Method for increasing the sphericity of particles in thermoplastic polymer powders
Infrared radiation and convective heating combined with controlled crystallization enhance the sphericity and flowability of thermoplastic polymer powders, addressing inefficiencies and thermal issues in existing methods.
Patent Information
- Application Number
- JP2024527765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-10
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for producing thermoplastic polymer powders with high sphericity are inefficient, costly, and often require toxic solvents or high temperatures, leading to low yield, poor flowability, and thermal degradation.
A method utilizing infrared radiation and convective heating to melt thermoplastic polymer particles in a transparent chamber, followed by spontaneous spheronization and controlled crystallization in a shielding gas, minimizing thermal exposure and agglomeration, and enhancing sphericity.
The method significantly improves the sphericity and flowability of thermoplastic polymer powders while reducing thermal degradation and increasing production yield and throughput.
Smart Images

Figure 2024544140000001 
Figure 2024544140000002 
Figure 2024544140000003
Abstract
Description
[Technical field]
[0001] The object of the present invention is a method for increasing the sphericity of particles of thermoplastic polymer powders. The term "sphericity" as used herein should also be understood as "ellipticity", "roundness" or "regularity". The term "grains" of a polymer powder as used herein should also be understood as "particles" of a polymer powder. The term "type II phase transition" as used herein should also be understood as "second-order phase transition" or "glass transition". The term "spontaneous spheronization" as used herein should be understood as a process in which a particle of any shape spontaneously changes shape to become a nearly perfect sphere. The particles are droplets of liquid polymer suspended in a fluid to such an extent that the effect of the Earth's gravity is negligible, and the process is mainly controlled by the surface tension, viscosity and size of the liquid polymer droplets. [Background technology]
[0002] Powders of thermoplastic polymers, both crystalline polymers that exhibit a melting point and amorphous polymers that exhibit a type II phase transition, are used as components of powder coatings, electrostatically applied paints, electrostatically applied layers from solutions and suspensions (EPD - electrophoretic deposition), feed materials for rotational molding processes, feedstock for the selective laser sintering (SLS) process in additive manufacturing techniques, feedstock for the multi-jet fusion (MJF) process in additive manufacturing techniques, abrasives for cosmetics, materials for polymer cold spray processes, or feedstock for polymer flame spray (FSA) processes, or for the manufacture of toners and inks. In particular, additive manufacturing techniques such as SLS and MJF require powders that are characterized by a high sphericity that allows efficient transport processes and good solidification at high temperatures. This is made possible by a high powder flowability (expressed by the Hausner ratio), which is positively correlated with the sphericity of the polymer particles. Many methods for producing polymer powders based on milling processes, including milling under cryogenic conditions, produce irregular powders with low sphericity, resulting in poor flowability, which severely limits the use of polymer powders in additive manufacturing techniques and other areas requiring high flowability.
[0003] Commonly known methods of obtaining powders with highly spherical particles of thermoplastic polymers can be classified with respect to the mechanism of action, namely controlled melting, spontaneous spheronization, controlled crystallization, and controlled precipitation from solution. These methods utilize the aforementioned mechanisms in combination with heat transfer by liquid or gas convection. One of the well-known methods is to prepare powders with high sphericity parameters by precipitating the polymer from solution, this precipitation process being triggered by lowering the temperature or adding a liquid that is a non-solvent for the polymer. This process is used for polyamide 12 (PA12), polypropylene (PP), polyamide 6 (PA6), polycarbonate (PC), polyamide 11 (PA11), polybutylene terephthalate (PBT), polyoxymethylene (POM), and polylactide derivatives (PLA). A feature of this method is the need to use toxic solvents and the need for strict selection of process conditions in pressure reactors, which is not favorable. An exemplary overview of known applications of this method is given in the paper (P. Hejmady et al, A processing route to spherical polymer particles via controlled droplet retraction, 388, 401-411, 2021). Furthermore, US Patent No. 5,932,687A describes the controlled precipitation of polyamide 12-based materials from aliphatic alcohols containing 1-13 carbon atoms at temperatures ranging from 130°C to 165°C in a high-pressure system, followed by cooling to a temperature of 110°C to 130°C. Another commonly known method is the spray drying process. The spray drying process can be used for a wide range of thermoplastic polymers, including high melting point polymers such as polysulfone (PSU). The main limitations of this method are low mass yields, the difficulty of selecting the optimal chamber temperature, and excessive solidification of the particles in the collection vessel. Another well-known process is the co-extrusion of a thermoplastic material with a matrix material, which can then be removed to leave thermoplastic particles with high sphericity.This solution is disadvantageous due to the need for removal and management of waste polymer matrix, as well as the fact that the particle size distribution is poorly controlled. The solution is known to be used for polypropylene and polyamide 12. Exemplary results described in (X.Yang et al., Preparation of spherical polymer powders for selective laser sintering from immiscible PA12 / PEO blends with high viscosity ratios, Polymer, 172, 58-65, 2019) show the formation of a fraction with a sieve size of less than 1 micrometer, which is undesirable for applications in additive manufacturing techniques and in applications where there is a risk of inhalation or ingestion of the powder material by humans. Patent application DE102006015791A1 describes water-soluble matrices based on poly(ethylene glycol) and poly(ethylene oxide). The scientific literature describes well-known methods that make it possible to convert thermoplastic polymer fibers into spherical particles by controlled heating in a liquid matrix, exploiting the Plateau-Rayleigh effect. This method is described, for example, in the publication (Y. Zhou et al., Preparation of near-spherical PA12 particles for selective laser sintering via Plateau-Rayleigh instability of molten fibers, Materials and Design, 190, 108578, 2020). It is limited in terms of efficiency, since it produces a very fine fraction by nature and also has a negative effect on the purity of the powder obtained, which can lead