Preparation method of rearview mirror rain suppressant coating
Through fine preparation of raw materials and process control, the problem of uneven coating of the rearview mirror rain agent is solved, the uniformity and service life of the coating are improved, and the durability and functional consistency of the coating are ensured.
Patent Information
- Application Number
- CN202411583858.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of existing rearview mirror rain agent coatings is not controlled accurately enough, resulting in uneven coating coatings and short service life.
By selecting suitable silicone resins, polyether modified polydimethylsiloxane leveling agents, silicone defoaming agents, isopropanol and fluorocarbon surfactants as preparation materials, combining surface pretreatment, curvature and roughness as the basis of the preparation materials Analysis, different application methods and gloss uniformity detection, monitoring the changes in water droplet contact angles, and adjusting the preparation process parameters to improve the uniformity and adhesion of the coating.
Effectively improve the accuracy of the preparation process of the rearview mirror rain agent coating, extend the service life of the coating, enhance the durability and scratch resistance of the coating, and ensure the functional consistency and reliability of the coating. .
Smart Images

Figure CN119060631A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coating preparation, and in particular to a method for preparing a waterproof coating for a rearview mirror. Background Art
[0002] With the continuous increase in the number of cars, road traffic safety issues have become increasingly prominent. Under severe weather conditions, such as heavy rain and heavy snow, the clarity of the rearview mirror is crucial to the driver's safety. Traditional rearview mirrors are prone to form water droplets and water mist when encountering rain, affecting the driver's line of sight and increasing the risk of traffic accidents. In order to solve this problem, it has become an urgent need to develop a rearview mirror coating with good rain-repelling effect. Many existing rearview mirror coatings will experience performance degradation after being used for a period of time. For example, the rain-repelling effect of the coating will gradually weaken, or it will be easily worn and scratched, affecting its service life.
[0003] Chinese patent application publication number: CN107699068B discloses a water-proof vapor-water-resistant coating stock solution and a preparation method thereof, as well as a water-proof vapor-water-resistant coating and its application, wherein the water-proof vapor-water-resistant coating stock solution comprises, by mass percentage, 10% to 20% of water-based resin, 1% to 5% of silicate, 75% to 90% of solvent and 0.1% to 1% of catalyst. The water-proof vapor-water-resistant coating stock solution is applied on a substrate to obtain a water-based coating having excellent high temperature resistance and water vapor barrier properties, as well as excellent anti-aging properties, environmental stability and temperature resistance, and has good adhesion to the coated substrate.
[0004] It can be seen that the existing technology has the problem of insufficiently precise control over the preparation process of the rearview mirror bullet rain agent coating, which results in uneven coating of the bullet rain agent coating and a low service life of the rearview mirror bullet rain agent coating. Summary of the invention
[0005] To this end, the present invention provides a method for preparing a rearview mirror bullet rain agent coating, so as to overcome the problem that the preparation process of the rearview mirror bullet rain agent coating in the prior art is not accurately controlled, resulting in uneven application of the bullet rain agent coating and a low service life of the rearview mirror bullet rain agent coating.
[0006] To achieve the above object, the present invention provides a method for preparing a rearview mirror anti-raining agent coating, comprising: Select 40 to 60 parts by weight of silicone resin, 1 to 3 parts by weight of polyether modified polydimethylsiloxane leveling agent, 0.5 to 1.5 parts by weight of silicone defoamer, 30 to 50 parts by weight of isopropanol, and 3 to 8 parts by weight of fluorocarbon surfactant as raw materials for preparing the rearview mirror bullet rain agent coating, and put the raw materials into a stirring device in order and stir to obtain a coating raw material mixed liquid; Pre-treating the surface of the rearview mirror, including sequentially cleaning, polishing and rinsing the surface of the rearview mirror, and determining whether to apply the coating raw material mixture to the surface of the rearview mirror based on the surface cleanliness and average roughness of the pre-treated rearview mirror surface; When it is determined to apply the coating raw material mixture to the rearview mirror surface, a coating difficulty area is determined based on the curvature and roughness of the rearview mirror area to be coated, and a coating method of the coating raw material mixture is determined according to the coating difficulty area and the complexity of the shape of the rearview mirror to be coated; Based on the gloss difference parameter and the color uniformity parameter of the rearview mirror after the application, it is judged whether the rearview mirror rain agent coating obtained after the application is uniform, and when the rearview mirror rain agent coating obtained is not uniformly applied, it is determined to optimize the judgment parameter of the difficult application area, wherein the judgment parameter includes a preset curvature and a preset roughness; Monitor the contact angle of water droplets on the surface of a uniformly applied rearview mirror anti-fouling agent coating, and determine whether to adjust the preparation process parameters of the rearview mirror anti-fouling agent coating based on the average decrease rate of the contact angle within a preset time and the difference between the maximum decrease rate and the average decrease rate of the contact angle within a preset time, wherein the preparation process parameters include a preset surface cleanliness and a preset average roughness.
