Precipitation Hardening Powder Metal Compositions
A powder metal composition with specific alloying elements and ceramic additives addresses the challenge of replicating the microstructure and mechanical properties of forged 6013 aluminum alloy, achieving comparable performance through compaction, sintering, and heat treatment, with hot swaging further enhancing properties.
Patent Information
- Application Number
- JP2024533006
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-03
- Filing Date
- 2022-07-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-29
AI Technical Summary
Existing powder metal processes struggle to replicate the microstructure and mechanical properties of forged 6013 aluminum alloy, leading to porosity and inferior material properties in sintered parts.
A powder metal composition is developed that includes aluminum-based powders with specific alloying elements like silicon, copper, and magnesium, optionally with manganese and tin, and can be compacted, sintered, and heat treated to achieve properties comparable to wrought 6013 aluminum alloy, with the addition of ceramic additives for improved wear resistance and strength.
The composition achieves sintered parts with densities exceeding 95% of theoretical density, showing mechanical properties such as Young's modulus, yield strength, and ultimate tensile strength comparable to forged 6013 aluminum alloy, particularly when combined with hot swaging and appropriate heat treatments.
Smart Images

Figure 2024544011000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of the filing date of U.S. Provisional Patent Application No. 63 / 285,804, entitled "Precipitation Hardening Powder Metal Compositions," filed on December 3, 2021, and claims the benefit of the filing date of U.S. Provisional Patent Application No. 63 / 285,871, entitled "Hot Deformation Treatment of Precipitation Hardening Powder Metal Alloys," filed on December 3, 2021, which are incorporated by reference herein for all purposes as if set forth in their entireties herein.
[0002] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT Not applicable.
[0003] The present disclosure relates to powder metallurgy formulations and sintered parts produced therefrom. In particular, the present disclosure relates to powder metal compositions that are replacements for wrought 6013 aluminum alloy. [Background technology]
[0004] 6013 aluminum alloy is a precipitation hardened aluminum alloy containing magnesium (Mg) and silicon (Si) as the primary alloying elements. It has excellent mechanical properties and weldability, and also has good corrosion resistance. This combination of properties makes it one of the most widely used aluminum alloys. Aluminum 6013 is used in a wide range of applications, including aerospace parts, automotive parts, valve parts, machine parts, munitions, braking systems, and hydraulic applications. As used herein, the composition of 6013 aluminum alloy should be understood to mean, in weight percent, 94.8%-97.8% aluminum, 0.8%-1.2% magnesium, 0.60%-1.0% silicon, 0.60%-1.1% copper, 0.20%-0.80% manganese, 0.50% or less iron, 0.25% or less zinc, 0.10% or less chromium, and 0.10% or less titanium, with the remaining elements each being 0.050% or less and totaling 0.15% or less.
[0005] In alloy 6013, magnesium and silicon are the basis for the heat treatment of this system, forming the Mg2Si intermetallic phase which improves the mechanical properties. Copper also contributes to the improvement of mechanical properties. Iron is present as an impurity and forms various intermetallic phases which affect corrosion and mechanical properties.
[0006] There are many methods for forming metal parts, but Powder Metal or "PM" processes represent one class of manufacturing technology for forming metal parts. Powder metallurgy generally involves producing or obtaining powdered metal material, compressing this powdered metal material with a tool and die set to form a green compact or preform that approximates the shape of the desired end product, and then sintering the green compact so that the powdered metal particles diffuse into each other and densify into a mechanically stronger body. Powder metallurgy is suitable for mass production of parts, has low scrap costs, and has the advantage of producing parts that do not require machining after forming.
[0007] While this is only a general overview of powder metal manufacturing processes, it can be seen that many of the powder metal processes are typically performed in the solid state or have limited amounts of liquid formed during the sintering process. However, it also highlights some of the challenges in using powder metal processes, since sintering is a diffusion dependent process and the resulting microstructure and porosity are a function of the powder formulation and processing conditions. Thus, when attempting to convert a wrought or cast alloy to a powder metal formulation, challenges can arise in creating a comparable microstructure and providing comparable mechanical properties. Summary of the Invention
[0008] Currently, there is no powder metal equivalent of a cast "wrought" 6013 aluminum alloy. From the Background section above, it can be seen that many such wrought alloys cannot be produced simply by combining various elemental powders, because the powder metal process relies on diffusion and the resulting morphology may not be comparable, for example, to a cast part with an otherwise similar chemical composition. Furthermore, because powder metal parts are made of various particles sintered together, there is usually some porosity after a conventional sintering process, which can adversely affect material properties compared to a fully dense part.
[0009] Disclosed herein is a powder metal composition that is comparable to wrought 6013 aluminum alloy. This powder metal 6013 aluminum alloy adds another potential alloy to the toolbox of materials that can be used in new applications and may open the door to parts made from powder metal that have previously been limited to wrought alloy production. Such an alloy would be particularly useful for the production of electric vehicle parts. Additionally, the 6013 powder metal composition and parts made therefrom can be supplemented with metal matrix composite (MMC) additives to improve wear resistance and strength.
[0010] According to one embodiment, the powder metal compositions are compacted, sintered, and heat treated to provide a powder metal material comparable to wrought 6013 aluminum alloy. The powder metal compositions include aluminum-based powder metals (defined herein as powder metals that contain pure aluminum with no significant alloying elements or that have alloying elements that are 2% or less by weight of the aluminum-based powder metal), aluminum-silicon powder metal, aluminum-copper powder metal, and elemental magnesium powder metal. The weight percentage of silicon in the powder metal composition is in the range of 0.6-1.0% by weight of the powder metal composition, the weight percentage of copper in the powder metal composition is in the range of 0.7-1.1% by weight of the powder metal composition, and the weight percentage of magnesium in the powder metal composition is in the range of 0.8-1.2% by weight of the powder metal composition.
[0011] In some embodiments, the aluminum-based powder metal may be pure aluminum with no significant alloying elements pre-alloyed to the aluminum-based powder metal. In this embodiment, the powder metal composition may further include elemental tin powder metal, and the weight percentage of tin in the powder metal composition may be within the range of 0.2% to 1.0% by weight of the powder metal composition. In some embodiments, the weight percentage of silicon in the powder metal composition is more narrowly within the range of 0.7-0.9% by weight of the powder metal composition, the weight percentage of copper in the powder metal composition is more narrowly within the range of 0.8-1.0% by weight of the powder metal composition, the weight percentage of magnesium in the powder metal composition is more narrowly within the range of 0.9-1.1% by weight of the powder metal composition, and the weight percentage of tin in the powder metal composition is more narrowly within the range of 0.4-0.6% by weight of the powder metal composition, with the remainder of the powder metal composition being aluminum with only trace amounts of other ineffective alloying elements added. More specifically, in one particular embodiment, in the powder metal composition, the weight percentage of silicon in the powder metal composition can be 0.8% by weight of the powder metal composition, the weight percentage of copper in the powder metal composition can be 0.9% by weight of the powder metal composition, the weight percentage of magnesium in the powder metal composition can be 1.0% by weight of the powder metal composition, and the weight percentage of tin in the powder metal composition can be 0.5% by weight of the powder metal composition.