to powder degradation due to excessive exposure to high temperatures. Another known method is described in US Patent Application No. 4345015A, which involves heating polymer particles suspended in a liquid that is a non-solvent for the polymer. A feature of this method is the need to wash the powder particles from the liquid residues, which is a drawback of this method.US Patent Application No. 6264861B1 describes another known method in which irregular particles of a thermoplastic polymer are homogenized with particles of a non-thermoplastic material and mixed at a temperature above the glass transition temperature of the thermoplastic polymer undergoing spheronization. This solution is inferior because it requires the separation of the non-thermoplastic material after the particle rounding process, which makes it unattractive for high purity, low cost powder applications. Other methods are known that involve heating a suspension of thermoplastic polymer powder particles in a gas by a tubular reactor heater. One such solution, which exists in the scientific and industrial literature under the name "Heated Downer Reactor", is exemplified in (M. Sachs et al., Characterization of a downer reactor for particle rounding, Powder Technology, 316, 1, 357-366, 2017). This method can be used for polystyrene powder, PBT powder, polyethylene (PE) powder, and other thermoplastics. Despite the large size of the equipment, this solution is characterized by a low process efficiency of about 70%, due to the uncontrolled deposition of molten thermoplastic particles on the reactor walls near the inlet of the powder lift gas. The method has a powder production capacity of about 200 g / h. This solution cannot be easily expanded, since the height of the tubular reactor is more than 4 meters, which would be necessary to achieve a favorable production capacity, considering that a large part of the supplied powder is destroyed during the process. US Patent Application No. 20120070666A1 describes another known solution using a NARA NHS device, which provides high shear forces acting on the powder particles, the powder being introduced at a temperature above the glass transition temperature but below the melting point of the material.
[0004] During the course of the research, it was unexpectedly found that infrared radiation is not only scattered, but also partially absorbed by the suspension of polymer powder particles in the gas. It was observed that if the thermoplastic polymer powder particles contain an infrared absorbing additive, the heating process can be accelerated and complete melting of the particles or a complete type II phase transition can be reached. It was observed that the process can be carried out even if the powder particles do not contain an infrared absorbing additive, and the aforementioned process proceeds with a decrease in mass efficiency and is based on the absorption of infrared radiation by the polymer. It was observed that the spheroidization process proceeds both by the radiation absorption mechanism and the convection heating mechanism, regardless of whether the particles contain a radiation absorbing additive. It was observed that if the powder particles are higher than room temperature and at the same time 20 ° C lower than the melting point of the thermoplastic polymer, the particles in the gas phase can be effectively melted by the mechanism of radiation absorption without maintaining the agglomeration of the thermoplastic polymer powder in the ejector and feed nozzle. It was observed that if the powder particles are introduced into the reactor when the gas temperature near the reactor inlet is in the range from room temperature to the melting point of the polymer, the powder particles can be efficiently melted by a mixed mechanism of radiation absorption and convection heating. It has been observed that if the powder particles are introduced into the reactor when the temperature of the gas near the reactor inlet is in the range from room temperature to the melting point of the polymer, the powder particles can be efficiently melted by a mixed mechanism of radiation absorption and convection heating, especially if the radiation heating zone and the convection heating zone are co-located. This situation is advantageously achieved by implementing a reactor made of a material that is partially transparent to radiation and has a low thermal conductivity coefficient. In the course of the research, it was found that the method of radiation spheroidization is effective if the particles of the polymer powder do not remain in an agglomerated state. Otherwise, spheroidization proceeds with an increase in the average particle size. It has been observed that a convenient way of feeding the powder to the process is to use a Venturi ejector to pulverize it with a shielding gas and to distribute the powder to the suction section of the ejector using one of the well-known methods that are not part of the present invention. It has been observed that an advantageous way of feeding the powder is to feed it under conditions close to free fall, especially through a sieve, an arrangement of several sieves, or an arrangement based on a sieve(s) and a powder agglomerate breaking element.It was observed that an advantageous way of feeding the powder is through a sieve, an arrangement of several sieves or an arrangement based on sieve(s) and powder agglomerate breaking elements under conditions close to free fall, the flow of powder and shielding gas being controlled by reducing the pressure near the reactor section outlet, whereby the shielding gas and the polymer powder are simultaneously drawn into the reactor. In the course of the research, it was observed that in order to avoid solidification of the molten particles, the invention should include a step of controlled crystallization of the molten particles after they leave the transparent chamber in which heating by radiation takes place, advantageously the controlled crystallization being carried out in a chemically inert shielding gas having a temperature ranging from room temperature to 50°C below the melting point of the thermoplastic powder. The object of the invention is visualized in the attached drawing. Summary of the Invention
[0005] The object of the present invention is a method for increasing the sphericity of powder particles of a thermoplastic polymer, characterized in that it reduces the temperature of the gas carrying the powder particles, shortens the time of exposure of the powder to high temperatures, reduces the degree of thermal degradation of the polymer being spheroidized and improves the achievable yield and throughput of the process.
[0006] The essence of the present invention is to increase the sphericity of thermoplastic polymer powder particles by using an apparatus based on a radiation heat transport mechanism for the controlled melting or controlled type II phase transition of the polymer particles, followed by spontaneous spheroidization, and finally controlled crystallization in a shielding gas, the temperature of the shielding gas carrying the polymer powder particles being lower than the melting temperature of the thermoplastic polymer particles.
