Advanced refining cell for aluminum scrap recycling

The aluminum refining cell with integrated reservoirs and inert gas maintenance addresses oxidation and energy inefficiencies, enabling efficient production of high-purity aluminum from scrap materials.

JP2024543460APending Publication Date: 2024-11-21ALCOA USA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024527808
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2022-11-14
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing aluminum refining processes face challenges in efficiently producing high-purity aluminum while minimizing oxidation and energy consumption, particularly when using scrap materials that are often contaminated and require complex collection and sorting.

Method used

The implementation of an aluminum refining cell with integrated reservoirs and a hermetically sealed design, utilizing inert gas to maintain an inert atmosphere, reduces oxidation and interference during the refining process, and includes a feed and tapping system to manage scrap feedstock efficiently.

Benefits of technology

This approach enhances the production of high-purity aluminum by limiting oxidation and reducing energy consumption, making the process more cost-effective and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543460000001_ABST
    Figure 2024543460000001_ABST
Patent Text Reader

Abstract

The present disclosure includes methods for refining aluminum. The methods include producing purified aluminum from an aluminum feedstock in an aluminum refining cell and flowing the purified aluminum from a cell chamber of the aluminum refining cell through an overflow passage to a refined metals reservoir located inside the aluminum refining cell. In some embodiments, a feed reservoir is located inside the aluminum refining cell and is accessible through a feed port located in a refractory top cover of the cell chamber. In some embodiments, the methods include removing the refined aluminum from the refined metals reservoir through a tapping port located in a refractory top cover of the cell chamber. In some embodiments, simultaneously with the removing step, the methods include limiting or preventing oxidation of the refined aluminum.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] <CROSS REFERENCE TO RELATED APPLICATIONS> This application claims priority to U.S. Provisional Patent Application No. 63 / 279,447, entitled "Advanced Purification Cell for Aluminum Scrap Recycling," filed on November 15, 2021, and U.S. Provisional Patent Application No. 63 / 335,984, entitled "Advanced Purification Cell for Aluminum Scrap Recycling," filed on April 28, 2022, each of which is hereby incorporated by reference in its entirety. [Background technology]

[0002] Aluminum has traditionally been produced as alumina (Al 2 O 3 ) has been made from alumina (Al 2 O 3 The conversion of aluminium to alumina (Al 2 O 3 ) is dissolved in cryolite, a flux, and then an electric current is passed through the mixture, dissolving the carbon from the carbon anode into dissolved alumina (Al 2 O 3 ) to obtain aluminum and carbon dioxide as by-products. Various efforts have been made to purify aluminum, including the "Hoopes Process" (see U.S. Pat. No. 1,534,315) and the process described in commonly owned international patent application WO2016 / 130823. Summary of the Invention

[0003] In general, the present disclosure relates to methods and systems for producing purified aluminum via an aluminum refining cell that may include one or more reservoirs internal to the cell. For example, in one embodiment, the cell may include one or both of (i) a feed reservoir internal to the cell, and (ii) a refined metal reservoir internal to the cell. Placing the one or more reservoirs internal to the cell may limit / prevent oxidation, at least in part, because the cell may be hermetically sealed. In some embodiments, fluids to and from the cell may be provided through ports to maintain a hermetic seal. For example, in one embodiment, a feed port may provide access to the feed reservoir, and / or a tapping port may provide access to the refined metal reservoir. In some examples, an inert gas may also be provided to the cell to further prevent / limit oxidation of the aluminum metal. When the one or more reservoirs are located internal to the cell, the inert gas may provide an inert atmosphere to the cell including the one or more reservoirs. In some embodiments, when producing refined aluminum, the one or more reservoirs may reduce cell disturbances by (i) feeding aluminum feedstock to the cell, and / or (ii) tapping refined aluminum from the refined metal reservoir. The present disclosure may also reduce heat losses and improve energy consumption during operation of an aluminum refining cell. The methods disclosed herein may be more cost effective, for example, in producing refined aluminum products.

[0004] In one aspect, the disclosure includes a method for refining aluminum, comprising: producing purified aluminum from an aluminum feedstock in an aluminum refining cell, the purified aluminum having a density less than an electrolyte of the aluminum refining cell, the electrolyte having a density less than a molten metal pad of the aluminum refining cell; and flowing the purified aluminum from a cell chamber of the aluminum refining cell through an overflow passage to a refined metal reservoir, the refined metal reservoir being located within the aluminum refining cell.

[0005] In some embodiments, the producing process includes providing an aluminum feedstock to an aluminum refining cell, where the aluminum feedstock includes aluminum metal (e.g., aluminum scrap), and the aluminum refining cell includes a molten metal pad and an electrolyte.

[0006] In some embodiments, the step of supplying the aluminum feedstock comprises flowing the aluminum feedstock into the molten metal pad via a supply reservoir located within the aluminum refining cell. In some embodiments, the aluminum feedstock is aluminum alloy scrap. In some embodiments, the aluminum alloy scrap comprises scrap of 1xxx series aluminum alloys, 2xxx series aluminum alloys, 3xxx series aluminum alloys, 4xxx series aluminum alloys, 5xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys, 8xxx series aluminum alloys, or any combination thereof. In some embodiments, the aluminum alloy scrap comprises new aluminum scrap and / or old aluminum scrap.

[0007] Aluminum scrap can be described as new scrap or old scrap. New aluminum scrap is aluminum scrap from the manufacturing process and old aluminum scrap is post-consumer aluminum scrap. New aluminum scrap is generated during the manufacturing of aluminum semi-manufactured and finished products. Old aluminum scrap is scrap from products that are recovered after disposal by consumers. Old aluminum scrap may be more contaminated than new aluminum scrap. Some examples of old aluminum scrap include, but are not limited to, end-of-life vehicles, dismantled buildings, dismantled construction materials, discarded packaging materials, home and office appliances, and machinery and equipment.

[0008] The collection and sorting of aluminium scrap, e.g. old aluminium scrap, can be a complex scheme involving millions of households, local and regional authorities, small and medium-sized collectors, and metal retailers. Waste and environmental policies can also have a strong influence on the effectiveness of collection schemes.

