Cold forging wire rod, steel part and manufacturing method thereof with improved delayed fracture resistance
A steel composition and manufacturing process with controlled microstructure improve delayed fracture resistance and reduce costs by using specific alloy elements and processes, ensuring high tensile strength and minimizing hydrogen traps in high-strength steel components.
Patent Information
- Application Number
- JP2024532841
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-01
AI Technical Summary
High-strength steel materials used in bolts for automobiles and structures face issues with delayed fracture due to hydrogen traps at grain boundaries, leading to inferior performance, especially when boron-added steel is used at pressures above 1.1 GPa, necessitating the development of cost-effective alternatives to Mo and V-added steels.
A steel composition with controlled microstructure, comprising specific alloy elements (C, Si, Mn, P, S, Cr, Ti, B) and a manufacturing process involving finish rolling, spheroidizing heat treatment, and quenching, results in a wire rod with over 90% martensite and carbides less than 15 nm, enhancing delayed fracture resistance.
The solution achieves improved delayed fracture resistance and cost reduction by maintaining tensile strength above 1200 MPa while minimizing hydrogen traps, thereby preventing cracks in high-strength steel components.
Smart Images

Figure 2024543998000001 
Figure 2024543998000002 
Figure 2024543998000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a wire rod for cold forging, a steel part, and a manufacturing method thereof, which have improved delayed fracture resistance, and more particularly to a wire rod for cold forging, a steel part, and a manufacturing method thereof, which have improved delayed fracture resistance by controlling a microstructure. [Background technology]
[0002] Wire rods used for fastening bolts in automobiles and structures are required to have high strength in order to reduce the weight of automobiles and the size of structures. To increase the strength of steel, metal strengthening mechanisms such as cold working, grain refinement, martensite strengthening, and precipitation strengthening are utilized. However, the electric potential, grain boundaries, martensite lath boundaries, and fine precipitate boundaries used as the strengthening mechanisms act as hydrogen traps in the steel, causing delayed fracture to deteriorate. Therefore, there is a problem that delayed fracture is deteriorated in high-strength bolts with a tensile strength of 1 GPa or more.
[0003] To solve these problems, Cr-Mo alloy steels containing Mo have been used for bolt steels with a strength of 1 GPa or higher and a tempered martensite structure. However, to meet the need for cost reduction due to the development of bolt manufacturing technology, there have been efforts to replace high-strength steels with 1 GPa or higher with boron-containing steels. As a result, after realizing cost reductions using boron-containing steels and confirming their safety, boron-containing steels are now being used in some fastening bolts for automobiles.
[0004] However, when using boron-added steel at 1.1 GPa or higher, there is a problem of hydrogen-induced delayed fracture (Ref. N. Uno et al.). Therefore, for high-strength steels at 1.1 GPa or higher, standard steels containing Mo have been used, or steel types developed by steel companies containing Mo and V have been used. However, for cost competitiveness, there is a need to develop high-strength steels that omit expensive carbide elements such as Mo and V. [Prior art documents] [Non-patent literature]
[0005] Nippon Steel Technical Report 2008 No.97 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above problems, an object of the present invention is to provide a wire rod for cold forging, a steel part, and a manufacturing method thereof, which can reduce costs and have improved delayed fracture resistance by controlling the microstructure through the alloy composition and manufacturing method. [Means for solving the problem]
[0007] The steel part with improved delayed fracture resistance of the present invention may contain, by weight%, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, and the volume fraction of automatically tempered martensite may be 90% or more. Furthermore, the steel part of the present invention with improved delayed fracture resistance may have an average thickness of carbides within prior austenite grains of 15 nm or less. Furthermore, the steel part of the present invention with improved delayed fracture resistance may have a tensile strength of 1200 MPa or more.
