Photocurable compositions having improved thermal stability

A photocurable composition with specific aromatic monomers and acrylate groups addresses thermal instability in inkjet adaptive planarization, achieving high thermal stability and carbon content for advanced processing.

JP2024544115APending Publication Date: 2024-11-28CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024521892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-09
Filing Date
2022-11-11
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing photocurable compositions for inkjet adaptive planarization lack sufficient thermal stability and high carbon content, leading to issues during subsequent processing steps that require temperatures above the glass transition temperature and near the melting point.

Method used

A photocurable composition comprising a photoinitiator and a polymerizable material with specific monomers, such as those with the formula (R1)x-Ar-(R2)y, where Ar is an aromatic ring and R1 and R2 contain acrylate groups, providing high carbon content and low vapor pressure, along with optional acrylate and vinylbenzene compounds, to enhance thermal stability and viscosity.

Benefits of technology

The composition achieves a photocured layer with high thermal stability, maintaining integrity at temperatures above 300°C, suitable for advanced processing techniques like inkjet adaptive planarization and nanoimprint lithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544115000001_ABST
    Figure 2024544115000001_ABST
Patent Text Reader

Abstract

The photocurable composition includes a polymerizable material and a photoinitiator, and the polymerizable material is represented by the formula (1): (R1) x -Ar-(R2) y where Ar is one or more substituted or unsubstituted aromatic rings, R1 is covalently bonded to Ar containing at least one acrylate group, x is 1-4, R2 is -CH=CH2 or -CCH3=CH2 covalently bonded to Ar, and y is 1-4.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocurable composition, and in particular to a photocurable composition suitable for forming a photocurable layer for inkjet compatible planarization. [Background technology]

[0002] Inkjet adaptive planarization (IAP) is a process of planarizing the surface of a substrate, such as a wafer containing electrical circuitry, by jetting droplets of a photocurable composition onto the surface of the substrate and directly contacting a planar superstrate with the applied liquid to form a planar liquid layer. The planar liquid layer is typically solidified by exposure to UV light, and after removal of the superstrate, a planar polymer surface is obtained that can be subjected to subsequent processing steps, such as baking, etching, and / or further deposition steps.

[0003] Subsequent baking of the formed photocurable layer is often carried out at a temperature above its glass transition temperature and close to its melting point, requiring high thermal stability and low shrinkage.

[0004] There is a need for improved IAP materials that result in planar photocurable layers that have high thermal stability during subsequent processing. Summary of the Invention

[0005] In one embodiment, the photocurable composition can include a photoinitiator and a polymerizable material, the polymerizable material having Formula (1): x -Ar-(R2) y where Ar is one or more substituted or unsubstituted aromatic rings, R1 is a structure covalently bonded to Ar that includes at least one acrylate group, x is 1-4, R2 is -CH=CH2, or -CCH3=CH2 covalently bonded to Ar, and y is 1-4.

[0006] In one embodiment of the photocurable composition, Ar in formula (1) may be selected from benzene, phenylbenzene, or naphthalene.

[0007] In certain embodiments, the first polymerizable monomer of the photocurable composition can include a structure of Formula (2) or Formula (3).

[0008] [ka] (2)

[0009] [ka] (3) Here, R3 is C1-C5 alkyl or oxyalkyl, x is 1-3, R4 is hydrogen or C1-C4 alkyl, y is 1-4, and z is 1-3.

[0010] In another particular embodiment, the first polymerizable monomer of the photocurable composition can include at least one monomer of the following structure:

[0011] [ka] (4)

[0012] [ka] (5)

[0013] [ka] (6)

[0014] [ka] (7)

[0015] In one embodiment, the first polymerizable monomer can have a vapor pressure of 0.01 mmHg or less at 25° C. In one particular embodiment, the crosslinker can have a vapor pressure of 0.001 mmHg or less at 25° C.

[0016] In one embodiment, the at least one first polymerizable monomer can further include at least one second polymerizable monomer having a structure different from that of formula (1). In one aspect, the at least one second polymerizable monomer can include at least one monofunctional acrylate monomer. In another aspect, the second polymerizable monomer can include at least one monofunctional monomer and at least one multifunctional monomer.

[0017] In one embodiment, the amount of the polymerizable material may be at least 80% by weight, based on the total weight of the photocurable composition.

