Lyocell material, filter for smoking article, smoking article, and method for producing same
Treating Lyocell multifilaments with hydrophobic oil agents enhances filter hardness and biodegradability, addressing the environmental and user experience issues of cellulose acetate and Lyocell filters.
Patent Information
- Application Number
- JP2024531019
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-28
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Cellulose acetate cigarette filters take a long time to biodegrade and are not environmentally friendly, while Lyocell filters are more degradable but suffer from reduced hardness due to high water absorption, leading to unfavorable user experience when saliva is introduced.
Treat Lyocell multifilaments with a hydrophobic oil agent comprising esterified products of fatty acids and aliphatic alcohols or sorbitan and fatty acids to reduce water absorption and maintain filter hardness.
The treated Lyocell filters exhibit improved hardness retention even when exposed to moisture, providing a comparable user experience to cellulose acetate filters and ensuring environmental sustainability.
Smart Images

Figure 2024543887000001 
Figure 2024543887000002 
Figure 2024543887000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0190180 filed December 28, 2021, and Korean Patent Application No. 10-2021-0190181 filed December 28, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a lyocell material, a filter and a smoking article containing the same, and methods for their manufacture. [Background technology]
[0003] To date, cellulose acetate fiber has been mainly used as a cigarette filter material. Cellulose acetate is known to be a biodegradable material, but smoking article filters made of cellulose acetate maintain their original shape for one to two years after being buried in soil, and it takes a considerable amount of time to completely biodegrade. Considering not only the amount of tobacco products that are collected and buried as garbage after use, but also the amount and toxicity of tobacco products that are thrown away and left in the living environment, it is necessary to further improve the biodegradability of smoking article filters. As a result, lyocell, which is more environmentally friendly, has been selected as a material to replace cellulose acetate in recent years.
[0004] In addition, the tow for smoking article filters may be treated with an oil. The moisture absorption rate of lyocell tow treated with a general oil is about 10%, which is measured using a moisture analyzer and a drying oven combined with a scale capable of measuring the moisture loss on drying, and is calculated by measuring the weight of a tow whose weight has been measured in advance, leaving it at about 105°C, and then measuring the weight when no further weight loss occurs, and comparing the weights. This is a higher level than the 5% of cellulose acetate tow. As a result, the hardness of a filter containing lyocell tow is lower than that of a filter containing cellulose acetate tow, and when a filter containing lyocell tow is used in actual use, the hardness is broken down by saliva more quickly. For example, when smoking (although this varies depending on the user or situation), the user holds a cigarette in their mouth, and in such a case, if saliva flows into the cigarette tip or filter, the hardness (hardness) that the filter for smoking articles originally has is weakened, and smokers perceive such a change as an undesirable quality. Therefore, tobacco manufacturers are trying to create products that do not disintegrate when exposed to saliva, or disintegrate only to a small extent, and that maintain the inherent shape of the filter formed during production.
[0005] Considering such points, there is a need for development of a filter material that can replace the conventional cellulose acetate material while providing excellent hardness, quality, and user satisfaction. Summary of the Invention [Problem to be solved by the invention]
[0006] One object of the present application is to provide a lyocell material that can replace commercially available cellulose acetate for use in smoking article filters.
[0007] Another object of the present application is to provide a Lyocell material for smoking article filters which is environmentally friendly in its manufacturing process and has excellent biodegradability when disposed of.
[0008] It is yet another object of the present application to provide a Lyocell material for smoking article filters that exhibits little change in hardness upon moisture penetration.
[0009] Yet another object of the present application is to provide a Lyocell filter for a smoking article.
[0010] It is yet another object of the present application to provide a smoking article (eg, a cigarette) that includes a lyocell filter.
[0011] Yet another object of the present application is to improve the processability involved in the manufacture of said lyocell materials, filters and smoking articles.
[0012] The above and other objects of the present application can be achieved by the present invention, which will be described in detail below. [Means for solving the problem]
[0013] According to an embodiment of the present application, a lyocell material, a filter including the same, and a smoking article may be provided.
[0014] Substituting lyocell tow for cellulose acetate tow, which has been used conventionally, is accompanied by the above-mentioned difficulties. That is, since the moisture absorption rate (or moisture content) of lyocell tow is generally higher than that of cellulose acetate tow, the hardness collapse phenomenon caused by saliva is exhibited earlier. In order to solve such problems, there have been attempts to treat the tow with a hydrophobic binder, but the method of treating lyocell, which has strong hydrophilicity, with a hydrophobic binder has limitations in improving the filter hardness due to compatibility problems. Moreover, the above-mentioned undesirable compatibility problems also have a negative impact on the manufacturing process of filters or smoking articles (e.g., cigarettes).
[0015] Taking such points into consideration, the inventors of the present application have completed the present invention, which treats a lyocell material with a specific oil agent, thereby overcoming the hydrophilicity of the lyocell surface, improving compatibility with the binder, and improving the degree of hardness reduction caused by saliva (e.g., providing a similar or equivalent level of hardness when compared to conventional cellulose acetate filters).
[0016] Specifically, according to one example of the present application, a lyocell material may be provided, which includes a crimped lyocell multifilament and an oil agent coated on the lyocell multifilament, the oil agent including (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol, and (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms.
[0017] According to another example related to the present application, a lyocell material can be provided that includes crimped lyocell multifilaments and an oil agent coated on the lyocell multifilaments, and has a sinking time in water of 6.0 seconds or more.
[0018] According to yet another specific example of the present application, there may be provided a filter for smoking articles comprising a lyocell material, the lyocell material comprising a crimped lyocell multifilament and an oil agent coated on the lyocell multifilament, the oil agent comprising (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol, and (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms.
[0019] According to yet another specific example of the present application, a filter for a smoking article can be provided that satisfies a filter diameter maintenance rate of 85% or more before water is injected, as calculated by the following formula 1-1, which expresses the degree of hardness change of the filter for a smoking article, and that satisfies a filter diameter maintenance rate of 80% or more after water is injected, as expressed by the following formula 1-2.
[0020] According to yet another embodiment of the present application, there may be provided a smoking article comprising the lyocell material or the filter.
[0021] According to still other embodiments of the present application, methods of producing the lyocell material, filters including the same, and smoking articles may be provided.
[0022] According to yet another embodiment of the present application, an oil can be provided that can modify the hydrophilicity of the surface of the lyocell material to hydrophobicity, thereby improving the degree of reduction in hardness of a smoking article filter caused by moisture.
[0023] In this specification, the term "smoking article" may refer to an article capable of generating an aerosol, such as a cigarette or a cigar. In this context, the smoking article may also include an aerosol-generating substance or an aerosol-forming substrate. The smoking article may also include a solid substance based on tobacco raw materials, such as flat tobacco, cut tobacco, or reconstituted tobacco. In addition, the smoking material may also include a volatile compound.
[0024] Unless otherwise specifically defined in this specification, when the properties of the lyocell material, the smoking article filter, and the components and structures related thereto are affected by temperature, the temperature at which the properties are confirmed or measured is also room temperature. In this case, the room temperature is a temperature in a state in which the temperature is not particularly reduced or increased, for example, a temperature between 10°C and 35°C, specifically, 15°C and 35°C, 20°C and 30°C, or about 25°C.
[0025] The present invention will be described in further detail below.
[0026] In one embodiment, the present application relates to a lyocell material that may be used in, but is not limited to, a filter for a smoking article.
[0027] Specifically, the lyocell material includes a lyocell multifilament to which a crimp has been applied, and an oil agent coated on the lyocell multifilament. The oil agent includes (a) an ester of a fatty acid having 16 or more carbon atoms with an aliphatic monohydric alcohol, and (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms. Such an oil agent can be applied to a part or the whole of the monofilament or multifilament constituting the lyocell material. The oil agent can also permeate between the filaments.
[0028] The oil agent containing at least the components (a) and (b) can have hydrophobicity. As a result, the oil agent can solve the problems of the hydrophilicity of the Lyocell surface, vulnerability to moisture, and the resulting decrease in hardness of the filter. In addition, the oil agent has excellent compatibility with the binder component described below.
[0029] In a specific example of the present application, the lyocell material may contain a predetermined amount of the oil. In this case, the amount of the oil may refer to the OPU (oil pick up ratio) (wt%) described later. For example, the lyocell material may contain an oil in an amount of 2.0 wt% or more based on 100 wt% of the total lyocell material. Specifically, the amount of the oil may be 2.5 wt% or more, 3.0 wt% or more, specifically 3.5 wt% or more, 4.0 wt% or more, 4.5 wt% or more, 5.0 wt% or more, 5.5 wt% or more, 6.0 wt% or more, 6.5 wt% or more, 7.0 wt% or more, 7.5 wt% or more, 8.0 wt% or more, 8.5 wt% or more, 9.0 wt% or more, or 9.5 wt% or more. The upper limit is, for example, 15.0 wt % or less, 14.5 wt % or less, 14.0 wt % or less, 13.5 wt % or less, 13.0 wt % or less, 12.5 wt % or less, 12.0 wt % or less, 11.5 wt % or less, 11.0 wt % or less, 10.5 wt % or less, 10 wt % or less, 9.5 wt % or less, 9.0 wt % or less, 8.5 wt % or less, 8.0 wt % or less, 7.5 wt % or less, 7.0 wt % or less, 6.5 wt % or less, 6.0 wt % or less, 5.5 wt % or less, 5.0 wt % or less, 4.5 wt % or less, 4.0 wt % or less, or 3.5 wt % or less.
[0030] The oil content (OPU) may be measured, for example, by an extrusion method. For example, a sample (e.g., 2 to 5 g, specifically, about 2.5 g) is collected (the weight of the collected sample is referred to as the sample weight) and placed in a syringe-shaped container. The material of the container is not particularly limited, but may be SUS (steel use stainless) material. Then, a solvent (e.g., methanol) is added to the container containing the sample (the amount of the solvent added may be 10 ml or less (e.g., about 8 ml)). When the solvent is added to the sample, a drop method is used, and the drop speed is uniformly controlled. Then, as described above, the solvent added to the container is allowed to drop from one end of the syringe-shaped container onto a plate. At this time, the weight of the plate is measured in advance (the measured weight is called plate weight A), and the plate is provided so that the solvent dropped onto the plume can jump out (i.e., be evaporated) at a temperature of 120°C to 130°C (e.g., 125°C). The above-mentioned solvent injection and solvent drop are carried out three times, and a pressure (e.g., 10 kgf / cm) is applied to the sample using a syringe-shaped container. 2 Below, 5kgf / cm 2 Less than or equal to 2-4kgf / cm 2 ) and press the sample once. Through this, the solvent and oil present in the sample are fully pushed out. Pressure is applied until no more solvent comes out and the sample is squeezed out. After that, the plate is stored in a desiccator for 5 to 10 minutes and the weight of the plate containing the sample is measured (plate weight B). Then, the oil content is calculated using the following formula.
[0031] [Formula] Extrusion oil content (OPU (% or wt%)) = {(Plate weight B - Plate weight A) / (Sample weight)} x 100
[0032] The lyocell material serving as the standard for the oil content is also a lyocell multifilament that has been at least oil-treated. For example, the lyocell material is a lyocell multifilament to which a first oil treatment (described below) has been applied, a lyocell multifilament to which a first oil treatment and a second oil treatment (described below) have been applied, or a lyocell multifilament to which a binder (described below) has been applied in addition to the above-mentioned oil treatment. As described above, the lyocell multifilament that has been treated with an oil and / or binder is also one to which crimping has been applied.