[0012] In some embodiments, the aluminum-based powder metal may be aluminum powder metal pre-alloyed with manganese such that the weight percentage of manganese in the powder metal composition is within the range of 0.2-1.2 wt.% of the powder metal composition. In this embodiment, the weight percentage of manganese in the powder metal composition may be more narrowly within the range of 0.4-0.6 wt.% of the powder metal composition. More specifically, in one particular embodiment, in the powder metal composition, the weight percentage of manganese in the powder metal composition may be 0.5 wt.% of the powder metal composition. When the aluminum-based powder metal is pre-alloyed aluminum powder metal alloyed with manganese, the powder metal composition further comprises elemental tin powder, and the weight percentage of tin in the powder metal composition may be within the range of 0.2 wt.% to 1.0 wt.% of the powder metal composition, and may be targeted to about 0.5 wt.%.
[0013] In various forms, the aluminum-based powder metal, and whether it is pure or pre-alloyed, the powder metal composition can further include elemental tin powder, with the weight percentage of tin in the powder metal composition being in the range of 0.2-1.0% by weight of the powder metal composition, and can be targeted to about 0.5% by weight.
[0014] In some forms, the aluminum-silicon powder metal may be an Al-12Si master alloy powder metal (about 88% aluminum and 12% silicon by weight) and the aluminum-copper powder metal may be an Al-50Cu master alloy powder metal (about 50% aluminum and 50% copper by weight).
[0015] In some embodiments, the powder metal composition further includes a lubricant, and the weight percentages of the alloying elements do not include the weight of the lubricant, which may be the case if the lubricant is configured to burn off during sintering of the powder metal composition.
[0016] In some embodiments, the powder metal composition may further include a ceramic powder additive to provide a metal matrix composite upon sintering. The ceramic powder additive may be less than 15 volume percent of the powder metal, and the weight of the ceramic powder is not considered when calculating the weight percent of the alloying elements. The ceramic powder additive may have a specific surface area of 2.0 m 2 The specific surface area of the aluminum nitride may be 1.8 to 3.8 m / g or less, and the particle size distribution may be 0.4 to 1.4 μm at D10%, 6 to 10 μm at D50%, and 17 to 35 μm at D90%. 2 / g, with particle size distributions of 0.2-0.6 μm at D10%, 1-3 μm at D50%, and 5-10 μm at D90%. Aluminum nitride (AlN) has a hexagonal crystal structure and is single phase. In some forms, the ceramic additive is silicon carbide (SiC). Beta silicon carbide is a synthetic SiC with a diamond-like cubic structure and has excellent physical and chemical properties. The Mohs hardness of β-SiC is second only to diamond at 10 on the Mohs hardness scale. In addition to high hardness, β-SiC is characterized by chemical stability, thermal conductivity, and a low coefficient of thermal expansion. In one embodiment, the amount of ceramic powder added in the powder metal composition is 2 vol.% β-SiC with an upper limit of 10 vol.% based on the total volume of the powder metal composition.
[0017] In some embodiments, the flow rate of the powder metal composition will be in the range of 2.0-3.0 g / s, which may indicate the powder morphology in ways that other parameters of the powder metal do not.
[0018] According to another aspect, a green compact may be formed (e.g., by compaction) from any of the powder metal compositions described above and herein. Similarly, a sintered powder metal part may be formed (e.g., by sintering) from such green compact. The sintered density of the sintered powder metal part may be greater than 95% of the theoretical density. Furthermore, the sintered powder metal part may have a Young's modulus of 61 GPa to 77 GPa, a yield strength of 324 MPa to 344 MPa, and an ultimate tensile strength (UTS) of 324 MPa to 379 MPa that have been sintered, solutionized, water quenched, aged, and air cooled in a T6 process.
[0019] These and other advantages of the present invention will become apparent from the detailed description and drawings. The following is merely a description of some preferred embodiments of the present invention. To assess the full scope of the present invention, reference should be made to the claims, as these preferred embodiments are not intended to be the only embodiments within the scope of the claims. [Brief description of the drawings]
[0020] [Figure 1A-1B] 1A and 1B are scanning electron microscope (SEM) images of the various powders used in the production of the 6013 powder metal variants. Figures 1A and 1B are SEM images of the base aluminum powder used in the powder metal 6013 variants. Figure 1A is an image of pre-alloyed Al-0.6Mn powder metal, and Figure 1B is an image of pure aluminum powder. [Fig. 1C-1D] Figures 1C and 1D are scanning electron microscope (SEM) images of the various powders used in the production of the 6013 powder metal variants. Figures 1C and 1D are SEM images of alloying additions, including elemental Mg powder metal in Figure 1C and Al-12Si master alloy powder metal in Figure 1D. [Fig. 1E-1F]Figures 1E and 1F are scanning electron microscope (SEM) images of the various powders used in the production of the 6013 powder metal variants. Figures 1E and 1F are SEM images of the alloying additions, including elemental tin powder in Figure 1E and Al-50Cu master alloy powder metal in Figure 1F. [Figure 2A-2B] Figures 2A and 2B are SEM images of the sintered microstructures of PM6013-Mn in Figure 2A and PM6013-Mn-Sn in Figure 2B. The specific powder metal formulations in both compositions and powder blends designated PM6013-Mn and PM6013-Mn-Sn are provided in the detailed description below. [Fig. 2C-2D] Figures 2C and 2D are SEM images of the sintered microstructures of PM6013 in Figure 2C and PM6013-Sn in Figure 2D. The specific powder metal formulations in both compositions and powder blends designated PM6013 and PM6013-Sn are provided in the detailed description below. [Figure 3A-3B] Figures 3A and 3B are SEM images of the sintered and swaged microstructures of powder metal 6013 and Al-0.6Mn+0.5 wt. % Sn powder metal (i.e., PM6013-Mn-Sn) in the as-sintered and swaged states, respectively. [Figure 3C-3D] Figures 3C and 3D are SEM images of the sintered and swaged microstructures in the as-swaged state, with Figure 3C being the powder metal 6013 using Al-0.6Mn+0 wt% Sn powder metal (i.e., PM6013-Mn) and Figure 3D being the powder metal 6013 using Al-0.6Mn+0.5 wt% Sn powder metal (i.e., PM6013-Mn-Sn). [Fig. 3E-3F]Figures 3E and 3F are SEM images of the sintered and swaged microstructures in the as-swaged state, with Figure 3E being the SEM image of powder metal 6013 using pure Al + 0 wt% Sn powder metal (i.e., PM6013) and Figure 3F being the SEM image of powder metal 6013 using pure Al + 0.5 wt% Sn powder metal (i.e., PM6013-Sn). [Figure 4A-4B] 4A and 4B are differential scanning calorimetry (DSC) heating traces obtained from 6013 powder metal variants, with FIG. 4A showing the DSC heating trace for PM6013-Mn and FIG. 4B showing the DSC heating trace for PM6013-Mn-Sn. [Fig. 4C-4D] 4C and 4D are differential scanning calorimetry (DSC) heating traces obtained from the 6013 powder metal variants, with FIG. 4C showing the DSC heating trace of PM6013 and FIG. 4D showing the DSC heating trace of PM6013-Sn. [Figure 5A-5B] Figures 5A and 5B are T6 age data for 6013 powder metal variants. Samples were sintered, hot swaged, and then