[0007] Further, the determining whether to apply the coating raw material mixture to the rearview mirror surface includes: The surface cleanliness and average roughness of the pre-treated rearview mirror surface are compared with the corresponding preset surface cleanliness and preset average roughness, respectively, wherein: If the surface cleanliness of the pre-treated rearview mirror surface is greater than or equal to the preset surface cleanliness and the average roughness is greater than or equal to the preset average roughness, determining to apply the coating raw material mixture to the rearview mirror surface; If the surface cleanliness of the rearview mirror surface after pretreatment is less than the preset surface cleanliness or the average roughness is less than the preset average roughness, it is determined to perform secondary pretreatment on the rearview mirror surface.
[0008] Furthermore, the preset surface cleanliness is determined according to a historical average value of the surface cleanliness of the pre-treated rearview mirror surface, and the preset average roughness is determined according to a historical average value of the average roughness of the pre-treated rearview mirror surface.
[0009] Further, when determining to apply the coating raw material mixture to the surface of the rearview mirror, determining the difficult-to-apply area includes: The curvature and roughness of the rearview mirror area to be painted are compared with the corresponding preset curvature and preset roughness, respectively, wherein: If the curvature of the rearview mirror area to be painted is greater than a preset curvature or the roughness of the rearview mirror to be painted is greater than a preset roughness, it is determined that the rearview mirror area to be painted is a difficult-to-paint area.
[0010] Furthermore, the preset curvature is determined based on a historical average value of the curvature of the rearview mirror area to be painted.
[0011] Furthermore, the method for determining the coating raw material mixture to be applied includes: If the rearview mirror area to be coated is a difficult coating area, determining that the coating raw material mixture is coated by a sponge coating method; If the rearview mirror area to be coated is not a difficult coating area and the shape complexity of the rearview mirror to be coated is greater than or equal to a preset complexity, determining that the coating raw material mixture coating method is an automatic dipping method; If the rearview mirror area to be coated is not a difficult-to-coat area and the shape complexity of the rearview mirror to be coated is less than a preset complexity, it is determined that the coating raw material mixture is coated by ordinary spraying.
[0012] Further, the determination of whether the rearview mirror bullet rain agent coating obtained after the application is completed is evenly applied includes: The gloss difference parameter and color uniformity parameter of the rearview mirror painted under the corresponding painting method are compared with the corresponding preset gloss difference parameter and preset color uniformity parameter, wherein: If the glossiness difference parameter of the rearview mirror coated under the corresponding coating method is less than the preset glossiness difference parameter and the color uniformity parameter is less than the preset color uniformity parameter, it is determined that the rearview mirror rain agent coating obtained after coating is uniformly coated; If the gloss difference parameter of the rearview mirror coated under the corresponding coating method is greater than or equal to the preset gloss difference parameter or the color uniformity parameter is greater than or equal to the preset color uniformity parameter, it is determined that the rearview mirror rain agent coating obtained after coating is unevenly coated.
[0013] Furthermore, when it is determined that the rearview mirror bullet rain agent coating obtained after the coating is unevenly coated, the preset curvature and the preset roughness are optimized.
[0014] Furthermore, the determining whether to adjust the preparation process parameters of the rearview mirror anti-repellent coating includes: The average decrease rate of the contact angle within the preset time and the difference between the maximum decrease rate and the average decrease rate of the contact angle within the preset time are compared with their corresponding preset decrease rates and preset differences, wherein: If the average decrease rate of the contact angle within the preset time is greater than or equal to the preset decrease rate and the difference between the maximum decrease rate and the average decrease rate of the contact angle within the preset time is less than the preset difference, it is determined that the preparation process parameters of the rearview mirror bullet rain agent coating are adjusted.
[0015] Furthermore, the adjustment amount of the preset surface cleanliness is positively correlated with the average reduction rate of the contact angle within a preset time, and the adjustment amount of the preset average roughness is positively correlated with the average reduction rate of the contact angle within a preset time.
[0016] Compared with the prior art, the beneficial effect of the present invention lies in that the coating raw material mixture is applied only when the surface cleanliness reaches or exceeds the preset standard, which can effectively avoid the presence of pollutants on the surface affecting the adhesion and uniformity of the coating, thereby reducing the service life and performance of the coating. When the average roughness meets the preset requirements, it is beneficial for the coating raw material mixture to better mechanically combine with the rearview mirror surface. The roughness can increase the contact area between the coating raw material mixture and the substrate, and improve the adhesion of the coating. By determining whether to apply the coating raw material mixture to the rearview mirror surface based on the surface cleanliness and the average roughness, the accuracy of the control of the preparation process of the rearview mirror rain agent coating is improved, thereby improving the uniformity of the rain agent coating application to avoid the problem of low service life of the rearview mirror rain agent coating.
[0017] Furthermore, the present invention can accurately determine the difficult-to-apply area by comparing the curvature and roughness of the rearview mirror area with preset values. For the difficult-to-apply area, the sponge application method can better adapt to the curved surface shape and ensure the integrity and consistency of the coating; for the area with higher roughness, the soft material of the sponge can better fill the tiny bumps on the surface and improve the adhesion of the coating. By selecting different application methods according to different situations, the advantages of each method can be maximized to improve the coating quality. The automatic dipping method is suitable for rearview mirrors with more complex shapes and can ensure that the coating evenly covers all parts; the ordinary spraying method is suitable for rearview mirrors with simple shapes. It is easy to operate and can quickly form a uniform coating. The above method improves the accuracy of the control of the preparation process of the rearview mirror rain agent coating and thereby improves the uniformity of the rain agent coating application to avoid the problem of low service life of the rearview mirror rain agent coating.