[0007] The method for increasing the sphericity of particles of thermoplastic polymer powder according to the invention is based on the introduction of thermoplastic polymer powder in a gas flow into a device ensuring the destruction of agglomerates of particles of the powder material, then the powder is transported through a nozzle (2) into an optically transparent flow chamber (4) located in the region of the radiation generated by a radiation source (3), then the powder absorbs the radiation causing a complete melting or a type II phase transition of the powder, then the molten particles are removed from the radiation region by being transported in a carrier gas continuously supplied through a pneumatic connection (5), while being transported by the carrier gas spontaneous sphericization of the liquid polymer occurs, then the polymer is allowed to crystallize in the carrier gas in a controlled crystallization chamber (6).
[0008] The method for increasing the sphericity of particles of a thermoplastic polymer powder according to the invention is characterized by a series of steps, in which the thermoplastic polymer powder is introduced into a device (9) that ensures the destruction of agglomerates of the particles of the powder, then the powder is introduced into a device (10) that ensures conditions close to the free fall of the particles and separates the shielding gas from the powder suspended in the carrier gas, then the powder suspension in gas and the shielding gas are transported into an optically transparent flow chamber (12) by reducing the pressure in the flow chamber with a reduced pressure generator (14), then radiation absorption, or radiation absorption accompanied by convective heat transfer from the walls of the flow chamber, then complete or partial melting of the particles due to absorption of energy or complete or partial type II phase transition occurs, then the molten particles are removed from the radiation zone by being carried in a gas drawn from the chamber (15) into a flow reactor under the action of the reduced pressure generator (14), then spontaneous spheronization of the liquid polymer particles occurs during transport in the carrier gas, then controlled crystallization occurs in the carrier gas in the controlled crystallization chamber (13).
[0009] Thermoplastic polymer powders are prepared by subjecting the polymers in question to a wide range of applications, in particular polyamide-4, polyamide-6, polyamide-7, polyamide-8, polyamide-9, polyamide-11, polyamide-12, polyamide-46, polyamide-66, polyamide-69, polyamide-510, polyamide-610, polyamide-613, polyamide-1010, polyamide-1012, polyamide-1212, polyamide-1313, polyamide-6T, polyamide-6 / 66, polyamide-6 / 12, polyamide-612, copolymers of these polyamides, polypropylene (PP), low density polyethylene (LDPE), high density polyethylene (HDPE), low density branched polyethylene (LLDPE), copolymers of polypropylene and polyethylene (PP-PE). The melting points or type II phase transition temperature ranges are always lower than the thermal decomposition onset temperature of polymer powders based on poly[(ethylene)-co-(vinyl acetate)] (EVA), polyethylene wax (low molecular weight polyethylene), paraffin wax with a melting point below 70 °C, ultra-high molecular weight polyethylene (UHDPE), poly(butylene terephthalate) (PBT), polyether ether ketone (PEEK), poly(oxymethylene) (POM), thermoplastic polyurethane elastomers (TPU), isotactic polystyrene, atactic polystyrene, poly(methyl methacrylate) isotactic, poly(methyl methacrylate) atactic, thermoplastic polyester elastomers (TPE), and thermoplastic polyamide elastomers (TPA).
[0010] Advantageously, the thermoplastic polymer powder comprises as additive a radiation absorber dispersed in the volume of the polymer particles or on the surface of the polymer particles in an amount of 0.01% to 10% by weight, advantageously the thermoplastic polymer powder comprises a radiation absorber additive homogeneously dispersed in the volume of the particles in an amount of 0.01% to 2% by weight.
[0011] Advantageously, the radiation absorbing additive is carbon black, carbon fibres less than 0.2 mm in length, carbon nanotubes, fullerene-C60, magnetite (Fe3O4), hematite (Fe2O3), black iron(II) oxide (FeO), copper(II) oxide (CuO), ultramarine, pigments based on cobalt(II,III) (Co3O4), copper phthalocyanine blue BN (CAS 147-14-8), cobalt blue (Thennard blue, CoAl2O4), polyaniline (CAS 25233-30-1), nigrosine or a mixture thereof, and advantageously, the infrared absorbing additive is a pigment based on carbon black or magnetite.
[0012] The device ensuring the breakup of agglomerates of the particles of the thermoplastic polymer powder is a Venturi ejector (1), the suction of which is connected by a hydraulic line (6) to a reservoir of the thermoplastic polymer powder.
[0013] The device (9) for ensuring the breakage of powder particle agglomerates according to the invention is a device equipped with a screw feeder and a sieve subjected to mechanical vibration and / or shaking.
[0014] The device (9) for ensuring the breakage of powder particle agglomerates according to the invention is a device comprising a screw feeder and a mechanical impact element subjected to mechanical vibration and / or oscillation.
[0015] Advantageously, the element (10) which ensures near free-fall conditions for the powder particles and separates the shielding gas from the powder suspended in the carrier gas is a perforated element.
[0016] Advantageously, the carrier gas (8) is a shielding gas in which controlled crystallization takes place and at the same time a substance or element from the group consisting of air, nitrogen, argon, helium, carbon dioxide, sulphur hexafluoride or mixtures thereof, advantageously the carrier gas is nitrogen, argon or sulphur hexafluoride.