[0009] Aluminum scrap may need to be separated, further sorted, and pre-treated before the metal can be recovered in a melting furnace. Separation of aluminum scrap at this stage can be accomplished by various mechanical actions such as magnetic, gravitational, eddy current, or color sensors. Further separation of different aluminum alloys may also be achieved by X-ray, X-ray fluorescence (XRF) spectroscopy, and / or laser-induced breakdown spectroscopy (LIBS) methods. For example, wrought and cast alloys can be separated prior to mechanical processes.

[0010] In some embodiments, the aluminum purification cell includes a cell chamber defined at least in part by a refractory sidewall, a refractory top cover, and a cell bottom, the cell bottom being located proximal to the base. In some embodiments, the disclosure includes providing access to the refined metal reservoir via a feed port that penetrates the refractory top cover of the cell chamber. In some embodiments, the disclosure includes providing an inert gas to the cell chamber via an inert gas inlet formed in the refractory top cover of the cell chamber, thereby providing an inert atmosphere to the cell chamber. In some embodiments, the disclosure includes maintaining an inert atmosphere in the cell chamber of the aluminum purification cell while feeding aluminum feedstock to the feed reservoir, producing refined aluminum, and removing refined aluminum from the aluminum purification cell via a tapping port.

[0011] In some embodiments, the disclosure includes removing the refined aluminum from the refined metal reservoir through a tapping port located in a refractory top cover of the cell chamber. In some embodiments, the disclosure includes limiting or preventing oxidation of the refined aluminum simultaneously with the removing step. In some embodiments, the disclosure includes a feed port of the feed reservoir and a tapping port of the refined metal reservoir at least partially defining a hermetic seal of the cell chamber.

[0012] In some embodiments, the disclosure includes at least one anode overlapping at least one cathode, thereby defining an anode-cathode overlap, where a distal end of the at least one cathode is proximal to a middle portion of the at least one anode, and where a distal end of the at least one anode is proximal to a middle portion of the at least one cathode. In some embodiments, the generating step includes passing a current through the electrolyte to the at least one anode and to the at least one cathode, where (i) the at least one anode and the at least one cathode are partially disposed within the electrolyte, and (ii) the at least one anode is partially disposed within the molten metal pad. In some embodiments, the generating step includes generating aluminum ions within the electrolyte and reducing at least a portion of the aluminum ions at or near at least one cathode of the aluminum purification cell. In some embodiments, the generating step includes generating aluminum ions from the at least one anode, transferring at least a portion of the aluminum ions into the electrolyte, and reducing at least a portion of the aluminum ions at or near at least one cathode of the aluminum purification cell.

[0013] In another aspect, the present disclosure includes an aluminum refining cell including a cell chamber including a cell bottom, a refractory sidewall, and a refractory top cover, at least one anode extending upwardly from the cell bottom, a cathode connector located proximate the refractory top cover, at least one cathode extending downwardly from the cathode connector, and an overflow passage extending from the cell chamber to a refined metal reservoir located within the aluminum refining cell.

[0014] In some embodiments, the aluminum refining cell further includes a tapping port 200 and a feed port located within the refractory top cover of the cell chamber. In some embodiments, the feed port and the tapping port at least partially define a hermetic seal of the cell chamber. In some embodiments, the aluminum refining cell further includes a feed reservoir located within the aluminum refining cell. In some embodiments, the feed reservoir directs the aluminum feedstock directly to the molten metal pad of the cell chamber. In some embodiments, the aluminum refining cell further includes an inert gas inlet formed within the refractory top cover and configured to provide an inert atmosphere to the cell chamber. In some embodiments, the distal end 92 of the at least one anode 90 and the distal end 152 of the at least one cathode 150 partially overlap.

[0015] Although the present disclosure is generally directed to refining aluminum, the devices, systems, and methods described herein are applicable to refining other metals (e.g., magnesium). [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic cutaway side view of one embodiment of an aluminum refining cell for refining aluminum, according to some embodiments.

[0017] [Diagram 2]FIG. 2 is a schematic cutaway side view of one embodiment of an aluminum refining cell for refining aluminum, according to some embodiments.

[0018] [Diagram 3] FIG. 3 illustrates one embodiment of a method for refining aluminum metal, such as aluminum scrap, in an aluminum refining cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present disclosure is further described with reference to the accompanying drawings, in which like structures are referred to by like numerals throughout the several views. The drawings constitute a part of this specification and include exemplary embodiments of the present disclosure, illustrating various objects and features thereof. Moreover, the drawings are not necessarily to scale, and some features may be exaggerated to show details of the components. Moreover, any dimensions, specifications, etc. shown in the figures are for illustrative purposes and not limiting. Therefore, specific structural and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art to various uses of the present disclosure.

[0020] Among these disclosed advantages and improvements, other objects and advantages of the present disclosure will become apparent from the following description taken in conjunction with the accompanying drawings. Detailed embodiments of the present disclosure are disclosed herein. However, it should be understood that the disclosed embodiments are merely exemplary of the present disclosure, which may be embodied in various forms. Moreover, each of the examples given in connection with the various embodiments of the present disclosure are intended to be illustrative and not limiting.

[0021] Throughout the specification and claims, the following terms have the meanings expressly associated therewith, unless the context clearly dictates otherwise. As used herein, the phrases "in one embodiment" and "in some embodiments" may refer to the same embodiment, but do not necessarily refer to the same embodiment. Additionally, as used herein, the phrases "in another embodiment" and "in some other embodiments" may refer to different embodiments, but do not necessarily refer to different embodiments. Thus, as described below, various embodiments of the present disclosure may be readily combined without departing from the scope or spirit of the present disclosure.

[0022] Additionally, the term "or" as used herein is an inclusive "or" operator and is equivalent to the term "and / or" unless the context clearly dictates otherwise. The term "based on" is not exclusive and acknowledges that a term may be based on another unlisted element unless the context clearly dictates otherwise. Additionally, throughout this specification, the meanings of "a," "an," and "the" include plural referents. The meaning of "in" includes "in" and "on."

[0023] As used herein, "aluminum source" means a material having at least 50% aluminum by weight.

[0024] As used herein, "refined aluminum" means a material having at least 99.5% aluminum by weight.

[0025] As used herein, "molten metal pad" means a reservoir of molten material disposed beneath the electrolyte, the molten material comprising aluminum.

[0026] As used herein, "aluminum wettable" means having a contact angle with molten aluminum of 90 degrees or less.

[0027] As used herein, "electrolyte" refers to a medium through which electric current flows by the movement of ions / ionic species. In one embodiment, the electrolyte may include a molten salt.