[0033] In the present application, the component (a) is a compound that can function as a kind of lubricant or oil, and is harmless to the human body so that it can be used in food. The component (a) provides lubricity to the fibers fed into the crimper. If the lubricity is insufficient, the lyocell will form clumps and will not be able to escape the crimper, and if the lubricity is too high, the crimp will not be formed well. The content of the component (a) can be controlled as described below, taking into account such functions.
[0034] The type of fatty acid having 16 or more carbon atoms forming the component (a) is not particularly limited. Fatty acids having 16 or more carbon atoms that can provide esterified products that are harmless to the human body and can be used in foods may be used.
[0035] For example, as the fatty acid having 16 or more carbon atoms, a saturated fatty acid and / or an unsaturated fatty acid can be used.
[0036] Examples of saturated fatty acids include palmitic acid (hexadecanoic acid (CH3(CH2) 14 COOH)), margaric acid (heptadecanoic acid (CH3(CH2) 15 COOH)), stearic acid (octadecanoic acid (CH3(CH2) 16 COOH)), nonadecylic acid (nonadecanoic acid (CH3(CH2) 17COOH)) or arachidic acid (eicosanoic acid (CH3(CH2) 18 However, the types of usable saturated fatty acids are not limited thereto.
[0037] Examples of unsaturated fatty acids include palmitoleic acid (CH3(CH2)5CH=CH(CH2)7COOH), oleic acid (CH3(CH2)7CH=CH(CH2)7COOH), linoleic acid (C 18 H 32 O2) or arachidonic acid (C 20 H 32 However, the types of saturated fatty acids that can be used are not limited to these.
[0038] The upper limit of the carbon number of the fatty acid having 16 or more carbon atoms is not particularly limited, and is, for example, 40 or less, 36 or less, 32 or less, 28 or less, 24 or less, or 20 or less.
[0039] The type of aliphatic monohydric alcohol forming the component (a) is not particularly limited. Any aliphatic monohydric alcohol capable of providing an esterification product that is harmless to the human body and can be used in foods may be used.
[0040] For example, they may be saturated or unsaturated fatty alcohols, and they may be linear or branched.
[0041] As one example, the carbon number of the aliphatic monohydric alcohol is 1 to 40. Specifically, the carbon number of the aliphatic monohydric alcohol is, for example, 4 or more, 8 or more, 12 or more, 16 or more, or 20 or more.
[0042] Examples of the aliphatic monohydric alcohol include, but are not limited to, methanol, ethanol, butanol, lauryl alcohol, isotridecanol, and stearyl alcohol.
[0043] In a specific example of the present application, the component (a) may be an ester of isotridecanol and stearic acid (e.g., isotridecyl stearate). However, the type of the component (a) that can be used is not limited thereto.
[0044] As described below, the content of the component (a) in the oil agent can be adjusted in consideration of the function of the oil agent or the function of the component (a).
[0045] The component (b), i.e., an ester of sorbitan with a fatty acid having 16 or more carbon atoms, is a compound that can function as a type of oil-forming agent, and is a component that is harmless to the human body and can be used in food.
[0046] Such component (b) has both hydrophilic and hydrophobic properties due to its alcohol (i.e., sorbitan), and therefore allows component (a), which provides lubricity to fibers, to disperse well in water, as described below. In addition, components (a) and (b) used together not only increase the dispersibility of the oil agent, as described above, but also lower the melting point, ensuring the ease of use and safety of the oil agent. The content of component (b) can be controlled in consideration of such functions, as described below.
[0047] The type of fatty acid having 16 or more carbon atoms forming the component (b) is not particularly limited. Fatty acids having 16 or more carbon atoms that can provide esterified products that are harmless to the human body and can be used in foods may be used.
[0048] For example, as the fatty acid having 16 or more carbon atoms, a saturated fatty acid and / or an unsaturated fatty acid can be used.
[0049] Examples of saturated fatty acids include palmitic acid (hexadecanoic acid (CH3(CH2) 14 COOH)), margaric acid (heptadecanoic acid (CH3(CH2) 15COOH)), stearic acid (octadecanoic acid (CH3(CH2) 16 COOH)), nonadecylic acid (nonadecanoic acid (CH3(CH2) 17 COOH)) or arachidic acid (eicosanoic acid (CH3(CH2) 18 However, the types of usable saturated fatty acids are not limited thereto.
[0050] Examples of unsaturated fatty acids include palmitoleic acid (CH3(CH2)5CH=CH(CH2)7COOH), oleic acid (CH3(CH2)7CH=CH(CH2)7COOH), and linoleic acid (C 18 H 32 O2) or arachidonic acid (C 20 H 32 However, the types of saturated fatty acids that can be used are not limited to these.
[0051] The upper limit of the carbon number of the fatty acid having 16 or more carbon atoms is not particularly limited, and is, for example, 40 or less, 36 or less, 32 or less, 28 or less, 24 or less, or 20 or less.
[0052] In a specific example of the present application, the component (b) may be an ester of sorbitan and oleic acid (e.g., sorbitan monooleate). However, the type of the component (b) that can be used is not limited thereto.
[0053] The content of component (b) can be adjusted taking into consideration the above-mentioned functions of component (b) and the functions of the oil.
[0054] In one example, the oil agent contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
[0055] Specifically, the oil agent of the present application may contain the (b) component in an amount of 25 parts by weight or more, 30 parts by weight or more, 35 parts by weight or more, 40 parts by weight or more, 45 parts by weight or more, or 50 parts by weight or more, relative to 100 parts by weight of the (a) component. The upper limit of the content of the (b) component relative to 100 parts by weight of the (a) component may be, for example, 55 parts by weight or less, 50 parts by weight or less, 45 parts by weight or less, 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less. When the content range is satisfied, the surface of the oil agent-treated lyocell multifilament or lyocell tow becomes hydrophobic, and as a result, the problem of excessive reduction in hardness of the filter due to penetration of moisture (e.g., saliva) can be solved.
[0056] In one example, the oil agent further contains an alkylene oxide adduct of the component (b) as the component (c). Such a component (c) can function as a kind of oiling agent. The compound can also be selected from those that are harmless to the human body and can be used in food.
[0057] The type of alkylene oxide in the component (c) is not particularly limited, but for example, the number of carbon atoms in the alkylene oxide is 2 to 4. Specifically, in the component (c), ethylene oxide, propylene oxide, and / or butylene oxide may be used, but is not limited thereto.
[0058] The number of moles of alkylene oxide added is not particularly limited, and may be, for example, 1 to 100, 5 to 80, 10 to 60, or 15 to 40.
[0059] In a specific example of the present application, the component (c) may be an ester of a polyethylene oxide (PEO) adduct of sorbitan and oleic acid (e.g., polyoxyethylene sorbitan monooleate). However, the type of component (c) that can be used is not limited thereto.
[0060] The component (c) improves processability by suppressing static electricity generation in lyocell staple during the manufacturing process of smoking article filters, thereby preventing thread breakage caused by static electricity generation. Specifically, the alkylene oxide-derived units adsorb moisture to the fiber surface, suppressing static electricity generation. The component (c) also plays a role in helping the oil to disperse effectively in water.
[0061] The content of component (c) can be adjusted taking into consideration the above-mentioned functions of component (c) and the functions of the oil agent.
[0062] In one example, the oil agent contains 10 to 50 parts by weight of the (c) alkylene oxide adduct of the ester (b) relative to 100 parts by weight of the (a) ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
[0063] Specifically, the oil agent of the present application contains 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 35 parts by weight or more, 40 parts by weight or more, or 45 parts by weight or more of the (c) component relative to 100 parts by weight of the (a) component. The upper limit of the content of the (c) component relative to 100 parts by weight of the (a) component is, for example, 45 parts by weight or less, 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, or 15 parts by weight or less.
[0064] In one example, the oil agent contains (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms in an excess amount relative to (c) an alkylene oxide adduct of the ester (b).
[0065] In one example, the oil contains 40 to 80% by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol, based on 100% by weight of the total oil. Specifically, based on 100% by weight of the total oil, the content of the component (a) is 45% by weight or more, 50% by weight or more, 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, or 75% by weight or more. The upper limit of the content is, for example, 75% by weight or less, 70% by weight or less, 65% by weight or less, 60% by weight or less, 55% by weight or less, 50% by weight or less, or 45% by weight or less.
[0066] In one example, the oil agent contains component (a) in the largest excess amount among components (a) to (c).
[0067] In one example, the oil agent contains 15 to 55 wt% of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, based on 100 wt% of the total weight of the oil agent. Specifically, based on 100 wt% of the total weight of the oil agent, the content of the (b) component is 20 wt% or more, 25 wt% or more, 30 wt% or more, 35 wt% or more, 40 wt% or more, 45 wt% or more, or 50 wt% or more. The upper limit of the content is, for example, 50 wt% or less, 45 wt% or less, 40 wt% or less, 35 wt% or less, 30 wt% or less, or 25 wt% or less.
[0068] In one example, the oil agent contains 10 to 30% by weight of component (c), i.e., an alkylene oxide adduct of (b), based on 100% by weight of the total weight of the oil agent. Specifically, based on 100% by weight of the total weight of the oil agent, the content of component (c) is 15% by weight or more, 20% by weight or more, or 25% by weight or more. The upper limit of the content is, for example, 25% by weight or less, 20% by weight or less, or 15% by weight or less.
[0069] In one example, the oil agent contains at least 15% by weight of (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms, and (c) an alkylene oxide adduct of (b), based on 100% by weight of the total weight of the oil agent. Specifically, based on 100% by weight of the total weight of the oil agent, the total content of the (b) component and the (c) component is 20% by weight or more, 25% by weight or more, 30% by weight or more, 35% by weight or more, 40% by weight or more, 45% by weight or more, or 50% by weight or more. The upper limit of the content is, for example, 55% by weight or less, 50% by weight or less, 45% by weight or less, 40% by weight or less, 35% by weight or less, 30% by weight or less, or 25% by weight or less.
[0070] In one embodiment, the oil agent further comprises (d) water. As described below, a small amount of water used helps the oiling.
[0071] The water content is not particularly limited, but may be the amount remaining after subtracting the total content of components (a) to (c) from the total 100% by weight of the oil. The water content in the oil (i.e., the amount remaining after subtracting the total content of the remaining components excluding water) is, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, or 1% by weight or less. The lower limit is, for example, 0% by weight or more, 0.1% by weight or more, 0.5% by weight or more, or 1% by weight or more.
[0072] The lyocell material of the present application is also a crimped tow having a fineness suitable for producing a filter for a smoking article and ensuring its function. For example, the total fineness of the tow is a factor related to the amount of filaments that can be inserted into the filter paper. If the total fineness is too low, a sufficient amount of filaments cannot be loaded into the filter paper, resulting in low draw resistance properties. If the total fineness is too high, the amount loaded into the filter paper will be too high, causing the filter paper to tear or making it difficult to adjust the tow loading amount to achieve the draw resistance required for the filter.
[0073] In one embodiment, the single filament fineness of the lyocell multifilament is 1.5 to 8.0 denier. In this case, the single filament fineness means the fineness of one monofilament separated from the multifilament.
[0074] Specifically, the filament single yarn fineness is, for example, 7.5 denier or less, 7.0 denier or less, 6.5 denier or less, 6.0 denier or less, 5.5 denier or less, 5.0 denier or less, 4.5 denier or less, 3.5 denier or less, or 3.0 denier or less. The lower limit is, for example, 2.0 denier or more, 2.5 denier or more, 3.0 denier or more, 3.5 denier or more, 4.0 denier or more, 4.5 denier or more, 5.0 denier or more, 5.5 denier or more, or 6.0 denier or more. Satisfying the above range is further advantageous for ensuring stable physical properties (e.g., hardness or drawing resistance) and processability of the smoking article filter.