[0008] In addition, the method for producing a steel part with improved delayed fracture resistance of the present invention includes the steps of forming a steel material containing, by weight%, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0.03% but not more than 0.03%, S: more than 0% but not more than 0.03%, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, finish rolling the steel material to form a wire material, coiling the wire material, drawing the coiled wire material and then subjecting it to a spheroidizing heat treatment, forming the spheroidizing heat treated wire material into a part, and quenching the part after austenitizing.
[0009] In the method for producing a steel part with improved delayed fracture resistance of the present invention, the finish rolling can be carried out at 880 to 980°C, and the coiling can be carried out at 830 to 930°C. In the method of the present invention for producing a steel part with improved delayed fracture resistance, the spheroidizing heat treatment can be carried out at a maximum temperature in the range of 745 to 765°C. In addition, in the method for producing a steel part having improved delayed fracture resistance according to one embodiment of the present invention, the austenitization can be carried out at 870 to 940°C. In addition, in the method for producing a steel part having improved delayed fracture resistance according to one embodiment of the present invention, the quenching can be performed with a coolant at 10 to 80°C.
[0010] The cold forging wire rod of the present invention may contain, by weight%, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, and may have a diameter of 5.5 to 20 mm. Effect of the Invention
[0011] According to the present invention, it is possible to provide a wire rod for cold forging, a steel part, and a manufacturing method thereof, which are capable of reducing costs and have improved delayed fracture resistance by controlling the microstructure through the alloy composition and manufacturing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The steel part with improved delayed fracture resistance of the present invention contains, by weight%, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, and the volume fraction of automatically tempered martensite is 90% or more.
[0013] The following examples are presented to fully convey the concept of the present invention to those skilled in the art to which the present invention pertains. The present invention is not limited to the examples presented herein and may be embodied in other forms. In the drawings, parts that are not relevant to the description are omitted in order to clarify the present invention, and the sizes of components are somewhat exaggerated in order to facilitate understanding. Throughout the specification, when a part is described as "comprising" certain elements, this does not mean to exclude other elements, but rather that it may further include other elements, unless specifically stated to the contrary. The singular expression includes the plural expression unless the context clearly dictates otherwise.
[0014] The reasons for limiting the contents of alloying elements in the examples of the present invention will be described below. In the following, the unit is weight percent unless otherwise specified.
[0015] The steel part with improved delayed fracture resistance of the present invention may contain, by weight, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities.
[0016] The C (carbon) content may be 0.18% or more and 0.25% or less. C is an element added to ensure the strength of the product. Taking this into consideration, C can be added in an amount of 0.18% or more. However, if the C content is too high, delayed fracture can be induced due to an increase in strength. Taking this into consideration, the upper limit of the C content can be limited to 0.25%.
[0017] The content of Si (silicon) may be 0.30% or more and 0.50% or less. Si may be added to deoxidize steel. In addition, Si is an effective element for ensuring strength through solid solution strengthening. In consideration of this, Si may be added in an amount of 0.30% or more. However, if the Si content is excessive, the impact properties and formability may be deteriorated. In consideration of this, the upper limit of the Si content may be limited to 0.50%. Preferably, the Si content may be 0.31% or more and 0.48% or less.
[0018] The Mn (manganese) content may be equal to or greater than 0.35% and equal to or less than 0.50%. Mn is a very effective element that improves hardenability and forms a substitutional solid solution in the matrix structure to exhibit a solid solution strengthening effect. In addition, if the Mn content is low, it may not sufficiently bond with S (sulfur) that flows into the steel as an impurity, which may induce continuous casting cracks. In consideration of this, Mn may be added in an amount of 0.35% or more. However, if the Mn content is excessive, coarse MnS may be formed, which may result in poor delayed fracture resistance. In consideration of this, the upper limit of the Mn content may be limited to 0.50%. Preferably, the Mn content may be 0.36% or more and 0.49% or less.