[0028] As used herein, "energy efficiency" means the amount of energy (in kilowatt-hours) consumed by an aluminum refining cell per kilogram of refined aluminum produced by the aluminum refining cell. Energy efficiency may therefore be expressed in kilowatt-hours per kilogram of aluminum produced (kWh / kg).

[0029] As used herein, "anode-cathode overlap" (ACO) means the vertical distance from the distal end of an anode (e.g., an elongated vertical anode) to the distal end of each cathode (e.g., an elongated vertical cathode).

[0030] As used herein, "anode-cathode distance" (ACD) means the horizontal distance separating an anode (eg, an elongated vertical anode) from each cathode (eg, an elongated vertical cathode).

[0031] 1 and 2 are schematic cutaway side views of one embodiment of an aluminum refining cell 1 for refining aluminum, according to some embodiments. The aluminum refining cell 1 comprises a cell chamber 210 having a cell bottom 60, a refractory sidewall 30, and a refractory top cover 40, at least one anode 90 extending upwardly from the cell bottom 60, a cathode connector 140 located proximate the refractory top cover 40, at least one cathode 150 extending downwardly from the cathode connector 140, and an overflow passage 250 extending from the cell chamber 210 to a refined metal reservoir 260 located inside the aluminum refining cell 1. An example of an aluminum refining cell 1 can be found in commonly owned U.S. Patent No. 10,407,786, entitled "Systems and Methods for Purifying Aluminum," filed February 11, 2016, which is incorporated by reference in its entirety.

[0032] The cell chamber 210 is at least partially defined by the refractory sidewall 30, the refractory top cover 40, and the cell bottom 60. The cell bottom 60 is located proximal to the base 10. In some embodiments, the cell chamber 210 includes a tapping port 200 and a feed port 170, both located within the refractory top cover 40 of the cell chamber 210. The feed port 170 and the tapping port 200 at least partially define a hermetic seal of the cell chamber 210. The feed port 170 connects to a feed reservoir 270. The feed reservoir 270 is located inside the aluminum refining cell 1. The tapping port 200 connects to a refined metal reservoir 260. The feed reservoir 270 is located inside the aluminum refining cell 1. The refined metal reservoir 260 and the feed reservoir 270 are located within the hermetically sealed environment of the aluminum refining cell 1.

[0033] The aluminum refining cell 1 further includes an inert gas inlet 220 formed in the refractory top cover 40 and configured to provide an inert atmosphere to the hermetically sealed cell chamber 210. In addition to the inert gas inlet 220, the supply reservoir 270 and the refined metal reservoir 260 may each have an inert gas inlet to provide an inert atmosphere for the hermetically sealed environment. Providing an inert gas 222 into the cell chamber 210 further prevents or limits oxygen from entering the cell chamber 210.

[0034] The design of the aluminum refining cell 1 allows the cell chamber 210 to be sealed from air and prevents or limits oxidation of the top metal of the refined aluminum 120 in the aluminum refining cell 1. The feed port 170 allows scrap (e.g., scrap containing aluminum) to be fed and mixed with the anode metal. The feed port 170 allows for reduced disturbance to the molten metal pad 100 in the cell chamber 210 during feeding of scrap to the cell chamber 210. Similarly, the tapping port 200 eliminates disturbance during metal tapping. The design of the aluminum refining cell 1, including the refined metal reservoir 260 and the feed reservoir 270 located therein, allows for feeding the aluminum feedstock 180 to the feed reservoir 270, refining the aluminum feedstock 180 to the refined aluminum 120 in the cell chamber 210, and removing the refined aluminum 120 from the refined metal reservoir 260 while maintaining a hermetic seal of the cell chamber 210.

[0035] In some embodiments, the supply reservoir 270 is carbon-based. In some embodiments, the supply reservoir 270 is an anode and is not electrically insulated. The supply reservoir 270 directs the aluminum feedstock 180 directly to the molten metal pad 100 in the cell chamber 210. In some embodiments, the molten metal pad 100 comprises at least 50% aluminum metal by weight. In some embodiments, the molten metal pad 100 comprises at least one alloy including Al, Si, at least 0.5% by weight of one or more of Cu, Fe, Sb, Gd, Cd, Sn, Pb, and impurities.

[0036] The refined metal reservoir 260 is located within the interior of the aluminum refining cell 1. In some embodiments, the refined metal reservoir 260 is substantially surrounded by a refractory material (e.g., refractory sidewall 30). In some embodiments, the refined metal reservoir 260 is partially surrounded by a refractory material. Access to the refined metal reservoir 260 is via a tapping port 200 that penetrates the refractory top cover 40 of the cell chamber 210.

[0037] Similar to the tapping port 200, the feed port 170 passes through the refractory top cover 40, thereby providing access to a feed reservoir 270. The feed reservoir 270 provides access to the lower portion of the cell chamber 210 which contains the molten metal pad 100.

[0038] In some embodiments, the fire resistant top cover 40 may be one piece or may have separate pieces. For example, the fire resistant top cover 40 may have separate, separate covers for the supply reservoir 270 and the supply port 170. Similarly, the fire resistant top cover 40 may have separate, separate covers for the refined metal reservoir 260 and the tapping port 200.

[0039] The cell bottom 60 includes an upper surface 80 and a lower surface 70. In some embodiments, the cell bottom 60 is flat. In some embodiments, the cell bottom 60 slopes downwardly towards the feed reservoir 270. In some embodiments, the slope of the cell bottom 60 has an angle of less than 10 degrees. In some embodiments, the slope of the cell bottom 60 has an angle of between 3 and 5 degrees.

[0040] The aluminum purification cell 1 includes a cathode connector 140 proximate the fire resistant top cover 40. The cathode connector 140 includes an upper connecting rod 130 configured to connect to an external power source. The cathode connector 140 includes a lower surface 142 and an upper surface 144. Opposite the cathode connector 140, the aluminum purification cell 1 includes an anode connector 50 in electrical communication with the cell bottom 60. The anode connector 50 is configured to connect to an external power source.

[0041] At least one anode 90 and at least one cathode 150 are electrodes. In some embodiments, some of the electrodes are made of the same material and some are made of different materials. In some embodiments, all of the electrodes are made of different materials. In some embodiments, all of the electrodes are made of the same material. In some embodiments, some of the electrodes are made of a carbonaceous material and some of the electrodes are made of a non-carbonaceous material.