[0075] In one embodiment, the crimped lyocell multifilament is also a crimped tow having a total fiber size of 15,000 to 45,000 denier. For example, the lower limit of the total fineness is, for example, 16,000 or more, 16,500 or more, 17,000 or more, 17,500 or more, 18,000 or more, 18,500 or more, 19,000 or more, 19,500 or more, 20,000 or more, 20,500 or more, 21,000 or more, 21,500 or more, 22,000 or more, 22,500 or more, 23,000 or more, 23,500 or more, 24,000 or more, 24,500 or more, 25,000 or more, 25,500 or more, 26,000 or more, 26,500 or more, 27,000 or more, 27,500 or more, 28,000 or more, 28,500 or more, 29,000 or more, 29,500 or more than 30,000, or more than 30,500, or more than 31,000, or more than 31,500, or more than 32,000, or more than 32,500, or more than 33,000, or more than 33,500, or more than 34,000, or more than 34,500, or more than 35,000, or more than 35,500, or more than 36,000, or more than 36,500, or more than 37,000, or more than 37,500, or more than 38,000 or more than 38,500, or more than 39,000, or more than 39,500, or more than 40,000 or more than 40,500, or more than 41,000, or more than 41,500, or more than 42,000, or more than 42,500, or more than 43,000, or more than 43,500, or more than 44,000.And the upper limit is, for example, 44,500 or less, 44,000 or less, 43,500 or less, 43,000 or less, 42,500 or less, 42,000 or less, 41,500 or less, 41,000 or less, 40,500 or less, 40,000 or less, 39,500 or less, 39,000 or less, 38,500 or less, 38,000 or less, 37,500 or less, 37,000 or less, 36,500 or less, 36,000 or less, 35,500 or less, 35,000 or less, 34,500 or less, 34,000 or less, 33,500 or less, 33,000 or less, 32,500 or less, 32,000 or less, 31,500 or less, 31,000 or less, 30,500 or less, 30,000 or less, 29,500 or less, 29,000 or less, 28,500 or less, 28,000 or less, 27,500 or less, 27,000 or less, 26,500 or less, 26,000 or less, 25,500 or less, 25,000 or less, 24,500 or less, 24,000 or less, 23,500 or less, 23,000 or less, 22,500 or less, 22,000 or less, 21,500 or less, 21,000 or less, 20,500 or less, 20,000 or less, 19,500 or less, 19,000 or less, 18,500 or less, 18,000 or less, 17,500 or less, 17,000 or less, 16,500 or less, 16,000 or less or 15,500 or less. If the total fineness of the tow is outside the above range, the processability of producing a filter for a smoking article is poor (continuous process is not possible due to thread breakage), and when producing a filter for a smoking article, the amount of tow inserted into the filter paper is excessively small or large, making it difficult to ensure sufficient filter properties (e.g., hardness, drawing resistance, etc.).
[0076] The method for measuring the fineness is not particularly limited, but for example, a 2 m sample of the tow to be measured is taken and left in a temperature-constant humidity room at a temperature of 20° C. and a humidity of 65% for 24 hours to keep it stable. One end of the stabilized tow is fixed, and a weight of 2 kg is attached to the other end. The tow in a state stretched by the load is kept for 5 seconds (stabilized), and then cut to 90 cm to obtain a sample, and the weight of the sample is measured (total fineness). The fineness is converted by multiplying the weight measured by the denier conversion method by 10,000. The total fineness is divided by the number of filaments to calculate the single yarn fineness.
[0077] The total fineness of the tow as described above can be determined by the single filament fineness and the number of crimps. In the method of the present application, since the single filament fineness and the number of crimps are controlled as described above, the total fineness of the tow as described above suitable for producing a smoking article filter and ensuring its function can be ensured.
[0078] In one example, the crimped lyocell multifilament may have 20 to 50 crimps per inch. For example, the number of crimps may be 25 ea / inch or more, 30 ea / inch or more, 35 ea / inch or more, 40 ea / inch or more, or 45 ea / inch or more, and the upper limit may be, for example, 45 ea / inch or less, 40 ea / inch or less, 35 ea / inch or less, 30 ea / inch or less, or 25 ea / inch or less. The number of crimps and their uniformity may be controlled through pressure and temperature conditions, etc., involved in the crimping step described below.
[0079] The number of crimps may be measured, for example, according to the KS K 0326 standard, without being particularly limited thereto. Specifically, 20 tow samples with undamaged crimps are taken, and each single fiber is attached to a piece of glossy paper (with a clearance of 25 mm) prepared in advance with 4 to 5% celluloid amyl acetate adhesive so that the attached length is extended by 25±5%, and then the adhesive is left to dry. Then, the sample is measured using a crimp tester, applying an initial load equivalent to 1.96 / 1,000cN (=2mgf) per De to each fiber, and the number of crimps in a 25mm interval is calculated. In this case, the number of crimps may be expressed by the upper and lower limits of the number of crimps measured for the 20 fibers. Alternatively, the number of crimps may be expressed by the arithmetic average value of the number of crimps measured for the 20 fibers.
[0080] Although not particularly limited, the lyocell material produced as described above can be used in filters for smoking articles.
[0081] In one embodiment, the lyocell material further includes a binder. The binder can be present, for example, on the surface of the crimped lyocell multifilament or between the crimped lyocell multifilaments (or monofilaments). The binder can further increase the hardness of the smoking article filter produced from the tow, and prevent problems such as filter tightness during the filter production process or smoking article (e.g., cigarette) production process.
[0082] The type of binder that can be used is not particularly limited, and any known binder may be used without impairing the object of the present invention. For example, a binder that provides sufficient compatibility with the oil used in the present application, can improve the hardness of the filter, and can provide excellent binding strength may be used.
[0083] In one example, the binder includes a polyester-based binder, a cellulosic binder, and / or a vinyl-based binder.
[0084] Although not particularly limited, the polyester-based binder may be a polyester binder containing at least one selected from the group consisting of alkylene, arylene, and heteroarylene having 5 to 12 carbon atoms.
[0085] Examples of the cellulose-based binder that may be used include, but are not limited to, hydroxypropylmethylcellulose (HPMC), ethylcellulose (EC) and / or methylcellulose (MC), carboxymethylcellulose (CMC), and the like.
[0086] Examples of the vinyl binder that may be used include, but are not limited to, polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA) and / or ethylene vinyl acetate (EVAc).
[0087] The method of applying (coating) the binder to the lyocell material will be described later.
[0088] In one example, the lyocell material is a lyocell material (crimped tow) having a settling time in water of 6.0 seconds or more, where the settling time means the time it takes for the lyocell material to fall to the bottom of a container (e.g., a beaker) filled with water after being poured therein (see the examples below for a specific measurement method).
[0089] In a specific example of the present application, the tow length (e.g., the length of the longest dimension of the tow shape) used in measuring the settling time may be, for example, 10 cm or less, 9 cm or less, 8 cm or less, 7 cm or less, 6 cm or less, or 5 cm or less, and the lower limit may be 1 cm or more, 2 cm or more, 3 cm or more, 4 cm or more, or 5 cm or more. In this case, the cutting size (length) may have an error of ±1 cm, ±0.5 cm, or ±0.1 cm.
[0090] In a specific example of the present application, the height of the water filled in the container for the settling time measurement is 12 to 13 cm, or about 12.5 cm, and the height may have an error within ±1 cm, ±0.5 cm, or ±0.1 cm.
[0091] The shorter the sinking time in water, the more hydrophilic the material is, and the longer the sinking time in water, the more hydrophobic the material is. As shown in the experiment described below, in the present application, a relatively long sinking time can be imparted to the lyocell material by using a predetermined amount of oil containing a predetermined component. In other words, the lyocell material of the present application can have a hydrophobic surface through the oil coating.
[0092] The settling time can be adjusted depending on the oil content (weight %) in the material; for example, the settling time can be 6.5 seconds or more, 7.0 seconds or more, 7.5 seconds or more, 8.0 seconds or more, 8.5 seconds or more, 9.0 seconds or more, 9.5 seconds or more, or 10 seconds or more, and can be 15 seconds or less, 14 seconds or less, 13 seconds or less, 12 seconds or less, 11 seconds or less, or 10 seconds or less.
[0093] Such settling time characteristics may also be expressed as settling velocity (cm / sec) in terms of the time and water height discussed below.
[0094] In another embodiment of the present application, the present application relates to a lyocell material having hydrophobic properties, for example, the lyocell material may exhibit a certain settling characteristic with respect to water.
[0095] Specifically, the lyocell material is a lyocell material (crimped tow) having a settling time in water of 6.0 seconds or more, where the settling time means the time it takes for the lyocell material to fall to the bottom of a container (e.g., a beaker) filled with water after being poured therein (see the examples below for a specific measurement method).
[0096] In a specific example of the present application, the tow length (e.g., the length of the longest dimension of the tow shape) used in measuring the settling time may be, for example, 10 cm or less, 9 cm or less, 8 cm or less, 7 cm or less, 6 cm or less, or 5 cm or less, and the lower limit may be 1 cm or more, 2 cm or more, 3 cm or more, 4 cm or more, or 5 cm or more. In this case, the cutting size (length) may have an error of ±1 cm, ±0.5 cm, or ±0.1 cm.
[0097] In a specific example of the present application, the height of the water filled in the container for the settling time measurement is 12 to 13 cm, or about 12.5 cm, and the height may have an error within ±1 cm, ±0.5 cm, or ±0.1 cm.
[0098] The shorter the sinking time in water, the more hydrophilic the material is, and the longer the sinking time in water, the more hydrophobic the material is. As shown in the experiment described below, in this application, a relatively long sinking time can be given to the lyocell material in order to apply the above-mentioned oil agent. That is, the lyocell material of this application can have a hydrophobic surface through the oil agent coating.
[0099] The settling time can be adjusted depending on the oil content (weight %) in the material; for example, the settling time can be 6.5 seconds or more, 7.0 seconds or more, 7.5 seconds or more, 8.0 seconds or more, 8.5 seconds or more, 9.0 seconds or more, 9.5 seconds or more, or 10 seconds or more, and can be 15 seconds or less, 14 seconds or less, 13 seconds or less, 12 seconds or less, 11 seconds or less, or 10 seconds or less.
[0100] In one embodiment, the sinking characteristics as described above can also be expressed as sinking velocity. For example, the Lyocell material of the present application has a sinking velocity in water of 2.1 cm / sec or less. A specific example of such a velocity can be calculated by the above-mentioned time and water height.
[0101] In one example, the lyocell material includes a lyocell multifilament having a crimp and an oil agent coated on the lyocell multifilament. The description of the lyocell filament, the oil agent, and the material including the same are the same as those described above, and therefore will not be repeated here.
[0102] Although not particularly limited, Lyocell materials exhibiting the above-mentioned settling properties can be used in filters for smoking articles.
[0103] In yet another embodiment of the present invention, the present application relates to a method for producing a lyocell material, by which the above-mentioned lyocell material for smoking article filters can be produced.
[0104] When the Lyocell material to which the hydrophobic oil is applied is manufactured into a smoking article filter, it can delay instantaneous moisture absorption. In addition, the oil of the present application is highly compatible with binders, so it can realize the physical properties (e.g., hardness or draw resistance) required for various smoking articles (e.g., cigarettes).
[0105] Specifically, the method for producing the lyocell material includes a step of treating a lyocell multifilament with an oil agent and a step of crimping the lyocell multifilament, and the oil agent includes at least (a) an ester of a fatty acid having 16 or more carbon atoms with an aliphatic monohydric alcohol, and (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms.
[0106] The oil treatment can be carried out, for example, by spraying the oil having the above-mentioned composition onto the lyocell filaments or by immersing the lyocell filaments in the oil. The method of the present application including the oil treatment can be carried out so that the oil content (e.g., OPU (wt%)) in the lyocell material satisfies a predetermined range described below.