[0019] The P (phosphorus) content may be more than 0% and not more than 0.03%. P segregates at grain boundaries, lowering toughness and decreasing delayed fracture resistance. Therefore, in the present invention, it can be controlled as an impurity. In consideration of this, the upper limit of the P content can be limited to 0.03%, and the closer to 0%, the more preferable.
[0020] The S (sulfur) content may be more than 0% and not more than 0.03%. Like P, S segregates at grain boundaries to reduce toughness and forms low melting point sulfides, which act as a cause of impeding hot rolling. Therefore, in the present invention, S can be controlled as an impurity. In consideration of this, the upper limit of the S content can be limited to 0.03%, and the closer to 0%, the more preferable.
[0021] The Cr (chromium) content may be equal to or greater than 0.45% and equal to or less than 0.60%. Cr is a very effective element that improves hardenability and forms a substitutional solid solution in the matrix structure to produce a solid solution strengthening effect. In consideration of this, Cr may be added in an amount of 0.45% or more. However, if the Cr content is excessive, the c / a ratio of corrosion pits increases due to the formation of a chromium oxide layer on the surface, and delayed fracture resistance may be deteriorated due to the notch effect. In consideration of this, the upper limit of the Cr content may be limited to 0.60%. Preferably, the Cr content may be 0.46% or more and 0.59% or less.
[0022] The Ti (titanium) content may be 0.015% or more and 0.03% or less. Ti is an effective element that prevents B (boron) from combining with N by combining with N to form titanium nitride. In consideration of this, Ti may be added in an amount of 0.015% or more. However, if the Ti content is excessive, coarse carbonitrides may be formed, resulting in poor delayed fracture resistance. In consideration of this, the upper limit of the Ti content may be limited to 0.03%. Preferably, the Ti content may be 0.023% or more and 0.026% or less.
[0023] The content of B (boron) may be 0.001% or more and 0.004% or less. B is an effective element for improving hardenability. Taking this into consideration, B may be added in an amount of 0.001% or more. However, if the B content is excessive, Fe may be mixed into the grain boundaries. 23 The formation of (CB)6 carbide may induce embrittlement of the austenite grain boundary, resulting in poor delayed fracture resistance. In consideration of this, the upper limit of the B content may be limited to 0.004%. Preferably, the B content may be 0.0018% or more and 0.0023% or less.
[0024] The remaining component of the present invention is iron (Fe). However, since unintended impurities may be inevitably mixed from raw materials or the surrounding environment during normal manufacturing processes, it is not possible to exclude them. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them will not be specifically mentioned in this specification.
[0025] The steel part of the present invention with improved delayed fracture resistance may have a volume fraction of auto-tempered martensite of 90% or more. If the auto-tempered martensite is less than 90%, it is difficult to ensure sufficient toughness and delayed fracture resistance may be inferior. Therefore, in the present invention, the auto-tempered martensite can be controlled to 90% through the alloy composition and manufacturing process. In particular, one of the features of the auto-tempered martensite structure is that it is automatically tempered during coiling without an additional tempering heat treatment process.
[0026] In addition, the steel part of the present invention with improved delayed fracture resistance can be automatically tempered at the time of coiling without an additional tempering heat treatment process, and the average thickness of carbides in prior austenite grains can be controlled to be 15 nm or less. It is known that the surface direction of carbides precipitated during automatic tempering in plate-type steels is not effective as a hydrogen trap because of its high coherency, whereas the side portion of the plate-type steel has low coherency and acts as a non-diffusible hydrogen trap, thereby improving hydrogen delayed fracture resistance. Therefore, when the average thickness of the carbides in the prior austenite grains is thin, the coherency of the carbide interface increases, making it difficult to improve hydrogen delayed fracture resistance. On the other hand, when the average thickness of the carbides in the prior austenite grains is thick, the number of carbides decreases, making it difficult to improve delayed fracture resistance. Therefore, in the present invention, the average thickness of the carbides in the prior austenite grains is controlled to be 15 nm or less to improve delayed fracture resistance.