[0042] The electrodes (i.e., at least one anode 90 and at least one cathode 150) are constructed from an aluminum wettable material. In some embodiments, the electrodes are constructed from TiB 2 , ZrB 2 , HfB 2 , SrB 2 , a carbonaceous material (e.g., graphite), a non-carbonaceous material, or a combination thereof. In some embodiments, the electrode is made of a non-carbonaceous material. In some embodiments, the electrode is made of a cermet or a ceramic. In some embodiments, the electrode is a ceramic. In some embodiments, the electrode is made of TiB2 In some embodiments, the electrode is made of multiple layers.

[0043] At least one anode 90 is disposed on the cell bottom 60 of the aluminum refining cell 1. The at least one anode 90 includes a proximal end 94 connected to the top surface 80 of the cell bottom 60. The at least one anode 90 includes a distal end 92 that extends upwardly toward the refractory top cover 40 of the aluminum refining cell 1. The at least one anode 90 includes an intermediate portion between the distal end 92 and the proximal end 94. In some embodiments, the at least one anode 90 is a vertical anode.

[0044] The at least one cathode 150 includes a proximal end 154 connected to the cathode connector 140 and a distal end 152 extending downward toward the base 10. The at least one cathode 150 includes an intermediate portion between the proximal end 154 and the distal end 152. In some embodiments, the at least one cathode 150 is a vertical cathode. The at least one anode 90 may be interleaved with the at least one cathode 150.

[0045] In some embodiments, at least one anode 90 overlaps with at least one cathode 150, thereby defining an anode-cathode overlap (ACO) 290. The distal end 92 of the at least one anode 90 and the distal end 152 of the at least one cathode 150 partially overlap. In some embodiments, the distal end 152 of the at least one cathode 150 is proximal to a middle portion of the at least one anode 90, and the distal end 92 of the at least one anode 90 is proximal to a middle portion of the at least one cathode 150. In some embodiments, the anode-cathode overlap (ACO) 290 is between 0 and 50 inches. In some embodiments, the anode-cathode overlap 290 is between 1 and 50 inches. In some embodiments, the anode-cathode overlap 290 is between 5 and 50 inches. In some embodiments, the anode-cathode overlap 290 is between 10 and 50 inches. In some embodiments, the anode-cathode overlap 290 is between 20 and 50 inches. In some embodiments, the anode-cathode overlap 290 is between 25 and 50 inches. In some embodiments, the anode-cathode overlap 290 is up to 12 inches of overlap, with at least some overlap. In some embodiments, the anode-cathode overlap 290 is at least a 2 inch overlap to a 10 inch overlap. In some embodiments, the anode-cathode overlap 290 is at least a 3 inch overlap to an 8 inch overlap. In some embodiments, the anode-cathode overlap 290 is at least a 3 inch overlap to a 6 inch overlap.

[0046] The lateral spacing distance between the at least one anode 90 and the at least one cathode 150 may be designated as an anode-cathode distance (ACD) 280. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 3 inches. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 2 inches. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 1 inch. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 1 / 4 inch. In some embodiments, the anode-cathode distance 280 may be between 1 / 4 inch and 1 / 2 inch. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 3 / 4 inch. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 1 inch. In some embodiments, the anode-cathode distance 280 may be between 1 / 8 inch and 1 / 2 inch.

[0047] In some embodiments, the aluminum refining cell 1 includes an outer shell 20. The outer shell 20 may include steel or other suitable material. In some embodiments, the outer shell 20 may include a shell floor located below the base 10. In some embodiments, the outer shell 20 may include a shell sidewall spaced from and surrounding the refractory sidewall 30.

[0048] In some embodiments, the aluminum refining cell 1 may include a cell lining 190 to provide thermal insulation to the cell chamber 210. The cell lining 190 may be located between the refractory sidewall 30 and the outer shell 20, and between the base 10 and the cell bottom 60. In some embodiments, the cell lining 190 may enclose substantially all of the cell chamber 210, or only a portion of the cell chamber 210. The cell lining 190 may facilitate high electrical efficiency of the aluminum refining cell 1.

[0049] 3 illustrates one embodiment of a method 300 for refining aluminum metal, such as aluminum scrap, in an aluminum refining cell. The method 300 for refining aluminum includes providing 310 an aluminum feedstock 180 to the aluminum refining cell 1, passing an electric current through at least one anode 90, directing aluminum metal in a molten metal pad 100 to an electrolyte 110, generating at least some ions in the electrolyte 110, and generating 320 refined aluminum 120 from the aluminum feedstock 180. The method 300 further includes flowing 330 the refined aluminum 120 from a cell chamber 210 of the aluminum refining cell 1 through an overflow passage 250 to a refined metal reservoir 260.

[0050] In some embodiments, the cell chamber 210 includes a molten metal pad 100, refined aluminum 120, and an electrolyte 110. The molten metal pad 100 is in contact with the cell bottom 60. The electrolyte 110 separates the refined aluminum 120 from the molten metal pad 100. The anode 90 extends upward from the cell bottom 60 through the molten metal pad 100 and terminates in the electrolyte 110. The cathode 150 extends downward from the cathode connector 140 and terminates in the electrolyte 110 such that the cathode 150 overlaps the anode 90 in the electrolyte 110. Thus, the cathode 150 is separated from the anode 90 by the electrolyte 110.

[0051] In the illustrated embodiment, the refined aluminum 120 has a density less than the electrolyte 110 of the aluminum refining cell 1. The electrolyte 110 has a density less than the molten metal pad 100 of the aluminum refining cell 1. The electrolyte 110 separates the top layer of the refined aluminum 120 from the molten metal pad 100. In this regard, the composition of the electrolyte 110 may be selected such that the electrolyte 110 has a lower density than the molten metal pad 100 and a higher density than the refined aluminum 120. In some embodiments, the electrolyte 110 includes a molten salt. In some embodiments, the electrolyte 110 includes at least one of a fluoride and / or a chloride. In some embodiments, the electrolyte 110 includes at least one of a fluoride and / or a chloride of, among others, Na, K, Al, Ba, Ca, Ce, La, Cs, Rb, or combinations thereof.