[0107] The crimping step may also be performed by applying steam and / or pressure to the lyocell multifilament.
[0108] The explanation regarding the oil component is the same as that described above, so it will be omitted.
[0109] The method for producing a lyocell material according to an embodiment of the present application, including the steps of oil treatment and crimping, is described in more detail below. The method of the present application may be carried out by including one or more of the steps described below.
[0110] Lyocell doped radiation stage (a) The step is to irradiate a Lyocell radiation dope containing Lyocell cellulose (or cellulose pulp) and N-methylmorpholine-N-oxide (NMMO).
[0111] Commercially available cellulose acetate filters have been pointed out as a major source of microplastic emissions. However, the amine oxide solvents used in the production of lyocell fibers are recyclable and biodegradable when disposed of, meaning that lyocell materials do not generate any pollutants during their production process. Furthermore, lyocell tow is biodegraded and removed within a relatively short period of time, making lyocell a more environmentally friendly material than cellulose acetate.
[0112] In one embodiment, the content of cellulose in the radiation dope is 5 to 15 wt% based on the total weight of the dope being 100 wt%. If the content of cellulose is too low, it is difficult to realize the characteristics of Lyocell fiber, and if the content exceeds the range, it is difficult to dissolve in a solvent. In consideration of this, the content of cellulose in the radiation dope is 6 wt% or more, 7 wt% or more, 8 wt% or more, 9 wt% or more, or 10 wt% or more, and its upper limit is, for example, 14 wt% or less, 13 wt% or less, 12 wt% or less, 11 wt% or less, 10 wt% or less, or 9 wt% or less.
[0113] In one embodiment, the radiation dope includes an aqueous solution of N-methylmorpholine-N-oxide (NMMO). The aqueous solution may include, for example, 80 to 95 weight ratios of N-methylmorpholine-N-oxide and 5 to 20 weight ratios of water, taking into consideration the degree of solubility of cellulose and the process temperature.
[0114] In one embodiment, the cellulose or cellulose pulp has an α-cellulose content of 85 to 97% by weight relative to 100% by weight of the total cellulose.
[0115] In a specific embodiment of the present application, the degree of polymerization (DPw) of the cellulose is also 600 to 1,700.
[0116] In the emitting step, the shape of a nozzle for discharging the emitting dope is not particularly limited. For example, a donut-shaped nozzle may be used.
[0117] The nozzle temperature of the radiation nozzle, specifically, the radiation temperature, can be appropriately selected by those skilled in the art. Considering that the viscosity of the radiation dope varies depending on the radiation temperature and the discharge may not be good, the radiation temperature can be, for example, 100°C to 120°C or less, or 100°C to 110°C or less.
[0118] In one embodiment, the step of emitting the radiant dope may be performed under controlled radiant conditions so that the filament has a single fiber fineness of 1.5 to 8.0 denier. For example, the radiant conditions of at least one of the discharge amount and the radiant speed of the radiant dope may be appropriately controlled so that the filament has a single fiber fineness of 1.5 to 8.0 denier. In this case, the single fiber fineness of the filament means the fineness of one monofilament separated from a multifilament.
[0119] Specifically, the filament single yarn fineness is, for example, 7.5 denier or less, 7.0 denier or less, 6.5 denier or less, 6.0 denier or less, 5.5 denier or less, 5.0 denier or less, or 4.5 denier or less. The lower limit is, for example, 2.0 denier or more, 2.5 denier or more, 3.0 denier or more, 3.5 denier or more, 4.0 denier or more, 4.5 denier or more, 5.0 denier or more, 5.5 denier or more, or 6.0 denier or more. Satisfying the above range is further advantageous for realizing a stable drawing resistance of the smoking article filter and ensuring processability.
[0120] The radiation dope discharged through the radiation nozzle undergoes a solidification stage, which will be described later.
[0121] Step (b) of coagulation and obtaining a multifilament In this step, the irradiated lyocell dope is solidified to obtain the lyocell multifilament.
[0122] The solidification may be carried out in a manner in which the radiation-induced dope is in contact with air and / or a solidification liquid.
[0123] In one example, the solidification also includes a primary solidification stage in which cooling air is supplied to the irradiated lyocell dope, and a secondary solidification stage in which the primarily solidified irradiated dope is introduced into a coagulation liquid to be solidified.
[0124] According to the above-mentioned solidification method, the lyocell dope discharged from the nozzle can be primarily solidified in the space (air gap section) between the nozzle and the solidification tank. For example, cooling air can be supplied from the inside to the outside of the nozzle to the air gap section from an air cooling section located inside the nozzle. In addition, primary solidification can be performed by a method or means of so-called air quenching, which is well known in the related field.
[0125] In one example, the upper limit of the temperature of the cooling air used for the primary solidification is, for example, 15° C. or less. Specifically, the cooling air is air having a temperature of 14° C. or less, 13° C. or less, 12° C. or less, 11° C. or less, or 10° C. or less. If the temperature exceeds the above range, the radiation doped solidification by air is not sufficient, and the radiation-related processability is not good.
[0126] The lower limit of the cooling air can be determined in consideration of the radiation processability and / or the cross-sectional uniformity of the filament. For example, if the temperature of the cooling air is less than 4°C, the surface of the die becomes cold, the surface of the filament becomes uneven, and the radiation processability is also deteriorated. Taking this into consideration, the cooling air temperature can be 5°C or more, 6°C or more, 7°C or more, 8°C or more, or 9°C or more.
[0127] The amount of cooling air supplied may be adjusted in consideration of sufficient solidification, radiation processability, and effects on the physical properties of the filament. For example, 70 to 300 Nm 3 / h. More specifically, the air flow rate is 100 Nm 3 / h or more or 150Nm 3 / h or more, and the upper limit of the air volume is, for example, 250Nm 3 / h or less or 200Nm 3 / h or less.
[0128] The radiation dope cooled after the primary solidification as described above may be supplied to a coagulation tank or bath containing a coagulation liquid (secondary solidification). For proper coagulation progress, the temperature of the coagulation liquid may be, for example, 30° C. or less or 25° C. or less. The temperature of the coagulation liquid may be 10° C. or more, 15° C. or more, or 20° C. or more. When the above temperatures are maintained, the coagulation rate may be properly maintained.
[0129] The type of the coagulation liquid for the secondary coagulation as described above is not particularly limited. For example, the coagulation liquid may contain one or more of water and N-methylmorpholine-N-oxide (NMMO).
[0130] Although not particularly limited, when the coagulation liquid contains water and N-methylmorpholine-N-oxide (NMMO), the content of water in the coagulation liquid is 60 to 90% by weight, and the content of N-methylmorpholine-N-oxide (NMMO) is 10 to 40% by weight. Alternatively, the coagulation liquid may contain 70 to 80% by weight of water and 20 to 30% by weight of N-methylmorpholine-N-oxide (NMMO). The concentration of such a coagulation liquid may be controlled to be maintained during the manufacturing process using a sensor or the like.
[0131] Water washing stage (c) If necessary, after the coagulation step and the multifilament step, the multifilament may be washed with water to remove N-methylmorpholine-N-oxide (NMMO) and / or other impurities remaining in the filament.
[0132] The method of washing is not particularly limited. For example, washing may be performed by introducing the solidified lyocell multifilament into a washing tank using a pulling roller. Alternatively, washing may be performed by spraying a washing liquid during the process of moving to the next stage by the pulling roller.
[0133] The components of the washing liquid are not particularly limited. For example, the washing liquid may contain water and may further contain known additives.
[0134] In consideration of reuse after washing, the washing water may be adjusted to a temperature of 100° C. or less.
[0135] Oil treatment stage (d) This step is a step of applying the oil of the above-mentioned composition to the surface of the filament. The friction applied to the filament is reduced through the oil treatment, and the crimp can be well formed in the crimping step described below. As described below, when the oil treatment is performed twice or more, it can be called a first oil treatment and a second oil treatment depending on the order.
[0136] Although not particularly limited, the oil treatment may be performed by immersing the multifilament in a bath filled with the oil so that the multifilament is completely immersed in the oil, or may be performed by spraying the oil solution during the process of moving to the next stage by a pulling roller.
[0137] As described above, in order to ensure that the amount of oil applied to the multifilament after the oil treatment is constant, an additional process may be performed before and / or after the oil treatment step, in which a roll or the like is positioned to squeeze out the oil from the surface of the multifilament.
[0138] In one example, the oil treatment may be performed so that the oil content (OPU: oil pick up ratio) (wt%) is 2.0 wt% or more based on 100 wt% of the multifilament treated with at least an oil. In this case, the multifilament treated with at least an oil may be, for example, a lyocell multifilament to which a primary oil treatment is applied, a lyocell multifilament to which a primary oil treatment and a secondary oil treatment (see the following description) are applied, or a lyocell multifilament to which a binder is applied in addition to the above-mentioned oil treatment. As described above, the lyocell multifilament treated with an oil and / or binder may be crimped.
[0139] Specifically, in at least the multifilament treated with an oil agent, the content of the oil agent is 2.5 weight% or more, 3.0 weight% or more, 3.5 weight% or more, 4.0 weight% or more, 4.5 weight% or more, 5.0 weight% or more, 5.5 weight% or more, 6.0 weight% or more, 6.5 weight% or more, 7.0 weight% or more, 7.5 weight% or more, 8.0 weight% or more, 8.5 weight% or more, 9.0 weight% or more, or 9.5 weight% or more. The upper limit may be, for example, 15.0 wt% or less, 14.5 wt% or less, 14.0 wt% or less, 13.5 wt% or less, 13.0 wt% or less, 12.5 wt% or less, 12.0 wt% or less, 11.5 wt% or less, 11.0 wt% or less, 10.5 wt% or less, 10 wt% or less, 9.5 wt% or less, 9.0 wt% or less, 8.5 wt% or less, 8.0 wt% or less, 7.5 wt% or less, 7.0 wt% or less, 6.5 wt% or less, 6.0 wt% or less, 5.5 wt% or less, 5.0 wt% or less, 4.5 wt% or less, 4.0 wt% or less, or 3.5 wt% or less. In this case, the content may refer to the dry weight after the solvent (e.g., water) or liquid component contained in the oil agent has evaporated.
[0140] When the oil of the above composition is administered within the above content range, it can complement the hydrophilic properties of the Lyocell material and, as described below, can suppress excessive decrease in hardness of the Lyocell filter due to penetration of moisture or saliva.
[0141] Optionally, after the oil treatment as described above, the oil may be dried.
[0142] In an embodiment of the present application, one or more of the above steps may be controlled so that the single filament fineness of the filament constituting the lyocell multifilament is 1.5 to 8.0 denier. The single filament fineness means the fineness of one monofilament separated from the multifilament.
[0143] Specifically, the filament single yarn fineness is, for example, 7.5 denier or less, 7.0 denier or less, 6.5 denier or less, 6.0 denier or less, 5.5 denier or less, 5.0 denier or less, or 4.5 denier or less. The lower limit is, for example, 2.0 denier or more, 2.5 denier or more, 3.0 denier or more, 3.5 denier or more, 4.0 denier or more, 4.5 denier or more, 5.0 denier or more, 5.5 denier or more, or 6.0 denier or more. Satisfying the above range is further advantageous for realizing a stable drawing resistance of the smoking article filter and ensuring processability.
[0144] Although not particularly limited, the step controlled to ensure the above-mentioned range of single filament size may be the above-mentioned spinning step, or the above-mentioned spinning, coagulation, water washing and oil treatment steps may all be controlled to ensure the above-mentioned range of single filament size.
