Aluminum alloy for casting motor rotors of new energy vehicles and its manufacturing method

A tailored aluminum alloy composition with controlled elemental ratios and centrifugal casting enhances the strength and conductivity of motor rotor castings, addressing the demands of new energy vehicles.

JP2024543863AActive Publication Date: 2024-11-26SHANDONG BOYUAN PRECISION MASCH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024529730
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-19
Filing Date
2022-01-06
Publication Date
2024-11-26
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

Existing aluminum alloys for casting motor rotors in new energy vehicles fail to meet the rapidly evolving demands for high strength, elongation, and electrical conductivity while maintaining cost-effectiveness.

Method used

An aluminum alloy composition comprising specific weight percentages of titanium, boron, silicon, iron, copper, magnesium, zinc, and manganese, along with high-purity aluminum, is formulated and produced through centrifugal casting to enhance strength and conductivity.

Benefits of technology

The alloy achieves tensile strengths of 80-95 MPa, yield strengths of 60-80 MPa, and elongation rates of 45-55%, with electrical conductivity ranging from 30-33 MS/m, significantly surpassing conventional alloys in mechanical and electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543863000001
    Figure 2024543863000001
  • Figure 2024543863000002
    Figure 2024543863000002
  • Figure 2024543863000003
    Figure 2024543863000003
Patent Text Reader

Abstract

This application discloses an aluminum alloy for casting motor rotors of new energy automobiles and its manufacturing method, which belongs to the field of new energy automobile motor technology, and contains titanium 0.05wt%-0.06wt%, boron 0.04wt%-0.06wt%, silicon 0.15wt%-0.5wt%, iron 0.01wt%-0.08wt%, copper 0.5wt%-0.7wt%, magnesium 0.3wt%-0.5wt%, zinc 0.01wt%-0.2wt%, manganese 0.02wt%-0.12wt%, and aluminum. By adding new elements and adjusting the ratio of each element, the strength of the aluminum alloy for casting can be significantly improved and excellent electrical conductivity can be maintained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to an aluminum alloy for casting motor rotors of new energy automobiles and its manufacturing method, which belongs to the field of motor technology of new energy automobiles.

[0002] This application claims priority to a Chinese patent application filed with the China Patent Office on November 19, 2021, bearing application number 202111400150.8 and entitled "Aluminum alloy for casting motor rotors of new energy vehicles and manufacturing method thereof," the entire contents of which are incorporated herein by reference. [Background technology]

[0003] With the worsening of global energy problems and environmental pollution problems, the development of new energy vehicles has become the mainstream of modern automobile enterprises, and the motor rotors in new energy vehicles are generally cast with pure aluminum, because aluminum has good electrical and thermal conductivity, low density, and meets the requirements for weight reduction. New energy vehicles are developing rapidly, and the requirements for motor rotors are becoming increasingly higher, for example, aluminum alloys for casting are required to have high strength and high elongation, as well as good electrical conductivity. The repeated update speed of requirements for parameters such as strength is fast, and technological innovation is required every year or even every six months to meet the latest standards.

[0004] In the prior art, titanium boron is mainly added to increase the crystal nucleus and improve the strength of the alloy, and iron, copper, magnesium, zinc has the effect of solid solution strengthening. However, the aluminum alloy produced by adding aluminum titanium boron additives still cannot meet the current demand in terms of parameters such as strength and elongation, so that in order to reduce the cost of production and development as much as possible, the process adjustment is generally reduced as much as possible, but in the formulation adjustment, the strength is always improved, but the parameters such as elongation and electrical conductivity are sacrificed, and it is difficult to synchronously improve the performance of each point and keep them all within a good range. Summary of the Invention [Problem to be solved by the invention]

[0005] In order to solve the above problems, the present invention provides an aluminum alloy for casting motor rotors for new energy vehicles, which can significantly improve the strength of the casting aluminum alloy while maintaining excellent electrical conductivity by adding new elements and adjusting the ratio of each element, and a manufacturing method thereof. [Means for solving the problem]

[0006] According to one aspect of the present application, there is provided an aluminum alloy for casting motor rotors for new energy automobiles, comprising 0.05 wt% to 0.06 wt% titanium, 0.04 wt% to 0.06 wt% boron, 0.15 wt% to 0.5 wt% silicon, 0.01 wt% to 0.08 wt% iron, 0.5 wt% to 0.7 wt% copper, 0.3 wt% to 0.5 wt% magnesium, 0.01 wt% to 0.2 wt% zinc, 0.02 wt% to 0.12 wt% manganese, and also aluminum.