[0017] Advantageously, the temperature of the carrier gas (8) is below the melting point or the Type II phase transition temperature of the thermoplastic polymer powder but above 25° C., advantageously the carrier gas is supplied at a temperature between 20° C. and 50° C. below the melting point or the Type II phase transition temperature of the thermoplastic polymer powder.
[0018] Advantageously, the carrier gas and the powder suspended in the carrier gas are introduced into the reactor as a result of the reduced pressure existing within the reactor.
[0019] The reduced pressure in the reactor is created by a vacuum pump or a venturi ejector. Advantageously, the reduced pressure in the reactor is created by a vacuum pump.
[0020] The radiation source is a filament-based infrared emitter.
[0021] The radiation source is a laser.
[0022] Advantageously, the filament of the infrared emitter (3) is heated to a temperature in the range of 600°C to 2500°C, advantageously, the filament of the infrared emitter is heated to a temperature of 2200°C ± 100°C, causing emission of a radiation spectrum having a maximum spectral irradiance per wavelength in the range of 1.0 μm to 1.4 μm.
[0023] Advantageously, the ratio of the nominal power of the filament infrared emitter to the cross-sectional area of the transparent chamber illuminated by said emitter is in the range from 6.7 kW / m2 to 670 kW / m2, advantageously in the range from 10 kW / m2 to 100 kW / m2.
[0024] Advantageously, the wavelength of the radiation emitted by the laser is one of the following: 0.01 mm (CO2 laser), 0.001064 mm (Nd-YAG laser), 0.001319 mm (Nd-YAG laser), 0.0008 mm (NIR diode laser) and 0.00045 mm (blue diode laser).
[0025] Advantageously, the radiation source, while located within the optically transparent chamber, is oriented perpendicular to the direction of powder flow, with the path of the radiation successively traversing the walls of the optically transparent chamber, the interior of the optically transparent chamber which is filled with polymer powder suspended in a flowing carrier gas, and the opposing wall of the optically transparent chamber.
[0026] Advantageously, the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, and the path of the radiation successively traverses the walls of the optically transparent chamber, the interior of the optically transparent chamber which is filled with polymer powder suspended in a flowing carrier gas, the walls of the optically transparent chamber, and a layer of metal mirror which reflects the radiation back into the interior of the optically transparent chamber.
[0027] Advantageously, the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, with the path of the radiation successively traversing the walls of the optically transparent chamber, the interior of the transparent chamber filled with polymer powder suspended in a flowing carrier gas, the walls of the transparent chamber, and the collimated radiation source.
[0028] Advantageously, the optically transparent chamber is made of borosilicate glass, sodium glass, lead glass or fused quartz characterized by an average transmittance of more than 90% within the wavelength range of radiation from 0.001 mm to 0.0025 mm, measured on a sample having a thickness of 2 mm; advantageously, the chamber is made from fused quartz characterized by an average transmittance having a value of more than 90% within the range of radiation wavelengths from 0.001 mm to 0.0025 mm, measured on a sample having a thickness of 2 mm; most advantageously, the chamber is made from fused quartz, commercially known under the name JGS-2 or JGS-3.
[0029] Advantageously, the controlled crystallization is carried out in a shielding gas having a temperature ranging from 25° C. to 20° C. below the melting point or the type II phase transition temperature of the polymer powder, and advantageously, the controlled crystallization is carried out in argon, nitrogen or sulfur hexafluoride having a temperature ranging from 25° C. to 50° C. below the melting point or the type II phase transition temperature of the polymer powder.
[0030] The advantage of the solution according to the invention is the use of a radiation heat transport mechanism to effect a controlled melting of the thermoplastic polymer powder undergoing spheronization. The invention is characterized by the use of a shielding gas temperature lower than the melting point of the polymer being spheronized, thereby minimizing the risk of thermal degradation of the thermoplastic polymer. Furthermore, this solution allows control over the exact location in the flow chamber where the particles of thermoplastic polymer are expected to melt. This solution reduces the problem of molten particles adhering to the walls of the flow chamber, known to exist in systems where the temperature of the shielding gas exceeds the melting point of the thermoplastic polymer particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Example 1) A powder material based on polyamide 12 with a D90 of less than 0.130 mm, a number-average circularity parameter of 0.70 and a number-average roundness parameter of 0.65 was fed into the reactor at 100° C. in air. The powder material was introduced into a transparent flow chamber made of borosilicate glass with a circular cross section, diameter 35 mm, wall thickness 1 mm and length 300 mm. The powder material was introduced at a rate of 0.03 kg / h. In this example, a filament infrared emitter with a nominal power to irradiated area ratio of 66 kW / m2 and an aluminum reflector layer conformal to the surface of the optically transparent chamber opposite the radiation source was used to reflect the unabsorbed radiation back into the transparent chamber. The powder was introduced through a flat nozzle with a variable cross section, the detailed shape of the cross section is not reported here as it is not the subject of this application. The controlled crystallization was carried out in air at room temperature. The resulting material was subjected to size distribution and shape analysis using microscopic image analysis, where the polymeric material was analyzed in suspension in liquid to avoid the formation of agglomerates that may interfere with the measurements. The powder material obtained after spheronization was characterized by a particle size with D90 less than 0.145 mm, a number average circularity coefficient of 0.79 and a number average circularity parameter of 0.75. The results indicate an improvement in the overall sphericity of the powder, exhibiting a more spherical and regular average particle shape than the feed material.