[0145] Crimping step (e) The crimping step is a step in which the oil-treated lyocell multifilament is subjected to pressure by steam and / or rollers to obtain a crimped tow, and may be referred to as a crimping step.
[0146] Through crimping, the multifilament can be given a wave and the fiber can have bulky properties. The crimping is performed using a known crimping device, such as a stuffer box and / or a steam box, and the crimping device that can be used is not particularly limited as long as it is a device that can apply steam pressure and roll pressure, which will be described later.
[0147] In one example, the crimping step may be performed by first supplying steam to the lyocell multifilament to preheat and swell the multifilament, and then pressing the multifilament with a press roller to form wrinkles in the multifilament. In this case, a steam box may be used to supply steam, and the steam box may be located at the front end of the crimping device.
[0148] In one example, the crimping step may be performed by simultaneously pressing the multifilaments with a press roller and applying steam.
[0149] In one example, the crimping step may be performed by first supplying steam to the lyocell multifilament to preheat and swell the multifilament, and then simultaneously pressing the multifilament with a press roller and applying steam.
[0150] In one embodiment, the crimping step applies a pressure of 0.1 to 2.0 kgf / cm to the multifilament before it is fed into a crimping device (specifically, a press roller). 2 In the embodiment of the present application, the steam is added at 0.2 kgf / cm 2 More than 0.3kgf / cm 2 Above 0.4kgf / cm 2 More than 0.5kgf / cm 2 or more than 0.6kgf / cm 2 More than 1.5 kgf / cm can be provided by the steam box. 2 Below, 1.4kgf / cm 2 Below, 1.3kgf / cm 2 Below, 1.2kgf / cm 2 Below, 1.1kgf / cm 2 Less than or equal to 1.0kgf / cm 2The following steam may be provided: If the steam supply amount or pressure is less than the above range, the crimp is not formed smoothly, and if it exceeds the above range, the filament becomes too flexible and is excessively crimped in the crimping device, so that it cannot pass through the crimping device.
[0151] In one embodiment, the crimping step uses a roller to apply a pressure of 1.5 to 4.0 kgf / cm to the multifilament fed into the crimping device. 2 In the embodiment of the present application, the pressure is 1.6 kgf / cm 2 More than 1.7kgf / cm 2 Above, 1.8kgf / cm 2 Above 1.9kgf / cm 2 Above 2.0kgf / cm 2 Above, 2.1kgf / cm 2 Above, 2.2kgf / cm 2 Above, 2.3kgf / cm 2 Above 2.4kgf / cm 2 or more than 2.5kgf / cm 2 The pressure of 3.9 kgf / cm or more can be applied to the multifilament through the press roller. 2 Below, 3.8kgf / cm 2 Below, 3.7kgf / cm 2 Below, 3.6kgf / cm 2 Below, 3.5kgf / cm 2 Below, 3.4kgf / cm 2 Below, 3.3kgf / cm 2 Below, 3.2kgf / cm 2 Below, 3.1kgf / cm 2 Below, 3.0kgf / cm 2 Below, 2.9kgf / cm 2 Below, 2.8kgf / cm 2 Below, 2.7kgf / cm 2 Below, 2.6kgf / cm 2 Less than or equal to 2.5kgf / cm 2The following pressures may be applied: If the roller pressure is below the above range, the desired number of crimps may not be sufficiently formed; if the roller pressure is above the above range, the pressing force may be too strong and the filament may not be smoothly fed into the crimping device or may not pass through the stuffer box. The press rollers providing the pressure may cause wrinkles in the multifilament.
[0152] In one example, the crimping step may be performed by applying a doctor blade that applies a predetermined pressure to the multifilament. The doctor blade adjusts the residence time of the filament fed into the crimper buffer box and contributes to the number of crimps (which affects the quality and filter performance of the tow). For example, such a doctor blade may be located in the path of travel of the multifilament that is discharged at the roller pressure point after being pressed by the roller.
[0153] In a specific example of the present application, the crimping step uses a doctor blade to apply a pressure of 0.1 to 2.0 kgf / cm to the multifilament that has passed through the rollers of the crimping device. 2 More specifically, the pressure applied by the doctor blade is 0.2 kgf / cm. 2 More than 0.3kgf / cm 2 Above 0.4kgf / cm 2 or more than 0.5kgf / cm 2 The upper limit of the pressure is, for example, 1.5 kgf / cm. 2 Below, 1.4kgf / cm 2 Below, 1.3kgf / cm 2 Below, 1.2kgf / cm 2 Below, 1.1kgf / cm 2 Less than or equal to 1.0kgf / cm 2 It is also the following.
[0154] In one example, the crimping step may be performed at a temperature in the range of 120 to 250° C. If the temperature is too low, the shape stabilization effect of the crimp may not be good, and if the temperature is too high, the concentration of the retaining agent may increase in the stuffer box, making it difficult to form the crimp. Therefore, taking into consideration the above-mentioned steam pressure, the temperature may be appropriately controlled in the range of 130° C. or more, 140° C. or more, or 150° C. or more, and 200° C. or less, 180° C. or less, or 160° C. or less.
[0155] Binder processing stage (f) In one example, the method further includes a step of coating the oil-treated lyocell multifilament or the lyocell multifilament obtained by the crimping step (i.e., crimped tow) with a binder.
[0156] When a filter for a smoking article is manufactured from tow, a binder is used to increase the hardness of the filter for a smoking article manufactured from the tow, and the binder can prevent problems such as the filter becoming too tight during the filter manufacturing process or the cigarette manufacturing process.
[0157] The method of coating the Lyocell crimped tow with the binder is not particularly limited. For example, the crimped tow may be oiled by immersing the crimped tow in a bath filled with the binder (or binder solution) so that the multifilament is completely immersed in the binder. Alternatively, the binder may be coated by injecting (or spraying) the binder (or binder solution) from a nozzle.
[0158] The types and components of the binders that can be used are as described above, and so a detailed description thereof is omitted here.
[0159] In one example, the binder (or binder solution) may further include a solvent in addition to the above-mentioned components. The solvent may include, but is not limited to, water, ethanol, propylene glycol, and / or glycerin. When the binder (or binder solution) includes a solvent, the content of the solvent may be, for example, about 20 to 80 wt % or 40 to 60 wt % based on 100 wt % of the total binder (or binder solution).
[0160] The binder treatment may be performed at a level that can achieve the above-mentioned purpose of the binder treatment. For example, the binder treatment may be performed so that the binder content is 20% by weight or less, for example, 8 to 15% by weight, based on 100% by weight of the multifilament treated with oil and binder. Here, the content may refer to the dry weight after evaporation of the solvent or liquid component contained in the binder.
[0161] After the binder is coated on the crimp tow, the binder may be dried. The drying temperature is not particularly limited, but may be, for example, room temperature (about 10° C. to 35° C.).
[0162] Other stages (g) After crimping, any appropriate post-processing may additionally be performed.
[0163] In one embodiment, a secondary oil treatment (g1) may be additionally performed. The secondary oil treatment may prevent static electricity from being generated in the tow and may impart flexibility to the tow. The secondary oil treatment may be the same as or similar to the above-mentioned (d) oil treatment step.
[0164] Specifically, the secondary oil treatment can be carried out by treating the lyocell tow with an oil after the crimping process. This can be advantageous in various processes carried out during the manufacture of a filter for a smoking article. For example, the secondary oil treatment not only allows the fibers and the filter to spread well in the air during the spreading process, but also allows the chains of the oil to hold the lyocell down during the stretching process, preventing the fibers from being cut. In order to achieve such advantages, it is necessary to use a component derived from a fatty acid having a certain number of carbon atoms or more, as described above.
[0165] The secondary oil treatment as described above can be performed before or after the binder treatment, or the secondary oil treatment can be performed with or without the binder treatment.
[0166] Even when the secondary oil treatment as described above is carried out, the secondary oil treatment step can be carried out so that the oil content or OPU content in the material satisfies the range as described above.
[0167] In one example, a drying process (g2) may be additionally performed. The drying may be performed, for example, at a temperature ranging from 100° C. to 130° C. The manner or method of the drying process is not particularly limited, and known techniques may be used. For example, the drying process may be performed by applying hot air to the tow, passing the tow in a temperature-controlled room for a certain period of time, or leaving the tow in the room.
[0168] According to an embodiment of the present application, a tow having 20 to 50 crimps per inch may be provided by a method including the crimping step as described above. For example, the number of crimps may be 25 ea / inch or more, 30 ea / inch or more, 35 ea / inch or more, 40 ea / inch or more, or 45 ea / inch or more, and the upper limit may be, for example, 45 ea / inch or less, 40 ea / inch or less, 35 ea / inch or less, 30 ea / inch or less, or 25 ea / inch or less. The number of crimps and their uniformity may be controlled via pressure and temperature conditions involved in the crimping step.
[0169] The manufacturing method of the present application can provide a tow having a fineness suitable for manufacturing a filter for a smoking article and ensuring its function. The total fineness of the tow is a factor related to the amount of filaments that can be inserted into the filter paper. If the total fineness is too low, a sufficient amount of filaments cannot be loaded into the filter paper, resulting in low draw resistance properties. If the total fineness is too high, the amount loaded into the filter paper is too high, causing the filter paper to tear or making it difficult to adjust the tow loading amount to achieve the draw resistance required for the filter. In relation to this, according to a specific example of the present application, a crimped tow having a total fineness of 15,000 to 45,000 denier can be provided. For example, the lower limit of the total fineness is, for example, 16,000 or more, 17,000 or more, 18,000 or more, 19,000 or more, or 20,000 or more, and the upper limit is, for example, 40,000 or less, 35,000 or less, 30,000 or less, or 25,000 or less. More specific values are as described above. If the total fineness of the tow is outside the above range, the processability of producing a filter for a smoking article is not good (continuous process is not possible due to thread breakage), and when producing a filter for a smoking article, the amount of tow inserted into the filter paper is too small or too large, making it difficult to ensure sufficient filter properties (e.g., drawing resistance).
[0170] The total fineness of the tow as described above can be determined by the filament single-yarn fineness and the number of crimps. In the method of the present application, since the single-yarn fineness and the number of crimps are controlled as described above, the total fineness of the tow as described above suitable for producing a smoking article filter and ensuring its function can be ensured.
[0171] Although not particularly limited, the lyocell material produced by the above method can be used in filters for smoking articles.
[0172] In yet another embodiment of the present application, the present application relates to a filter for a smoking article, said filter for a smoking article comprising a lyocell material, said lyocell material also being the same as previously described.
[0173] Specifically, the smoking article filter of the present application is a smoking article filter containing a lyocell material, the lyocell material including a crimped lyocell multifilament and an oil agent coated on the lyocell multifilament, and the oil agent includes at least (a) an ester of a fatty acid having 16 or more carbon atoms with an aliphatic monohydric alcohol, and (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms.
[0174] In addition, the lyocell material contains the oil in an amount of 2.0% by weight or more based on 100% by weight of the total lyocell material. Other than that, the oil components and their contents according to the specific examples of the present application are the same as those described above.
[0175] In one embodiment, the filament fineness of the single filament constituting the lyocell multifilament is 1.5 to 8.0 denier, the specific values being the same as those mentioned above.
[0176] In one embodiment, the crimped lyocell multifilament is also a crimped tow having a total fineness of 15,000 to 45,000 denier, the specific values being the same as those mentioned above.
[0177] In one embodiment, the crimped lyocell multifilament may have 20 to 50 crimps per inch, the specific values being the same as those described above.
[0178] In one embodiment, the smoking article filter further includes a binder on the surface of the crimped lyocell multifilament or between the crimped lyocell multifilament. The binder increases the hardness of the smoking article filter made of the tow and prevents problems such as the filter becoming too tight during the filter manufacturing process or the cigarette manufacturing process. The types, components, and amounts of the binder that can be used are the same as those described above.