[0018] In another embodiment, the viscosity of the photocurable composition at a temperature of 23° C. may be 50 mPa·s or less.

[0019] In one embodiment, the photocurable composition may be essentially free of solvent.

[0020] In another embodiment, the photocurable composition can include a solvent in an amount of at least 15% by volume, based on the total volume of the photocurable composition.

[0021] In one embodiment of the photocurable composition, the amount of the at least one first polymerizable monomer can be in the range of 50% to 100% by weight based on the total weight of the polymerizable material.

[0022] In another embodiment, a laminate can include a substrate and a photocurable layer overlying the substrate, the photocurable layer can be formed from a photocurable composition as described above.

[0023] In one embodiment of the laminate, the photocurable layer can have an Onishi number of 3.2 or less.

[0024] In a further aspect of the laminate, the photocurable layer can have a degradation temperature of greater than 300°C.

[0025] In one embodiment, a method of forming a cured layer on a substrate can include applying a layer of a photocurable composition onto the substrate, the photocurable composition can include a photoinitiator and a polymerizable material, the polymerizable material having Formula (1): x -Ar-(R2) y where Ar is one or more substituted or unsubstituted aromatic rings, R1 is a structure covalently bonded to Ar that contains at least one acrylate group, x is 1 to 4, R2 is -CH=CH2, or -CCH3=CH2 covalently bonded to Ar, and y is 1 to 3. The method also includes contacting the photocurable composition with a template or superstrate, irradiating the photocurable composition with light to form a photocured layer, and removing the template or superstrate from the photocured layer.

[0026] In one embodiment of the method, the first polymerizable monomer can include a structure of formula (2) or formula (3).

[0027] [ka] (2)

[0028] [ka] (3) Here, R3 is C1-C5 alkyl or oxyalkyl, x is 1-4, R4 is hydrogen or C1-C4 alkyl, y is 1-4, and z is 1-3.

[0029] In a further embodiment, a method of making an article can include applying a layer of a photocurable composition onto a substrate, wherein the photocurable composition comprises a polymerizable material and a photoinitiator, the polymerizable material having a structure represented by Formula (1): (R1): x -Ar-(R2) y where Ar is one or more substituted or unsubstituted aromatic rings, R1 is a structure covalently bonded to Ar that contains at least one acrylate group, x is 1-4, R2 is -CH=CH2, or -CCH3=CH2 covalently bonded to Ar; and y is 1-3. The method also includes contacting the photocurable composition with a template or superstrate, irradiating the curable composition with light to form a cured layer, removing the template or superstrate from the photocured layer, forming a pattern on the substrate, treating the substrate with the pattern, and fabricating an article from the treated substrate. [Brief description of the drawings]

[0030] Embodiments are illustrated by way of example and not limitation in the accompanying figures. [Figure 1] FIG. 1 includes a graph showing two TGA curves of photocured materials made from photocurable compositions according to embodiments. [Figure 2A] FIG. 2A shows the decrease in the peak at 809 cm −1 at various stages of curing of photocurable layers prepared from a photocurable composition according to one embodiment. [Figure 2B] FIG. 2B includes a graph comparing the absorbance peak at 809 cm −1 of photocurable compositions including C2 and S7 before and after curing, according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The following description is provided to aid in understanding the teachings disclosed herein and focuses on specific implementations and embodiments of the teachings. This focus is provided to help explain the teachings and should not be construed as a limitation on the scope or applicability of the teachings.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one skilled in the art to which this invention belongs. The materials, methods, and examples are illustrative only and are not intended to be limiting. To the extent not described herein, many details regarding specific materials and processing acts are conventional and can be found in textbooks and other sources within imprint and lithography technology.

[0033] As used herein, the terms "comprises," "includes," "including," "including," "having," "having" or any other variations thereof are intended to cover an open-ended inclusion. For example, a process, method, article, or apparatus that includes a list of features is not necessarily limited to only those features and may include other features that are not expressly listed or that are inherent to such process, method, article, or apparatus.

[0034] As used herein, unless expressly stated to the contrary, "or" refers to an inclusive or and not an exclusive or. For example, a condition A or B is satisfied by any one of: A is true (or present) and B is false (or not present), A is false (or not present) and B is true (or present), and both A and B are true (or present).

[0035] Additionally, the use of "a" or "an" is used to describe elements and components described herein. This is used merely for convenience to give a general sense of the scope of the invention. The specification should be read to include one or at least one, and the singular also includes the plural, unless it is clear that no plural is intended.