[0007] Optionally, the aluminum alloy has a tensile strength of 80 MPa to 95 MPa.

[0008] Optionally, the aluminum alloy has a tensile strength of 85 MPa to 95 MPa.

[0009] Optionally, the aluminum alloy has a yield strength of 60 MPa to 80 MPa.

[0010] Optionally, the aluminum alloy has an elongation of 45% to 55%.

[0011] Optionally, the electrical conductivity of the aluminum alloy is between 30 MS / m and 33 MS / m.

[0012] Available components are 0.05wt%~0.06wt% titanium, 0.04wt%~0.06wt% boron, 0.15wt%~0.5wt% silicon, 0.01wt%~0.08wt% iron, 0.5wt%~0.7wt% copper, 0.3wt%~0.5wt% magnesium, 0.01wt%~0.2wt% zinc, 0.02wt%~0.12wt% manganese, and aluminum.

[0013] Optionally, the aluminum is high purity aluminum, which is pure aluminum with a purity of more than 99.8%. 0.2% of inevitable impurities in high purity aluminum does not affect the technical effect of the present application.

[0014] According to another aspect of the present application, a method for producing a molten aluminum alloy includes the steps of: (1) melting an aluminum ingot, adding each elemental component, and uniformly stirring the mixture; and (2) preheating the rotor mold cavity and centrifugal casting to produce the aluminum alloy for casting motor rotors.

[0015] Alternatively, the temperature in step (1) is 700-760°C, and the preheating temperature in step (2) is 680-720°C. Effect of the Invention

[0016] The beneficial effects of the present application include, but are not limited to:

[0017] 1. In the aluminum alloy for motor rotor casting of the present application, titanium and boron can strengthen the crystal nucleus and refine the crystal grains, but the addition of excessive titanium and boron will increase the amount of second phases formed by the two, and there will be excessive dissolution concentration, which will significantly reduce the electrical conductivity; the present application limits the titanium content to 0.05wt%-0.06wt% and the boron content to between 0.04wt%-0.06wt%, significantly increasing the titanium content, so as to significantly improve the strength while still maintaining good electrical conductivity; the present application adds manganese element, limiting it to 0.02wt%-0.12wt%, and reduces the iron content, limiting it to 0.01wt%-0.08wt%, so that the strength can be improved by micro-alloying manganese, and at the same time changing the iron microphase, making the iron from the original needle-like form to agglomerated, neutralizing the harmful effect of iron, thereby simultaneously improving the elongation and electrical conductivity of the alloy.

[0018] 2. In the present aluminum alloy for casting motor rotors, the magnesium content is limited to 0.3 wt%-0.5 wt%, which significantly increases the magnesium element content, and the silicon content is limited to between 0.15 wt%-0.5 wt%, which increases the silicon content, improves the casting performance and corrosion resistance, and reduces the tendency of weld cracking. In addition, some of the magnesium plays the role of solid solution strengthening, and the other part of the magnesium can form new hetero-crystalline nuclei with the high silicon content to form Mg2Si phase, which is beneficial to crystal refinement, and further improves the tensile strength and yield strength.

[0019] 3. In the present aluminum alloy for casting motor rotors, the copper content is further limited to 0.5wt%~0.7wt%, which significantly increases the copper content and enhances the precipitation strengthening effect. The high copper and aluminum content can form more θ-CuAl2 precipitation strengthening phase, and the excess magnesium and excess copper can also form a part of the better strengthened S-CuMgAl2 precipitation strengthening phase, which improves the dispersion of each precipitation phase, removes the manganese-containing coarse brittle phase and grain boundary network brittle phase, reduces the aging effect, and thereby improves the strength of the alloy.

[0020] 4. According to the aluminum alloy for motor rotor casting of the present application, if the electrical conductivity requirement reaches 30 MS / m or more, the demand can be met. However, the tensile strength of the motor rotor aluminum alloy currently provided by manufacturers needs to reach at least 70 MPa or 80 MPa or more according to different product levels. The present application significantly improves the mechanical performance parameters such as strength of the motor rotor aluminum alloy while slightly reducing the electrical conductivity to meet the demand. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present application will be described in detail below with reference to examples, but the present application is not limited to these examples.