[0179] In one example, the smoking article filter further includes a wrapping paper (which may be called wrapping paper, filter paper, or filter wrapping paper). For example, the wrapping paper may be a porous or non-porous paper that covers and encases the lyocell tow (i.e., tow that has been at least oil-treated and crimped) and can maintain the filter shape (e.g., a cylinder or a cylindrical shape).
[0180] In one example, when a porous wrapper paper is used, the wrapper paper may have a porosity of 10 to 50,000 CU (coresta unit). Specifically, the lower limit of the porosity of the wrapper paper is, for example, 1,000 CU or more, 5,000 CU or more, 10,000 CU or more, 15,000 CU or more, 20,000 CU or more, 25,000 CU or more, 30,000 CU or more, 35,000 CU or more, 40,000 CU or more, or 45,000 CU or more, and the upper limit is, for example, 45,000 CU or less, 40,000 CU or less, 35,000 CU or less, 30,000 CU or less, 25,000 CU or less, or 20,000 CU or less. In an embodiment of the present application, the wrapper may have a porosity in the range of 22,000 to 26,000 CU, or 23,000 to 25,000 CU.
[0181] In one example, the basis weight of the wrapper is 15 to 60 g / cm 2 Specifically, the lower limit of the basis weight of the wrapper paper is, for example, 20 g / cm 2 More than 25g / cm 2 More than 30g / cm 2 Above, 35g / cm 2 More than 40g / cm 2 More than 45g / cm 2 More than 50g / cm 2 or more than 55g / cm 2 The upper limit is, for example, 55 g / cm 2 Below, 50g / cm 2 Below, 45g / cm 2 Below 40g / cm 2 Below 35g / cm 2 Below 30g / cm 2 Below, 25g / cm 2 Less than or equal to 20g / cm 2 In a specific example of the present application, the wrapping paper has a density of 16 g / cm 2 More than 17g / cm 2 More than 18g / cm 2 More than 19g / cm 2 More than 20g / cm 2 or more than 21g / cm 2 Above, and 25g / cm 2 Below, 24g / cm 2 Below, 23g / cm 2 Below, 22g / cm 2 or less than 21g / cm 2 It may have the following basis weights:
[0182] In an embodiment of the present application, the smoking article filter may have a predetermined shape and size.
[0183] For example, the filter may have a rod shape. More specifically, the smoking article filter may have a cylinder-like shape.
[0184] The filter may have a length of, for example, 10 to 50 mm. Specifically, the length of the filter may have a lower limit of 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, 35 mm or more, 40 mm or more, or 45 mm or more, and an upper limit of 45 mm or less, 40 mm or less, 35 mm or less, 30 mm or less, 25 mm or less, 20 mm or less, or 15 mm or less.
[0185] In a specific example of the present application, the filter having said length has a circular cross section and a circumference of said circular cross section of 10 to 40 mm. For example, the circumference of said filter has a lower limit of 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, or 35 mm or more, and an upper limit of 35 mm or less, 30 mm or less, 25 mm or less, 20 mm or less, or 15 mm or less.
[0186] In one example, the filter for smoking articles may satisfy a filter diameter maintenance rate (or hardness maintenance rate) of 85% or more before water is injected, calculated by the following formula 1-1.
[0187] [Formula 1-1] Filter diameter (or filter hardness) retention rate (%) before water injection = {(initial filter diameter (mm) - length of filter pushed when a weight of a specific weight (300g) is used (mm)) / (initial filter diameter (mm))} x 100
[0188] Although not particularly limited, in relation to Equation 1-1, the initial filter diameter or the length to which the filter is pressed can be determined via cross sections of both ends of the filter to a predetermined length.
[0189] For example, the filter diameter (or filter hardness) retention rate before water injection calculated by the above-mentioned formula 1-1 is 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, or 95% or more. If the filter diameter (or filter hardness) retention rate (%) before water injection calculated by the above-mentioned formula 1-1 is below the above-mentioned range, it means that the hardness of the filter is insufficient.
[0190] In one example, the filter for smoking articles may satisfy a filter diameter maintenance rate (or hardness maintenance rate) of 80% or more after water is injected, which is expressed by the following formula 1-2.
[0191] [Formula 1-2] Filter diameter (or filter hardness) retention rate (%) after water injection = {(Initial filter diameter (mm) - length of filter pushed (mm) when the filter is pushed with a weight of a specific weight (300g) after water is injected) / (Initial filter diameter (mm))} x 100
[0192] Although not particularly limited, the initial filter diameter or the length to which the filter is pressed may be determined through cross sections of both ends of the filter in relation to Equation 1-2.
[0193] In relation to the above formula 1-2, the type of water to be injected is not particularly limited. For example, the water may be distilled water or tap water.
[0194] In a specific example of the present application, the amount of water injected according to Formula 1-2 is 20 μl. In this case, the amount of water injected may have an error of ±5 μl, ±4 μl, ±3 μl, ±1 μl, ±0.5 μl, or ±0.1 μl.
[0195] In a specific example of the present application, the diameter maintenance ratio in the above formula 1-2 is measured 5 minutes after water is poured into the filter, and the time at which the diameter maintenance ratio is measured may have an error of ±3 minutes, ±2 minutes, ±1 minute, or ±30 seconds.
[0196] Furthermore, water may be injected into the filter by dividing the water into equal portions along the filter's length (the direction of the longest dimension of the filter's shape, or the direction of the axis of symmetry if the filter is symmetrical). For example, when 20 μl of water is injected, the filter may be divided into thirds along the filter's length (the direction of the longest dimension of the filter's shape), and 6 to 7 μl of water may be injected into any point (e.g., the center) or region of each of the thirds.
[0197] For example, the filter diameter (or filter hardness) retention rate after water injection calculated by the above formula 1-2 is 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, or even 92% or more. If the filter diameter (or filter hardness) retention rate after water injection calculated by the above formula 1-2 is less than the above range, it means that the filter hardness change due to water penetration is large. As shown in the experiment described below, the filter for smoking articles of the present application suppresses hardness change even after water injection because of the application of the oil agent as described above, and therefore can show a high level of diameter (or filter hardness) retention rate.
[0198] In one example, the filter for smoking articles has a moisture disintegration rate of 8.0% or less, calculated by the following Equation 2:
[0199] [Formula 2] Moisture disintegration rate (%) = {(Filter diameter maintenance rate before water injection - Filter diameter maintenance rate after water injection) / (Filter diameter maintenance rate before water injection)} x 100
[0200] In Equation 2, the filter diameter maintenance rate before water injection can be calculated by Equation 1-1, and the filter diameter maintenance rate after water injection can be calculated by Equation 1-2.
[0201] For example, the moisture disintegration degree calculated by the above Equation 2 is 7.5% or less or 7.0% or less, specifically, 6.5% or less, 6.0% or less, 5.5% or less, 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, or 2.0% or less. If the moisture disintegration degree is satisfied, it means that even if a certain amount of moisture penetrates into the filter, the degree of collapse of the filter due to hardness change is not large. As shown in the experiment described below, the filter for smoking article of the present application can show a low moisture disintegration degree because of the application of the oil agent as described above.
[0202] Although not particularly limited, the diameter change (hardness change) and water disintegration degree according to the above-mentioned formula 1-1, formula 1-2, and formula 2 are measured for a rod-shaped filter weighing 50 mg or more. Specifically, the weight of the filter may have a lower limit of 100 mg or more, 150 mg or more, or 200 mg or more, and an upper limit of 500 mg or less, 450 mg or less, 400 mg or less, 350 mg or less, 300 mg or less, 250 mg or less, or 200 mg or less.
[0203] In yet another example of the present application, the present application relates to a filter for smoking articles that exhibits a characteristic that the hardness does not decrease significantly even when moisture penetrates, that is, that can effectively prevent the hardness of the filter from decreasing due to the smoker's saliva, etc. The above-mentioned characteristics can be calculated by the following Equations 1-1, 1-2, and 2.
[0204] In a specific example of the present application, the filter for smoking articles can satisfy a filter diameter maintenance rate (or hardness maintenance rate) before water injection, calculated by the following formula 1-1, of 85% or more.
[0205] [Formula 1-1] Filter diameter (or filter hardness) retention rate (%) before water injection = {(initial filter diameter (mm) - length of filter pushed when a weight of a specific weight (300g) is used (mm)) / (initial filter diameter (mm))} x 100
[0206] Although not particularly limited, in relation to Equation 1-1, the initial filter diameter or the length to which the filter is pressed can be confirmed via cross sections of both ends of the filter to a predetermined length.
[0207] For example, the filter diameter (or filter hardness) retention rate before water injection calculated by the above-mentioned formula 1-1 is 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, or 95% or more. If the filter diameter (or filter hardness) retention rate (%) before water injection calculated by the above-mentioned formula 1-1 is below the above-mentioned range, it means that the hardness of the filter is insufficient.
[0208] In a specific example of the present application, the filter for smoking articles may satisfy a filter diameter maintenance rate (or hardness maintenance rate) after water is injected, which is expressed by the following formula 1-2, of 80% or more.
[0209] [Formula 1-2] Filter diameter (or filter hardness) retention rate (%) after water injection = {(Initial filter diameter (mm) - length of filter pushed (mm) when the filter is pushed with a weight of a specific weight (300g) after water is injected) / (Initial filter diameter (mm))} x 100
[0210] Although not particularly limited, the initial filter diameter or the length to which the filter is pressed may be determined through cross sections of both ends of the filter in relation to Equation 1-2.
[0211] In relation to the above formula 1-2, the type of water to be injected is not particularly limited. For example, the water may be distilled water or tap water.
[0212] In a specific example of the present application, the amount of water injected according to Formula 1-2 is 20 μl. In this case, the amount of water injected may have an error of ±5 μl, ±4 μl, ±3 μl, ±1 μl, ±0.5 μl, or ±0.1 μl.
[0213] In a specific example of the present application, the diameter maintenance ratio in the above formula 1-2 is measured 5 minutes after water is poured into the filter, and the time at which the diameter maintenance ratio is measured may have an error of ±3 minutes, ±2 minutes, ±1 minute, or ±30 seconds.
[0214] Furthermore, water may be injected into the filter by dividing the water into equal portions along the filter's length (the direction of the longest dimension of the filter's shape, or the direction of the axis of symmetry if the filter is symmetrical). For example, when 20 μl of water is injected, the filter may be divided into thirds along the filter's length (the direction of the longest dimension of the filter's shape), and 6 to 7 μl of water may be injected into any point (e.g., the center) or region of each of the thirds.
[0215] For example, the filter diameter (or filter hardness) retention rate after water injection calculated by the above formula 1-2 is 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, 90% or more, 91% or more, or even 92% or more. If the filter diameter (or filter hardness) retention rate after water injection calculated by the above formula 1-2 is less than the above range, it means that the filter hardness change due to water penetration is large. As shown in the experiment described below, the filter for smoking articles of the present application suppresses hardness change even after water injection because of the application of the oil agent as described above, and therefore can show a high level of diameter (or filter hardness) retention rate.
[0216] In one example, the filter for smoking articles has a moisture disintegration rate calculated by Equation 2 of 8.0% or less.
[0217] [Formula 2] Moisture disintegration rate (%) = {(Filter diameter maintenance rate before water injection - Filter diameter maintenance rate after water injection) / (Filter diameter maintenance rate before water injection)} x 100
[0218] In Equation 2, the filter diameter maintenance rate before water injection can be calculated by Equation 1-1, and the filter diameter maintenance rate after water injection can be calculated by Equation 1-2.