[0018] Furthermore, in the present invention, whether the coating is uniform is determined based on the gloss difference parameter and color uniformity parameter of the rearview mirror coated under the coating method. The uniformity of gloss is often closely related to the physical and chemical properties of the coating. Uniform gloss usually means that the thickness, hardness and wear resistance of the coating are consistent, which can improve the durability and scratch resistance of the rearview mirror rain agent coating and extend the service life of the product. For example, in actual use, a coating with uniform gloss can better resist the erosion of the external environment, such as ultraviolet rays, rain, dust, etc., so as to maintain good performance. For some rain agent coatings with special functions, color uniformity may also affect the performance of their functions. For example, if the color of the coating is uneven, it may cause different optical properties in different parts, thereby affecting the anti-glare effect or rain repelling performance of the rearview mirror. Ensuring color uniformity can ensure the functional consistency of the coating on the entire rearview mirror surface, improve the reliability and practicality of the product, and improve the accuracy of the control of the preparation process of the rearview mirror rain agent coating through the above method, thereby improving the uniformity of the rain agent coating coating to avoid the problem of low service life of the rearview mirror rain agent coating.
[0019] Furthermore, the present invention can directly reflect the hydrophobic performance of the coating by monitoring the change in the contact angle of water droplets on the coating surface. When the average decrease rate of the contact angle is less than the preset decrease rate, it indicates that the hydrophobic performance of the coating is relatively stable. When the average decrease rate of the contact angle is greater than or equal to the preset decrease rate, it is necessary to compare the difference between the maximum decrease rate and the average decrease rate of the contact angle with the preset difference to determine whether the rearview mirror bullet rain agent coating is damaged due to scratches or friction. When the difference is greater than or equal to the preset difference, it indicates that the rearview mirror bullet rain agent coating is damaged. The layer is damaged by scratches or friction, which does not mean that the preparation process is unqualified. At this time, it is determined that there is no need to adjust the preparation process parameters of the rearview mirror bullet rain agent coating. When the difference is greater than or equal to the preset difference, it means that the preparation process is unqualified. At this time, it is necessary to use an adjustment coefficient to increase the preset surface cleanliness and the preset average roughness to increase the service life of the rearview mirror bullet rain agent coating. The above method improves the accuracy of the control of the preparation process of the rearview mirror bullet rain agent coating and thus improves the uniformity of the application of the bullet rain agent coating to avoid the problem of low service life of the rearview mirror bullet rain agent coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The following is a working flow chart of a method for preparing a rain-repellent coating for a rearview mirror according to an embodiment of the present invention; Figure 2 The present invention is a flowchart of determining whether to apply the coating raw material mixture to the rearview mirror surface in the method for preparing the rearview mirror bullet rain agent coating according to an embodiment of the present invention; Figure 3A flowchart of determining a difficult-to-apply area in a method for preparing a rearview mirror rain-repellent coating according to an embodiment of the present invention; Figure 4 The present invention is a workflow diagram for determining whether to adjust the preparation process parameters of the rearview mirror bullet rain agent coating in the preparation method of the rearview mirror bullet rain agent coating in an embodiment of the present invention. DETAILED DESCRIPTION
[0021] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0022] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0023] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0024] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0025] See also Figure 1-Figure 4 As shown, Figure 1 The following is a working flow chart of a method for preparing a rain-repellent coating for a rearview mirror according to an embodiment of the present invention; Figure 2 The present invention is a flowchart of determining whether to apply the coating raw material mixture to the rearview mirror surface in the method for preparing the rearview mirror bullet rain agent coating according to an embodiment of the present invention; Figure 3 A flowchart of determining a difficult-to-apply area in a method for preparing a rearview mirror rain-repellent coating according to an embodiment of the present invention; Figure 4 The present invention is a workflow diagram for determining whether to adjust the preparation process parameters of the rearview mirror bullet rain agent coating in the preparation method of the rearview mirror bullet rain agent coating in an embodiment of the present invention.
[0026] The method for preparing the rain-repellent coating of a rearview mirror according to an embodiment of the present invention comprises: Step S1, selecting 40 to 60 parts by weight of an organosilicon resin, 1 to 3 parts by weight of a polyether-modified polydimethylsiloxane leveling agent, 0.5 to 1.5 parts by weight of an organosilicon defoaming agent, 30 to 50 parts by weight of isopropanol, and 3 to 8 parts by weight of a fluorocarbon surfactant as raw materials for preparing a rearview mirror bullet rain agent coating, and placing the raw materials in a stirring device in order and stirring to obtain a coating raw material mixed solution; Step S2, pre-treating the rearview mirror surface, including sequentially cleaning, polishing and rinsing the rearview mirror surface, and determining whether to apply the coating raw material mixture to the rearview mirror surface based on the surface cleanliness and average roughness of the pre-treated rearview mirror surface; Step S3, when it is determined to apply the coating raw material mixture to the surface of the rearview mirror, determine the coating difficulty area based on the curvature and roughness of the rearview mirror area to be coated, and determine the coating method of the coating raw material mixture according to the coating difficulty area and the complexity of the shape of the rearview mirror to be coated; Step S4, judging whether the rearview mirror rain agent coating obtained after the application is uniform based on the gloss difference parameter and the color uniformity parameter of the rearview mirror after the application is completed, and determining the judgment parameters for optimizing the difficult application area when the rearview mirror rain agent coating obtained is unevenly applied, wherein the judgment parameters include a preset curvature and a preset roughness; Step S5, monitor the contact angle of water droplets on the evenly applied surface of the rearview mirror anti-fouling agent coating, and determine whether to adjust the preparation process parameters of the rearview mirror anti-fouling agent coating based on the average decrease rate of the contact angle within a preset time and the difference between the maximum decrease rate and the average decrease rate of the contact angle within a preset time, wherein the preparation process parameters include a preset surface cleanliness and a preset average roughness.