solution treated at 540°C for Figure 5A and 560°C for Figure 5B, then water quenched and aged at 190°C. [Figure 5C] Figure 5C is the T6 age data for the 6013 powder metal variant. The sample was sintered, hot swaged, and then solution treated at 580°C in Figure 5C, then water quenched and aged at 190°C. [Figure 6A-6B] 6A and 6B show the SEM images of the microstructures of PM6013 variants processed by the sinter-swage-T6 sequence, respectively, including PM6013-Mn in Fig. 6A and PM6013-Mn-Sn in Fig. 6B. [Figure 6C-6D] 6C and 6D show the SEM images of the microstructures of PM6013 variants processed by sinter-swage-T6 sequence, respectively, including PM6013 in Fig. 6C and PM6013-Sn in Fig. 6D. [Figure 7A-7B]Figures 7A and 7B are T8 aging data for powder metal 6013 variants where the samples were sintered, hot swaged, solution annealed at 560°C, water quenched, cold worked, and then aged for the specified times at 190°C. Figure 7A is the T8 aging data for PM6013-Mn, and Figure 7B is the T8 aging data for PM6013-Mn-Sn. [Figure 7C-7D] Figures 7C and 7D are T8 aging data for powder metal 6013 variants where the samples were sintered, hot swaged, solution annealed at 560°C, water quenched, cold worked, and then aged for the specified times at 190°C. Figure 7C is the T8 aging data for PM6013 and Figure 7D is the T8 aging data for PM6013-Sn. [Figure 8A-8B] 8A and 8B show the microstructures of PM6013 variants processed by the sinter-swage-T8 sequence, including PM6013-Mn in FIG. 8A and PM6013-Mn-Sn in FIG. 8B. [Fig. 8C-8D] 8C and 8D are the microstructures of PM6013 variants processed by the sinter-swage-T8 sequence, including PM6013 in FIG. 8C and PM6013-Sn in FIG. 8D. [Figure 9A-9B] Figures 9A and 9B are graphs showing the tested mechanical properties of PM6013 variants across a range of conditions and alloys, with Figure 9A showing Young's modulus values ("E value") and Figure 9B showing elongation to break values. [Fig. 9C-9D] Figures 9C and 9D are graphs showing the tested mechanical properties of PM6013 variants across a range of conditions and alloys: Figure 9C shows the 0.2% offset yield value, and Figure 9D shows the ultimate tensile strength (UTS). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The powder metal compositions disclosed herein are comparable to the composition of aluminum alloy 6013. Below, exemplary powder metal compositions and several variations thereof are disclosed.
[0022] Four alloys were considered as powder metal counterparts of the wrought 6013 aluminum alloy. All of these have the same concentrations of magnesium, silicon, and copper. Alloy variations were prepared with and without pre-alloyed manganese and mixed tin. Manganese is used in wrought 6031 and was found in two of the four variations. Two variations without manganese were also prepared, as pre-alloying the aluminum often increases the yield strength of the powder metal and can complicate the compaction behavior of the die. For each of the manganese-containing and manganese-free formulations, the addition of tin was also considered, with one formulation containing no tin and the other containing a trace amount of 0.5 wt% tin. Tin was considered because it helps catalyze the densification reaction of powder metal alloys.
[0023] These four variant compositions were designated PM6013-Mn, PM6013-Mn-Sn, PM6013, and PM6013-Sn, and the compositions of each system are shown in Table 1, with all percentages referring to the weight percent of the total powder metal weight (excluding lubricant). [Table 1]
[0024] The PM6013-Mn and PM6013-Mn-Sn compositions were Al-0.6Mn powder metal (0.6 wt.% manganese pre-alloyed with aluminum, with the remainder of the Al-0.6Mn powder (approximately 99.4 wt.%) being aluminum) [D 50 = 103 μm], Al-12Si powder metal (master alloy powder with 12 wt.% Si and the remainder aluminum) [D 50 = 33 μm], Al-50Cu (master alloy powder with 50 wt. % Cu and the remainder aluminum) [D 50 = 31 μm], and magnesium individual mixed elemental powder metal [D 50 = 31 μm], and in the case of PM6013-Mn-Sn compound, tin [D 50 = 4 μm]. The PM6013 and PM6013-Sn compositions were made from a mixture of pure aluminum powder metal [D50 =116μm] to Al-12Si powder metal [D 50 =33μm], Al-50Cu powder metal [D 50 = 31 μm], and magnesium [D 50 = 31 μm] of separate mixed elemental powder metal additives (tin [D 50 = 4 μm]. All powders were manufactured by Kymera International (Raleigh, NC), except for the elemental magnesium powder, which was manufactured by inert gas atomization by Tangshan Weihao Magnesium Powder Company Ltd. (Qian'an, Hebei, China). In all formulations, the various powder metal constituents were combined in ratios and proportions to achieve the target composition, and although the exact powder quantities are not given here, given the powder metal "ingredients" listing for each formulation or variant, it is easy to work backwards to find the exact powder metal percentages that were combined in each case.
[0025] 1A through 1F, scanning electron microscope images of the various powder metals mixed to create these alloy compositions are shown: Figure 1A shows powder metal Al-0.6Mn, Figure 1B shows pure aluminum, Figure 1C shows elemental magnesium, Figure 1D shows Al-12Si, Figure 1E shows elemental Sn, and Figure 1F shows Al-50Cu (50% Cu by weight, balance aluminum).
[0026] For each powder metal composition, 1.5 wt.% LicoWax® C (available from Clariant Corporation, Louisville, Kentucky) was added to all mixes to facilitate compaction. LicoWax® C is a lubricant / wax that helps hold the powder particles together to hold the compacted green part together, and also aids in the removal of the green part from the tool and die set after compaction. The lubricant typically burns off during the sintering process in the preheat zone. Therefore, the alloy percentages listed above should be understood to be 100% of the powder metal, as this 1.5 wt.% is based on the powder metal component itself being 100 wt.%, and the powder metal component plus the lubricant is actually 101.5 wt.%.
[0027] It is further envisioned that these 6013 powder metal variants can be used to provide ceramic additives of up to 15% by volume to create metal matrix composites that provide improved wear and strength. The primary additive being explored for the 6013 powder metal variants is Aluminum Nitride (AlN), although Silicon Carbide (SiC) is another ceramic additive being explored as a viable additive.
[0028] With respect to aluminum nitride (AlN) MMC additives, these aluminum nitride additives may be, for example, grade AT aluminum nitride (agglomerated powder with a broader particle size distribution) or grade BT aluminum nitride (non-agglomerated powder with a relatively finer particle size). Both grades may be used in the disclosed powder metal formulations, depending on the processing and properties.
[0029] Both AT and BT grades of aluminum nitride are single phase with a hexagonal crystal structure. To characterize the chemical content of these aluminum nitride additives, the mass fractions of both AT and BT grades are 32.0% minimum N, 0.15% maximum C, and 0.05% maximum Fe. However, the AT grade contains 1.3% maximum O, while the BT grade contains 1.5% maximum O. The specific surface area of the AT grade is 2.0 m2 / g or less, whereas the specific surface area of the BT grade is 1.8 to 3.8 m 2 / g. The particle size distribution of the two different grades is shown in Table 2 below. [Table 2]
[0030] Aluminum nitride as an MMC additive improves the wear, ductility and thermal conductivity of powder metal formulations. Tool wear is minimized compared to traditional MMC additives such as Al2O3 and SiC.