[0219] For example, the moisture disintegration degree calculated by the above Equation 2 is 7.5% or less or 7.0% or less, specifically, 6.5% or less, 6.0% or less, 5.5% or less, 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, or 2.0% or less. If the moisture disintegration degree is satisfied, it means that even if a certain amount of moisture penetrates into the filter, the degree of collapse of the filter due to hardness change is not large. As shown in the experiment described below, the filter for smoking article of the present application can show a low moisture disintegration degree because of the application of the oil agent as described above.
[0220] In one example, a filter for a smoking article for which measurements related to the above Equations 1-1, 1-2, and 2 are taken may have a predetermined shape and size.
[0221] For example, the filter may have a rod shape. More specifically, the smoking article filter may have a cylinder-like shape.
[0222] The filter may have a length of, for example, 10 to 50 mm. Specifically, the length of the filter may have a lower limit of 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, 35 mm or more, 40 mm or more, or 45 mm or more, and an upper limit of 45 mm or less, 40 mm or less, 35 mm or less, 30 mm or less, 25 mm or less, 20 mm or less, or 15 mm or less.
[0223] In a specific example of the present application, the filter having said length has a circular cross section and a circumference of said circular cross section of 10 to 40 mm. For example, the circumference of said filter has a lower limit of 15 mm or more, 20 mm or more, 25 mm or more, 30 mm or more, or 35 mm or more, and an upper limit of 35 mm or less, 30 mm or less, 25 mm or less, 20 mm or less, or 15 mm or less.
[0224] In one example, the smoking article filter also includes a lyocell tow (i.e., a crimped lyocell multifilament), an oil agent coated on the lyocell multifilament, and a filter paper. The description of the lyocell tow and the oil agent is the same as that described above, and therefore will be omitted.
[0225] The wrapper paper is a porous or non-porous paper that can cover and encase the above-mentioned lyocell tow (i.e., tow that has been at least oil-treated and crimped) and maintain the filter shape (e.g., columnar or cylindrical).
[0226] In one example, when a porous wrapper paper is used, the wrapper paper may have a porosity of 10 to 50,000 CU (coresta unit). Specifically, the lower limit of the porosity of the wrapper paper is, for example, 1,000 CU or more, 5,000 CU or more, 10,000 CU or more, 15,000 CU or more, 20,000 CU or more, 25,000 CU or more, 30,000 CU or more, 35,000 CU or more, 40,000 CU or more, or 45,000 CU or more, and the upper limit is, for example, 45,000 CU or less, 40,000 CU or less, 35,000 CU or less, 30,000 CU or less, 25,000 CU or less, or 20,000 CU or less. In an embodiment of the present application, the wrapper may have a porosity in the range of 22,000 to 26,000 CU or 23,000 to 25,000 CU.
[0227] In one example, the basis weight of the wrapper is 15 to 60 g / cm 2Specifically, the lower limit of the basis weight of the wrapper paper is, for example, 20 g / cm 2 More than 25g / cm 2 More than 30g / cm 2 Above, 35g / cm 2 More than 40g / cm 2 More than 45g / cm 2 More than 50g / cm 2 or more than 55g / cm 2 The upper limit is, for example, 55 g / cm 2 Below, 50g / cm 2 Below, 45g / cm 2 Below 40g / cm 2 Below 35g / cm 2 Below 30g / cm 2 Below, 25g / cm 2 or less than 20g / cm 2 In a specific example of the present application, the wrapping paper has a density of 16 g / cm 2 More than 17g / cm 2 More than 18g / cm 2 More than 19g / cm 2 More than 20g / cm 2 or more than 21g / cm 2 Above, and 25g / cm 2 Below, 24g / cm 2 Below, 23g / cm 2 Below, 22g / cm 2 or less than 21g / cm 2 It may have the following basis weights:
[0228] Although not particularly limited, the diameter change (hardness change) and water disintegration degree according to the above-mentioned formula 1-1, formula 1-2, and formula 2 are measured for a rod-shaped filter weighing 50 mg or more. Specifically, the weight of the filter may have a lower limit of 100 mg or more, 150 mg or more, or 200 mg or more, and an upper limit of 500 mg or less, 450 mg or less, 400 mg or less, 350 mg or less, 300 mg or less, 250 mg or less, or 200 mg or less.
[0229] Other than that, the description of the filter for smoking articles and the materials contained therein is the same as that described above, so they will be omitted.
[0230] In yet another embodiment of the present invention, the present invention relates to a method for producing a filter for a smoking article, the method being a method for producing a filter for a lyocell smoking article as described above, the method also comprising a method for producing the lyocell material as described above.
[0231] Specifically, the method for manufacturing a filter for a smoking article according to the present application includes a step of treating a lyocell multifilament with an oil agent, a step of crimping the lyocell multifilament, and a step of manufacturing a filter using the crimped lyocell multifilament.
[0232] In the above method, the oil applied to the multifilament includes (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol, and (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms.
[0233] According to a specific example of the present application, the lyocell multifilament included in the smoking article filter contains the oil in an amount of 2.0% by weight or more, based on 100% by weight of the entire lyocell multifilament. In this case, the lyocell multifilament included in the smoking article filter is a multifilament that has been at least treated with an oil, and for example, the lyocell material is a lyocell multifilament to which a primary oil treatment has been applied, a lyocell multifilament to which a primary oil treatment and a secondary oil treatment have been applied, or a lyocell multifilament to which a binder, which will be described later, has been applied in addition to the oil treatment as described above. As described above, the lyocell multifilament that has been treated with an oil and / or binder is also one to which crimping has been applied. Specific values related to the content of the oil are as described above.
[0234] Regarding the method for manufacturing a filter for a smoking article, the remaining steps except for the step of manufacturing the filter are the same as those described above for the lyocell material, so the description thereof will be omitted. Also, the description that overlaps with the above will be omitted.
[0235] The step of manufacturing the filter can be appropriately performed by a person skilled in the art using a known method. For example, the filter can be manufactured by forming a tow-filled wrapper paper into a rod shape. Alternatively, the filter can be manufactured by cutting a rod-shaped tow-filled filter paper to an appropriate length. The description of the wrapper paper is as above.
[0236] Although not particularly limited, before filling the filter paper with the tow, the tow may be additionally subjected to fiber opening treatment and plasticizer treatment.
[0237] In yet another embodiment of the present application, the present application relates to a smoking article comprising a lyocell material having the composition and / or properties as described above, the description of which is omitted here.
[0238] In yet another embodiment of the present application, the present application relates to a smoking article including a filter for a smoking article, the filter for a smoking article having the configuration and / or characteristics as described above, and the description thereof will be omitted.
[0239] In yet another embodiment of the present application, the present application relates to an oil that can be applied (e.g., coated) to lyocell tow. The oil of the present application can overcome the hydrophilicity of the surface of a lyocell material for a smoking article filter and improve the degree of reduction in hardness of the lyocell material caused by moisture.
[0240] In a specific example of the present application, the oil agent contains (a) an ester of a fatty acid having 16 or more carbon atoms with an aliphatic monohydric alcohol, and (b) an ester of sorbitan with a fatty acid having 16 or more carbon atoms. In another example, the oil agent further contains, as component (c), an alkylene oxide adduct of component (b).
[0241] A specific description of each component contained in the oil agent is the same as that described above, and will not be repeated here. Effect of the Invention
[0242] According to the present application, a lyocell material for smoking article filters that can replace commercially available cellulose acetate (CA) and a smoking article filter containing the same are provided. Specifically, the present application not only provides a lyocell material with excellent manufacturing processability and biodegradability, but also has the inventive effect of improving the filter hardness and the physical properties of smoking articles (e.g., cigarettes). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0243] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, which are presented as examples of the invention and are not intended to limit the scope of the present invention in any way.
[0244] <Experiment 1: Evaluation of settling time of lyosceltoe> The Lyocell material was produced through the process described in the following production examples. Unless otherwise specified, the conditions were within the scope of the above description.
[0245] Manufacturing Example A cellulose pulp having a degree of polymerization (DPw) of 820 and an α-cellulose content of 93.9% was mixed with an N-methylmorpholine-N-oxide (NMMO) / H2O solvent having a propyl gallate content of 0.01 wt% to produce a radiation dope for tow production with a concentration of 11 wt%. The radiation dope was then radiated from a radiation nozzle by appropriately adjusting the discharge amount and radiation speed while maintaining the radiation temperature at 110°C.
[0246] The dope on the filament discharged from the nozzle was fed through the air gap section to the coagulation liquid (containing 75 wt% water and 25 wt% N-methylmorpholine-N-oxide (NMMO) and having a temperature of about 25°C) in the coagulation tank. At this time, the cooling air in the air gap section was at a temperature of 8°C and a pressure of 200 Nm 3 The radiation dope was solidified by blowing air at a rate of 1 / h. The concentration of the solidified solution was continuously monitored using a sensor and a refractometer.
[0247] The solidified lyocell filaments were then washed with water. Specifically, the filaments were introduced into a pulling roll, and N-methylmorpholine-N-oxide (NMMO) remaining in the filaments was removed with water sprayed from a water washing device. The washed filaments were then immersed in a bath designed to have a predetermined oil concentration.
[0248] The filament is rolled at 2kgf / cm by the nip roll installed at the bath discharge section. 2 The fabric was then subjected to pressure treatment and placed in a crimp machine for crimping. Specifically, the steam pressure was set at 0.5 kgf / cm in a steam box. 2 The pressure of the crimping device roller is 2.5kgf / cm 2 and the doctor blade pressure is 0.5kgf / cm 2 Then, a tow was produced.
[0249] The produced tow was subjected to a secondary oil treatment to prevent static electricity and impart flexibility, and immediately after the treatment, it was passed through a continuous drying device set at 120°C to obtain a dried tow product.
[0250] The tow produced has a single yarn fineness of 3.0 to 3.5 denier, a total fineness of 36,000 to 40,000 denier, and a crimp count of 25 to 35 ea / inch.
[0251] For reference, the types (components) of oils and / or oil treatment levels (OPU) used in each of the examples and comparative examples are different from each other as shown below.
[0252] Example 1 Lyocell tow was used that had been oil-treated as in the previous preparation example, except that the oil used in preparing the tow contained about 60% by weight of isotridecyl stearate, about 22% by weight of sorbitan monooleate, about 16% by weight of polyoxyethylene sorbitan monooleate, and the balance water, with an OPU of 5.6% by weight.
[0253] Example 2 The lyocell tow was treated with an oil as in the above-mentioned preparation example. The oil used in the preparation of the tow contained about 50% by weight of isotridecyl stearate, about 27% by weight of sorbitan monooleate, about 21% by weight of polyoxyethylene sorbitan monooleate, and the balance of water, and the OPU was 5.1% by weight.
[0254] Example 3 The same lyocell tow was used as in Example 1, except that the OPU was 3.16 wt%.
[0255] Example 4 The same lyocell tow was used as in Example 1, except that the OPU was 2.15 wt%.
[0256] Comparative Example 1 Lyocell tow was used in the same manner as in the above-mentioned manufacturing example, except that no oil treatment was carried out.
[0257] Comparative Example 2 The lyocell tow was treated with an oil as in the above-mentioned manufacturing example. The oil used in the manufacturing of the tow was JKP-107C, which can be classified as a hydrophilic oil, and the OPU was 2.1% by weight. The JKP-107C is known to contain about 40% by weight or more of polyoxyethylene alkyl ether, about 10% by weight or more of polyethylene glycol, about 20% by weight or more of polyethylene glycol alkyl ester, about 13% by weight or more of polyoxyethylene alkyl phosphate, about 9% by weight or more of dialkyl sulfosuccinate and / or its salt, about 3% by weight or more of aliphatic alcohol amine, and about 5% by weight or more of water.