[0032] Example 2) A powder material based on polyamide 12 with a D90 of less than 0.130 mm, a number average circularity of 0.70, and a number average circularity of 0.65 was fed into the reactor at 150 °C in air. The powder material was introduced into a transparent flow chamber with a circular cross-sectional shape, an inner diameter of 40 mm, a wall thickness of 3 mm, and a length of 300 mm, made of quartz glass with the commercial designation JGS-2. The powder material was introduced at a rate of 0.03 kg / h. In this example, a filament infrared emitter with a nominal power to irradiated area ratio of 66 kW / m2 and an aluminum reflective layer conformal to the surface of the optically transparent chamber opposite the radiation source was used to reflect the unabsorbed radiation back into the transparent chamber. The powder was introduced through a flat nozzle with a variable cross-sectional area, the detailed shape of the cross-section is not the subject of this application and is not reported here. The controlled crystallization was carried out in air at room temperature. The resulting material was subjected to granulation distribution and shape analysis using microscopic image analysis, where the polymeric material was analyzed in suspension in liquid to avoid the formation of agglomerates that could interfere with the measurements. The resulting powder material was characterized by a particle size with a D90 of less than 151 μm, a number average circularity parameter of 0.81, and a number average circularity coefficient of 0.79. The results indicate an improvement in the overall sphericity of the powder, exhibiting a more spherical and regular average particle shape than the feed material.
[0033] Example 3) A polyamide 12-based powder material with a D90 of 0.146 mm, number-average circularity of 0.62, and circularity of 0.55 was fed into the reactor at 100° C. in air. The powder material was introduced into a transparent flow chamber with a circular cross-sectional shape, made of fused quartz, commercially known as JGS-2, with an inner diameter of 17 mm, a wall thickness of 1.5 mm, and a height of 300 mm. The powder material was introduced at a rate of 0.002 kg / h. In this example, a filament infrared emitter with a nominal power-to-irradiation area ratio of 70 kW / m2 and a gold reflector layer coherent with the optically transparent chamber surface located on the opposite side to the radiation source was used to reflect unabsorbed radiation back into the transparent chamber. The powder was fed through a screw feeder integrated with a vibrating-oscillating screen feeder and then directed into a perforated element that ensures near-free-fall conditions for the powder particles and separates the shielding gas from the powder suspended in the carrier gas. The controlled crystallization was carried out at 70 °C in air. The resulting material was subjected to particle size distribution and shape analysis using microscopic image analysis, where the polymeric material was analyzed while suspended in a non-solvent to avoid the formation of aggregates that may interfere with the measurements. The powder material obtained after spheronization by the method described in this example was characterized by a particle size of D90 of 167 μm, a number average circularity parameter of 0.91, and a number average circularity coefficient of 0.81. The results show an improvement in the overall sphericity of the powder, and a shift towards a more spherical and regular average particle shape than the feed material.
[0034] Example 4) A polypropylene-based powder material with a D90 of 0.125 mm, number average circularity of 0.68, and circularity of 0.63 was fed into the reactor at 100°C in air. The powder material was introduced into a transparent flow chamber with a circular cross-sectional shape, made of fused quartz, commercially known as JGS-2, with an inner diameter of 17 mm, a wall thickness of 1.5 mm, and a height of 300 mm. The powder material was introduced at a rate of 0.0015 kg / h. In this example, a filament infrared emitter with a nominal power to irradiation area ratio of 70 kW / m2 and a gold reflector layer coherent with the optically transparent chamber surface located on the opposite side to the radiation source was used to reflect unabsorbed radiation back into the transparent chamber. The powder was fed through a screw feeder integrated with a vibrating-oscillating screen feeder and then directed into a perforated element that ensures near free-fall conditions for the powder particles and separates the shielding gas from the powder suspended in the carrier gas. The controlled crystallization was carried out at 70 °C in air. The resulting material was subjected to particle size distribution and shape analysis using microscopic image analysis, where the polymeric material was analyzed while suspended in a non-solvent to avoid the formation of aggregates that may interfere with the measurements. The powder material obtained after spheronization by the method described in this example was characterized by a particle size of D90 of 160 μm, a number average circularity parameter of 0.89, and a number average circularity coefficient of 0.85. The results show an improvement in the overall sphericity of the powder, and a shift towards a more spherical and regular average particle shape than the feed material.
[0035] Example 5) Powder material based on thermoplastic polyurethane (TPU), with D90 of 0.143 mm, number average circularity of 0.82, and circularity of 0.62, was fed into the reactor at 100°C in air. The powder material was introduced into a transparent flow chamber with a circular cross-sectional shape, made of fused quartz, commercially known as JGS-2, with an inner diameter of 17 mm, a wall thickness of 1.5 mm, and a height of 300 mm. The powder material was introduced at a rate of 0.0027 kg / h. In this example, a filament infrared emitter with a nominal power to irradiation area ratio of 70 kW / m2 and a gold reflector layer coherent with the optically transparent chamber surface located on the side opposite the radiation source was used to reflect unabsorbed radiation back into the transparent chamber. The powder was fed through a screw feeder integrated with a vibrating-oscillating screen feeder and then directed into a perforated element that ensures near free-fall conditions of the powder particles and separates the shielding gas from the powder suspended in the carrier gas. The controlled crystallization was carried out at 70 °C in air. The resulting material was subjected to particle size distribution and shape analysis using microscopic image analysis, where the polymeric material was analyzed while suspended in a non-solvent to avoid the formation of aggregates that may interfere with the measurements. The powder material obtained after spheronization by the method described in this example was characterized by a particle size of D90 of 152 μm, a number average circularity parameter of 0.90 and a number average circularity coefficient of 0.93. The results show an improvement in the overall sphericity of the powder and a shift towards a more spherical and regular average particle shape than the feed material. [Brief description of the drawings]
[0036] [Figure 1] FIG. 1 shows a schematic diagram of the spheronization of thermoplastic polymer powder. [Diagram 2] FIG. 2 shows particles of thermoplastic polymer subjected to a spheronization process according to Example 1. [Diagram 3] FIG. 3 shows a schematic diagram of the spheronization of thermoplastic powders using a free-fall technique and a mechanism for drawing the powder and shielding gas into a reactor by a partial vacuum.