[0031] In some embodiments, the ceramic additive can be silicon carbide (SiC). Beta silicon carbide is a synthetic SiC with a diamond-like cubic structure, which has excellent physical and chemical properties. β-SiC has a Mohs hardness rating of 10, second only to diamond on the Mohs hardness scale. In addition to its high hardness, β-SiC is characterized by good chemical stability, high thermal conductivity, and a low coefficient of thermal expansion. In one embodiment, the ceramic powder additive in the powder metal composition is 2% by volume of β-SiC, with an upper limit of 10% by volume, based on the total volume of the powder metal composition.
[0032] If a ceramic additive is used, the powder metal, aluminum nitride or other ceramic additive, and lubricant are mixed during powder preparation, preferably in a high intensity mixer, to uniformly distribute the various particles, especially fine particles, throughout the powder metal composition mixture and to avoid segregation.
[0033] The following methods were used for alloy preparation and manufacturing of the powder metal samples investigated:
[0034] First, the starting powders were mixed in the appropriate proportions using a Turbula shaker mixer. The alloying additives were added sequentially to the required base aluminum powder, applying a mixing time of 30 minutes between each addition. Apparent density was assessed for each mix using an Arnold Meter according to MPIF Standard 48, and flow characteristics were measured by passing 25g of each powder mix through a Carney Apparatus, giving the values in Table 3 below. [Table 3]
[0035] The alloys containing manganese had higher apparent density and lower flow rates compared to those prepared using pure aluminum as the base powder. Both of these responses may be related to the morphology of the base aluminum powder. The powder pre-alloyed with manganese (Figure 1A) had a spherical morphology, whereas the unalloyed base powder (Figure 1B) had an irregular shape. Particles with irregular morphology will experience greater interparticle friction. Higher interparticle friction will result in greater separation between particles, fewer particles per unit volume, and lower apparent density. By this principle, the flow rates of PM6013 and PM6013-Sn should be slower than the manganese-containing alloys, but in fact they are slightly faster. This may be due to the slightly coarser particle size of the pure aluminum base powder, which allows the particles to flow more efficiently.
[0036] The addition of tin was found to have no statistically significant effect on flow rate, but did increase apparent density. Since tin is a relatively heavy element (118.7 g / mol), even small additions can increase the density of lightweight aluminum alloys to a significant extent. For example, as shown in Table 4 below, the addition of 0.5 wt.% tin increased the calculated theoretical density by 0.09 g / cc (approximately 3.3%). A somewhat similar increase was observed in the apparent density values, so the results are believed to be primarily a direct reflection of the heavy element addition.
[0037] Once the powder metal was prepared, samples were die pressed at 220 MPa using an Instron 5594-200HVL test frame with a target green density of 2.50 g / cc for the green compact. Three different sample geometries were produced. These were a transverse rupture strength (TRS) sample (nominal 31.7 mm x 12.7 mm x 9.7 mm), a Charpy sample (nominal 75 mm x 10 mm x 10 mm), and a larger rectangular sample (nominal 20 mm x 92 mm x 10 mm). Green density was determined using a "wet" approach in accordance with MPIF Standard 42. Green strength was determined using the three-point bend method outlined in MPIF Standard 15. Both were completed using TRS bars.
[0038] The compression response of various variations of 6013 powder metal is shown below in Table 4. For each formulation, the theoretical density of each composition is given first, followed by the measured green strength and green density (as a percent of theoretical density). [Table 4]
[0039] The addition of tin did not have a statistically significant effect on these properties of the green compacts, but significant differences were observed for systems using pre-alloyed manganese. PM6013 and PM6013-Sn showed an approximately four-fold increase in green strength over their manganese-containing counterparts. As with flowability and apparent density, this difference is believed to be due to the morphology of the base powder particles. Particle shape can be a factor influencing the green strength of the compacts, and the spherical shape of the manganese-prealloyed base powder may limit surface contact between particles and result in poor green strength. In contrast, the irregular shape of the unalloyed aluminum base powder may provide more opportunities for mechanical interlocking of the particles during compaction, resulting in higher green strength. Pre-alloying the base powder with manganese further enhances this effect by strengthening the spherical particles, making them more resistant to the plastic deformation required for interlocking.
[0040] These samples were then sintered in a three-zone Lindberg tube furnace under flowing high purity (99.999%) nitrogen gas. Prior to heating, the samples were evacuated multiple times (10 -2 The furnace atmosphere was adjusted by a sequence of 1000 psi (3000 psi) (torr) and backfill, after which a static gas flow rate of 9.4 liters / min was maintained for the duration of the sintering cycle. The thermal profile of the sintering furnace was 420°C for 20 minutes for desliding and 630°C for 30 minutes for sintering for the TRS and Charpy samples. The larger rectangular bars were held at 630°C for 50 minutes to ensure complete sintering. After the sintering time had elapsed, the samples were gas quenched by sliding them into the water jacketed end of the tube furnace and cooled to ambient temperature under nitrogen. The TRS samples were used to monitor the general sintering behavior of the alloy. Data was compiled on sintered density, dimensional change, and mass change caused by sintering. Measurements of width, length, overall length (OAL) or thickness of each sample before and after sintering were taken to quantify the dimensional change. Sintered density was evaluated using the oil penetration Archimedes method according to MPIF Standard 42. Density measurements were reported as a percentage of the theoretical full density calculated for the alloy using a method specified by the Aluminum Association. This data is reported in Table 5 below. [Table 5]
[0041] All alloys showed a mass loss of about 1.5 wt.%, corresponding to the lubricant boiling off and evaporating during sintering, but there was considerable variation in sintered density and compact warpage. The manganese-containing alloy variants (PM6013-Mn and PM6013-Mn-Sn) did not respond favorably to sintering. Here, the sintered density was inferior to the green density, and the compacts practically experienced a net expansion in all dimensions. The manganese-free alloys (PM6013 and PM6013-Sn) sintered to a much higher extent. The sintered density of these manganese-free material variants was greater than 96%, a measurable improvement compared to the density of the starting green compacts. This improvement was consistent with the dimensional change, as shrinkage was observed in all directions.
[0042] The addition of tin did not enhance the sintering response of PM6013-Mn, as it both expanded and reduced the sintered density. However, when comparing PM6013 and PM6013-Sn, the sintering response of PM6013 was further improved by the addition of tin. This may be related to the behavior of tin during liquid phase sintering. Since tin has a lower melting point than other alloying additions, it usually forms part of the liquid phase that densifies the compact. Therefore, the addition of tin to PM6013-Mn-Sn and PM6013-Sn was expected to result in a slightly higher fraction of liquid being present during liquid phase sintering of these alloys than in PM6013-Mn and PM6013. A high liquid fraction in liquid phase sintering leads to rapid densification, but dimensional control can become difficult as densification progresses. However, since only small amounts of tin were added, this does not fully explain the observed effect. Aluminum powder necessarily reacts with oxygen to form a thin alumina layer (Al2O3) on the surface of the powder. The increased apparent density of the manganese-containing alloys indicates that the particles are more densely packed, resulting in a higher amount of oxide per unit volume than the manganese-free alloys. The inability of tin to wet alumina is likely responsible for the difference in the sintering response of the two tin-containing alloys.
