METHOD FOR PRODUCING A MATTE MULTILAYER SURFACE WITH INCREASED HAPTIC EFFECT AND MULTILAYER SURFACE - Patent application
By pre-stabilizing electrocurable varnish layers with UV or LED radiation and electron beam treatment, the method produces stable multilayer matte surfaces with a thickness of 20-30 μm, addressing defects and enhancing tactile experience.
Patent Information
- Application Number
- JP2024527268
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-15
- Filing Date
- 2022-11-13
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods struggle to produce multilayer matte surfaces with a thickness greater than 20 μm and a distinct tactile effect, as they often result in defects such as pinhead highlights and unstable coating structures due to excessive varnish application and incomplete curing.
A method involving pre-stabilization of electrocurable varnish layers through UV or LED radiation followed by electron beam treatment, and subsequent matting with excimer light, ensuring consistent thickness and stability of each pore.
The method achieves stable multilayer matte surfaces with a thickness of 20-30 μm, avoiding defects and providing a consistent tactile effect.
Smart Images

Figure 2024543364000001_ABST
Abstract
Description
[Technical field]
[0001] The subject of the invention is a method for producing a matt multi-layer surface with increased tactile effect on a carrier such as paper or plastic foil, in particular BOPP, CPP, PVC, PET, etc. The subject of the invention is also a multi-layer surface obtained by such a method, and furniture comprising a matt multi-layer surface according to the invention.
[0002] The invention can be applied in the manufacture of furniture surfaces. It can also be used to provide structure in the manufacture of melamine surfaces. [Background technology]
[0003] Concave three-dimensional coated surfaces are known, whose structures are printed, for example, with special paints having anti-adhesive properties, as well as convex surfaces, whose structures are obtained by overprinting with paints having extenders or varnishes. Another division divides the surfaces into synchronous surfaces, whose three-dimensional structure reflects elements of the printed pattern, and asynchronous surfaces, whose three-dimensional structure does not reflect the printed pattern.
[0004] For practical reasons and taking into account the aesthetic taste of consumers, furniture manufacturers use boards with a matte finish for furniture manufacturing. Currently known technologies allow the use of coatings, both water-based and EB (where the polymerization of the coating is activated by electron beam) as well as UV (where the polymerization of the coating is activated by ultraviolet light) coatings with matting agents to obtain a matte finish on the coated surface.
[0005] An example of such a finish is the product of the company Schattdecor: flat surface Smartfoil, three-dimensional concave Smartfoil Real and three-dimensional convex Smartfoil Evo and Smartfoil 3D. Matting agents have a negative effect on the rheological properties of the coating and complicate the coating process, among other things, by depositing on the applicator device, e.g. paint roller. The application of matting agents in coatings used for printing three-dimensional structures also limits the possibility of obtaining structures with a wide range of screen rulings due to the large size of the matting particles. In practice, it is very difficult to achieve chemical and mechanical standards for furniture foils with a gloss value of less than 10° (measured in 60° geometry).
[0006] A method is also known for obtaining a gloss of less than 10° on a surface by exposing a special type of varnish to an excimer lamp emitting light with a wavelength of 172 nm. The UV excimer lamp operating at a wavelength of 172 nm causes a gelling effect in the top layer of the varnish, which creates a microstructure and gives a deep matte optical effect. These surfaces are then fully cured, i.e. a full crosslinking is achieved, by treating the surface with UV radiation of a longer wavelength or with an electron beam with a defined dose. However, this method only results in a uniform, monolayer surface.
[0007] Patent specification JP 236233 B1 discloses a method of surface treatment with an excimer lamp to obtain a matt effect. The method discloses the use of adhesion-enhancing additives and the gelling of a layer when a subsequent layer is applied on it. This results in a multi-layered three-dimensional surface, maintaining the quality required for the furniture industry, with a thickness ranging from 3 to 20 μm. The most desirable effect of surface mattification with an excimer lamp is obtained in the range of applied coatings or structures having a thickness of 5 to 20 μm. This thickness maintains the stability of the applied layer.