Claims
1. 1. A method for increasing the sphericity of particles of a thermoplastic polymer powder, comprising the successive steps of: (a) introduction of the polymer powder (by entrainment in a gas flow) into a device ensuring the destruction of agglomerates of the powder particles; (b) transport of the deagglomerated powder through a nozzle (2) into an optically transparent flow chamber (4) located in the area covered by the radiation generated by a radiation source (3); (c) absorption of the radiation by the powder, causing either complete melting of the polymer powder particles or a type II phase transition; (d) removal of the molten powder particles from the radiation zone by suspension in a carrier gas continuously supplied via a pneumatic connection (5); (e) spontaneous spheronization of the molten polymer particles while being entrained by the gas; and (f) the process of controlled crystallization of the polymer in the carrier gas, which takes place in a controlled crystallization chamber (6).
2. Said thermoplastic polymer powders are preferably made from the polymers in question, in particular polyamide-4, polyamide-6, polyamide-7, polyamide-8, polyamide-9, polyamide-11, polyamide-12, polyamide-46, polyamide-66, polyamide-69, polyamide-510, polyamide-610, polyamide-613, polyamide-1010, polyamide-1012, polyamide-1212, polyamide-1313, polyamide-6T, polyamide-6 / 66, polyamide-6 / 12, polyamide-612, copolymers of these polyamides, polypropylene (PP), low density polyethylene (LDPE), high density polyethylene (HDPE), low density branched polyethylene (LLDPE), copolymers of polypropylene and polyethylene (PP-PE), poly[ 2. The method of claim 1, wherein the melting point or type II phase transition temperature range is always lower than the onset of thermal decomposition temperature of polymer powders based on [(ethylene)-co-(vinyl acetate)] (EVA), polyethylene wax (low molecular weight polyethylene), paraffin wax with a melting point below 70° C., ultra-high molecular weight polyethylene (UHDPE), poly(butylene terephthalate) (PBT), polyether ether ketone (PEEK), poly(oxymethylene) (POM), thermoplastic polyurethane elastomers (TPU), isotactic polystyrene, atactic polystyrene, poly(methyl methacrylate) isotactic, poly(methyl methacrylate) atactic, thermoplastic polyester elastomers (TPE), and thermoplastic polyamide elastomers (TPA).
3. 3. The method according to claim 2, wherein the thermoplastic polymer powder comprises as additive a radiation absorber dispersed in the volume of the polymer particles or on the surface of the polymer particles in an amount of 0.01% to 10% by weight, advantageously the thermoplastic polymer powder comprises a radiation absorber additive homogeneously dispersed in the volume of the particles in an amount of 0.01% to 2% by weight.
4. 4. The method according to claim 3, wherein the radiation absorbing additive is carbon black, carbon fibres less than 0.2 mm in length, carbon nanotubes, fullerene-C60, magnetite (Fe3O4), hematite (Fe2O3), black iron(II) oxide (FeO), copper(II) oxide (CuO), ultramarine, pigments based on cobalt(II,III) (Co3O4), copper phthalocyanine blue BN (CAS 147-14-8), cobalt blue (Tennard blue, CoAl2O4), polyaniline (CAS 25233-30-1), nigrosine or a mixture thereof, advantageously the infrared absorbing additive is a pigment based on carbon black or magnetite.
5. 2. The method according to claim 1, wherein the device ensuring the breakage of agglomerates of the thermoplastic polymer powder particles is a Venturi ejector (1), the suction of which is connected by a hydraulic line (6) to a reservoir of the thermoplastic polymer powder.
6. 2. The method according to claim 1, wherein the temperature of the carrier gas (8) is below the melting point or the type II phase transition temperature of the thermoplastic polymer powder but not below 25°C below said temperature, advantageously the carrier gas is supplied at a temperature between 20°C and 70°C below the melting point or the type II phase transition temperature of the thermoplastic polymer powder.
7. 2. The method according to claim 1, wherein the temperature of the carrier gas (8) is below the melting point or the type II phase transition temperature of the thermoplastic polymer powder but above 25°C, advantageously the carrier gas is supplied at a temperature between 20°C and 50°C below the melting point or the type II phase transition temperature of the thermoplastic polymer powder.
8. The method of claim 1 , wherein the radiation source is a filament-based infrared emitter.
9. The method of claim 1 , wherein the radiation source is a laser.
10. 9. The method according to claim 8, wherein the filament of the infrared emitter (3) is heated to a temperature in the range of 600°C to 2500°C, advantageously the filament of the infrared emitter is heated to a temperature of 2200°C ± 100°C, causing emission of a radiation spectrum having a maximum spectral irradiance per wavelength in the range of 1.0 μm to 1.4 μm.
11. 2. The method according to claim 1, wherein the ratio of the nominal power of the filament infrared emitter to the cross-sectional area of the transparent chamber illuminated by the emitter is in the range of 6.7 kW / m2 to 670 kW / m2, preferably in the range of 10 kW / m2 to 100 kW / m2.