[0036] The present invention relates to a photocurable composition comprising a photoinitiator and a polymerizable material, the polymerizable material being represented by formula (1): (R1) x -Ar-(R2) y where Ar is one or more substituted or unsubstituted aromatic rings; R1 is a structure covalently bonded to Ar that includes at least one acrylate group; x is 1 to 4; R2 is -CH=CH2 or -CCH3=CH2 covalently bonded to Ar; and y is 1 to 4. In certain embodiments, Ar can be benzene, phenylbenzene, or naphthalene.

[0037] Without being bound by theory, photocurable compositions comprising monomers having the structure of formula (1) containing at least one vinyl group and at least one acrylate group covalently bonded to an aromatic ring structure may benefit by combining the properties of aromatic vinyl monomers, e.g., high carbon content, low viscosity, high etch resistance, with desirable properties typical of acrylate monomers, e.g., high cure speed and low vapor pressure compared to vinyl monomers.

[0038] As used herein, the term first polymerizable monomer having the structure of formula (1) is also referred to herein interchangeably as a "crosslinker", unless otherwise indicated. Without being bound by theory, it is believed that the monomer may be self-crosslinking when used as the only monomer in the polymerizable material, but may also assist in the crosslinking of other monomers contained in the composition, referred to herein as at least one second polymerizable monomer.

[0039] In an embodiment, the crosslinking agents of the present disclosure can have a vapor pressure at 25° C. of 0.01 mmHg or less, or 0.05 mmHg or less, or 0.001 mmHg or less, or 0.0005 mmHg or less, or 0.0003 mmHg or less.

[0040] In certain embodiments, the crosslinker can have a structure shown in formula (2) or formula (3).

[0041] [ka] (2)

[0042] [ka] (3) R3 is C1-C5 alkyl or oxyalkyl, x is 1-4, R4 is hydrogen or C1-C4 alkyl, y is 1-4, and z is 1-3.

[0043] In certain embodiments, the crosslinker may include 3-vinylbenzyl acrylate (structure 4), 2(4-vinyl)-phenyl; 1,3-propane diacrylate (structure 5); 3,5-bivinylbenzyl acrylate (structure 6); and 5-vinyl 1,3-xylylene diacrylate (structure 7).

[0044] [ka] Structure 4

[0045] [ka] Structure 5

[0046] [ka] Structure 6

[0047] [ka] ···Structure(7)

[0048] The photocurable compositions of the present disclosure can be adapted for use in inkjet adaptive planarization (IAP) or nanoimprint lithography (NIL).

[0049] The first polymerizable monomer of Formula 1 can have the advantage of a high carbon content, which can contribute to a high final carbon content in the formed photocured layer. In one embodiment, the carbon content of the first polymerizable monomer can be at least 70% by weight, or at least 72% by weight, or at least 76% by weight, or at least 78% by weight, based on the total molecular weight of the first monomer.

[0050] In one aspect, the viscosity of the photocurable composition can be 50 mPa·s or less, e.g., 40 mPa·s or less, 30 mPa·s or less, 25 mPa·s or less, 20 mPa·s or less. In other particular embodiments, the viscosity can be at least 2 mPa·s, or at least 3 mPa·s, or at least 5 mPa·s. As used herein, all viscosity values ​​refer to viscosities measured at a temperature of 23° C. using the Brookfield method using a Brookfield viscometer.

[0051] The at least one second polymerizable monomer of the photocurable composition of the present disclosure can include at least one second polymerizable monomer having a structure different from that of the first polymerizable monomer. In one embodiment, the at least one second polymerizable monomer can be at least one acrylate monomer. In a particular embodiment, the at least one acrylate monomer can include two acrylate monomers, three acrylate monomers, four acrylate monomers, or five acrylate monomers. The term "acrylate monomer" as used herein refers to unsubstituted or alkyl-substituted acrylate monomers, such as methacrylate monomers.

[0052] In another embodiment, the at least one second polymerizable monomer can be a monofunctional monomer or a multifunctional monomer. In a particular embodiment, the at least one first monomer of the polymerizable material can include at least one difunctional acrylate monomer or at least one trifunctional acrylate monomer. In a further embodiment, the second polymerizable monomer can include a non-acrylic monomer, such as a monofunctional or multifunctional vinylbenzene compound. In a particular embodiment, the vinylbenzene compound can be divinylbenzene.