[0008] However, studies have shown that if several layers are applied and then matted by the excimer lamp to a total thickness of more than 20 μm, certain defects that are not acceptable in the design of decorative surfaces occur, for example pinhead highlights on the surface of the pores, but smaller in size. Sometimes there are several highlights on the surface of one pore. The reason for such defects is the over-application of varnish locally. Immediately after exposure to the excimer lamp, due to these defects, the structure may collapse or behave in an uncontrollable manner. Since the excimer affects only the outer 0.1-0.5 nm of the top layer of the varnish, the coating in the remaining range is unstable, which causes partial exposure of the bottom layer, which then becomes visible on the surface in the form of highlights. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Polish Patent No. 236233B1 Summary of the Invention [Problem to be solved by the invention]
[0010] The object of the present invention is to develop a method for producing multi-layer matt surfaces, characterized by a matt finish, with a three-dimensional structural effect, with a thickness of more than 20 μm and with a very clear tactile effect. [Means for solving the problem]
[0011] The invention achieves this by pre-stabilizing the electronically curable varnish layer (called pore layer for the purposes of the invention), i.e. slightly gelling it throughout its thickness just before the excimer treatment. This is achieved by treating the applied electronically curable varnish layer with UV radiation having a wavelength of 254 (PAC lamp) or 395 nm (LED lamp), each previously applied layer being pre-polymerized with an electron beam having a generator power of 2-7 kGy, which causes a varnish pre-polymerization. This treatment results in a stable coating structure with a total thickness in the range of 20 μm-30 μm, which structure is matted in the next step by the action of the excimer light. This effect of the slight gelling of the structure before matting it is mainly to ensure a constant height and stability of each of the pores applied with the cylinder.
[0012] It has been found that if the previously applied electronically curable varnish layers are slightly gelled and matted with excimer and all electronically curable varnish layers are finally cured, then exposing the last applied electronically curable varnish layer to light having a wavelength of 254 (PAC lamp) or 395 nm (LED lamp) makes it possible to obtain a layer having a thickness of 20-30 μm.
[0013] For the purposes of this invention, when referring to layers called electron-curable varnish layers (4,6), it should be assumed that they mean layers that can be prepolymerized (gelled) by the action of an electron beam generator with a low dose in the range of 2-7 kGy or by exposing them to a sufficient dose of UV radiation. At the same time, layers so named sometimes already exhibit a finished polymerized and / or cured surface / structure.
[0014] The essence of the invention is a method for producing multi-coated matte surfaces which can subsequently be used for the production of decorative materials in the furniture industry. Possible surfaces are substrates with decoration in the form of wood, stone or fantasy motifs. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a cross-sectional view of a multilayer surface of Example 1. [Diagram 2] FIG. 1 is a cross-sectional view of a multilayer surface of Example 2. [Diagram 3] FIG. 11 is a cross-sectional view of a multilayer surface of Example 3. [Figure 4] FIG. 1 is a cross-sectional view of a multilayer surface of Example 4. [Diagram 5] FIG. 11 is a cross-sectional view of a multilayer surface of Example 5. [Figure 6] FIG. 13 is a cross-sectional view of a multilayer surface of Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The method according to the present invention comprises the following steps: a) providing a carrier layer (1); b) applying a protective layer (3); c) drying the protective layer (3); d) applying a topcoat electronic curable varnish layer (4); e) exposing the layer obtained in step d) to an excimer lamp emitting radiation having a wavelength of 172 nm; f) exposing the surface obtained in step e) to electron beam radiation having a dose in the range of 2-7 kGy; g) applying a subsequent structural electronic curable varnish layer (5), h) exposing the layer obtained in step g) to an LED lamp emitting UV radiation having a wavelength of 395 nm or a PAC lamp having a wavelength of 254 nm; i) exposing the structure obtained in step h) to an excimer lamp emitting radiation having a wavelength of 172 nm; j) exposing the structure obtained in step i) to electron beam radiation having a minimum dose of 40 kGy to complete the curing of all varnish layers.