[0027] Furthermore, the steel part of the present invention with improved delayed fracture resistance may have a tensile strength of 1200 MPa or more by controlling the alloy composition and manufacturing method.
[0028] Next, the method for producing a steel part having improved delayed fracture resistance according to the present invention will be described. The method for producing a steel part with improved delayed fracture resistance of the present invention includes the steps of forming a steel material containing, by weight%, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0.03% but not more than 0.03%, S: more than 0% but not more than 0.03%, Cr: 0.45% or more and 0.60% or less, Ti: 0.005% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, finish rolling the steel material to form a wire material, coiling the wire material, drawing the coiled wire material and then subjecting it to a spheroidizing heat treatment, forming the spheroidizing heat treated wire material into a part, and quenching the part after austenitizing.
[0029] The reasons for limiting the range of the components of each alloy composition are as described above, and will be described in more detail below with respect to each manufacturing step. First, a steel material satisfying the above alloy composition can be formed, and then it can go through a series of steps including finish rolling, coiling, adsorption heat treatment, forming, austenitization, and quenching. First, the steel material is finish-rolled at 880 to 980°C to form a wire rod, and the wire rod is coiled at 830 to 930°C. When the finish rolling temperature or the coiling temperature is low, the surface layer is in a quasi-two-phase region, and a surface ferrite decarburized layer may be formed due to phase transformation. Therefore, when the finish rolling temperature or the coiling temperature is low, a surface ferrite decarburized layer may be formed even during heat treatment of the steel part, resulting in poor delayed fracture resistance. In consideration of this, the finish rolling temperature may be 880°C or higher, or the coiling temperature may be 830°C or higher. On the other hand, when the finish rolling temperature or the coiling temperature is high, decarburization is accelerated by diffusion, and a ferrite decarburized layer is formed on the surface, which may result in poor delayed fracture resistance. In consideration of this, the finish rolling temperature may be 980°C or less, or the coiling temperature may be 930°C or less.
[0030] Next, the wound wire may be drawn according to the purpose, and then subjected to a spheroidizing heat treatment at a maximum temperature in the range of 745 to 765°C. If the maximum temperature of the spheroidizing heat treatment is too low or too high, the hardness of the spheroidized heat treatment material increases due to the low spheroidizing rate, which may induce cracks due to poor formability during processing of steel parts. Taking this into consideration, the maximum temperature of the spheroidizing heat treatment can be set to 745 to 765°C. The wire rod that has been subjected to the spheroidizing heat treatment can be shaped according to the purpose to form a steel part, and then austenitized at 870 to 940°C.
[0031] When the austenitizing temperature is low, the austenite reverse transformation does not occur sufficiently, so that the martensite structure after coiling becomes non-uniform, and the toughness may become inferior. In consideration of this, the austenitizing temperature may be 870°C or higher. However, when the austenitizing temperature is high, the austenite grain size becomes coarse, and the delayed fracture resistance may become inferior. In consideration of this, the upper limit of the austenitizing temperature may be limited to 940°C.
[0032] The austenitized steel part may then be quenched in a coolant at 10 to 80°C. If the temperature of the quenching coolant is low, fine quenching cracks may occur due to thermal deformation of the steel parts, which may lead to delayed fracture. In consideration of this, the temperature of the quenching coolant may be 10°C or higher. However, if the temperature of the quenching coolant is high, the self-tempering effect may become high, making it difficult to achieve the desired strength. In consideration of this, the upper limit of the quenching coolant temperature may be limited to 80°C. From the above process, the final microstructure of the steel part can realize 90% or more of auto-tempered martensite structure without tempering process, and can realize a structure in which carbides having an average thickness of 15 nm or less are precipitated in the prior austenite grains. Therefore, by controlling the microstructure, delayed fracture resistance can be improved.