[0053] In one embodiment, the amount of the first polymerizable monomer of the polymerizable material can be at least 5 wt%, or at least 10 wt%, or at least 15 wt%, or at least 20 wt%, or at least 30 wt%, or at least 40 wt%, or at least 50 wt%, or at least 60 wt% based on the total weight of the polymerizable material. In another embodiment, the amount of the at least one first polymerizable monomer can be 100 wt% of the total weight of the polymerizable material, or 95 wt% or less, or 90 wt% or less, or 80 wt% or less, or 70 wt% or less, or 60 wt% or less based on the total weight of the polymerizable material. In an aspect, the amount of the first polymerizable monomer can range from 50 wt% to 100 wt%, or 60 wt% to 97 wt%, or 70 wt% to 95 wt% based on the total weight of the polymerizable material. In yet another aspect, the amount of the first polymerizable monomer can range from 5 wt% to 40 wt%, or 10 wt% to 30 wt% based on the total weight of the polymerizable material.

[0054] In another particular embodiment, the polymerizable material can consist essentially of at least one first polymerizable monomer of formula (1) and at least one additional acrylate monomer, where the at least one additional acrylate monomer is related to the at least one second polymerizable monomer, and by consisting essentially, it is meant that up to 1% by weight of the polymerizable material can be a different polymerizable compound.

[0055] The amount of polymerizable material in the photocurable composition can be at least 30% by weight, e.g., at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 85% by weight, at least 90% by weight, or at least 95% by weight, based on the total weight of the photocurable composition. In another embodiment, the amount of polymerizable material can be 99% by weight or less, e.g., 98% by weight or less, or 97% by weight or less, or 95% by weight or less, based on the total weight of the photocurable composition. The amount of polymerizable material can be any value between the minimum and maximum values ​​listed above. In a particular embodiment, the amount of polymerizable material can be at least 80% by weight, 98% by weight or less.

[0056] In another embodiment, the polymerizable material of the photocurable composition can include an amount of a polymerizable monomer, oligomer, or polymer in addition to the crosslinker and at least one first polymerizable monomer.

[0057] The photocurable composition can be adapted so that the photocured layer formed therefrom has high thermal stability. In one embodiment, the onset temperature of thermal degradation of the photocurable layer can be greater than 250°C, or greater than 300°C, or greater than 350°C, or greater than 375°C, or greater than 400°C. As used herein, onset thermal degradation temperature, also referred to as "thermal degradation temperature", refers to the temperature of the TGA curve where deviation of the curve from a nearly linear plateau is first observed, immediately prior to the rapid degradation of the sample.

[0058] In one embodiment, the first photocurable composition of the present disclosure may be essentially free of solvent.

[0059] As used herein, unless otherwise indicated, the term solvent refers to a compound that can dissolve or disperse polymerizable monomers and crosslinkers, but does not itself polymerize during photocuring of the photocurable composition. The term essentially solvent-free herein means an amount of solvent that is 5 wt% or less based on the total weight of the photocurable composition. In certain embodiments, the amount of solvent can be 3 wt% or less, 2 wt% or less, 1 wt% or less, or the photocurable composition can be solvent-free, except for unavoidable impurities.

[0060] In other specific embodiments, the photocurable composition can include a solvent in an amount of at least 6% by weight, or at least 8% by weight, at least 10% by weight, at least 15% by weight, at least 20% by weight, at least 30% by weight, or at least 50% by weight, based on the total weight of the photocurable composition. In other embodiments, the amount of solvent can be 80% by weight or less, or 50% by weight or less, or 40% by weight or less, or 30% by weight or less, or 20% by weight or less, or 15% by weight or less.

[0061] One or more photoinitiators may be included in the photocurable composition to initiate photocuring of the composition when exposed to light.

[0062] In some embodiments, curing can also be accomplished by a combination of light and heat curing.

[0063] The photocurable composition may further contain one or more optional additives. Non-limiting examples of the optional additives may be stabilizers, dispersants, solvents, surfactants, inhibitors, or any combination thereof.

[0064] In one embodiment, the photocurable composition can be coated onto a substrate to form a photocured layer. As used herein, the combination of the substrate and the photocured layer overlying the substrate is referred to as a laminate.

