 is then carried out (Fig. 7B). The molecular bonding is, for example, performed by bonding a layer of Si on the surface of the structure of Fig. 2 with a layer of SiO 2 The layer may be formed between the first layer and the second layer.

[0085] Figure 7C shows a subsequent cutting step by fracturing the handle substrate 1 in the weakened area 3. An additional step of post-removal of the remaining thickness can then be performed (Figure 7D), which is typically performed by planarization (CMP).

[0086] The semiconductor layer 120 is at level N. 1 Once transferred onto the component, it is now possible to carry out at least one amorphization implantation (FIG. 7E).

[0087] A transistor is then formed, for example, according to the method previously described in connection with Figures 1A-1F.

[0088] Optionally, as shown in Figure 7A, the semiconductor layer 120 disposed on the handle substrate 1 can be placed facing an etch stop layer 170 made of a different semiconductor material and capable of being selectively etched with respect to the material of the layer 120. For example, when the semiconductor layer 120 is made of silicon, the etch stop layer 170 can be made of SiGe.

[0089] Once the transfer of the semiconductor layer 120 as performed in Figures 7B-7C has been performed, the surface semiconductor layer is thinned and smoothed to remove therefrom the roughness created by the fracturing step, and any residual defects that may be introduced into the crystal due to the implantation to create the weak regions are removed or reduced.

[0090] The presence of the stop layer 170 makes it better possible to control the thickness of the layer 120 and to reduce its roughness at low temperatures.

[0091] According to another implementation possibility, a substrate 1 is coated with a semiconductor layer 120 and thereon a level N 1 It is possible to create an amorphous sublayer in the semiconductor layer 120 even before assembly by molecular bonding with the substrate 10 on which the components are formed.

[0092] Thus, in the exemplary embodiment shown in Figures 8A-8C, a weakened area 3 is formed.

[0093] Then (FIG. 8B), amorphization by implantation of a sublayer of the semiconductor layer 120 is carried out.

[0094] Next, assembly by molecular bonding followed by severing by fracturing the handle substrate 1 at the weakened region 3 is performed (FIG. 8C).

[0095] According to a variant (not shown) of the method just described in relation to Figures 8A to 8C, it is also possible to carry out amorphization of the semiconductor layer 120 on the handle substrate 1 even before the step of creating the weak region 3.

[0096] As in the exemplary embodiment previously described with reference to Figures 7A-7E, an etch stop layer 170 may be optionally provided for the semiconductor layer 120. [Explanation of symbols]

[0097] 1 Second board, handle board 3 Vulnerable areas 10 First substrate 12 Layer of semiconductor material, semiconductor layer, first semiconductor layer 25 Metallic Interconnects 100 support 110 Insulating layer 120 Semiconductor layer 120C area 121 Lower Sublayer 122 Upper Sublayer 125 Doped Region 126 Expansion Area 131 Gate Dielectric Region 132 Transistor Gate Block 135 Fine protective layer 137 Insulating spacer 145 Semiconductor blocks, semiconductor regions 170 Etch stop layer 925 Semiconductors 926 Undoped layer 932 Spacer, Gate Block

Claims

1. Multiple superimposed levels of electronic components (N 1 , N 2 1. A method for producing a microelectronic device comprising: (a) First level (N 1 ), said support (100) being covered by an insulating layer (110), said insulating layer itself being a second level (N 2 ), said semiconductor layer (120) comprising at least one lower sublayer (121) in contact with said insulating layer and an upper sublayer (122) disposed on said lower sublayer, a first of said lower and upper sublayers being made of a crystalline semiconductor material (C) while a second of said lower and upper sublayers being made of an amorphous semiconductor material (A); (b) forming at least one transistor gate block (132) on the semiconductor layer (120); (c) implanting dopants into the semiconductor layer (120) on either side of the gate block (132) to form doped regions (125) on either side of a semiconductor region positioned facing the gate block (132) and intended to accommodate a channel of the transistor; (d) performing at least one heat treatment to perform a recrystallization of the second amorphous sublayer while using the first crystalline sublayer as a starting region of a crystallization plane for performing the activation of the dopants; A method comprising the steps, in this order:

2. The step (a) comprises forming the second level (N 2 2. The method of claim 1, further comprising an amorphization implant into the semiconductor layer (120) of a thickness of about 1000 nm.

3. 2. The method of claim 1, wherein the second sublayer made of an amorphous semiconductor material (A) extends over the entire surface such that the support (100) is entirely covered by the second sublayer.

4. 4. The method according to claim 1, wherein in step (a), the first sublayer made of an amorphous material (A) is the upper sublayer (122) and the second sublayer made of a crystalline material (C) is the lower sublayer (121).

5. 4. The method of claim 1, wherein in step (a), the first sublayer that is amorphous is the bottom sublayer and the second sublayer that is crystalline is the surface sublayer.

6. The forming of the structure in step (a) comprises: The first level (N 1 providing a first substrate (10) comprising the components: bonding a second substrate (1) comprising the semiconductor layer (120) onto the first substrate (10); removing a portion of the second substrate (1) while preserving the semiconductor layer (120) bonded to the first substrate (10); The method according to claim 4 or 5, comprising the sub-step consisting of:

7. The step (a) includes, prior to the bonding, forming the second semiconductor sublayer, the second level (N 2 7. The method of claim 6 when dependent on claim 5, further comprising the step of amorphizing said semiconductor layer (120) of .

8. 8. The method of claim 7, wherein an implantation of the first substrate (10) is performed prior to the bonding to create a weak region (3), and the amorphization of the semiconductor layer (120) is performed after the creation of the weak region.

9. 9. The method according to claim 6, wherein an etch stop layer (170) is disposed on the second substrate facing the semiconductor layer (120), and the removing of the portion of the second substrate (1) further comprises selective etching of the etch stop layer with respect to the semiconductor layer (120).

10. After step (b), Formation of insulating spacers (137) on either side of the gate block Including, said step (c) of forming said doped regions (125) includes implanting a dopant prior to said forming of said insulating spacers (137); or The formation of insulating spacers (137) on either side of the gate block. Including, 10. The method of any one of claims 1 to 9, wherein the step (c) of forming the doped region (125) comprises an implantation of a dopant performed after the formation of the insulating spacers (137).

11. The method of any one of claims 1 to 10, further comprising, after step (d), growing a semiconductor block (145) on the semiconductor layer (120) on either side of the gate block (132).

12. 12. The method of claim 11 , wherein in step (a), the first sublayer that is amorphous is the bottom sublayer and the second sublayer that is crystalline is the surface sublayer, the method further comprising removing an undoped surface region after step (d) and prior to the growth of the semiconductor block.

13. 13. A method according to any one of the preceding claims, wherein the recrystallization heat treatment is carried out at a temperature below 700°C, preferably below 550°C, advantageously below 500°C.

14. The first level (N 1 14. The method according to claim 1, wherein the components of are produced in a layer (12) of semiconductor material.