[0017] During the application of the topcoat electronically curable varnish layer (4) formed in steps d), e) and f), and before the application of the subsequent structural electronically curable varnish layer (5) applied in step g), it is advantageous for the method according to the invention to comprise the following steps: f1) applying at least one subsequent structural electronic curable varnish layer (6), f2) exposing the layer obtained in step f1) to an excimer lamp emitting radiation having a wavelength of 172 nm; f3) exposing the structure obtained in step f2) to electron beam radiation having a dose in the range of 2-7 kGy.
[0018] Advantageously, a decorative layer (2) (printed by rotogravure, flexographic or digital printing processes) is applied to the carrier layer (1). In rotogravure printing according to the invention, the method of transferring the print or varnish to the carrier layer (1) consists of pressing it against the printing cylinder with a special roller coated with a layer of rubber of suitable hardness. The cylinder is immersed in a rotating toner container with a feed roller. Excess paint is removed by an adjustable scraper blade on the printing cylinder.
[0019] When the decorative layer (2) is applied to the carrier layer (1), a structural electronically curable varnish layer (5) can be applied to match the imprinted design. The structural electronically curable varnish layer (5) can be synchronized with the individual decorative elements or can be asynchronous.
[0020] The subject of the invention is also a multi-layer matt surface with increased haptic effect, consisting of: a) a carrier layer made of a paper-based material or a polymer film; b) protective layer (3), c) a topcoat electron curable varnish layer (4) having a thickness of 5-9 μm, applied over the entire width of the carrier 1, the varnish being matted using an excimer lamp emitting radiation having a wavelength of 172 nm; d) a structural electronically curable varnish layer EB (5) having a thickness of 20-30 μm, which has been matted using an excimer lamp emitting radiation having a wavelength of 172 nm; The varnish coating is finally fully cured using an electron beam with a minimum dose of 40 kGy. The final layer, which is the structural electronically curable varnish layer (5), is characterized in that the varnish is pregelled by irradiating it with an LED lamp emitting UV radiation with a wavelength of 395 nm or a PAC lamp with a wavelength of 254 nm.
[0021] It is advantageous if the multilayer surface according to the invention on the topcoat electronically curable varnish layer (4) formed in step c) comprises at least one subsequent structural electronically curable varnish layer (6) which has been previously matted with radiation from an excimer lamp having a wavelength of 172 nm.
[0022] Advantageously, the carrier layer (1) comprises a decorative layer (2).
[0023] The carrier layer (1) referred to in step a) is advantageously in the form of a film made of natural materials such as paper or of artificial materials such as biaxially oriented polypropylene (BOPP), cast polypropylene (CPP), polyvinyl chloride (PVC) or polyethylene terephthalate (PET). The carrier layer 1 can also be made of a wood-based panel.
[0024] The protective layer (3) applied in step b) is an acrylate-based mixture which improves the chemical resistance and is also beneficially applied using an intaglio cylinder.
[0025] It is also advantageous if the electronically curable varnish layer EB (4, 5, 6) comprises an additive that increases the adhesive strength of the varnish, selected from the group of additives made on the basis of micronized waxes based on high-sensitivity polyethylene to which propoxylated glycerol triacrylate has been added.
[0026] The topcoat electronically curable varnish layer (4) is made of varnishes available in the prior art, including FLE 27800 varnish, which is also a component of the structural electronically curable varnish layer (6).