[0065] The combination of at least one first polymerizable monomer with at least one second polymerizable monomer of the polymerizable material, or the use of at least one first polymerizable monomer as the only monomer of the polymerizable material, can result in a high carbon content in the formed photocured layer. In one embodiment, the carbon content of the photocured layer can be at least 70%, such as at least 72%, at least 73%, at least 74%, or at least 75%.

[0066] In another embodiment, the photocurable layer of the laminate can have an Onishi number of 3.2 or less, or 3.0 or less, or 2.9 or less, or 2.8 or less, or 2.7 or less, or 2.6 or less. In another embodiment, the Onishi number can be at least 1.8, such as at least 1.9, at least 2.0, at least 2.1, at least 2.2, or at least 2.3.

[0067] In certain embodiments, the photocured layer may have a carbon content of at least 70% and an Onishi number of 2.9 or less.

[0068] The present disclosure further relates to a method of forming a photocurable layer, which may include applying a layer of the photocurable composition described above onto a substrate, contacting the photocurable composition with a template or superstrate, irradiating the photocurable composition with light to form the photocurable layer, and removing the template or superstrate from the photocurable layer.

[0069] The substrate and solidified layer may be subjected to additional processing, such as an etching process, to transfer an image to the substrate that corresponds to the pattern of one or both of the solidified layer and / or the patterned layer underlying the solidified layer. The substrate may be further subjected to known steps and processes for device (article) manufacturing, including, for example, curing, oxidation, layering, deposition, doping, planarization, etching, formable material removal, dicing, bonding, and packaging.

[0070] In addition, the film may be used as an interlayer insulating film in semiconductor devices such as LSI, system LSI, DRAM, SDRAM, RDRAM, and D-RDRAM, or as a resist film used in the semiconductor manufacturing process.

[0071] As further demonstrated in the examples, it has been surprisingly discovered that a particular combination of polymerizable monomers containing a crosslinker of formula (1) in a photocurable composition can have properties that are particularly suitable for IAP and NIL processing. The photocurable composition can form a photocured layer with high thermal stability. In one embodiment, the polymerizable material of the photocurable composition of the present disclosure can essentially consist of a crosslinker and other acrylate monomers and can have thermal stability of more than 300°C.

[0072] Working Example The following non-limiting examples illustrate the concepts described herein. Example 1 Preparation of the first polymerizable monomer (crosslinker).

[0073] A variety of cross-linkers were prepared by acrylation of the OH groups of the corresponding starting compounds.

[0074] 3-Vinylbenzyl acrylate (VBA) (S4) 40 g of 3-vinylbenzenemethanol (0.3 mol) and 45.9 g of triethylamine (Et)3N (0.45 mol) were dissolved in 900 ml of dry dichloromethane (CH2Cl2) and cooled to 0°C in an ice-water bath. To this solution, a solution of 32.6 g of acryloyl chloride dissolved in 100 ml of CH2Cl2 was added dropwise with stirring. The resulting mixture was allowed to warm to room temperature and stirred for 12 hours. The organic phase was washed with saturated brine and dried over Na2SO4. After drying, the solvent was removed by distillation under reduced pressure.

[0075] The chemical reaction scheme is outlined below.

[0076] [ka]

[0077] Using a method similar to that described above for the synthesis of 3-vinylbenzyl acrylate, the compounds 2-(4-vinyl)-phenyl-1,3-dipropane diacrylate (5); 3,5-vinylbenzyl acrylate (6); and 5-vinyl 1,3-xylylene diacrylate (7) were synthesized. The reaction schemes for these reactions are summarized below.

[0078] 2-(4-vinyl)-phenyl, 1,3-dipropane diacrylate (VPDD) (S5):

[0079] [ka]

[0080] 3,5-Divinylbenzyl acrylate (DVBA) (S6):

[0081] [ka]

[0082] 5-Vinyl 1,3-xylylene diacrylate (VXDA) (S7):

[0083] [ka]

[0084] Example 2 Comparison of crosslinking agent properties The crosslinkers made in Example 1, such as samples S4, S5, S6, and S7, were analyzed by their viscosity, vapor pressure, and thermal stability.

[0085] As comparative samples, monomers containing only acrylate and vinyl groups were selected and analyzed in the same manner as the representative crosslinkers of the present disclosure containing both acrylate and vinyl groups. The following comparative monomers were tested: C1: benzyl acrylate (BZA), C2: m-xylylene diacrylate (MXDA); C3: styrene monomer (SM); and C4: divinylbenzene (DVB).