[0033] Next, the cold forging wire rod of the present invention will be described. The wire rod for cold forging of the present invention may contain, by weight, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.005% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities, and may have a diameter of 5.5 to 20 mm. The reasons for limiting the numerical values of the ranges of the components of each alloy composition are as described above, and the cold forging wire rod of the present invention may be manufactured with a diameter of 5.5 to 20 mm, but is not limited thereto and may be manufactured with various diameters depending on the purpose.
[0034] The present invention will be described in more detail with reference to the following examples. However, the description of the examples is merely for illustrating the implementation of the present invention, and the present invention is not limited by the description of the examples. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred from the claims.
[0035] <Example> Steel materials were manufactured for various alloy composition ranges shown in Table 1 below, and then finish-rolled at 910°C to form wire rods with a diameter of 15 mm, which were then wound into a coil shape at 880°C. The wound wire rods were spheroidized at a maximum temperature of 755°C, formed into bolts with M12 threads, austenitized at 890°C, and quenched with a coolant at 60°C. The spheroidized heat treatment temperature means the highest heating temperature.
[0036] [Table 1]
[0037] The tensile strength, carbide thickness, and delayed fracture performance of the bolts produced above are shown in Table 2. The tensile strength was measured using a Zwick / Roell ZWICK Z250 tensile tester. The tensile strength measurement test was performed on a tensile test piece with a diameter of 10 mm and a gauge diameter of 6.25 mm. The thickness of the carbide was measured using an FEI Tecnai OSIRIS transmission electron microscope (TEM). The thickness of the carbide was measured at five random points on the replica specimen and expressed as the average thickness. The minor axis of the plate-type carbide was defined as the thickness. The delayed fracture performance evaluation test method was carried out by fastening the bolt to a structure with the fastening force of the yield strength, and then immersing it in 5% hydrochloric acid + 95% distilled water solution for 10 minutes, before and after which the presence or absence of cracks was observed on the threads, which are the stress concentration areas, using a delayed fracture simulation method. As a result of the delayed fracture performance evaluation, if a crack occurred, it was indicated with "O", and if no crack occurred, it was indicated with "X".
[0038] [Table 2]
[0039] As shown in Table 2, Examples 1 to 8 satisfied the alloy composition, component range, and manufacturing process proposed by the present invention. Thus, Examples 1 to 8 satisfied the tensile strength of 1200 MPa or more, the carbide thickness of 15 nm or less, and the delayed fracture performance evaluation showed that no cracks occurred. However, Comparative Example 1 did not satisfy the tensile strength of 1200 MPa or more due to the low C content. In addition, in Comparative Example 2, the C content was high and the thickness of the carbides exceeded 15 nm, and the delayed fracture performance evaluation showed that cracks occurred. In addition, in Comparative Example 3, the tensile strength did not satisfy the requirement of 1200 MPa or more due to the low Si content. In addition, in Comparative Example 4, since the Mn content was high, coarse MnS was formed, and as a result of the delayed fracture performance evaluation, cracks were generated. In addition, in Comparative Example 5, since the Cr content was low, a bainite contaminated structure was formed in the microstructure, and as a result of the delayed fracture performance evaluation, cracks were generated. In addition, in Comparative Example 6, since the Cr content was high, sharp corrosion pits were formed during corrosion with hydrochloric acid, and as a result of the delayed fracture performance evaluation, cracks were generated.
[0040] Next, Table 3 below shows the presence or absence of cracks based on the delayed fracture performance evaluation results after steel materials were manufactured with the alloy components of Example 5 in Table 1 above and bolts were manufactured at the finish rolling temperature, coiling temperature, maximum spheroidizing heat treatment temperature, and austenitizing temperature shown in Table 3 below.