[0043] Interestingly, the alloys that achieved higher green density, PM6013-Mn and PM6013-Mn-Sn, also had lower sintered densities and therefore lower densities during sintering. In theory, a compact that sintered well should measure higher green densities since density is generally a function of green density. This was not the case here, an unexpected and surprising result. It is instructive to examine the net change in apparent and green density for PM6013-Mn and PM6013-Mn-Sn. PM6013-Mn and PM6013-Mn-Sn have net changes in apparent and green density of 1.2g / cc and 1.1g / cc, respectively. In contrast, PM6013 and PM6013-Sn show slightly higher net changes of 1.3g / cc and 1.4g / cc, respectively. This indicates that there was less material movement in the compression of PM6013-Mn and PM6013-Mn-Sn than in the compression of the manganese-free alloys. This suggests that the particles were not bonded mechanically as effectively, which is also seen in the relatively low green strengths of these two alloys. The material movement also serves to break down the oxide film on the powder and provide sites for metal-to-metal mechanical bonding. With less material movement, fewer sites of metal-to-metal contact are established between the particles, which can inhibit sintering. The increased interparticle contact of PM6013 and PM6013-Sn allows these alloys to sinter more efficiently.
[0044] The difference between these two sintering responses was particularly pronounced microstructurally, as shown in Figures 2A-2D.
[0045] The as-sintered microstructures observed by scanning electron microscopy are shown in Figures 2A-2D. Figure 2A corresponds to PM6013-Mn, Figure 2B corresponds to PM6013-Mn-Sn, Figure 2C corresponds to PM6013, and Figure 2D corresponds to PM6013-Sn. All of these samples are shown in the as-sintered state without swaging. For microstructural evaluation, the specimens were hot mounted in conductive epoxy and then polished using a Struers Tegramin semi-automatic polisher. Standard polishing media such as silicon carbide paper, diamond paste, and colloidal silica were used. Optical microscopy was performed using a Zeiss Axiotech upright microscope and a Keyence VK-X1000 laser confocal microscope (optical mode). Electron microscopy was performed using a Hitachi S-4700 cold field emission scanning electron microscope (SEM) operated at an accelerating voltage of 20 kV and a beam current of 20 mA. Energy dispersive spectroscopy (EDS) was performed using an Oxford Instruments X-Max 80mm 2 This was carried out using an EDS detector.
[0046] Alloys PM6013-Mn (Figure 2A) and PM6013-Mn-Sn (Figure 2B) were found to have poor sintering quality. Evidence of the morphology of the starting powders remained and the microstructure showed many irregular and interconnected pores (black features). These factors indicate that sintering bonding was achieved only at an early stage.
[0047] In contrast, the samples produced without manganese (PM6013 (Figure 2C) and PM6013-Sn (Figure 2D)) were sintered with much higher quality: the raw powder particles were no longer visible and the few remaining pores were rounded and discontinuous.
[0048] Sintered bars of each alloy were then processed by hot swaging. The sintered rectangular samples were processed into cylindrical shapes (18 mm diameter, 90 mm length), preheated to 485°C, and then hot swaged in a laboratory-scale apparatus, using multiple passes through successively smaller dies until a final diameter of 12.7 mm was achieved, resulting in an approximately 50% reduction in area for a 2:1 extrusion ratio. The samples were reheated at 485°C for 5 min between each pass.
[0049] Macroscopically, the response of all alloys was good and no visible defects were observed in the finished parts after swaging, considering Figures 3B-3F, which show the various microstructures after swaging. Microstructurally, the effect of swaging was immediately evident in the manganese-containing alloys when comparing the microstructures before swaging (e.g., Figures 2A, 2B, 3A) with those after swaging (e.g., Figure 3B). The swaging process closed most of the porosity that remained in the sintered material. The pores that remained were smaller and less continuous. For clarity, Figure 3A shows only the sintered PM6013-Mn-Sn sample, while Figure 3B shows a comparison of the sintered and swaged PM6013-Mn-Sn samples. 3C-3F show images of the sintered and swaged microstructures of PM6013-Mn (FIG. 3C), PM6013-Mn-Sn (FIG. 3D), PM6013 (FIG. 3E), and PM6013-Sn (FIG. 3F).
[0050] From Figures 3B-3F above, it can be seen that swaging was performed on all Powder Metal 6013 variants. Qualitative observations indicated that all alloy formulations swaged well and were free of external cracks or fissures. Additionally, swaging homogenized the microstructures. All microstructures were dominated by white alpha aluminum grains and there was no evidence of coarsening of secondary grain boundary phases as a result of the heat applied during hot swaging. A small fraction of residual porosity remained in all microstructures, consistent with swaged density measurements. The residual porosity was observed to be primarily grain boundary in nature.
[0051] When viewed longitudinally, the grains are elongated in the direction of swaging, similar to industrial extrusion processes, and there is also evidence of metal flow when viewed at the edges of the microstructure, as would be expected from hot deformation processes.
[0052] To further characterize the differences between the "as sintered" and "as swaged" samples, the as swaged density of each formulation was collected and compared to the as sintered density (the average sintered density for each formulation is also shown in Table 5 above). These are shown in Table 6 below, again expressed as a percent of the theoretical density for the particular formulation. [Table 6]
[0053] From Table 6 above, it can be seen that the density of all swaged powder metal alloy compositions was improved by swaging, including the sample containing Al-0.6Mn, which did not show densification upon sintering. The swaged sample made with Al-0.6Mn powder metal (as opposed to a combination of pure aluminum and elemental magnesium) was slightly longer due to more porosity being closed. No significant differences in the swaging response of the alloys were observed among the four swaged powder metals. The average swaged densities were all greater than 99% of the theoretical density, with the two samples made with pure aluminum being slightly closer to the theoretical density than the two samples made with Al-0.6Mn, which may be due in part to the higher starting density before swaging.
[0054] The sintered densities of PM6013 and PM6013-Sn were significantly higher, so the differences in microstructure before and after swaging were less pronounced. However, the amount of residual porosity in each alloy was measurably reduced, and all materials had densities above 99% of the theoretical value after swaging. Specifically, the swaged densities of PM6013 and PM6013-Sn were 99.5% and 99.4% of the theoretical value, respectively. In contrast, the densities of PM6013-Mn and PM6013-Mn-Sn were both slightly lower, at 99.1%. The slight improvement measured for PM6013 and PM6013-Sn is due to their higher sintered densities (see Table 5) and, at the same time, significantly less residual porosity to be removed.
[0055] As wrought 6013 is a heat treatable alloy, the effects of the T6 and T8 processes on variants of PM6013 were also investigated. Both begin with a solutionizing stage whose main purpose is to dissolve precipitate forming elements into solid solution. Establishing the appropriate temperature for this step is important and is frequently investigated using Differential Scanning Calorimetry (DSC). DSC testing provides data on the melting behavior of the alloy, which can guide the study of the appropriate solutionizing temperature range.
[0056] Therefore, the melting behavior of the swaged specimens was evaluated using a Netzsch 404 F1 differential scanning calorimeter. Temperature and sensitivity calibrations were performed before testing. All tests were carried out under a controlled atmosphere with high purity nitrogen gas flowing at 50 ml / min. Circular samples were machined from the swaged rods (4 mm diameter, 2 mm thickness). The samples were heated to 700 °C at a rate of 20 °C / min and then cooled to ambient temperature at the same rate.