[0086] viscosity Viscosity was measured using a Brookfield DV-11+Pro viscometer with spindle #18. For each viscosity measurement, 6-7 ml of sample was taken, added to the sample chamber, and allowed to equilibrate for 15-20 minutes until the target temperature of 23°C was reached. Viscosity was measured at a speed of 135 rpm with spindle #18. For each sample, measurements were repeated three times and the average value was calculated.

[0087] An overview of the invention of the measured viscosities (each related to 100% monomer, excluding unavoidable impurities) is given in Table 1.

[0088] [Table 1]

[0089] Table 1 From the data in Table 1, it can be seen that the comparative monomer C2, which contains two acrylate groups (MXDA), had a viscosity four times higher than the acrylate monomer C1 (BZA), which has only one acrylate group. The lowest viscosities were measured for the comparative samples C3 (styrene monomer) and C4 (divinylbenzene), which contain only vinyl groups and no acrylate groups.

[0090] Crosslinkers S4, S5, S6 and S7, which contain a combination of vinyl and acrylate groups covalently bonded to the benzene ring, had viscosities higher than those of the comparative monomers and were in the suitable range for use in IAP or NIL processing.

[0091] Vapor pressure Table 1 also summarizes the calculated vapor pressures of all the monomers listed. Monomers S4, S5, S6, and S7 all have vapor pressures at least 10 times lower than the equivalent monomers C1-C4. Monomers with low vapor pressures are desirable in IAP and NIL processing to avoid loss of resist composition after applying the resist on the substrate and before photocuring.

[0092] Vapor pressure is EPISuite TM The calculations were made using a US Environmental Protection Agency software program called version 4.1. In a comparison example of Styrene Monomer (SM) and DVB, the calculations were found to be correct. The difference between the calculated vapor pressure and the actual tested vapor pressure was less than 6 percent of the total vapor pressure value.

[0093] Light-curable and heat-stable Crosslinkers S5 (VPDD) and S7 (VXDA) were photocured with a radiation energy of 2.4 J and the cured data were analyzed by thermal analysis (TGA). TGA was performed using a LINSEIS STA PT1000 instrument (Linseis Messgeraete GmbH, Germany). All measurements were performed under nitrogen at a rate of 5 liters per hour. Samples (approximately 25 mg per test) were heated at a rate of 20 °C / min and the mass loss was continuously recorded. The TGA curves are shown in Figure 1. Decomposition of the materials began at temperatures above 380 °C. The exact decomposition temperatures were 388.6 °C for monomer S5 and 399.5 °C for monomer S7. As used herein, degradation temperature refers to the initial degradation temperature T(X), which is the temperature of the TGA curve at which a deviation of the curve from the approximately linear plateau shape is first observed immediately prior to a rapid drop in the mass of the sample, i.e., degradation.

[0094] 1 further includes a TGA curve of a photocured layer formed by photocuring a photocurable composition containing Monomer S7 and Monomer C2 in a uniform weight percent ratio of 1:1. The initial degradation temperature T(X) of this data was 398°C.

[0095] The curing of functional groups (acrylate and vinyl groups) was observed at 809 cm for the photocured sample of the crosslinker. -1 The change in the absorption peak at 100° C. was evaluated by observing the change in the absorption peak at 100° C. in the FTIR spectrum. The absorption peaks are related to the C═C double bonds of the vinyl group and the acrylate group.

[0096] For these tests, a layer of monomer approximately 10 μm thick was applied onto a NaCl window and an emission wavelength of 365 nm and 38 mW / cm 2 The photocured layer was prepared by photocuring the layer with a dose of 10 J for 263 seconds with a light beam of 1000 nm. The photocured layer was baked on a hot plate at a temperature of 250 °C for 2 minutes. After cooling to room temperature and measuring the FTIR spectrum, the same test was repeated by placing the photocured layer on a hot plate at 350 °C for 2 minutes. A summary of the test results is shown in Table 2.

[0097] The same test was performed on comparative sample C2, a difunctional acrylate monomer. Sample C2 was cured with a cure energy of 1.2 J.