12. 10. The method of claim 9, wherein the wavelength of the radiation emitted by the laser is one of: 0.01 mm (CO2 laser), 0.001064 mm (Nd-YAG laser), 0.001319 mm (Nd-YAG laser), 0.0008 mm (NIR diode laser), and 0.00045 mm (blue diode laser).
13. 2. The method of claim 1, wherein the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, and the path of the radiation successively traverses a wall of the optically transparent chamber, an interior of the optically transparent chamber filled with polymer powder suspended in the flowing carrier gas, and an opposing wall of the optically transparent chamber.
14. 2. The method of claim 1, wherein the radiation source is oriented perpendicular to the direction of powder flow while positioned within the optically transparent chamber, and the path of the radiation successively traverses the walls of the optically transparent chamber, the interior of the optically transparent chamber filled with polymer powder suspended in the flowing carrier gas, the walls of the optically transparent chamber, and a layer of metal mirror that reflects the radiation into the interior of the optically transparent chamber.
15. 2. The method of claim 1, wherein the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, and the path of the radiation successively traverses the walls of the optically transparent chamber, the interior of the transparent chamber filled with polymer powder suspended in the flowing carrier gas, the walls of the transparent chamber, and the collimated radiation source.
16. 2. The method of claim 1, wherein the optically transparent chamber is made of borosilicate glass, sodium glass, lead glass, or fused quartz characterized by an average transmittance of more than 90% in the radiation wavelength range of 0.001 mm to 0.0025 mm, measured on a sample with a thickness of 2 mm, advantageously the chamber is made from fused quartz characterized by an average transmittance having a value of more than 90% in the radiation wavelength range of 0.001 mm to 0.0025 mm, measured on a sample with a thickness of 2 mm, and most advantageously the chamber is made from fused quartz commercially known under the name JGS-2 or JGS-3.
17. 2. The method according to claim 1, wherein the controlled crystallization is carried out in a shielding gas having a temperature ranging from 25° C. to 20° C. below the melting point or type II phase transition temperature of the polymer powder, advantageously the controlled crystallization is carried out in argon, nitrogen or sulfur hexafluoride having a temperature ranging from 25° C. to 50° C. below the melting point or type II phase transition temperature of the polymer powder.
18. A method for increasing the sphericity of particles of a thermoplastic polymer powder, comprising: (a) introducing the polymer powder into a device (9) that ensures the destruction of agglomerates of the powder particles; (b) transporting the deagglomerated powder to a device (10) that ensures near free-fall motion of the powder and separates the shielding gas from the powder suspended in the carrier gas; (c) transporting the suspended powder and the shielding gas into an optically transparent flow chamber (12) caused by reducing the pressure in the flow chamber by the action of a vacuum generator (14); and (d) transporting the suspended powder and the shielding gas into an optically transparent flow chamber (12) by radiation absorption or a combination of radiation absorption and convective heat transfer. (e) complete or partial melting or complete or partial Type II phase transition of the particles of the powder as a result of the energy transfer; (f) removal of the molten particles from the radiation zone by the carrier gas drawn from a chamber (15) into an optically transparent flow reactor under the action of the vacuum generator (14) while the liquid polymer particles undergo spontaneous spheronization; and (g) the process of controlled crystallization of the polymer in the carrier gas occurring in a controlled crystallization chamber (13).
19. Said thermoplastic polymer powders are preferably selected from the polymers in question, in particular polyamide-4, polyamide-6, polyamide-7, polyamide-8, polyamide-9, polyamide-11, polyamide-12, polyamide-46, polyamide-66, polyamide-69, polyamide-510, polyamide-610, polyamide-613, polyamide-1010, polyamide-1012, polyamide-1212, polyamide-1313, polyamide-6T, polyamide-6 / 66, polyamide-6 / 12, polyamide-612, copolymers of these polyamides, polypropylene (PP), low density polyethylene (LDPE), high density polyethylene (HDPE), low density branched polyethylene (LLDPE), copolymers of polypropylene and polyethylene (PP-PE), poly[( 19. The method of claim 18, wherein the melting point or type II phase transition temperature range is always lower than the onset of thermal decomposition temperature of polymer powders based on: [(ethylene)-co-(vinyl acetate)] (EVA), polyethylene wax (low molecular weight polyethylene), paraffin wax with a melting point below 70° C., ultra-high molecular weight polyethylene (UHDPE), poly(butylene terephthalate) (PBT), polyether ether ketone (PEEK), poly(oxymethylene) (POM), thermoplastic polyurethane elastomers (TPU), isotactic polystyrene, atactic polystyrene, poly(methyl methacrylate) isotactic, poly(methyl methacrylate) atactic, thermoplastic polyester elastomers (TPE), and thermoplastic polyamide elastomers (TPA).
20. 20. The method according to claim 19, wherein the thermoplastic polymer powder comprises as additive a radiation absorber dispersed in the volume of the polymer particles or on the surface of the polymer particles in an amount of 0.01% to 10% by weight, advantageously the thermoplastic polymer powder comprises a radiation absorber additive homogeneously dispersed in the volume of the particles in an amount of 0.01% to 2% by weight.