[0022] Unless otherwise stated, all raw materials in the examples of this application are purchased through commercial approaches, the manufacturing method adopts conventional centrifugal casting and smelting processes, and other undisclosed parameters, such as stirring speed, are all parameters used in the prior art. Example 1: Preparation of aluminum alloy 1#

[0023] The composition of aluminum alloy 1# is 0.05wt% titanium, 0.05wt% boron, 0.2wt% silicon, 0.05wt% iron, 0.6wt% copper, 0.4wt% magnesium, 0.1wt% zinc, 0.08wt% manganese, and high-purity aluminum, which is pure aluminum with a purity of greater than 99.8%.

[0024] The manufacturing method is as follows: (1) melt an aluminum ingot at 720°C, add each elemental component, and stir uniformly; (2) The rotor mold cavity was preheated to 700°C, and aluminum alloy 1# for motor rotor casting was produced using a conventional centrifugal casting process. Example 2: Preparation of aluminum alloy 2#

[0025] The composition of aluminum alloy 2# is 0.05wt% titanium, 0.04wt% boron, 0.15wt% silicon, 0.01wt% iron, 0.5wt% copper, 0.3wt% magnesium, 0.05wt% zinc, 0.02wt% manganese, and high-purity aluminum, which is pure aluminum with a purity of greater than 99.8%.

[0026] The manufacturing method is as follows: (1) melt an aluminum ingot at 700°C, add each elemental component, and stir uniformly; (2) The rotor mold cavity was preheated to 680°C, and aluminum alloy 2# for motor rotor casting was produced using a conventional centrifugal casting process. Example 3: Preparation of aluminum alloy 3#

[0027] The composition of aluminum alloy 3# is 0.06wt% titanium, 0.06wt% boron, 0.5wt% silicon, 0.08wt% iron, 0.7wt% copper, 0.5wt% magnesium, 0.2wt% zinc, 0.12wt% manganese, and high-purity aluminum, which is pure aluminum with a purity of greater than 99.8%.

[0028] The manufacturing method is as follows: (1) melt an aluminum ingot at 760°C, add each elemental component, and stir uniformly; (2) The rotor mold cavity was preheated to 720°C, and aluminum alloy 3# for motor rotor casting was produced using a conventional centrifugal casting process. Comparative Examples 1 to 6: Production of Aluminum Alloys 4# to 9#

[0029] The manufacturing methods for aluminum alloys 4# to 9# are all the same as for aluminum alloy 1#, and the differences in composition are shown in Table 1.

[0030] [Table 1]

[0031] Example 4 Performance characteristics of aluminum alloys 1#-9# For motor rotor aluminum alloys 1#~9#, the corresponding end surfaces were sampled, the size of the electrical conductivity sample conformed to the requirements of GB / T12966-2008, and electrical conductivity tests were performed. The size standard of the mechanical performance test sample conformed to ASTM E8, and tensile performance analysis was performed. The mechanical performance and electrical conductivity test results are shown in Table 2.

[0032] [Table 2]

[0033] The results show that the motor rotor aluminum alloys 1# to 3# manufactured by adopting the elemental components limited in this application have excellent tensile strength and yield strength, with the tensile strength reaching up to 95MPa and the yield strength reaching up to 80MPa, fully meeting the latest manufacturers' requirements for tensile strength of 70MPa or more. In addition, by adding a limited proportion of manganese element, the elongation is also significantly improved, and the electrical conductivity can still meet the demand for 30MS / m or more, and the electrical conductivity is excellent. In addition, by limiting the proportion of copper and magnesium elements, a small amount of electrical conductivity is sacrificed, and the tensile strength, yield strength and elongation are significantly improved, which meets the manufacturers' relatively high requirements for strength and ensures the excellent electrical conductivity of the aluminum alloy.