[0027] The method of placing the prepared raw materials in a stirring device in order and stirring to obtain a coating raw material mixture includes but is not limited to selecting a suitable stirring device, such as a stainless steel stirring kettle with a speed regulating function. The material of the stirring kettle must be able to withstand the chemical properties of the raw materials to avoid chemical reactions and contamination of the raw materials. The shape and size of the stirring paddle must be suitable for stirring the liquid mixture with moderate viscosity. Generally, a three-blade stirring paddle can be selected to ensure that the raw materials can be fully stirred. When pouring the prepared raw materials into the stirring device, first pour isopropanol into the stirring kettle, turn on the stirring device, and then slowly add the silicone resin. , keep stirring, and observe the liquid state in the stirring tank. When the liquid is uniform and there are no obvious particles, it means that the silicone resin has been completely dissolved. After the silicone resin is completely dissolved, add the polyether modified polydimethylsiloxane leveling agent and silicone defoamer. During the addition process, pour it slowly and evenly, stirring while pouring, this is to ensure that the additives can be fully dispersed in the solution. Continue stirring to make the leveling agent and defoamer evenly distributed in the solution. Finally, add the fluorocarbon surfactant, and also pour it slowly and continue stirring to ensure that the fluorocarbon surfactant is fully integrated into the solution to obtain a uniform coating raw material mixture.
[0028] In one embodiment of the present invention, 40 parts by weight of silicone resin, 1 part by weight of polyether modified polydimethylsiloxane leveling agent, 0.5 parts by weight of silicone defoaming agent, 30 parts by weight of isopropanol, and 3 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing the rearview mirror bullet rain agent coating, and the raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixture.
[0029] In another embodiment of the present invention, 50 parts by weight of silicone resin, 2 parts by weight of polyether modified polydimethylsiloxane leveling agent, 1 part by weight of silicone defoaming agent, 40 parts by weight of isopropanol, and 5 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing the rearview mirror bullet rain agent coating, and the prepared raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixture.
[0030] In one embodiment of the present invention, 60 parts by weight of silicone resin, 3 parts by weight of polyether modified polydimethylsiloxane leveling agent, 1.5 parts by weight of silicone defoaming agent, 50 parts by weight of isopropyl alcohol, and 8 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing the rearview mirror bullet rain agent coating, and the prepared raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixture.
[0031] Specifically, in step S2, when determining whether to apply the coating raw material mixture to the rearview mirror surface, it is determined whether to apply the coating raw material mixture to the rearview mirror surface according to the comparison results of the surface cleanliness and average roughness of the pre-treated rearview mirror surface with the corresponding preset surface cleanliness and preset average roughness; When the surface cleanliness of the pre-treated rearview mirror surface is greater than or equal to the preset surface cleanliness and the average roughness is greater than or equal to the preset average roughness, determining to apply the coating raw material mixture to the rearview mirror surface; When the surface cleanliness of the pre-treated rearview mirror surface is less than a preset surface cleanliness or the average roughness is less than a preset average roughness, it is determined that the rearview mirror surface is subjected to secondary pretreatment.
[0032] In the embodiment of the present invention, the preset surface cleanliness is the historical average value of the surface cleanliness of the rearview mirror surface after pretreatment, and the preset average roughness is the historical average value of the average roughness of the rearview mirror surface after pretreatment, but the above values are not limited to this, and technical personnel in this field can also adjust the values according to actual needs.
[0033] The surface cleanliness of the rearview mirror surface in the embodiment of the present invention can be measured by using a surface cleanliness tester, and the average roughness can be determined by evenly dividing the rearview mirror surface into 10 areas, using a surface roughness meter to measure the roughness of the 10 areas and taking the average value to determine the average roughness.
[0034] In the present invention, the coating raw material mixture is applied only when the surface cleanliness reaches or exceeds the preset standard, which can effectively avoid the presence of pollutants on the surface affecting the adhesion and uniformity of the coating, thereby reducing the service life and performance of the coating. When the average roughness meets the preset requirements, it is beneficial for the coating raw material mixture to better mechanically combine with the rearview mirror surface. The roughness can increase the contact area between the coating raw material mixture and the substrate, and improve the adhesion of the coating. By determining whether to apply the coating raw material mixture to the rearview mirror surface based on the surface cleanliness and the average roughness, the accuracy of the control of the preparation process of the rearview mirror rain agent coating is improved, thereby improving the uniformity of the rain agent coating application to avoid the problem of low service life of the rearview mirror rain agent coating.