[0258] Comparative Example 3 The same lyocell tow was used as in Example 1, except that the OPU was 0.23 wt%.
[0259] The settling time of each of the tows of Examples 1 to 3 and Comparative Examples 1 to 4 produced as described above was evaluated by the following method.
[0260] Sinking time (seconds) evaluation method The tow (oil-treated tow) of the examples and comparative examples was cut to a size of 8 cm. The sample tow prepared from the examples and comparative examples was placed in a beaker filled with 1,000 ml of water (the outer diameter of the beaker was 108 mm, the height was 158 mm, and the height of the water filled was about 12.5 cm), and the time (seconds) for the tow to fall to the bottom of the sample was measured. The settling times listed in Table 1 below are arithmetic average values obtained after repeating the above experiment three times for the sample tow taken from each example or comparative example.
[0261] [Table 1] *OPU (oil pick-up ratio): Measured by the method described above.
[0262] It can be seen from Table 1 that the tow settling time of the examples is longer than that of the comparative examples. This means that the tow surface of the examples has stronger hydrophobicity. When the tow having stronger hydrophobicity is used as a filter material for smoking articles, it can more effectively suppress the hardness collapse caused by saliva. This is also confirmed by the following experiment.
[0263] <Experiment 2: Evaluation of hardness change of filters containing lyocell tow> Example 4 The lyocell tow of Example 1 was used as a wrapping paper (24,000 CU porous paper, grammage approximately 21 g / cm 2 ) to prepare a cylindrical filter rod (weight 150-200 mg) having an axial length of 27 mm and a circumference of 24.22 mm.
[0264] Example 5 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Example 2 was used.
[0265] Example 6 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Example 3 was used.
[0266] Comparative Example 5 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Comparative Example 1 was used.
[0267] Comparative Example 6 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Comparative Example 2 was used.
[0268] Comparative Example 7 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Comparative Example 3 was used.
[0269] Comparative Example 8 A filter rod was prepared in the same manner as in Example 4, except that the lyocell tow of Comparative Example 4 was used.
[0270] The example filters and the comparative example filters manufactured as described above were each evaluated for hardness change (or diameter change) by the following method.
[0271] Filter hardness change (%) or diameter change (%) 20 μl of water (e.g., distilled water or tap water) was injected into the filters manufactured in Examples 5 to 8 and Comparative Examples 4 to 7, and the change in hardness (diameter change) was confirmed before and after 5 minutes of water injection. At this time, water was injected into three portions at positions of 4.5 mm, 13.5 mm, and 22.5 mm into one end of a 27 mm long filter rod. The amount of water injected was a value set after a group of smokers voluntarily measured the amount of moisture remaining in the filter after smoking a tobacco product.
[0272] The change in filter hardness due to water penetration into the filter and the degree of collapse of the filter due to water can be calculated from the change in filter diameter as follows. For such measurements, Filtrona's DHT 200 TM The equipment was used.
[0273] [Formula 1-1] Filter diameter (or filter hardness) retention rate (%) before water injection = {(initial filter diameter (mm) - length of filter pushed when a weight of a specific weight (300g) is used (mm)) / (initial filter diameter (mm))} x 100
[0274] [Formula 1-2] Filter diameter (or filter hardness) retention rate (%) after water injection = {(Initial filter diameter (mm) - length of filter pushed (mm) when the filter is pushed with a weight of a specific weight (300g) after water is injected) / (Initial filter diameter (mm))} x 100
[0275] [Formula 2] Moisture disintegration rate (%) = {(Filter diameter maintenance rate before water injection - Filter diameter maintenance rate after water injection) / (Filter diameter maintenance rate before water injection)} x 100
[0276] [Table 2] *OPU (oil pick-up ratio): Measured by the method described above. Defective filter production: This refers to the case where the tow does not spread evenly during the spreading process in filter production, resulting in clumps, or where the filter rod is not cut smoothly due to lack of hardness.
[0277] It can be seen from Table 2 that the hardness change (especially the hardness change after water injection) of the examples is larger than that of the comparative examples. This means that the tow surface of the examples has stronger hydrophobicity. When the tow having stronger hydrophobicity is used as a filter material for smoking articles, it can more effectively suppress the hardness destruction caused by saliva.
Claims
1. A lyocell material for a smoking article filter, comprising: a lyocell multifilament having a crimp; and an oil agent coated on the lyocell multifilament; The oil agent comprises: (a) an esterification product of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an esterification product of sorbitan and a fatty acid having 16 or more carbon atoms, The lyocell material for smoking article filters contains the oil in an amount of 2.0% by weight or more relative to 100% by weight of the entire lyocell material.
2. The oil agent contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
3. The lyocell material for smoking article filters according to claim 1 , wherein the oil further comprises an alkylene oxide adduct (c) of the esterified product (b).
4. The oil agent contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
5. The crimped lyocell multifilament is 2. The lyocell material for smoking article filters according to claim 1, having a total denier of 15,000 to 45,000 and 20 to 50 crimps per inch.
6. A smoking article comprising the lyocell material of claim 1.
7. A crimped lyocell multifilament and an oil agent coated on the lyocell multifilament, A lyocell material for smoking article filters having a settling time in water of 6.0 seconds or more (wherein the settling time means the time it takes for the lyocell material, cut to a length of 10 cm or less, to fall to the bottom of a container filled with water to a height of 12 to 13 cm).
8. The lyocell material for smoking article filters contains the oil in an amount of 2.0% by weight or more based on 100% by weight of the entire lyocell material, The lyocell material for smoking article filters according to claim 7, wherein the oil comprises: (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms.
9. The oil agent contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
10. The lyocell material for smoking article filters according to claim 8, wherein the oil further comprises (c) an alkylene oxide adduct of the ester (b).
11. The oil agent contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
12. 8. The lyocell material for smoking article filters according to claim 7, wherein the lyocell multifilaments have a total fineness of 15,000 to 45,000 denier and 20 to 50 crimps per inch.
13. A smoking article comprising the lyocell material of claim 7.
14. A method for producing a lyocell material for a smoking article filter, comprising the steps of treating a lyocell multifilament with an oil agent and crimping the lyocell multifilament, The oil agent comprises: (a) an esterification product of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an esterification product of sorbitan and a fatty acid having 16 or more carbon atoms, The lyocell material for smoking article filters comprises the oil in an amount of 2.0% by weight or more based on 100% by weight of the entire lyocell material.
15. The method for producing a lyocell material for a smoking article filter according to claim 14, wherein the oil contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
16. The method for producing a lyocell material for a smoking article filter according to claim 14, wherein the oil further comprises (c) an alkylene oxide adduct of the ester (b).
17. The method for producing a lyocell material for a smoking article filter according to claim 14, wherein the oil contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
18. 15. The method for producing a lyocell material for a smoking article filter according to claim 14, comprising providing a lyocell multifilament having a total fineness of 15,000 to 45,000 denier and 20 to 50 crimps per inch.
19. A filter for a smoking article comprising a lyocell material, The lyocell material includes a lyocell multifilament having a crimp and an oil agent coated on the lyocell multifilament, The oil agent comprises: (a) an esterification product of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an esterification product of sorbitan and a fatty acid having 16 or more carbon atoms, The lyocell material contains the oil in an amount of 2.0% by weight or more based on 100% by weight of the entire lyocell material.
20. The filter for smoking articles according to claim 19, wherein the oil agent contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
21. The filter for smoking articles according to claim 19, wherein the oil further comprises (c) an alkylene oxide adduct of the ester (b).
22. The filter for smoking articles according to claim 19, wherein the oil agent contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
23. The crimped lyocell multifilament is 20. A filter for a smoking article according to claim 19, having a total denier of 15,000 to 45,000 and 20 to 50 crimps per inch.
24. A smoking article comprising the filter for a smoking article according to claim 18.
25. A filter for a smoking article comprising a lyocell material and a wrapping paper that covers and wraps the lyocell material, The lyocell material includes a lyocell multifilament having a crimp and an oil agent coated on the lyocell multifilament, The filter diameter maintenance rate before water injection calculated by the following formula 1-1 is 85% or more. A filter for a smoking article, which satisfies a filter diameter maintenance rate after water injection of 80% or more, as expressed by the following mathematical formula 1-2: [Formula 1-1] Filter diameter maintenance rate before water injection (%) = {(initial filter diameter (mm) - length (mm) of the filter pushed when the filter is pushed with a weight of a specific weight (300 g)) / (initial filter diameter (mm))} x 100 [Formula 1-2] Filter diameter maintenance rate after water injection (%) = {(initial filter diameter (mm) - length (mm) of the filter pushed when the filter is pushed with a weight of a specific weight (300 g) after water is poured) / (initial filter diameter (mm))} x 100 However, in the above formula 1-2, the amount of water injected into the filter is 20 μl, and the diameter maintenance rate in formula 1-2 is also measured 5 minutes after the water was injected into the filter.
26. The filter for smoking articles according to claim 25, which satisfies a moisture decay rate calculated by the following formula 2 of 8.0% or less: [Formula 2] Moisture disintegration rate (%)={(filter diameter maintenance rate before water injection calculated by the above-mentioned Formula 1-1)−(filter diameter maintenance rate after water injection calculated by the above-mentioned Formula 1-2) / filter diameter maintenance rate before water injection calculated by the above-mentioned Formula 1-1}×100.
27. The lyocell material contains the oil in an amount of 2.0% by weight or more based on 100% by weight of the entire lyocell material, The filter for smoking articles according to claim 25, wherein the oil comprises: (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms.
28. The filter for smoking articles according to claim 25, wherein the oil agent contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
29. The filter for smoking articles according to claim 25, wherein the oil further comprises (c) an alkylene oxide adduct of the ester (b).
30. The filter for smoking articles according to claim 25, wherein the oil agent contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
31. 26. A filter for a smoking article according to claim 25, wherein the lyocell multifilament has a total fineness of 15,000 to 45,000 denier and 20 to 50 crimps per inch.
32. A smoking article comprising the smoking article filter of claim 25.
33. A method for manufacturing a filter for a smoking article, comprising the steps of treating a lyocell multifilament with an oil agent, crimping the lyocell multifilament, and manufacturing a filter using the crimped lyocell multifilament, The oil agent comprises: (a) an esterification product of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol; and (b) an esterification product of sorbitan and a fatty acid having 16 or more carbon atoms, The lyocell multifilament included in the filter for smoking articles contains the oil in an amount of 2.0% by weight or more based on 100% by weight of the entire lyocell multifilament.
34. The method for producing a filter for smoking articles according to claim 33, wherein the oil contains 20 to 60 parts by weight of (b) an ester of sorbitan and a fatty acid having 16 or more carbon atoms, relative to 100 parts by weight of (a) an ester of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
35. The method for producing a filter for a smoking article according to claim 33, wherein the oil further comprises (c) an alkylene oxide adduct of the ester (b).
36. The method for producing a filter for smoking articles according to claim 33, wherein the oil contains 10 to 50 parts by weight of the alkylene oxide adduct (c) to the ester (b) relative to 100 parts by weight of the ester (a) of a fatty acid having 16 or more carbon atoms and an aliphatic monohydric alcohol.
37. The method for producing a filter for a smoking article according to claim 33, wherein the lyocell multifilament has a total fineness of 15,000 to 45,000 denier and 20 to 50 crimps per inch.
Citation Information
Patent Citations
LYOCELL fiber containing chitin / chitosan and preparation method thereof
CN112323161A
Lyocell material for cigarette filter and its manufacturing method
JP2018504897A
Regenerated cellulose substrate for aerosol delivery device
US20210315255A1