[0098] Further, a composition was prepared by mixing sample C2 with sample S5 in a weight percent ratio of 1:4, and similarly, sample C2 was mixed with sample S7 in a weight percent ratio of 1:4.

[0099] For each photocurable composition, Irgacure 907 was used as the photoinitiator in an amount of 2 wt %, based on the total weight of the photocurable composition.

[0100] The results summarized in Table 2 demonstrate that photocured layers made from the crosslinkers of the present disclosure are stable at temperatures of 250°C and 350°C, with further curing (reaction) of the functional groups occurring at higher temperatures. In contrast, the difunctional acrylate sample C2 was already cured to a high percentage at room temperature (23°C). Sample C2 could not withstand baking at 350°C, but combinations of C2 with S5 or S7 at a weight percent ratio of 1:4 could improve thermal stability and baking at 250°C and 350°C could be performed.

[0101] Furthermore, the percentage of cure (C=C conversion) at room temperature could be increased by combining monomer C2 with monomers S5 or S7 in a weight percent ratio of 1:4. The combination of monomers C2 and S7 in a weight percent ratio of 1:1 further increased the conversion at room temperature to 78.14% conversion.

[0102] Figure 2A shows the 809 cm peaks at each stage of curing, including uncured (d), room temperature curing (c), baking at 250°C (b), and baking at 350°C (a). -1 The peak maximum value of 809 cm -1 The peak observed at 809 cm is a characteristic peak of a -C=Cn double bond. FIG. 2B shows the peak at 809 cm for the composition containing C2 and S7, comparing the uncured composition with the layer formed after curing at room temperature (23 °C). -1 The decrease in the absorption peak maximum at

[0103] [Table 2]

[0104] Table 2 Carbon content and Onishi number Further important properties for developing photocurable compositions suitable for IAP and NIL processing are the carbon content and the Ohnishi number.

[0105] Table 3 shows a summary of the calculated carbon contents and Ohnishi numbers for the representative crosslinkers prepared in Example 1.

[0106] The Onishi number (ON) is known to be an empirical parameter and is the total number of atoms in a polymer repeat unit (N t ) is expressed as the number of carbon atoms (Nc) and oxygen atoms (N O ) divided by the difference between ON and N t / (N C -N O For the calculation of the Ohnishi number, the cured data was assumed to contain 100% by weight of polymerized monomer units formed by addition polymerization (no atoms lost during polymerization).

[0107] Carbon content was calculated as the percentage of carbon atoms based on the total molecular weight of the compound.

[0108] From Table 3 it can be seen that all of the crosslinkers had a carbon content greater than 70 percent and a Maximum Axis Number less than 3.2.

[0109] [Table 3]

[0110] Table 3 The specification and illustrations of the embodiments described herein are intended to provide a general understanding of the structure of the various embodiments. The specification and illustrations are not intended to be exhaustive and comprehensive descriptions of all of the elements and features of the apparatus and systems that use the structures or methods described herein. Separate embodiments may also be provided in combination in a single embodiment, and conversely, for brevity, various features described in the context of a single embodiment may be provided separately or in any subcombination. Furthermore, references to values ​​described in ranges include each and every value within that range. Many other embodiments may be apparent to those skilled in the art only after reading this specification. Other embodiments may be used and derived from this disclosure, such that structural substitutions, logical substitutions, or other changes may be made without departing from the scope of this disclosure. Thus, this disclosure should be considered as illustrative and not restrictive.

Claims

1. A photocurable composition comprising a polymerizable material and a photoinitiator, the polymerizable material being represented by formula (1): (R 1 ) x -Ar-(R 2 ) y wherein the polymerizable monomer comprises at least one first polymerizable monomer having a structure: Ar is one or more substituted or unsubstituted aromatic rings; R 1 is covalently bonded to Ar containing at least one acrylate group; x is 1 to 4; R 2 -CH=CH 2 or -CCH covalently bonded to Ar 3 =CH 2 and y is 1 to 4; A photocurable composition comprising:

2. Ar is selected from benzene, phenylbenzene or naphthalene; The photocurable composition according to claim 1 .

3. the at least one first polymerizable monomer comprises a structure of formula (2) or formula (3): 【Chemistry 19】 ...Formula (2) 【Chemistry 20】 ...Formula (3) Here, R 3 is C1-C5 alkyl or oxyalkyl, x is 1-4, R 4 is hydrogen or C1-C4 alkyl, y is 1-4, and z is 1-3; The photocurable composition according to claim 2 .