[0052] In some embodiments, the molten metal pad 100 comprises at least 5% by weight aluminum metal, or at least 10% by weight aluminum metal, or at least 15% by weight aluminum metal, or at least 20% by weight aluminum metal, or at least 25% by weight aluminum metal, or at least 30% by weight aluminum metal, or at least 35% by weight aluminum metal, or at least 40% by weight aluminum metal, or at least 45% by weight aluminum metal, or at least 50% by weight aluminum metal, or at least 55% by weight aluminum metal, or at least 60% by weight aluminum metal, or at least 65% by weight aluminum metal, or at least 70% by weight aluminum metal, or at least 75% by weight aluminum metal, or at least 80% by weight aluminum metal, or at least 85% by weight aluminum metal, or at least 90% by weight aluminum metal, or at least 95% by weight aluminum metal.

[0053] In some embodiments, the molten metal pad 100 comprises at least one alloy including one or more of Al, Si, Cu, Fe, Sb, Gd, Cd, Sn, Pb, and impurities. In some embodiments, the composition of the wettable material on the anode 90 in the aluminum refining cell 1 is the same as or substantially similar to the molten metal pad 100. In some embodiments, the composition of the wettable material is a metal. In some embodiments, the metal comprises aluminum, or at least aluminum and magnesium. In some embodiments, the metal comprises at least 5% by weight aluminum, or at least 10% by weight aluminum, or at least 15% by weight aluminum, or at least 20% by weight aluminum, or at least 25% by weight aluminum, or at least 30% by weight aluminum, or at least 35% by weight aluminum, or at least 40% by weight aluminum, or at least 45% by weight aluminum, or at least 50% by weight aluminum, or at least 55% by weight aluminum, or at least 60% by weight aluminum, or at least 65% by weight aluminum, or at least 70% by weight aluminum, or at least 75% by weight aluminum, or at least 80% by weight aluminum, or at least 85% by weight aluminum, or at least 90% by weight aluminum, or at least 95% by weight aluminum. In some embodiments, the metal is selected from the group consisting of aluminum alloys, metallic aluminum, and combinations thereof.

[0054] The method 300 includes producing 320 purified aluminum 120 from the aluminum feedstock 180 by passing an electric current through the electrolyte 110 to the at least one anode 90 and to the at least one cathode 150. In some embodiments, passing the electric current includes passing a direct current through the electrolyte 110 from the at least one anode 90 to the at least one cathode 150. When producing 320 purified aluminum 120, the at least one anode 90 and the at least one cathode 150 may be partially disposed within the electrolyte 110, and the at least one anode 90 may be partially disposed within the molten metal pad 100. Directing the aluminum metal of the molten metal pad 100 toward the electrolyte 110 may include passing the aluminum metal toward the electrolyte 110 and providing an electric current to the at least one anode 90.

[0055] The aluminum refining cell 1 includes a molten metal pad 100 and an electrolyte 110. In some embodiments, supplying 310 the aluminum feedstock 180 includes flowing the aluminum feedstock 180 into the molten metal pad 100 via a supply reservoir 270 located inside the aluminum refining cell 1.

[0056] As discussed herein, supplying 310 the aluminum feedstock 180 may be through the aluminum purification cell 1. In some embodiments, the supplying step 310 includes continuously supplying the aluminum feedstock 180 during operation of the aluminum purification cell 1. In some embodiments, the supplying step 310 includes periodically adding the aluminum feedstock 180 to the aluminum purification cell 1. In some embodiments, the supplying step 310 includes metering the aluminum feedstock 180 to the aluminum purification cell 1 at a first supply rate. The first supply rate may be kept constant or may vary, including stopping and starting the supply 310 of the aluminum feedstock 180 to the aluminum purification cell 1. In some embodiments, the supplying step 310 includes periodically adding the aluminum feedstock 180 to the aluminum purification cell 1.

[0057] In some embodiments, aluminum source 180 includes aluminum metal. In some embodiments, aluminum source 180 includes at least one other metal other than aluminum metal. In some embodiments, aluminum source 180 includes a transition metal. In some embodiments, aluminum source 180 includes at least 50% aluminum metal by weight, or at least 55% aluminum metal by weight, or at least 60% aluminum metal by weight, or at least 65% aluminum metal by weight, or at least 70% aluminum metal by weight, or at least 75% aluminum metal by weight, or at least 80% aluminum metal by weight, or at least 85% aluminum metal by weight, or at least 90% aluminum metal by weight, or at least 95% aluminum metal by weight.

[0058] In some embodiments, the aluminum feedstock 180 includes impurities. In some embodiments, the impurities of the aluminum feedstock 180 can include Cr, Cu, Fe, Mg, Mn, Ni, Si, Ti, and Zn. In some embodiments, the aluminum feedstock 180 can have aluminum with up to 2% Mg by weight, in addition to other impurities. In some embodiments, the aluminum feedstock 180 includes 0.5% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes impurities. In some embodiments, the aluminum feedstock 180 includes 0.5% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 5.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 10.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 15.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 20.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 25.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 30.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 35.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 40.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 45.0% to 50.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 contains between 0.5% and 45.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 contains between 0.5% and 40.0% impurities by weight of the aluminum feedstock 180.In some embodiments, the aluminum feedstock 180 includes 0.5% to 35.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 30.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 25.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 20.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 15.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 10.0% impurities by weight of the aluminum feedstock 180. In some embodiments, the aluminum feedstock 180 includes 0.5% to 5.0% impurities by weight of the aluminum feedstock 180.

[0059] In some embodiments, an additive (e.g., copper) is added to the aluminum feedstock 180 to increase density and retain the metal of the aluminum feedstock 180 in a molten metal pad 100 on the bottom of the aluminum refining cell 1. In some examples, the aluminum feedstock 180 comprises at least 5% copper by weight, at least 10% copper by weight, at least 15% copper by weight, at least 20% copper by weight, at least 25% copper by weight, at least 30% copper by weight, at least 35% copper by weight, at least 40% copper by weight, at least 45% copper by weight, or at least 50% copper by weight. Thus, the molten metal pad 100 may comprise a relatively large amount of copper. In some embodiments, the molten metal pad 100 comprises at least 5% by weight copper, at least 10% by weight copper, at least 15% by weight copper, at least 20% by weight copper, at least 25% by weight copper, at least 30% by weight copper, at least 35% by weight copper, at least 40% by weight copper, at least 45% by weight copper, at least 50% by weight copper, or more.