[0057] 4A-4D, differential scanning calorimetry data in the form of heat flux traces for samples made from 6013 powder metal variants are provided over the range 100° C.-700° C. under controlled atmosphere. As previously mentioned, FIG. 4A is PM6013-Mn, FIG. 4B is PM6013-Mn-Sn, FIG. 4C is PM6013, and FIG. 4D is PM6013-Sn.
[0058] The "A" and "B" indicators in these figures indicate melting events at the particular temperatures indicated. It can be seen that two melting events are observed for PM6013-Mn-Sn and PM6013-Sn, but only one melting event is observed for PM6013-Mn and PM6013. All plots show a primary melting event, labeled "A". The peak magnitude was relatively consistent throughout the alloy, beginning at approximately 580°C. This event was likely to have corresponded to the overall melting of the alloy as the temperature increased through the semi-solid state. The heat traces of the tin-containing alloys (Figures 4B and 4D) contained a smaller secondary event (peak B) that occurred between approximately 540°C and 580°C. This is assumed to indicate the initial melting of the tin-containing phase. The heat traces in Figures 4A and 4C also show small variations around the same location as peak "B". This likely indicates that melting did begin in these alloys as well, but the effect was enhanced by the addition of tin, as shown by the clearly higher values of peak "B" in the traces in Figures 4B and 4D.
[0059] The solution temperature itself needs to be higher than the solvus temperature, but usually not so high that partial melting occurs. A typical solution temperature for wrought 6013 is 570°C. This is below the onset of bulk melting, but lies in the central valley of event "B". Therefore, the same temperature cannot be arbitrarily applied to powder metal systems, as it may cause liquid formation and reduce the concentration of alloying elements dissolved in solid solution. Therefore, a series of solution temperature experiments above and below peak B were required. For this purpose, solution tests at 540°C, 560°C, and 580°C were selected.
[0060] Two post-swaging heat treatments were considered: T6 and T8. In the T6 condition, the swaged rods were solution treated in air at 560°C for 2 hours (Lindberg box furnace), water quenched, and then aged at 190°C (Heratherm mechanical convection oven). To achieve the T8 condition, samples underwent the same solution / quench treatment, but were then cold worked to reduce the average thickness by 11%, and then aged at 190°C.
[0061] T6 aging curves were also constructed using the solution treatment temperatures identified by the DSC evaluation and are shown in Figure 5A for the 540°C solution treatment temperature, Figure 5B for the 560°C solution treatment temperature, and Figure 5C for the 580°C solution treatment temperature. All curves showed an increase in hardness to a peak at approximately 5 hours of artificial aging. For all alloys, the lowest hardness measurements were consistently obtained at 580°C, suggesting a microstructure with less precipitate formation. This indicates that the solution treatment temperature was too high. There was little to distinguish between the 540°C and 560°C aging curves. The 560°C aging curve showed less consistency between hardness measurements when compared to the curve made at 540°C. However, when 560°C was used as the solution treatment temperature, the highest hardness measurements were obtained across the alloys during the construction of the aging curves. For convenience and clarity, the peak hardness (T6 at 560° C. solution temperature) in FIG. 5B was 102 HRE for PM6013-Mn, 98 HRE for PM6013-Mn-Sn, 102 HRE for PM6013, and 100 HRE for PM6013-Sn.
[0062] From these results, it was found that the effective T6 heat treatment cycle for all variations was solution treatment at 560°C, followed by water quenching and ageing at 190°C for 5 hours. These heat treatment parameters were used for the remainder of the study.
[0063] SEM images of the samples in the T6 state are shown in Figures 6A-6D. In all cases, a small percentage of residual porosity was evident, as was a secondary grain boundary component. In PM6013-Mn (Figure 6A), the grain boundary structure was light gray, relatively coarse, and in some cases fractured. The latter was likely caused during hot swaging, as no cracks within this structure were observed in the as-sintered micrograph in Figure 2A. EDS analysis showed predominantly aluminum with elevated concentrations of manganese (25 wt%) and silicon (10 wt%). Similar phases were also seen within PM6013-Mn-Sn (Figure 6B), which also showed evidence of fracture. A secondary grain boundary structure was also observed in the alloy. This was brighter than the Mn-containing structure (left image), and was confirmed by EDS to be enriched in tin. As PM6013 contained neither manganese nor tin, the microstructure in Figure 6C did not show any of the previously mentioned grain boundary features. Here, the secondary features were finer and somewhat more uniformly distributed throughout the microstructure. EDS showed mostly aluminum with high and varying concentrations of silicon (4-7 wt%), magnesium (1-2 wt%), and copper (1-4 wt%). In Figure 6D of PM6013-Sn, a tandem of grain boundary features was again seen. One was similar to that seen in PM6013, but this time it contained a small amount of tin (about 1 wt%). The second was brighter and had a higher concentration of tin (47 wt%) and magnesium (22 wt%) with the remainder being aluminum. No evidence of cracking was seen in any of the grain boundary features in PM6013 or PM-6013-Sn.
[0064] The evaluation of the T8 aging response was then completed. Figures 7A-7D show data on hardness as a function of aging time for samples of PM6013-Mn, PM6031-Mn-Sn, PM6013, and PM6013-Sn variants, respectively. The samples were sintered, hot swaged, solution treated at 560 °C, water quenched, cold worked, and aged at 190 °C for the times specified. All alloys were very similar in this respect, with similar peak hardnesses (70-76 HRB), respectively. In general, hardness steadily decreased with aging time beyond the initial period considered (1 h). This behavior indicates that the peak of the curves was likely missed during the aging experiments. However, since all curves showed a relatively gradual slope in the early stages, the difference between the true peak value and that suggested by the data was probably minimal. In this study, 1 h was adopted as the aging time required to achieve the highest hardness with the T8 treatment. From Figures 5A-5C, the samples that underwent T6 treatment exhibited the highest hardness values ranging from 65 to 76 HRB (i.e., 98 to 101 HRE). Thus, the highest values recorded for the T8 samples are quite similar to those achieved by the T6 treatment.
[0065] SEM images were acquired for all samples in the T8 condition and are shown in Figures 8A-8D. PM6013-Mn is shown in Figure 8A, PM6013-Mn-Sn in Figure 8B, PM6013 in Figure 8C, and PM6013-Sn in Figure 8D. In all cases, the T8 microstructure is very similar to the T6 counterpart (Figures 6A-6D). The only difference is in the case of PM6013-Mn, where the cracks are no longer confined to the boundaries of the grain structure but extend throughout the microstructure as sporadic cracks several hundred microns long. This is due to the cold working stage of the T8 process.