[0041] [Table 3]
[0042] In Comparative Example 7, the finish rolling temperature and coiling temperature were high, so that the size of the prior austenite crystal grains became large, and as a result of the delayed fracture performance evaluation, cracks occurred. In Comparative Example 8, the finish rolling temperature and coiling temperature were low, so that a ferrite decarburized layer was formed in the wire rod, and as a result of the delayed fracture performance evaluation, cracks occurred. In Comparative Example 9, since the austenitizing temperature was high, the size of the prior austenite crystal grains became large, and as a result of the delayed fracture performance evaluation, cracks were generated. In Comparative Example 10, since the austenitizing temperature was low, the material entered the quasi-two-phase region, and a ferrite decarburized layer was formed during heating. As a result of the delayed fracture performance evaluation, cracks were generated. In Comparative Examples 11 and 12, the maximum temperature of the spheroidizing heat treatment was low or high, respectively, so that the spheroidizing heat treatment was not performed sufficiently, resulting in poor formability. Therefore, in Comparative Examples 11 and 12, cracks were formed during the forming of the thread portion, and the performance evaluation of delayed fracture showed that cracks occurred.
[0043] [Table 4]
[0044] Comparative Examples 13 to 16 utilize steel materials having the same alloy components and composition range as Example 5. However, compared to Example 5, the automatic martensite fraction and carbide thickness do not satisfy the ranges of the present application, and it can be confirmed that cracks are generated as a result of the delayed fracture performance evaluation. [Industrial Applicability]
[0045] According to the present invention, by controlling the microstructure through the alloy composition and manufacturing method, it is possible to provide a wire rod and a steel part for cold forging that can reduce costs and have improved delayed fracture resistance, and the industrial applicability is recognized.
Claims
1. The steel contains, by weight, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, and the remainder being Fe and unavoidable impurities, A steel part having improved delayed fracture resistance, characterized in that the volume fraction of auto-tempered martensite is 90% or more.
2. 2. A steel part with improved delayed fracture resistance according to claim 1, characterized in that the average thickness of carbides in prior austenite grains is 15 nm or less.
3. 2. A steel part with improved delayed fracture resistance according to claim 1, characterized in that the tensile strength is 1200 MPa or more.
4. forming a steel material containing, by weight percent, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, with the remainder being Fe and unavoidable impurities; finish rolling the steel material to form a wire rod; winding the wire; the coiled wire is drawn and then heat-treated for spheroidization; forming the spheroidized heat treated wire into a part; and The method of claim 1, further comprising the step of quenching the part after austenitizing the part.
5. The finish rolling is carried out at 880 to 980°C, The method for producing a steel part with improved delayed fracture resistance according to claim 4, wherein the coiling is carried out at a temperature of 830 to 930°C.
6. 5. The method for producing a steel part having improved delayed fracture resistance according to claim 4, wherein the spheroidizing heat treatment is performed at a maximum temperature in the range of 745 to 765°C.
7. The method for producing a steel part with improved delayed fracture resistance according to claim 4, characterized in that the austenitization is carried out at a temperature of 870 to 940°C.
8. The method for producing a steel part with improved delayed fracture resistance according to claim 4, characterized in that the quenching is carried out with a coolant at 10 to 80°C.
9. The steel contains, by weight, C: 0.18% or more and 0.25% or less, Si: 0.30% or more and 0.50% or less, Mn: 0.35% or more and 0.50% or less, P: more than 0% and 0.03% or less, S: more than 0% and 0.03% or less, Cr: 0.45% or more and 0.60% or less, Ti: 0.015% or more and 0.03% or less, B: 0.001% or more and 0.004% or less, and the remainder being Fe and unavoidable impurities, A wire rod for cold forging having improved delayed fracture resistance, characterized in that the wire rod has a diameter of 5.5 to 20 mm.
Citation Information
Patent Citations
Wire rod for cold forging and its manufacture
JP2000336457A
Hot forming method, and hot-formed member
JP2004353026A
Hot-pressed steel sheet member, manufacturing method therefor and steel sheet to be hot-pressed
JP2006152427A
High-strength steel sheet and manufacturing method therefor
JP2009203550A
Spring steel, spring steel wire and spring
JP2012132097A