[0060] In some embodiments, the aluminum feedstock 180 is aluminum alloy scrap. In some embodiments, the aluminum alloy scrap includes at least one of a 1xxx series aluminum alloy, a 2xxx series aluminum alloy, a 3xxx series aluminum alloy, a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, a 6xxx series aluminum alloy, a 7xxx series aluminum alloy, an 8xxx series aluminum alloy, or any combination thereof.

[0061] In some embodiments, the generating step 320 includes generating aluminum ions in the electrolyte 110 and reducing at least a portion of the aluminum ions at or near the at least one cathode 150 of the aluminum purification cell 1. In some embodiments, the generating step 320 includes migrating the aluminum ions through the electrolyte 110 toward the at least one cathode 150.

[0062] The refined aluminum 120 product above the electrolyte 110 defines a top layer. In some embodiments, the refined aluminum 120 product comprises an aluminum purity of at least 99.5% to up to 99.999% by weight. In some embodiments, the refined aluminum 120 product comprises an aluminum purity of at least 99.8% to up to 99.999% by weight. In some embodiments, the refined aluminum 120 product comprises an aluminum purity of at least 99.9% to up to 99.999% by weight. In some embodiments, the refined aluminum 120 product comprises an aluminum purity of at least 99.9% to up to 99.999% by weight. In some embodiments, the refined aluminum 120 product comprises an aluminum purity of at least 99.98% to up to 99.999% by weight.

[0063] In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 1-15 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 1-10 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 1-8 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 1-6 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 1-4 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 5-15 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product may be produced through the aluminum purification cell 1 with an energy efficiency of 10-15 kWh / kg of purified aluminum. In some embodiments, refined aluminum 120 product may be produced via aluminum purification cell 1 with an energy efficiency of 12-15 kWh / kg of refined aluminum.

[0064] As mentioned above, the method 300 further includes flowing 330 the refined aluminum 120 from the cell chamber 210 of the aluminum refining cell 1 to the refined metal reservoir 260 via the overflow passage 250. In other words, the overflow passage 250 extends from the cell chamber 210 to the refined metal reservoir 260 located inside the aluminum refining cell 1. The overflow passage 250 provides access to the refined metal reservoir 260 from the top of the cell chamber 210. When the refined aluminum 120 reaches the level of the overflow passage 250, the refined aluminum 120 flows from the top of the cell chamber 210 to the refined metal reservoir 260. The refined aluminum 120 can then be tapped from the refined metal reservoir 260 via the tapping port 200.

[0065] In some embodiments, the disclosure includes providing an inert gas 222 to the cell chamber 210 via an inert gas inlet 220 formed in a refractory top cover 40 of the cell chamber 210, thereby providing an inert atmosphere to the cell chamber 210. In some embodiments, the disclosure includes maintaining an inert atmosphere in the cell chamber 210 of the aluminum purification cell 1 while feeding aluminum feedstock 180 to a feed reservoir 270, producing purified aluminum 120, and removing the purified aluminum 120 from the aluminum purification cell 1 via a tapping port 200.

[0066] The refined aluminum 120 may be removed from the refined metals reservoir 260 via a tapping port 200 located in the fire-resistant top cover 40 of the cell chamber 210. In some embodiments, simultaneously with removing the refined aluminum 120, the method includes limiting, reducing, or preventing air oxidation of the refined aluminum 120 in the cell chamber 210 when removing the refined aluminum 120 from the refined metals reservoir 260. In some embodiments, removing the refined aluminum 120 from the refined metals reservoir 260 includes removing the refined aluminum 120 via a tapping port 200 located in the fire-resistant top cover 40 of the cell chamber 210.

[0067] In some embodiments, the disclosure includes removing at least a portion of a top layer of the refined aluminum 120 from the refined metal reservoir 260 via the tapping port 200. In some embodiments, the refined aluminum 120 may be removed continuously during operation of the aluminum purification cell 1. In some embodiments, the first removal rate may be controlled, for example, based at least in part on the second removal rate. In some embodiments, the refined aluminum 120 may be removed periodically during operation of the aluminum purification cell 1. In some embodiments, the removal step may be performed using equipment (e.g., alumina, graphite, and / or TiB) configured to remove the refined aluminum 120 product without contaminating the product. 2 This is completed using a tapping device.

[0068] The present disclosure achieves limiting, reducing, or preventing air oxidation of the refined aluminum 120 in the cell chamber 210 by preventing air from entering the cell chamber 210. The design of the aluminum purification cell 1 allows the cell chamber 210 to be sealed from air, preventing oxidation of the top metal of the refined aluminum 120 in the aluminum purification cell 1.

[0069] Although many embodiments of the present disclosure have been described, it is understood that these embodiments are illustrative and not limiting, and that many modifications may become apparent to one of ordinary skill in the art. The various steps may be performed in any desired order (and any desired steps may be added and / or any desired steps may be removed). For example, the features and characteristics of the aluminum refining cell 1 may be used with any other system and / or product, or alone. For example, in some embodiments, only one of the refined metal reservoir 260 and the feed reservoir 270 may be integrated with and within the aluminum refining cell 1. The features and characteristics of the aluminum refining cell 1 described in any of the embodiments may be used in any other embodiment described herein. The exemplary embodiments of the aluminum refining cell 1 are not meant to be exhaustive. The features and characteristics of the present disclosure may be combined in any manner.

Claims

1. 1. A method for refining aluminum, comprising: (a) producing refined aluminum from an aluminum feedstock in an aluminum refining cell, the refined aluminum having a density less than an electrolyte of the aluminum refining cell, the electrolyte having a density less than a molten metal pad of the aluminum refining cell; (b) flowing the refined aluminum from a cell chamber of the aluminum refining cell through an overflow passage to a refined metal reservoir, the refined metal reservoir being located within the aluminum refining cell.

2. Prior to the generating step (a), providing the aluminum feedstock to the aluminum refining cell; The aluminum source contains aluminum metal, The method of claim 1 , wherein the aluminum refining cell comprises the molten metal pad and the electrolyte.

3. The step of supplying the aluminum raw material comprises:

3. The method of claim 2 comprising flowing the aluminum source into the molten metal pad via a feed reservoir located within the aluminum refining cell.

4. The method according to any one of claims 1 to 3, wherein the aluminum source material comprises aluminum alloy scrap.

5. 5. The method of claim 4, wherein the aluminum alloy scrap comprises 1xxx series aluminum alloys, 2xxx series aluminum alloys, 3xxx series aluminum alloys, 4xxx series aluminum alloys, 5xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys, 8xxx series aluminum alloys, or any combination thereof.