[0035] Specifically, in step S3, when it is determined to apply the coating raw material mixture to the rearview mirror surface, the coating difficult area is determined according to the comparison result of the curvature and roughness of the rearview mirror area to be coated with the corresponding preset curvature and preset roughness; When the curvature of the rearview mirror area to be painted is greater than a preset curvature or the roughness of the rearview mirror to be painted is greater than a preset roughness, determining that the rearview mirror area to be painted is a difficult-to-paint area; When the curvature of the rearview mirror area to be painted is less than or equal to a preset curvature and the roughness of the rearview mirror to be painted is less than or equal to a preset roughness, it is determined that the rearview mirror area to be painted is not a difficult-to-paint area.
[0036] In the embodiment of the present invention, the curvature of the rearview mirror area to be painted can be measured by a curvature measuring instrument. The division method of the rearview mirror area to be painted is the same as the method for measuring the average roughness. The preset curvature is the historical average value of the curvature of the rearview mirror area to be painted, and the preset roughness is 1.1 times the preset average roughness. However, the above values are not limited to this, and technical personnel in this field can also adjust the values according to actual needs.
[0037] Specifically, in step S3, when determining the coating material mixture coating method, the coating material mixture coating method is determined according to whether the rearview mirror area to be coated is a coating difficult area and the comparison result of the shape complexity of the rearview mirror to be coated with the preset complexity; When the rearview mirror area to be coated is a difficult coating area, the coating raw material mixture is coated by a sponge coating method; When the rearview mirror area to be coated is not a difficult coating area and the shape complexity of the rearview mirror to be coated is greater than or equal to a preset complexity, determining that the coating raw material mixture coating method is an automatic dipping method; When the rearview mirror area to be coated is not a difficult-to-coat area and the shape complexity of the rearview mirror to be coated is less than a preset complexity, it is determined that the coating raw material mixture is coated by a common spraying method.
[0038] The shape complexity of the rearview mirror to be painted in the embodiment of the present invention can be determined according to the number of curved surfaces on the surface of the rearview mirror and the maximum curvature change degree. The shape complexity is positively correlated with the number of curved surfaces, and the shape complexity is positively correlated with the maximum curvature change degree. The preset complexity is the historical average value of the shape complexity of the rearview mirror to be painted, but the above value is not limited to this. Technical personnel in this field can also adjust the value according to actual needs.
[0039] The sponge coating method described in the embodiment of the present invention includes gently dipping the sponge into the coating raw material mixture, allowing the sponge to fully absorb the solution, and gently applying the coating raw material mixture to the difficult-to-apply area with the sponge; the automatic dipping method includes the automatic dipping method using gravity and capillary action to immerse the rearview mirror in an immersion tank filled with the coating raw material mixture, so that a layer of the coating raw material mixture is evenly attached to the surface of the rearview mirror. When the rearview mirror is lifted out of the immersion tank, excess coating raw material mixture will drip under the action of gravity to form a uniform coating; the ordinary spraying method includes holding a spray gun, maintaining an appropriate distance (15-30 cm) and angle (perpendicular to the surface of the rearview mirror), and spraying the coating raw material mixture evenly on the surface of the rearview mirror.
[0040] The present invention can accurately determine the difficult-to-apply area by comparing the curvature and roughness of the rearview mirror area with preset values. For the difficult-to-apply area, the sponge application method can better adapt to the curved surface shape and ensure the integrity and consistency of the coating; for the area with higher roughness, the soft material of the sponge can better fill the tiny bumps on the surface and improve the adhesion of the coating. Different application methods are selected according to different situations, which can maximize the advantages of each method and improve the coating quality. The automatic dipping method is suitable for rearview mirrors with more complex shapes and can ensure that the coating evenly covers all parts; the ordinary spraying method is suitable for rearview mirrors with simple shapes, which is easy to operate and can quickly form a uniform coating. The above method improves the accuracy of the control of the preparation process of the rearview mirror rain agent coating and thus improves the uniformity of the rain agent coating application to avoid the problem of low service life of the rearview mirror rain agent coating.
[0041] Specifically, in step S4, when judging whether the rearview mirror rain agent coating obtained after the application is evenly applied, it is determined whether the rearview mirror rain agent coating obtained after the application is evenly applied according to the comparison result of the gloss difference parameter and color uniformity parameter of the rearview mirror applied under the corresponding application method and the corresponding preset gloss difference parameter and preset color uniformity parameter; When the gloss difference parameter of the rearview mirror coated under the corresponding coating method is less than the preset gloss difference parameter and the color uniformity parameter is less than the preset color uniformity parameter, it is judged that the rearview mirror rain agent coating obtained after coating is uniformly coated; When the gloss difference parameter of the rearview mirror coated under the corresponding coating method is greater than or equal to the preset gloss difference parameter or the color uniformity parameter is greater than or equal to the preset color uniformity parameter, it is determined that the rearview mirror rain agent coating obtained after coating is unevenly coated.
[0042] In the embodiment of the present invention, the gloss difference parameter of the rearview mirror coated by the corresponding coating method can be obtained by using a professional gloss meter to measure different areas of the rearview mirror, recording the gloss value of each measured area, and calculating the standard deviation to obtain the gloss difference parameter; the color uniformity parameter of the rearview mirror coated by the corresponding coating method can be obtained by using a spectrophotometer to measure the color of different areas of the rearview mirror, recording the color value of each measured area, and calculating the standard deviation to obtain the color uniformity parameter. The area division method is the same as the area division method when measuring the average roughness. The preset gloss difference parameter is one twentieth of the average gloss value of the rearview mirror coated by the corresponding coating method, and the preset color uniformity parameter is one twentieth of the average color value of the rearview mirror coated by the corresponding coating method, but the above values are not limited to this, and those skilled in the art can also adjust the values according to actual needs.