[0027] To obtain a matte effect, the layers (4,6) are first exposed to an excimer lamp emitting light with a wavelength of 172 nm. This procedure does not completely cure the varnish layer (4,6), only its surface is slightly crosslinked, which causes a matte appearance on the surface. After treatment with the excimer lamp, the varnish coating has a surface with a topography, which makes it difficult to adhere to the next layer. For this reason, additives that increase the adhesive strength, preferably FZ 2720 for example, are used in both varnish layers, as well as gelling of the layers is performed. The excimer-treated topcoat electron-curable varnish layer (4) is then transferred to an electron beam generator and exposed to an electron beam with a dose in the range of 2-7 kGy. This does not guarantee complete crosslinking and is not enough to complete the polymerization. Due to this, the topcoat layer is not completely cured, so another layer is applied on top. The thickness of the topcoat layer (4) is 5-9 μm.
[0028] The structural electronically curable varnish layer (5) is made of a varnish available in the prior art. The layer (5) is first subjected to the stabilization process described in step h) by exposure to a lamp emitting UV light with a wavelength of 254 nm for PAC lamps and 395 nm for LED lamps. This wavelength is necessary to obtain the desired degree of polymerization, taking into account the thickness of the applied layer, i.e. 20-30 μm. The structural electronically curable varnish layer (5) is slightly polymerized without disturbing its surface, only the technological effect of improving the stiffness of the following layer is obtained, for which a constant thickness and stability of each of the applied pores by the cylinder is ensured. To obtain a matte effect, as in the case of the topcoat electronically curable varnish layer (4), the structural electronically curable varnish layer (5) is exposed to an excimer lamp emitting light with a wavelength of 172 nm. This procedure does not completely cure the structural electronically curable varnish layer (5), only its surface is slightly disturbed, causing a matte appearance on the surface. The excimer treated structural electronically curable varnish layer (5) is then transferred to an electron beam generator and exposed to an electron beam having a minimum dose of 40 kGy, which is necessary to complete the polymerization of layer (4) and the curing of the structural electronically curable varnish layer (5).
[0029] In one embodiment, the carrier layer (1) is provided with a decorative layer (2) that mimics a wood grain pattern. Before applying the second radiation-curable structural electronically curable varnish layer (5) in step g), the method according to the invention has the effect of forming a coating as shown in FIG. 6 and can further comprise the following steps: f1) applying a subsequent structural electronic curable varnish layer (6); f2) exposing the structure obtained in step f1) to an excimer lamp emitting radiation having a wavelength of 172 nm; f3) exposing the structure obtained in step f2) to electron beam radiation having a dose of 4 kGy (2-7 kGy).
[0030] The subsequent structural electronically curable varnish layer (6) is made of a varnish available in the prior art. The excimer treatment used in step f2) does not completely cure the subsequent structural electronically curable varnish layer (6), the surface is slightly disturbed, the surface appears matte, and the second structural electronically curable varnish layer (6) is then transferred to an electron beam generator and exposed to an electron beam with a dose of 4 kGy (2-7 kGy). This does not guarantee complete crosslinking and is not enough to complete the polymerization. This allows more layers to be applied on top, since the layer is not completely cured. Then another layer of electronically curable varnish, for example structural electronically curable varnish layer (5), could be applied on the surface.
[0031] The advantage of PAC or LED lamps is that they are compact devices with dimensions much smaller than electron beam generators, while still maintaining good production efficiency parameters. At the same time, they allow the gelling of structures with increased thickness (porous varnish), which avoids the aforementioned highlight defects on the surfaces of the pores. EXAMPLES
[0032] <Example 1: Positive mold, synchronization effect> The foil manufacturing process is based on the use of a printing and varnishing machine.
[0033] The wood-like design pattern forming the decorative layer 2 is applied onto a carrier 1 made of paper film. The design is transferred to the band by pressing it onto the printing cylinder with a special roller coated with rubber of sufficient hardness. The cylinder is immersed in a rotating toner container equipped with a feed roller. Excess ink is removed by an adjustable scraper blade on the printing cylinder. The band with the applied ink is then dried in a hot air chamber before being transported to the next printing unit. The carrier passes through three printing stations. Water-soluble inks are used in this process.
[0034] Each of the printing stations has a drying chamber where the applied ink is cured on the carrier at temperatures between 50°C-150°C.