6. The method of claim 4 , wherein the aluminum alloy scrap comprises new aluminum scrap and / or old aluminum scrap.

7. 7. The method of claim 1, wherein the aluminum refining cell further comprises a cell chamber defined at least in part by a refractory sidewall, a refractory top cover, and a cell bottom, the cell bottom being located proximate a base.

8. The method of any of claims 1 to 7, further comprising providing access to the refined metal reservoir through a feed port that passes through a refractory top cover of the cell chamber.

9. 9. The method of claim 1, further comprising providing an inert gas to the cell chamber via an inert gas inlet formed in a refractory top cover of the cell chamber, thereby providing an inert atmosphere in the cell chamber.

10. 10. The method of claim 9, further comprising: maintaining the inert atmosphere in the cell chamber of the aluminum refining cell while feeding the aluminum feedstock to a supply reservoir; producing the refined aluminum; and removing the refined aluminum from the aluminum refining cell via a tapping port.

11. The method of claim 10 , wherein a feed port of the feed reservoir and the tapping port of the refined metal reservoir at least partially define a hermetic seal of the cell chamber.

12. The method of any of claims 1 to 11, further comprising removing the refined aluminum from the refined metal reservoir through a tapping port located in a refractory top cover of the cell chamber.

13. 13. The method of claim 12 including limiting or preventing oxidation of the purified aluminum simultaneously with the removing step.

14. 14. The method of any of claims 1 to 13, wherein at least one anode overlaps at least one cathode, thereby defining an anode-cathode overlap, and a distal end of the at least one cathode is proximal to a middle portion of the at least one anode, and a distal end of the at least one anode is proximal to a middle portion of the at least one cathode.

15. The generating step (a) passing an electric current through the electrolyte to at least one anode and to at least one cathode; (i) the at least one anode and the at least one cathode are partially disposed within the electrolyte; The method of any preceding claim, wherein (ii) said at least one anode is partially disposed within said molten metal pad.

16. The generating step (a) 16. The method of any of claims 1 to 15, comprising generating aluminum ions from the at least one anode, transferring at least a portion of the aluminum ions into the electrolyte, and reducing the at least a portion of the aluminum ions at or near at least one cathode of the aluminum purification cell.

17. 1. An aluminum refining cell comprising: (a) a cell chamber including a cell bottom, a refractory sidewall, and a refractory top cover; (b) at least one anode extending upwardly from the bottom of the cell; (c) a cathode connector located proximate to the fire resistant top cover; and (d) at least one cathode extending downwardly from the cathode connector; (e) an overflow passage extending from the cell chamber to a refined metal reservoir located within the aluminum refining cell.

18. 20. The aluminum refining cell of claim 17, further comprising a tapping port and a feed port located within the refractory top cover of the cell chamber.

19. 20. The aluminum refining cell of claim 18, wherein the supply port and the tapping port at least partially define a hermetic seal for the cell chamber.

20. The aluminium refining cell of any of claims 1 to 19, further comprising a feed reservoir located within the aluminium refining cell.

21. 21. The aluminum refining cell of claim 20, wherein the supply reservoir directs aluminum feedstock directly to a molten metal pad in the cell chamber.

22. 22. The aluminum purification cell of claim 21, wherein the molten metal pad comprises at least 5 wt.% aluminum metal, or at least 10 wt.% aluminum metal, or at least 15 wt.% aluminum metal, or at least 20 wt.% aluminum metal, or at least 25 wt.% aluminum metal, or at least 30 wt.% aluminum metal, or at least 35 wt.% aluminum metal, or at least 40 wt.% aluminum metal, or at least 45 wt.% aluminum metal, at least 50 wt.% aluminum metal, at least 55 wt.% aluminum metal, at least 60 wt.% aluminum metal, at least 65 wt.% aluminum metal, at least 70 wt.% aluminum metal, at least 75 wt.% aluminum metal, at least 80 wt.% aluminum metal, at least 85 wt.% aluminum metal, at least 90 wt.% aluminum metal, or at least 95 wt.% aluminum metal.

23. 23. The aluminum refining cell of claim 21 or claim 22, wherein the molten metal pad comprises at least one alloy.

24. 24. The aluminum refining cell of claim 23, wherein the at least one alloy comprises one or more of Al, Si, Cu, Fe, Sb, Gd, Cd, Sn, Pb, or any combination thereof.

25. 25. The aluminum refining cell of any of claims 1 to 24, wherein the composition of wettable material on the at least one anode in the aluminum refining cell is the same as or substantially similar to the molten metal pad.

26. 26. The aluminum refining cell of claim 25, wherein said composition of said wettable material is a metal.

27. 27. The aluminum refining cell of claim 26, wherein the metal comprises aluminum, magnesium, or any combination thereof.

28. 27. The aluminum purification cell of claim 26, wherein the metal comprises at least 5 wt.% aluminum, or at least 10 wt.% aluminum, or at least 15 wt.% aluminum, or at least 20 wt.% aluminum, or at least 25 wt.% aluminum, or at least 30 wt.% aluminum, or at least 35 wt.% aluminum, or at least 40 wt.% aluminum, or at least 45 wt.% aluminum, at least 50 wt.% aluminum, at least 55 wt.% aluminum, at least 60 wt.% aluminum, at least 65 wt.% aluminum, at least 70 wt.% aluminum, at least 75 wt.% aluminum, at least 80 wt.% aluminum, at least 85 wt.% aluminum, at least 90 wt.% aluminum, or at least 95 wt.% aluminum.

29. 27. The aluminum refining cell of claim 26, wherein the metal is selected from the group consisting of an aluminum alloy, aluminum metal, and combinations thereof.

30. The aluminum refining cell comprises:

30. The aluminum refining cell of any of claims 1-29, further comprising an inert gas inlet formed in the refractory top cover, the inert gas inlet configured to provide an inert atmosphere to the cell chamber.

31. 31. The aluminum refining cell of any one of claims 1 to 30, wherein a distal end of the at least one anode and a distal end of the at least one cathode partially overlap.

32. 22. The aluminum refining cell of claim 21, wherein the aluminum source comprises aluminum metal.

33. 33. The aluminum refining cell of claim 21 or claim 32, wherein the aluminum source comprises at least one other metal other than aluminum metal.

34. 34. The aluminum refining cell of any one of claims 21, 32, or 33, wherein the aluminum source comprises a transition metal.