[0066] With the heat treatment parameters established, the focus of the study shifted to evaluating the mechanical properties of each alloy system in the T6 and T8 tempers, including the effects of swaging. Mechanical testing included measurements of hardness, tensile properties, and bending fatigue performance. Hardness data was obtained on the Rockwell Hardness E scale (HRE) and Rockwell Hardness B scale (HRB) using a Wilson Rockwell 2000 testing machine. Reported values were taken as the average of four measurements. Tensile properties were evaluated according to ASTM standard E8-M. The swaged rods and Charpy bars were machined into threaded end tensile specimens and then loaded to failure on an Instron 5594-200HVL load frame equipped with a 50 kN load cell and an Epsilon Model 3542 extensometer. The extensometer was attached to each sample until failure. Reported tensile properties for the T6 and T8 samples are average values obtained from three and two test samples, respectively. Flexural fatigue properties were evaluated according to MPIF standard 56, applying the step method, with a step size of 5 MPa under three-point loading conditions. All samples were rectangular (31.7 mm x 12.7 mm x 9.7 mm) and were tested using an Instron 1332 servo-hydraulic frame equipped with an MTS 642 bending fixture that maintained a span of 24.7 mm between the two lower pins. Loads were applied at 25 Hz (R = 0.1) to a runout limit of 106 cycles. 10%, 50% and 90% residual stress values were calculated from the resulting data.
[0067] Tensile properties were obtained for the T6 pressed and sintered (post-sintered), T6 swaged, and T8 swaged parts. This data is summarized graphically in Figures 9A-9D, followed by the table and explanations below. Figures 9A-9D show data comparisons for various measured properties (Figure 9A: Young's modulus, Figure 9B: elongation at break, Figure 9C: offset yield, and Figure 9D: UTS) across various conditions and compositions.
[0068] Various tensile properties of 6013 powder metal were measured on samples that had been processed through the sintering T6 sequence, then solution treated at 560°C for 2 hours, water quenched, aged at 190°C for 5 hours, and air cooled. These tensile properties are listed below in Table 7, which includes a forged 6013 aluminum alloy sample for comparison. [Table 7]
[0069] From the above table, it can be seen that pressed and sintered samples made from 6013 powder metal variations (especially PM6013-Sn) have very similar or nearly equivalent mechanical properties to the forged 6013 aluminum alloy samples. However, it can also be seen that the as-sintered samples (without further swaging) made from Al-0.6Mn (i.e. PM6013-Mn and PM6013-Mn-Sn) have relatively poor mechanical performance. Thus, all powder metal systems performed poorly compared to their forged counterparts, but the differences were most pronounced for those containing pre-alloyed manganese. These materials had exceptionally low values for all properties (Table 5 above) as a direct result of the high levels of residual porosity present in them. In contrast, PM6013 and PM6013-Sn performed better in terms of stiffness and yield strength, with these particular properties being within about 10% of the typical forged values. The UTS of PM6013 was significantly lower than the wrought, but improved for PM6013-Sn. The average tensile ductility of the pressed and sintered samples was approximately 13 times lower than the typical wrought value. This significant difference can be attributed to the presence of residual porosity in all powder metal systems, which is nearly absent in the wrought alloy. Overall, PM6013-Sn exhibited the most desirable T6 tensile properties, supporting the beneficial role of tin.
[0070] By adding a swaging step to the processing sequence, the performance difference between the forged 6013 in Table 7 and all of the powder metal variants shown below in Table 8 was significantly reduced. For ease of comparison, the post-sintered data from Table 7 is copied below and identified as "Pressed & Sintered". [Table 8]
[0071] The improvements in 0.2% offset yield strength and UTS for all powder metals were particularly notable for the swaged parts, with these properties being virtually equivalent to the forged parts. An improvement in ductility was also noted, although none of the powder metal systems achieved net values that matched the forging threshold.
[0072] On average, the swaged T6 powder metal samples exhibited approximately nine times greater ductility than those processed as sintered T6 without swaging.
[0073] Hot swaging reduced the residual porosity levels in all powder metal materials, but did not completely eliminate them. This effect may have been the basis for the significant gains achieved, but it also led to the powder metal systems being unable to maintain ductility comparable to wrought 6013, as the residual porosity served as a crack initiation site, limiting net ductility. Hot swaging likely contributed to the ductility improvement by destroying the semi-continuous oxide network that is also typically present in sintered products. During sintering, the alumina shells at the surface of the raw aluminum powder react with magnesium to form spinel crystallites (MgAl2O3). This brittle ceramic remains throughout the sintered product, reducing tensile ductility. It has been observed that hot forging destroys the spinel network, thereby improving tensile ductility. It is reasonable to assume that the same mechanism is at work here. It is also noteworthy that the fractured grain boundary phase observed in Figures 6A and 6B does not significantly reduce ductility. Other tensile properties are relatively constant for all four alloys. Overall, PM6013-Sn was identified as the powder metal alloy offering the best overall combination of properties, combining the highest ductility with yield strength, UTS, and stiffness values comparable to wrought products.
[0074] Data for PM6013 variants processed with the sinter-swage-T8 sequence (solution treatment at 560°C for 2 hours, followed by water quenching, sizing and ageing at 190°C) are shown in Table 9 below. [Table 9]
[0075] These particular materials showed the highest yield strength and UTS of all the sequences considered, with no significant trends due to the presence or absence of manganese or tin. The higher values are due to a slight decrease in tensile ductility compared to the material that underwent the sinter-swaged T6 process. This decrease can be partly attributed to the cold work stage of the T8 heat treatment, which increases the concentration of dislocations present, leading to strain hardening and a concomitant decrease in ductility. The nature and distribution of precipitates must have changed as a result of the T8 treatment and were also influencing factors. In this sense, cold work could change the rate and extent of hardening, as precipitates nucleate preferentially on dislocations and increase the concentration of precipitates in the microstructure. The additional strengthening brought about by this change could have been accompanied by a decrease in ductility. Overall, the PM6013-Mn had the lowest ductility. This is probably due to a combination of the previously mentioned mechanisms and the cracks seen in the microstructure (Figure 8A).
[0076] It can also be seen that alloys containing pure aluminum in the base aluminum powder are more ductile than alloys in which aluminum has been pre-alloyed into the base aluminum powder (Al-0.6Mn), that alloys containing tin are more ductile than alloys without tin, and that alloys without tin have higher UTS values compared to tin.
[0077] In summary, powder metal 6013 systems processed with the sinter-swage-T6 / T8 sequence performed relatively well compared to wrought 6013. In particular, PM6013-Sn exhibited properties closest to those achieved by forging and outperformed all other powder metal alloys in terms of tensile ductility, regardless of the processing sequence employed. Therefore, the final stage of the fatigue evaluation was focused only on this particular powder metal system.
[0078] Finally, data on the fatigue performance of PM6013-Sn for the three processing sequences considered are presented in Table 10. [Table 10]
[0079] The sintered T6 product showed the lowest resistance to fatigue loading. The inclusion of a hot swaging step (i.e., sintered swaged T6) increased the median bending fatigue strength by 102 MPa (about 68%). This is significant because hot swaging addresses two factors known to have a negative effect on fatigue: residual porosity and the oxide network present. Considering the former, fatigue generally increases exponentially with density, and even a small reduction in the volume fraction of residual porosity can have a significant effect by reducing the number of sites available for crack nucleation and growth. Thus, although the enhancement in density of PM6013-Sn by swaging was relatively small (about 1%), the net effect on fatigue appears to have been decidedly positive. As for the latter, as previously mentioned, the destruction of the oxide network by hot swaging contributed to the improved fatigue resistance, as well as the improved tensile ductility. By dispersing fine particles of the brittle spinel phase throughout the material, the crack nucleation sites are reduced, resulting in further strengthening through the action of mechanisms similar to those present in metal matrix composites.