[0035] The next step is to coat the printed carrier 1 with a protective layer 3. This is achieved by a unit with a special intaglio cylinder for the application of primer 20-97.10. The cylinder has a density of about 6 g / m 2 of primer is applied which is cured like an ink in a gas dryer at a temperature of 140° C. until the water evaporates from the applied primer and the dry weight of the dispersion on the band is maintained.
[0036] The structure is then coated with a first layer of electronically curable varnish 4 in a 3WS coating system. The Hesse varnish used has the following composition: ·FL 27692-0.9 part ·FLE 27800-0.1 part ·FZ 2711-0.07 part ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.01 parts
[0037] 8g / m 2 The resulting coating 4, having a basis weight of 1000 g, is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. The layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator parameter settings are as follows: Dose 2kGy 100kV high voltage
[0038] The resulting surface has a gloss of 5° when measured in 60° geometry. The carrier band then advances to an intaglio cylinder station which carries synchronised patterns for the individual elements of the main design of the decorative layer 2.
[0039] A second structural electronically curable varnish layer 5 is applied, the varnish having the following composition: ·FLE 27800-1 copy ·FZ 2720-0.15 part ·Photoinitiator Omnirad TPO-L-0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0040] The surface is stabilized under the action of ultraviolet light with a wavelength of 395 nm using an LED lamp. The surface is then exposed to an excimer lamp emitting radiation with a wavelength of 172 nm. Following this treatment, a final curing is carried out in the generator over the full thickness area of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0041] The multilayer surface, a cross section of which is shown in Figure 1, also provides a tactile sensation in addition to the visual effect of the imprinted design. The applied 27 μm thick porous structure, which correlates with the individual elements of the main design, has a gloss value of 1°-2° measured in a 60° geometry.
[0042] <Example 2: Positive mold, asynchronous effect> A decorative layer 2 is applied to a carrier 1 in the form of a plastic film band in the same way as described in example 1. The printed carrier 1 is then coated with a protective layer 3, which is primer FG 2810. This coating is carried out using an intaglio cylinder, which has a weight of approximately 5 g / m 2 This layer is cured in an oven at a temperature of 75°C.
[0043] The structure is then coated with a first layer of topcoat electronically curable varnish 4 using a 3WS coating system. The varnish used in this step has the following composition: ·FL 27694-0.8 part ·FLE 27800-0.2 part ·FZ 2711-0.07 part ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.01 parts
[0044] 8g / m 2 The resulting coating of topcoat electron curable varnish layer 4 having a basis weight of 1000 g is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. Layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator parameter settings are as follows: Dose 2kGy 100kV high voltage
[0045] The resulting surface has a gloss of 7° when measured in a 60° geometry.
[0046] The coated band then proceeds to an intaglio cylinder station with a pattern that is asynchronous with the individual main decorative elements (decorative layer 2). At this stage a structural electronically curable varnish layer 5 is applied, the varnish having the following composition: ·FLE 27800-1 copy ·FZ 2720-0.15 part Photoinitiator Omnirad 819 - 0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0047] The structural coating formed by electron curable varnish (5) is stabilized under the action of ultraviolet light having a wavelength of 254 nm using a PAC lamp. The surface is then exposed to an excimer lamp emitting radiation having a wavelength of 172 nm. Following this treatment, a final curing is carried out in an electron beam generator over the entire thickness area of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0048] The multi-layer surface, the cross section of which is shown in FIG. 2, also provides a tactile sensation in addition to the visual effect of the imprinted design.
[0049] The applied 22 μm thick asynchronous porous structure does not correlate with the individual elements of the main design and has a gloss value of 1°-2° when measured in a 60° geometry.
[0050] <Example 3: Negative mold, synchronization effect> The decorative layer 2 and the protective layer 3 are applied to the carrier layer 1 as described in Example 1.