35. 35. The aluminum refining cell of any one of claims 21 or 32-34, wherein the aluminum source comprises at least 50 wt.% aluminum metal, at least 55 wt.% aluminum metal, at least 60 wt.% aluminum metal, at least 65 wt.% aluminum metal, at least 70 wt.% aluminum metal, at least 75 wt.% aluminum metal, at least 80 wt.% aluminum metal, at least 85 wt.% aluminum metal, at least 90 wt.% aluminum metal, or at least 95 wt.% aluminum metal.

36. The aluminium refining cell of any one of claims 21 or 32-35, wherein the aluminium feedstock comprises impurities.

37. 37. The aluminum refining cell of claim 36, wherein the impurities of the aluminum source comprise Cr, Cu, Fe, Mg, Mn, Ni, Si, Ti, Zn, or any combination thereof.

38. 38. The aluminium refining cell of any one of claims 21 or 32-37, wherein the aluminium feedstock contains, in addition to other impurities, up to 2 wt.% Mg.

39. The aluminum raw material contains 0.5% by weight to 50.0% by weight of impurities of the aluminum raw material, 5.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 10.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 15.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 20.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 25.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 30.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 35.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 40.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 45.0% by weight to 50.0% by weight of the aluminum raw material 39. The aluminum refining cell according to any one of claims 21 or 32 to 38, comprising: 0.5% by weight to 45.0% by weight of the aluminum feed; 0.5% by weight to 40.0% by weight of the aluminum feed; 0.5% by weight to 35.0% by weight of the aluminum feed; 0.5% by weight to 30.0% by weight of the aluminum feed; 0.5% by weight to 25.0% by weight of the aluminum feed; 0.5% by weight to 20.0% by weight of the aluminum feed; 0.5% by weight to 15.0% by weight of the aluminum feed; 0.5% by weight to 10.0% by weight of the aluminum feed; or 0.5% by weight to 5.0% by weight of the aluminum feed.

40. 40. The aluminum refining cell of any one of claims 21 or 32-39, wherein the aluminum feedstock comprises at least 5 wt.% copper, at least 10 wt.% copper, at least 15 wt.% copper, at least 20 wt.% copper, at least 25 wt.% copper, at least 30 wt.% copper, at least 35 wt.% copper, at least 40 wt.% copper, at least 45 wt.% copper, or at least 50 wt.% copper.

41. 41. The aluminium refining cell of any one of claims 21 or 32-40, wherein the aluminium source comprises aluminium alloy scrap.

42. 42. The aluminum refining cell of claim 41, wherein the aluminum alloy scrap comprises a 1xxx series aluminum alloy, a 2xxx series aluminum alloy, a 3xxx series aluminum alloy, a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, a 6xxx series aluminum alloy, a 7xxx series aluminum alloy, an 8xxx series aluminum alloy, or any combination thereof.

43. 42. The aluminum refining cell of claim 41, wherein the aluminum alloy scrap comprises new aluminum scrap and / or old aluminum scrap.

44. 44. The aluminum refining cell of any one of claims 21 to 43, wherein the molten metal pad comprises at least 5 wt.% copper, at least 10 wt.% copper, at least 15 wt.% copper, at least 20 wt.% copper, at least 25 wt.% copper, at least 30 wt.% copper, at least 35 wt.% copper, at least 40 wt.% copper, at least 45 wt.% copper, or at least 50 wt.% copper.

45. The method of any one of claims 1 to 16, wherein the aluminum source comprises aluminum metal.

46. The method of any of claims 1 to 16 or 45, wherein the aluminum source comprises at least one other metal than aluminum metal.

47. The method of any one of claims 1 to 16, 45, or 46, wherein the source of aluminum comprises a transition metal.

48. 48. The method of any of claims 1-16 or 45-47, wherein the aluminum source comprises at least 50% by weight aluminum metal, at least 55% by weight aluminum metal, at least 60% by weight aluminum metal, at least 65% by weight aluminum metal, at least 70% by weight aluminum metal, at least 75% by weight aluminum metal, at least 80% by weight aluminum metal, at least 85% by weight aluminum metal, at least 90% by weight aluminum metal, or at least 95% by weight aluminum metal.

49. The method according to any one of claims 1 to 16 or 45 to 48, wherein the aluminum source contains impurities.

50. 50. The method of claim 49, wherein the impurities of the aluminum source comprise Cr, Cu, Fe, Mg, Mn, Ni, Si, Ti, Zn, or any combination thereof.

51. 51. The method of any of claims 1 to 16 or 45 to 50, wherein the aluminium source contains, in addition to other impurities, up to 2 wt.% Mg.

52. The aluminum raw material contains 0.5% by weight to 50.0% by weight of impurities of the aluminum raw material, 5.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 10.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 15.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 20.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 25.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 30.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 35.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 40.0% by weight to 50.0% by weight of impurities of the aluminum raw material, 45.0% by weight to 50.0% by weight of the aluminum raw material. 0% by weight of impurities, 0.5% by weight to 45.0% by weight of the aluminum raw material, 0.5% by weight to 40.0% by weight of the aluminum raw material, 0.5% by weight to 35.0% by weight of the aluminum raw material, 0.5% by weight to 30.0% by weight of the aluminum raw material, 0.5% by weight to 25.0% by weight of the aluminum raw material, 0.5% by weight to 20.0% by weight of the aluminum raw material, 0.5% by weight to 15.0% by weight of the aluminum raw material, 0.5% by weight to 10.0% by weight of the aluminum raw material, or 0.5% by weight to 5.0% by weight of the aluminum raw material.

53. 53. The method of any of claims 1 to 16 or 45 to 52, wherein the aluminum source comprises at least 5 wt.% copper, at least 10 wt.% copper, at least 15 wt.% copper, at least 20 wt.% copper, at least 25 wt.% copper, at least 30 wt.% copper, at least 35 wt.% copper, at least 40 wt.% copper, at least 45 wt.% copper, or at least 50 wt.% copper.

54. 54. The method of any of claims 1-16 or 45-53, wherein the molten metal pad comprises at least 5% by weight copper, at least 10% by weight copper, at least 15% by weight copper, at least 20% by weight copper, at least 25% by weight copper, at least 30% by weight copper, at least 35% by weight copper, at least 40% by weight copper, at least 45% by weight copper, or at least 50% by weight copper.