[0080] The samples obtained with the sintered swaged T8 process also showed a significant improvement over the sintered T6 material (about 43% increase) for the same reasons mentioned above, but were inferior to the sintered swaged T6 product (about 15%). The reduced ductility of the T8 samples observed in the tensile properties is likely to have contributed to these results.
[0081] From the above discussion and disclosure, it can be seen that: First, pre-alloying the base aluminum powder with manganese reduces compaction and sintering behavior. Second, all powder metal alloys based on 6013 responded well to hot swaging as they achieved near theoretical density (>99% of theoretical) without visible defects. Third, the addition of hot swaging to the processing sequence significantly improved the yield strength, UTS, ductility, and fatigue performance of the T6 and T8 tempers. Finally, sintered swaged T6PM6013-Sn was the overall best performing system in terms of response to powder metal processing and mechanical property comparison to wrought 6013-T6. While other variations can certainly be used, this processing route and configuration shows the most promise as a powder metal comparable to wrought 6013.
[0082] It is to be understood that various other modifications and changes can be made to the preferred embodiment within the spirit and scope of the present invention. Accordingly, the present invention should not be limited to the described embodiment. Reference should be made to the following claims to ascertain the full scope of the present invention.
Claims
1. 1. A powder metal composition which can be compacted, sintered and heat treated to provide a powder metal material comparable to wrought 6013 aluminum alloy, comprising: The powder metal composition comprises: an aluminum-based powder metal; aluminum-silicon powder metal; Aluminum-copper powder metal; Elemental magnesium powder metal; Including, the weight percentage of silicon in said powder metal composition is in the range of 0.6 to 1.0 weight percent of said powder metal composition; the weight percent of copper in said powder metal composition is in the range of 0.7 to 1.1 weight percent of said powder metal composition; the weight percentage of magnesium in said powder metal composition is in the range of 0.8 to 1.2 weight percent of said powder metal composition; Powder metal composition.
2. The aluminum-based powder metal is pure aluminum with no significant alloying elements pre-alloyed in the aluminum-based powder metal.
10. The powder metal composition of claim 1.
3. the powder metal composition further comprises elemental tin powder metal; the weight percent of tin in the powder metal composition is between 0.2% and 1.0% by weight of the powder metal composition; 3. The powder metal composition of claim 2.
4. the weight percentage of silicon in said powder metal composition is more narrowly within the range of 0.7 to 0.9 weight percent of said powder metal composition; the weight percent of copper in said powder metal composition is more narrowly within the range of 0.8 to 1.0 weight percent of said powder metal composition; the weight percent of magnesium in said powder metal composition is more narrowly within the range of 0.9 to 1.1 weight percent of said powder metal composition; the weight percent of tin in said powder metal composition is more narrowly within the range of 0.4 to 0.6 weight percent of said powder metal composition; The remainder of the powder metal composition is aluminum with only trace amounts of other ineffective alloying elements.
4. The powder metal composition of claim 3.
5. the weight percent of silicon in said powder metal composition is 0.8 weight percent of said powder metal composition; the weight percent of copper in said powder metal composition is 0.9 weight percent of said powder metal composition; the weight percent of magnesium in said powder metal composition is 1.0 weight percent of said powder metal composition; the weight percent of tin in said powder metal composition is 0.5 weight percent of said powder metal composition; 5. The powder metal composition of claim 4.
6. said aluminum based powder metal being aluminum powder metal pre-alloyed with manganese such that the weight percentage of manganese in said powder metal composition is within the range of 0.2 to 1.2 weight percent of said powder metal composition; 10. The powder metal composition of claim 1.
7. the weight percent of manganese in the powder metal composition is narrower and falls within the range of 0.4 to 0.6 weight percent of the powder metal composition; 7. The powder metal composition of claim 6.
8. the weight percent of manganese in said powder metal composition is 0.5 weight percent of said powder metal composition; 8. The powder metal composition of claim 7.
9. the powder metal composition further comprises elemental tin powder, the weight percentage of tin in the powder metal composition being within the range of 0.2% to 1.0% by weight of the powder metal composition; 7. The powder metal composition of claim 6.
10. the powder metal composition further comprises elemental tin powder, the weight percentage of tin in the powder metal composition being within the range of 0.2% to 1.0% by weight of the powder metal composition; 10. The powder metal composition of claim 1.
11. the aluminum-silicon powder metal is an Al-12Si master alloy powder metal; the aluminum-copper powder metal is an Al-50Cu master alloy powder metal; 10. The powder metal composition of claim 1.
12. the powder metal composition further comprising a lubricant; the weight percentages of alloying elements exclude the weight of the lubricant since the lubricant is configured to combust during sintering of the powder metal composition; 10. The powder metal composition of claim 1.
13. further comprising a ceramic powder additive to provide a metal matrix composite upon sintering; the ceramic powder additive is less than 15 volume percent of the powder metal; The weight of said ceramic powder additives is not taken into account when calculating the weight percentage of the alloying elements.
10. The powder metal composition of claim 1.
14. The ceramic powder additive has a specific surface area of 2.0 m 2 / g or less, and the particle size distribution is 0.4 to 1.4 μm at D10%, 6 to 10 μm at D50%, and 17 to 35 μm at D90%.
10. The powder metal composition of claim 1.
15. The aluminum nitride (AlN) has a specific surface area of 1.8 to 3.8 m 2 / g, and the particle size distribution is 0.2 to 0.6 μm at D10%, 1 to 3 μm at D50%, and 5 to 10 μm at D90%.
15. The powder metal composition of claim 14.
16. The aluminum nitride (AlN) has a hexagonal crystal structure and is single-phase; 15. The powder metal composition of claim 14.
17. the ceramic powder additive is silicon carbide; 14. The powder metal composition of claim 13.
18. the silicon carbide is beta-silicon carbide and is in the range of 2% to 10% by volume of the powder metal, the weight of the ceramic powder additives not being taken into account when calculating the weight percentage of the alloying elements; 20. The powder metal composition of claim 17.
19. The flow rate of the powder metal composition is 2.0 to 3.0 g / sec.
10. The powder metal composition of claim 1.
20. A green compact formed from the powder metal composition of claim 1.
21. 21. A sintered powder metal part formed from the green compact of claim 20.
22. 22. The sintered powder metal part of claim 21 , wherein the sintered density of the sintered powder metal part is greater than 95% of theoretical density.
23. The sintered powder metal part, which has been sintered, solution treated, water quenched, aged, and air cooled to a T6 treatment, has a Young's modulus of 61 GPa to 77 GPa, a yield strength of 324 MPa to 344 MPa, and an ultimate tensile strength (UTS) of 324 MPa to 379 MPa.
22. The sintered powder metal part of claim 21.
Citation Information
Patent Citations
Aluminum alloy powder and manufacturing method of aluminum alloy object
CN108070752A
Aluminium-alloy powder, sintered aluminium-alloy, and method for producing the sintered aluminum-alloy
EP0436952A1
Manufacture of superplasticity silicon nitride whisker reinforced aluminum alloy composite
JP1991107433A
Aluminum-aluminum nitride composite material and its production
JP1996003601A
Mixture of aluminum alloy powder metals
JP2012505312A