[0051] The next step is to apply a topcoat electronically curable varnish layer 4 in a 3WS coating system. The varnish used in this step has the following composition: ·FLE 27800-1 copy ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.02 parts
[0052] 8g / m 2 The resulting coating of topcoat electron curable varnish layer 4 having a basis weight of 172 nm is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. Layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator settings are as follows: Dose 2kGy 100kV high voltage
[0053] The resulting surface has a gloss value between 1° and 2° when measured in 60° geometry.
[0054] The next step in the manufacturing process according to the invention is the application of a structural electronically curable varnish layer 5, which is synchronized with each part of the design as shown in figure 3. A structure is applied in which the varnish has the following composition: ·FL 27694-0.9 part ·FLE 27800-0.1 part ·FZ 2711-0.07 part ·FZ 2720-0.15 part Photoinitiator Omnirad 2022 - 0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0055] The surface is stabilized under the action of ultraviolet light with a wavelength of 395 nm using an LED lamp. The surface is then exposed to an excimer lamp emitting radiation with a wavelength of 172 nm. Following this treatment, a final curing is carried out in an electron beam generator over the entire thickness of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0056] The multi-layer structure, the cross section of which is shown in FIG. 3, provides a tactile sensation in addition to the visual effect of the imprinted design.
[0057] The layer of cured varnish applied with a negative intaglio cylinder has a thickness of 25 μm and a gloss of 8° measured in 60° geometry.
[0058] Example 4: Off-line varnish coating, asynchronous negative mold The decorative layer 2 and the protective layer 3 are applied to the carrier layer 1 as described in Example 1.
[0059] In the next technological cycle a topcoat electronically curable varnish layer 4 is applied using a 3WS coating system. The varnish used has the following composition: ·FLE 27800-1.0 part ·FZ 2720-0.1 part Photoinitiator UZ 7381 - 0.01 parts
[0060] 8g / m 2 The resulting coating of the topcoat electron curable varnish layer 4 having a basis weight of 1000 g is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. The topcoat electron curable varnish layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator settings are as follows: Dose 3 kGy 100kV high voltage
[0061] The resulting surface has a gloss value between 1° and 2° measured in 60° geometry.
[0062] The semi-finished product thus prepared is wound onto rolls and is ready for further processing steps.
[0063] In the next offline technological cycle, an asynchronous structural electronically curable varnish layer 5 is applied in a separate varnishing machine to the individual elements of the wood-like design.
[0064] At this stage of the process the varnish has the following composition: ·FL 27692-0.9 part ·FLE 27800-0.1 part ·FZ 2711-0.07 part ·FZ 2720-0.2 part Photoinitiator Omnirad 2100 - 0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0065] The surface of the structural electronically curable varnish layer 5 is stabilized under the action of ultraviolet light with a wavelength of 395 nm using an LED lamp. The surface is then exposed to an excimer lamp emitting radiation with a wavelength of 172 nm. Following this treatment, a final curing in an electron beam generator is carried out in the area of the entire thickness of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0066] The layer of hardened varnish, a cross section of which is shown in FIG. 4, provides a tactile sensation in addition to the visual effect of the imprinted design.
[0067] The layer of hardened varnish, applied with a negative intaglio cylinder, has a thickness of 29 μm and a gloss of 6° measured in 60° geometry.
[0068] Example 5: Varnish coating without print on carrier As shown in Example 1, the protective layer 3 is applied directly to the carrier layer 1, ie the paper, and has no decorative imprinted design.
[0069] Then, over the entire width of the band, a topcoat electronically curable varnish layer 4 is applied using a 3WS varnishing system. At this stage of the process, the varnish used has the following composition: ·FL 27694-0.9 part ·FLE 27800-0.1 part ·FZ 2711-0.07 part ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.01 parts
[0070] 8g / m 2 The resulting topcoat electron curable varnish layer 4, having a basis weight of 172 nm, is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. The layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator settings are as follows: Dose 2kGy 100kV high voltage
[0071] The resulting surface has a gloss of 8° measured in 60° geometry.