[0034] Aluminum alloy 4# is a compound in the prior art, and the difference between the types and proportions of elements in the present application is significant. The final results show that it has excellent electrical conductivity, but mechanical properties such as strength cannot meet the latest demand, and the tensile strength and yield strength are both low. The manganese content in Aluminum alloy 5# is lower than the range specified in the present application, and as a result, each performance is far lower than Aluminum alloy 1#. Specifically, this is because the amount of manganese is too small to eliminate the harmful effects of iron. The manganese content in Aluminum alloy 6# is higher than the range specified in the present application, and as a result, the elongation and electrical conductivity are relatively good, but the strength is insufficient. This is because the amount of manganese is relatively high, and a relatively large amount of coarse brittle phase (Mn,Fe)Al6 is generated, which affects the strength.

[0035] The iron content in Aluminum alloy 7# exceeds the range specified in the present application, and as a result, its electrical conductivity is relatively low, and its parameters such as strength do not meet the standards. The magnesium content in Aluminum alloy 8# is lower than the range specified in the present application, and as a result, its strength is insufficient and much lower than that of Aluminum alloy 1#. The copper content in Aluminum alloy 9# is lower than the range specified in the present application, and as a result, each of its parameters is lower than that of Aluminum alloy 1#. Analysis shows that this is because the copper content cannot produce a relatively large amount of precipitation strengthening phase.

[0036] The above description is merely an embodiment of the present application, and the scope of protection of the present application is not limited to these specific embodiments, but is determined by the claims of the present application. Those skilled in the art can make various modifications and changes to the present application. Any modifications, equivalent replacements, improvements, etc. made within the technical ideas and principles of the present application should be included in the scope of protection of the present application.

Claims

1. An aluminum alloy for casting motor rotors of new energy vehicles, containing 0.05wt%-0.06wt% titanium, 0.04wt%-0.06wt% boron, 0.15wt%-0.5wt% silicon, 0.01wt%-0.08wt% iron, 0.5wt%-0.7wt% copper, 0.3wt%-0.5wt% magnesium, 0.01wt%-0.2wt% zinc, 0.02wt%-0.12wt% manganese, and other aluminum.

2. 2. The aluminum alloy for casting motor rotors according to claim 1, wherein the aluminum alloy has a tensile strength of 80 MPa to 95 MPa.

3. 3. The aluminum alloy for casting motor rotors according to claim 2, wherein the aluminum alloy has a tensile strength of 85 MPa to 95 MPa.

4. 2. The aluminum alloy for casting motor rotors according to claim 1, wherein the aluminum alloy has a yield strength of 60 MPa to 80 MPa.

5. 2. The aluminum alloy for casting motor rotors according to claim 1, wherein the elongation of said aluminum alloy is 45% to 55%.

6. 2. The aluminum alloy for casting motor rotors according to claim 1, wherein the electrical conductivity of the aluminum alloy is 30 MS / m to 33 MS / m.

7. 2. The aluminum alloy for casting motor rotors according to claim 1, comprising: 0.05 wt% to 0.06 wt% titanium, 0.04 wt% to 0.06 wt% boron, 0.15 wt% to 0.5 wt% silicon, 0.01 wt% to 0.08 wt% iron, 0.5 wt% to 0.7 wt% copper, 0.3 wt% to 0.5 wt% magnesium, 0.01 wt% to 0.2 wt% zinc, 0.02 wt% to 0.12 wt% manganese, and aluminum in addition.

8. 8. The aluminum alloy for casting motor rotors according to claim 7, wherein the aluminum is high purity aluminum, the high purity aluminum being pure aluminum having a purity of greater than 99.8%.

9. Using each element component in claim 1, Step (1) of melting an aluminum ingot, adding each elemental component, and uniformly stirring the mixture; and (2) preheating the rotor mold cavity and centrifugal casting to produce the aluminum alloy for casting motor rotors.

10. The method according to claim 9, wherein the temperature in step (1) is 700 to 760°C, and the preheating temperature in step (2) is 680 to 720°C.

Citation Information

Patent Citations

  • Fabrication die for centrifugal casting of squirrel cage motor rotor

    CN201768890U

  • Baking hardenability al-mg-si alloy sheet excellent in press formability and its manufacture

    JP1993112840A

  • Method for manufacturing precast-forming billet of aluminum alloy for transport equipment

    JP2003136174A

  • Method for producing 6000 series aluminum alloy sheet having excellent paint bake hardenability and production method therefor