4. The at least one first polymerizable monomer comprises at least one of the following structures: 【Chemistry 21】 ・・・(4) 【Chemical 22】 ・・・(5) 【Chemistry 23】 ・・・(6) 【Chemistry 24】 ・・・(7) The photocurable composition according to claim 3 .

5. the at least one first polymerizable monomer has a vapor pressure of 0.01 mmHg or less at 25° C.; The photocurable composition according to claim 1 .

6. the at least one first polymerizable monomer has a vapor pressure of 0.001 mmHg or less at 25° C.; The photocurable composition according to claim 5 .

7. the polymerizable material further comprises at least one second polymerizable monomer having a structure different from the structure of formula (1); The photocurable composition according to claim 1 .

8. the at least one second polymerizable monomer comprises at least one monofunctional acrylate monomer; The photocurable composition according to claim 7 .

9. the at least one second polymerizable monomer comprises at least one monofunctional monomer and at least one multifunctional monomer; The photocurable composition according to claim 7 .

10. the amount of said polymerizable material is at least 80% by weight based on the total weight of said photocurable composition; The photocurable composition according to claim 1 .

11. The viscosity of the photocurable composition at 23° C. is 50 mPa·s or less. The photocurable composition according to claim 1 .

12. the photocurable composition comprises a solvent in an amount of at least 15 volume percent based on the total volume of the photocurable composition; The photocurable composition according to claim 1 .

13. the photocurable composition is essentially free of solvent; The photocurable composition according to claim 1 .

14. the amount of the first polymerizable monomer is in the range of 50% by weight to 100% by weight based on the total weight of the polymerizable material; The photocurable composition according to claim 1 .

15. 13. A laminate comprising a substrate and a photocurable layer overlying said substrate, said photocurable layer being comprised of the photocurable composition of claim 1.

16. The photocurable layer has an Onishi number of 3.2 or less. The laminate according to claim 15 .

17. The photocurable layer has a degradation temperature of at least 300° C. The laminate according to claim 15 .

18. 1. A method for forming a photocurable layer on a substrate, comprising: applying a layer of a photocurable composition onto the substrate, the photocurable composition comprising a photoinitiator and a polymerizable material, the polymerizable material having the formula (1): (R 1 ) x -Ar-(R 2 ) y where Ar is one or more substituted or unsubstituted aromatic rings, and R 1 is a structure covalently bonded to Ar containing at least one acrylate group, x is 1 to 4, and R 2 -CH=CH 2 or -CCH covalently bonded to Ar 3 =CH 2 and y is 1 to 4; contacting the photocurable composition with a template or superstrate; A step of irradiating the photocurable composition with light to form a photocured layer; removing the template or the superstrate from the photocurable layer; The method according to claim 1, further comprising:

19. The crosslinking agent comprises a structure of formula (2) or formula (3), 【Chemistry 25】 ・・・(2) 【Chemistry 26】 ・・・(3) Here, R 3 is C1-C5 alkyl or oxyalkyl, x is 1-4, R 4 is hydrogen or C1-C4 alkyl, y is 1-4, and z is 1-3; 20. The method of claim 18 .

20. 1. A method of manufacturing an article, comprising the steps of: applying a layer of a photocurable composition onto a substrate, the photocurable composition comprising a polymerizable material and a photoinitiator, the polymerizable material having the formula (1): (R 1 ) x -Ar-(R 2 ) y where Ar is one or more substituted or unsubstituted aromatic rings, and R 1 is a structure covalently bonded to Ar containing at least one acrylate group, x is 1 to 4, and R 2 -CH=CH 2 or -CCH covalently bonded to Ar 3 =CH 2 and y is 1 to 4; contacting the photocurable composition with a template or superstrate; A step of irradiating the photocurable composition with light to form a cured layer; removing the template or the superstrate from the light cured layer; forming a pattern on the substrate; processing the substrate on which the pattern is formed; manufacturing an article from the substrate processed in the processing step; The method according to claim 1, further comprising:

Citation Information

Patent Citations

  • Lens material for eye

    JP1990196809A

  • Copolymer and its production

    JP1991160007A

  • Oxygen permeable material

    JP2002308954A

  • Composition for nanoimprint, pattern, and patterning method therefor

    JP2010109092A

  • Photocurable composition

    US20200339828A1