[0043] In the present invention, whether the coating is uniform is judged according to the gloss difference parameter and color uniformity parameter of the rearview mirror coated under the coating method. The uniformity of gloss is often closely related to the physical and chemical properties of the coating. Uniform gloss usually means that the thickness, hardness and wear resistance of the coating are consistent, which can improve the durability and scratch resistance of the rearview mirror rain agent coating and extend the service life of the product. For example, in actual use, a coating with uniform gloss can better resist the erosion of the external environment, such as ultraviolet rays, rain, dust, etc., so as to maintain good performance. For some rain agent coatings with special functions, color uniformity may also affect the performance of their functions. For example, if the color of the coating is uneven, it may cause different optical properties in different parts, thereby affecting the anti-glare effect or rain repelling performance of the rearview mirror. Ensuring color uniformity can ensure the functional consistency of the coating on the entire rearview mirror surface, improve the reliability and practicality of the product, and improve the accuracy of the control of the preparation process of the rearview mirror rain agent coating through the above method, thereby improving the uniformity of the rain agent coating coating to avoid the problem of low service life of the rearview mirror rain agent coating.
[0044] Specifically, in step S4, when it is determined that the rearview mirror bullet rain agent coating obtained after coating is unevenly coated, it is determined to optimize the preset curvature and the preset roughness with an optimization coefficient.
[0045] In the embodiment of the present invention, the value range of the optimization coefficient is set to 0.85-0.97, and the value of the optimization coefficient is preferably 0.92, but the above value is not limited thereto, and those skilled in the art may also adjust the value according to actual needs.
[0046] Specifically, in step S5, when determining whether to adjust the preparation process parameters of the rearview mirror bullet rain agent coating, it is determined whether to adjust the preparation process parameters of the rearview mirror bullet rain agent coating according to the comparison result of the average reduction rate of the contact angle within the preset time and the difference between the maximum reduction rate of the contact angle within the preset time and the average reduction rate and the corresponding preset reduction rate and preset difference; When the average decrease rate of the contact angle within the preset time is greater than or equal to the preset decrease rate and the difference between the maximum decrease rate and the average decrease rate of the contact angle within the preset time is less than the preset difference, it is determined that the preparation process parameters of the rearview mirror bullet rain agent coating need to be adjusted; When the average decrease rate of the contact angle within the preset time is less than the preset decrease rate or the average decrease rate of the contact angle within the preset time is greater than or equal to the preset decrease rate and the difference between the maximum decrease rate and the average decrease rate of the contact angle is greater than or equal to the preset difference, it is determined that there is no need to adjust the preparation process parameters of the rearview mirror bullet rain agent coating.
[0047] In the embodiment of the present invention, the preset time is preferably 30 days, and the contact angle of the monitored water droplets on the evenly applied rearview mirror rain agent coating surface can be measured by a contact angle meter; the average decrease rate of the contact angle within the preset time is to measure the contact angle of the water droplets on the evenly applied rearview mirror rain agent coating surface once at one tenth of the preset time, and subtract the contact angle obtained by the last measurement from the contact angle obtained by this measurement to obtain the difference, the ratio of the difference to the time is the decrease rate, the average decrease rate is the average value of the decrease rate calculated 10 times, the preset decrease rate is the historical average value of the average decrease rate of the contact angle of the water droplets on the evenly applied rearview mirror rain agent coating surface, and the preset difference is one tenth of the average decrease rate, but the above values are not limited to this, and those skilled in the art can also adjust the value according to actual needs.
[0048] Specifically, in step S5, when it is determined to adjust the preparation process parameters of the rearview mirror anti-fouling agent coating, it is determined to adjust the preset surface cleanliness and the preset average roughness by the adjustment coefficient.
[0049] In the embodiment of the present invention, the adjustment amount of the preset surface cleanliness is positively correlated with the average reduction rate of the contact angle within the preset time, and the adjustment amount of the preset average roughness is positively correlated with the average reduction rate of the contact angle within the preset time. The value range of the adjustment coefficient is set to 1.05-1.25, and the adjustment coefficient is preferably 1.12, but the above values are not limited to this, and technical personnel in this field can also adjust the value according to actual needs.
[0050] The present invention can directly reflect the hydrophobic performance of the coating by monitoring the change of the contact angle of water droplets on the coating surface. When the average decrease rate of the contact angle is less than the preset decrease rate, it indicates that the hydrophobic performance of the coating is relatively stable. When the average decrease rate of the contact angle is greater than or equal to the preset decrease rate, it is necessary to compare the difference between the maximum decrease rate and the average decrease rate of the contact angle with the preset difference to determine whether the rearview mirror bullet rain agent coating is damaged due to scratches or friction. When the difference is greater than or equal to the preset difference, it indicates that the rearview mirror bullet rain agent coating is damaged due to scratches or friction. If the bullet rain agent coating is damaged due to scratches or friction, it does not mean that the preparation process is unqualified. At this time, it is determined that there is no need to adjust the preparation process parameters of the rearview mirror bullet rain agent coating. When the difference is greater than or equal to the preset difference, it means that the preparation process is unqualified. At this time, it is necessary to use an adjustment coefficient to increase the preset surface cleanliness and the preset average roughness to increase the service life of the rearview mirror bullet rain agent coating. The above method improves the accuracy of the control of the preparation process of the rearview mirror bullet rain agent coating and thus improves the uniformity of the application of the bullet rain agent coating to avoid the problem of low service life of the rearview mirror bullet rain agent coating.