[0072] The carrier band then advances to the intaglio cylinder station. A second structural electro-curable varnish layer 5 is applied, the varnish having the following composition: ·FLE 27800-1 copy ·FZ 2720-0.15 part ·Photoinitiator Omnirad TPO-L-0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0073] The surface of the structure electron curable varnish layer 5 is stabilized under the action of ultraviolet light with a wavelength of 254 nm using a PAC lamp. The structure is then exposed to an excimer lamp emitting radiation with a wavelength of 172 nm. Following this treatment, a final curing in an electron beam generator is carried out in the area of the entire thickness of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0074] The 23 μm thick multilayer “porous” structure, the cross section of which is shown in FIG. 5, has a tactile feel and a glossiness of 1°-2° when measured in a 60° geometry.
[0075] Example 6: Offline varnish coating, positive mold, asynchronous effect, three layers of electronic curing varnish The decorative layer 2 and the protective layer 3 are applied to the carrier layer 1 as described in Example 1.
[0076] In the next technological cycle the first topcoat electronically curable varnish layer 4 is applied using a 3WS coating system. The varnish used has the following composition: ·FL 27692-0.8 part ·FLE 27800-0.2 part ·FZ 2711-0.07 part ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.02 parts
[0077] 8g / m 2 The resulting topcoat electron curable varnish layer 4, having a basis weight of 172 nm, is exposed to an excimer lamp emitting radiation having a wavelength of 172 nm, which makes the coating matte. The layer 4 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator settings are as follows: Dose 2kGy 100kV high voltage
[0078] The resulting surface has a gloss of 3° measured in 60° geometry.
[0079] The band then advances to an intaglio cylinder station with a pattern which is asynchronous with the individual main decorative elements formed in the decorative layer 2. A structural electronically curable varnish layer 6 is applied, the varnish having the following composition: ·FLE 27692-0.9 part ·FLE 27800-0.1 part ·FZ 2720-0.15 part Photoinitiator UZ 7381 - 0.01 parts
[0080] The surface is exposed to an excimer lamp emitting radiation with a wavelength of 172 nm, which results in a matt surface. The structural electron curable varnish layer 6 is then subjected to a prepolymerization (gelling) process in an electron beam generator. The generator parameter settings are as follows: Dose 3 kGy 100kV high voltage
[0081] After this process, a decorative structure is obtained with a thickness of 4 μm and a gloss value of 5°, measured in a 60° geometry.
[0082] In the next offline technological cycle the next structural electronically curable varnish layer EB5 is applied. The layer is applied using an intaglio cylinder with a greater engraving depth than in the application step of electronically curable varnish layer 6. The varnish composition in this part of the process is as follows: ·FLE 27800-1 copy ·FZ 2720-0.15 part Photoinitiator Omnirad 819 - 0.005 parts Photoinitiator UZ 7381 - 0.01 parts
[0083] The surface is then stabilized under the action of ultraviolet light with a wavelength of 395 nm using an LED lamp. The surface is then exposed to an excimer lamp emitting radiation with a wavelength of 172 nm. Following this treatment, a final curing is carried out in an electron beam generator in the area of the full thickness of all varnish layers. The generator parameters are as follows: Dose 40 kGy 110kV high voltage
[0084] The resulting surface, a cross-section of which is shown in Figure 6, gives a tactile sensation in addition to the visual effect of the imprinted design.The total thickness of the electronically curable varnish layer 5 is 30 μm and the surface has a gloss value of 1°-2° measured in 60° geometry.
[0085] In all the variants of the invention presented in the above examples, the varnish mixture in both application units contains special additives that improve the adhesive strength between the individual layers. An additional condition for achieving good adhesive strength is that each layer of varnish is subjected to a prepolymerization (gelling) prior to the last layer, in a step that produces a matte surface.
Claims
1. A method for producing a substrate having a matt multi-coated surface with an increased surface tactile effect and a decoration in the form of wood, stone or fancy motifs, characterized in that it comprises the following steps: a) providing a carrier layer (1); b) applying a protective layer (3); c) drying the protective layer (3); d) applying a topcoat electronic curable varnish layer (4); e) exposing the layer obtained in step d) to an excimer lamp emitting radiation having a wavelength of 172 nm; f) exposing the surface obtained in step e) to electron beam radiation having a dose in the range of 2-7 kGy; g) applying a subsequent structural electronic curable varnish layer (5); h) exposing the layer obtained in step g) to an LED lamp emitting UV radiation having a wavelength of 395 nm or a PAC lamp having a wavelength of 254 nm; i) exposing the structure obtained in step h) to an excimer lamp emitting radiation having a wavelength of 172 nm; j) exposing the structure resulting from step i) to electron beam radiation having a minimum dose of 40 kGy to complete the curing of all layers.
2. 2. The method according to claim 1, characterized in that after applying the topcoat electronically curable varnish layer (4) formed in steps d), e) and f) and before applying the subsequent structural electronically curable varnish layer (5) applied in step g), the following steps are carried out: f1) applying at least one subsequent structural electronically curable varnish layer (6), f2) exposing the layer obtained in step f1) to an excimer lamp emitting radiation having a wavelength of 172 nm; f3) exposing the structure obtained in step f2) to electron beam radiation having a dose in the range of 2-7 kGy.
3. 3. The method according to claim 1 or 2, characterized in that a decorative layer (2) is applied to the carrier layer (1) by printing with a rotogravure, flexographic or digital printing process.
4. 4. A method according to claim 3, characterized in that the structural electronically curable varnish layer (5) is applied in such a way that it matches the imprinted design synchronously or asynchronously with the individual decorative elements.
5. a) a carrier layer (1) made of a paper-based material or a polymer film; b) a protective layer (3); and c) a topcoat electron curable varnish layer (4) having a thickness of 5-9 μm, applied over the entire width of the carrier 1, the varnish being matted using an excimer lamp emitting radiation having a wavelength of 172 nm; d) a structural electronically curable varnish layer EB (5) having a thickness of 20-30 μm, which is matted using an excimer lamp emitting radiation having a wavelength of 172 nm; It is composed of The varnish coating layer is finally fully cured using an electron beam with a minimum dose of 40 kGy, resulting in a multi-layer matt surface with increased tactile effect, 1. A multi-layer matt surface, characterized in that the last layer, which is the structural electronically curable varnish layer (5), is pregelled by irradiating the varnish with an LED lamp emitting UV radiation with a wavelength of 395 nm or with a PAC lamp with a wavelength of 254 nm.
6. 6. Multilayer surface according to claim 5, characterized in that on the topcoat electronically curable varnish layer (4) formed in step c) there is present at least one subsequent structural electronically curable varnish layer (6) which has been previously matted with radiation from an excimer lamp having a wavelength of 172 nm.
7. 7. The multi-layer surface according to claim 5 or 6, characterized in that the carrier layer (1) comprises a decorative layer (2).
8. 7. Multilayer surface according to claim 5 or 6, characterized in that the carrier layer (1) referred to in step a) is in the form of a film made of natural materials such as paper or wood board, or made of artificial materials such as biaxially oriented polypropylene (BOPP) or cast polypropylene (CPP) or polyvinyl chloride (PVC) or polyethylene terephthalate (PET).
9. 7. Multilayer surface according to claim 5 or 6, characterized in that the protective layer (3) applied in step b) is an acrylate-based mixture, improving the chemical resistance, and is applied by means of an intaglio cylinder.
10. 7. Multilayer surface according to claim 5 or 6, characterized in that the electronically curable varnish layer (4, 5, 6) contains an additive that increases the adhesive strength of the varnish, selected from the group of additives made on the basis of micronized waxes based on high-sensitivity polyethylene to which propoxylated glycerol triacrylate has been added.
Citation Information
Patent Citations
Method of producing a matt varnished multilayer surface and a product comprising a matt varnished multilayer surface