[0051] Example 1: 40 parts by weight of silicone resin, 1 part by weight of polyether modified polydimethylsiloxane leveling agent, 0.5 parts by weight of silicone defoaming agent, 30 parts by weight of isopropanol, and 3 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing a rearview mirror bullet rain agent coating, and the raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixture, and a rearview mirror bullet rain agent coating is prepared by the preparation method of the present invention, and the rearview mirror coated with the bullet rain agent coating is placed in a QUV aging test box, and the ultraviolet wavelength is set to 340nm, the irradiance is set to 0.89W / m², the illumination and condensation cycle period is 4 hours of illumination (60°C) and 4 hours of condensation (50°C), and after a certain period of time (such as 250-1000 hours) of circulation, the gloss change data of the coating is recorded in Table 1.
[0052] Example 2: 50 parts by weight of silicone resin, 2 parts by weight of polyether modified polydimethylsiloxane leveling agent, 1 part by weight of silicone defoamer, 40 parts by weight of isopropanol, and 5 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing a rearview mirror bullet rain agent coating, and the raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixture, and a rearview mirror bullet rain agent coating is prepared by the preparation method of the present invention, and the rearview mirror coated with the bullet rain agent coating is placed in a QUV aging test box, and the ultraviolet wavelength is set to 340nm, the irradiance is set to 0.89W / m², the illumination and condensation cycle period is 4 hours of illumination (60°C) and 4 hours of condensation (50°C), and after a certain period of time (such as 250-1000 hours) of circulation, the gloss change data of the coating is recorded in Table 1.
[0053] Comparative Example: 40 parts by weight of silicone resin, 1 part by weight of polyether modified polydimethylsiloxane leveling agent, 0.5 parts by weight of silicone defoaming agent, 30 parts by weight of isopropyl alcohol, and 3 parts by weight of fluorocarbon surfactant are selected as raw materials for preparing the rearview mirror bullet rain agent coating, and the prepared raw materials are placed in a stirring device in sequence and stirred to obtain a coating raw material mixed liquid, and the rearview mirror bullet rain agent coating is prepared by a general preparation method, and the rearview mirror coated with the bullet rain agent coating is placed in a QUV aging test box, and the ultraviolet wavelength is set to 340nm, the irradiance is set to 0.89W / m², the illumination and condensation cycle period is 4 hours of illumination (60°C) and 4 hours of condensation (50°C), and after a certain period of time (such as 250-1000 hours) of circulation, the gloss change data of the coating is recorded in Table 1.
[0054] Group record data Initial gloss (GU) Gloss after 250 hours (GU) Gloss after 500 hours (GU) Gloss after 1000 hours (GU) Average value (GU) Example 1 80 78 70 65 73.25 Example 2 80 77 68 63 72 Comparative Example 80 72 60 40 63 From the data in Table 1, it can be concluded that the rate of gloss reduction of the rearview mirror bullet rain agent coating prepared by the present invention under long-term exposure to outdoor radiation is much lower than that of the rearview mirror bullet rain agent coating prepared by the general method. Therefore, the rearview mirror bullet rain agent coating prepared by the present invention has the advantage of long service life compared with the rearview mirror bullet rain agent coating prepared by the general method.
[0055] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a rearview mirror anti-raining agent coating, characterized in that: include: Select 40 to 60 parts by weight of silicone resin, 1 to 3 parts by weight of polyether modified polydimethylsiloxane leveling agent, 0.5 to 1.5 parts by weight of silicone defoamer, 30 to 50 parts by weight of isopropanol, and 3 to 8 parts by weight of fluorocarbon surfactant as raw materials for preparing the rearview mirror bullet rain agent coating, and put the raw materials into a stirring device in order and stir to obtain a coating raw material mixed liquid; Pre-treating the surface of the rearview mirror, including sequentially cleaning, polishing and rinsing the surface of the rearview mirror, and determining whether to apply the coating raw material mixture to the surface of the rearview mirror based on the surface cleanliness and average roughness of the pre-treated rearview mirror surface; When it is determined to apply the coating raw material mixture to the rearview mirror surface, a coating difficulty area is determined based on the curvature and roughness of the rearview mirror area to be coated, and a coating method of the coating raw material mixture is determined according to the coating difficulty area and the complexity of the shape of the rearview mirror to be coated; Based on the gloss difference parameter and the color uniformity parameter of the rearview mirror after the application, it is judged whether the rearview mirror rain agent coating obtained after the application is uniform, and when the rearview mirror rain agent coating obtained is not uniformly applied, it is determined to optimize the judgment parameter of the difficult application area, wherein the judgment parameter includes a preset curvature and a preset roughness; Monitor the contact angle of water droplets on the surface of a uniformly applied rearview mirror anti-fouling agent coating, and determine whether to adjust the preparation process parameters of the rearview mirror anti-fouling agent coating based on the average decrease rate of the contact angle within a preset time and the difference between the maximum decrease rate and the average decrease rate of the contact angle within a preset time, wherein the preparation process parameters include a preset surface cleanliness and a preset average roughness.
2. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 1, characterized in that: The determining whether to apply the coating raw material mixture to the rearview mirror surface comprises: The surface cleanliness and average roughness of the pre-treated rearview mirror surface are compared with the corresponding preset surface cleanliness and preset average roughness, respectively, wherein: If the surface cleanliness of the pre-treated rearview mirror surface is greater than or equal to the preset surface cleanliness and the average roughness is greater than or equal to the preset average roughness, determining to apply the coating raw material mixture to the rearview mirror surface; If the surface cleanliness of the rearview mirror surface after pretreatment is less than the preset surface cleanliness or the average roughness is less than the preset average roughness, it is determined to perform secondary pretreatment on the rearview mirror surface.
3. The method for preparing the anti-raining agent coating for rearview mirror according to claim 2, characterized in that: The preset surface cleanliness is determined according to a historical average of the surface cleanliness of the pre-treated rearview mirror surface, and the preset average roughness is determined according to a historical average of the average roughness of the pre-treated rearview mirror surface.
4. The method for preparing the anti-raining agent coating for rearview mirror according to claim 3, characterized in that: When determining to apply the coating raw material mixture to the surface of the rearview mirror, the determination of the difficult-to-apply area includes: The curvature and roughness of the rearview mirror area to be painted are compared with the corresponding preset curvature and preset roughness, respectively, wherein: If the curvature of the rearview mirror area to be painted is greater than a preset curvature or the roughness of the rearview mirror to be painted is greater than a preset roughness, it is determined that the rearview mirror area to be painted is a difficult-to-paint area.
5. The method for preparing the anti-raining agent coating for rearview mirror according to claim 4, characterized in that: The preset curvature is determined based on a historical average value of the curvature of the rearview mirror area to be painted.
6. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 5, characterized in that: The method for determining the coating raw material mixture to be applied comprises: If the rearview mirror area to be coated is a difficult coating area, determining that the coating raw material mixture is coated by a sponge coating method; If the rearview mirror area to be coated is not a difficult coating area and the shape complexity of the rearview mirror to be coated is greater than or equal to a preset complexity, determining that the coating raw material mixture coating method is an automatic dipping method; If the rearview mirror area to be coated is not a difficult-to-coat area and the shape complexity of the rearview mirror to be coated is less than a preset complexity, it is determined that the coating raw material mixture is coated by a common spraying method.
7. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 6, characterized in that: The step of judging whether the rearview mirror bullet rain agent coating obtained after the application is evenly applied comprises: The gloss difference parameter and color uniformity parameter of the rearview mirror painted under the corresponding painting method are compared with the corresponding preset gloss difference parameter and preset color uniformity parameter, wherein: If the gloss difference parameter of the rearview mirror coated under the corresponding coating method is less than the preset gloss difference parameter and the color uniformity parameter is less than the preset color uniformity parameter, it is determined that the rearview mirror rain agent coating obtained after coating is uniformly coated; If the gloss difference parameter of the rearview mirror coated under the corresponding coating method is greater than or equal to the preset gloss difference parameter or the color uniformity parameter is greater than or equal to the preset color uniformity parameter, it is determined that the rearview mirror rain agent coating obtained after coating is uneven.
8. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 7, characterized in that: When it is determined that the rearview mirror bullet rain agent coating obtained after the coating is unevenly coated, the preset curvature and the preset roughness are optimized.
9. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 8, characterized in that: The step of determining whether to adjust the parameters of the preparation process of the rearview mirror bullet rain agent coating comprises: The average decrease rate of the contact angle within the preset time and the difference between the maximum decrease rate and the average decrease rate of the contact angle within the preset time are compared with their corresponding preset decrease rates and preset differences, wherein: If the average reduction rate of the contact angle within the preset time is greater than or equal to the preset reduction rate and the difference between the maximum reduction rate and the average reduction rate of the contact angle within the preset time is less than the preset difference, the preparation process parameters of the rearview mirror rain agent coating are determined to be adjusted.
10. The method for preparing the anti-raining agent coating for a rearview mirror according to claim 9, characterized in that: The adjustment amount of the preset surface cleanliness is positively correlated with the average reduction rate of the contact angle within the preset time, and the adjustment amount of the preset average roughness is positively correlated with the average reduction rate of the contact angle within the preset time.
Citation Information
Patent Citations
Super hydrophobic paint and preparation and construction methods thereof
CN107267030A
Water vapor resisting water-borne coating stock solution and preparation method thereof and water vapor resisting water-borne coating and application thereof
CN107699068A
High-weather-resistance water-based argil-imitating coating and preparation method thereof
CN113308191A
Hardcoat agent composition, molded article and lens
JP2009227801A
Surface-treating agent
JP2013116972A
Cited By
Preparation method of quick-hydrophobic elastic rain agent coating
CN120502482A
A method for preparing a fast hydrophobic rain-repellent coating
CN120502482B