21. 21. The method according to claim 20, wherein the radiation absorbing additive is carbon black, carbon fibres less than 0.2 mm in length, carbon nanotubes, fullerene-C60, magnetite (Fe3O4), hematite (Fe2O3), black iron(II) oxide (FeO), copper(II) oxide (CuO), ultramarine, pigments based on cobalt(II,III) (Co3O4), copper phthalocyanine blue BN (CAS 147-14-8), cobalt blue (Tennard blue, CoAl2O4), polyaniline (CAS 25233-30-1), nigrosine or a mixture thereof, advantageously the infrared absorbing additive is a pigment based on carbon black or magnetite.
22. 20. The method of claim 19, wherein the thermoplastic polymer powder does not include the radiation absorber additive, and the radiation absorption is provided by the polymer that undergoes the spheronization.
23. 19. The method according to claim 18, wherein the device (9) for ensuring the breakage of powder agglomerates is a device comprising a screw feeder and a screen mesh subjected to mechanical vibration and / or agitation.
24. 19. The method according to claim 18, wherein the device (9) for ensuring the breakage of the powder agglomerates is a device comprising a screw feeder and a mechanical impact element subjected to mechanical vibration and / or oscillation.
25. 20. The method of claim 18, wherein the element (10) that provides conditions approximating the free-fall motion of the powder particles and separates the shielding gas from the powder suspended in the carrier gas is a perforated element that is subjected to mechanical vibration.
26. 19. The method according to claim 18, wherein the carrier gas is supplied at a temperature below the melting point or the Type II phase transition temperature of the thermoplastic polymer powder but at the same time above 25°C, advantageously the carrier gas is supplied at a temperature between 20°C and 70°C below the melting point or the Type II phase transition temperature of the thermoplastic polymer powder.
27. 19. The method according to claim 18, wherein the temperature of the carrier gas (8) is below the melting point or the type II phase transition temperature of the thermoplastic polymer powder but above 25°C, advantageously the carrier gas is supplied at a temperature between 20°C and 50°C below the melting point or the type II phase transition temperature of the thermoplastic polymer powder.
28. 20. The method of claim 18, wherein the radiation source is a filament-based infrared emitter.
29. 20. The method of claim 18, wherein the radiation source is a laser.
30. 29. The method according to claim 28, wherein the filament of the infrared emitter (3) is heated to a temperature in the range of 600°C to 2500°C, advantageously the filament of the infrared emitter is heated to a temperature of 2200°C ± 100°C causing emission of a radiation spectrum having a maximum spectral irradiance per wavelength in the range of 1.0 μm to 1.4 μm.
31. 19. The method according to claim 18, wherein the ratio between the nominal power of the filament infrared emitter and the cross-sectional area of the transparent chamber illuminated by the emitter is in the range of 1 kW / m2 to 1000 kW / m2, advantageously in the range of 10 kW / m2 to 100 kW / m2.
32. 30. The method of claim 29, wherein the wavelength of the radiation emitted by the laser is one of: 0.01 mm (CO2 laser), 0.001064 mm (Nd-YAG laser), 0.001319 mm (Nd-YAG laser), 0.0008 mm (NIR diode laser), and 0.00045 mm (blue diode laser).
33. 20. The method of claim 18, wherein the radiation source is oriented perpendicular to the direction of powder flow while positioned within the optically transparent chamber, and the path of the radiation successively traverses a wall of the optically transparent chamber, an interior of the optically transparent chamber filled with polymer powder suspended in the flowing carrier gas, and an opposing wall of the optically transparent chamber.
34. 20. The method of claim 18, wherein the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, and the path of the radiation successively traverses a wall of the optically transparent chamber, an interior of the optically transparent chamber filled with polymer powder suspended in the flowing carrier gas, a wall of the optically transparent chamber, and a layer of a metal mirror that reflects the radiation into the interior of the optically transparent chamber.
35. 20. The method of claim 18, wherein the radiation source is oriented perpendicular to the direction of powder flow while located within the optically transparent chamber, and the path of the radiation successively traverses the walls of the optically transparent chamber, the interior of the transparent chamber filled with polymer powder suspended in the flowing carrier gas, the walls of the transparent chamber, and the collimated radiation source.
36. 20. The method of claim 18, wherein the radiation source is oriented perpendicular to the direction of powder flow while positioned within the optically transparent chamber, and the path of the radiation successively traverses a wall of the optically transparent chamber, an interior of the transparent chamber filled with polymer powder suspended in the flowing carrier gas, and a layer of a metal mirror that reflects the radiation into the interior of the optically transparent chamber.
37. 19. The method according to claim 18, wherein the optically transparent chamber is made of borosilicate glass, sodium glass, lead glass or fused quartz characterized by an average transmittance of more than 90% in the radiation wavelength range of 0.001 mm to 0.0025 mm measured on a sample having a thickness of 2 mm, advantageously the chamber is made from fused quartz characterized by an average transmittance having a value of more than 90% in the radiation wavelength range of 0.001 mm to 0.0025 mm measured on a sample having a thickness of 2 mm, and most advantageously the chamber is made from fused quartz commercially known under the name JGS-2 or JGS-3.
38. 19. The method according to claim 18, wherein the controlled crystallization is carried out in a shielding gas having a temperature ranging from 25° C. to 20° C. below the melting point or type II phase transition temperature of the polymer powder, advantageously the controlled crystallization is carried out in argon, nitrogen or sulfur hexafluoride having a temperature ranging from 25° C. to 50° C. below the melting point or type II phase transition temperature of the polymer powder.
39. 19. The method according to claim 18, wherein the powder suspended in the shielding gas and the carrier gas is introduced into the reactor under the effect of a reduced pressure in the reactor, the reduced pressure being generated by a vacuum pump or a venturi ejector, advantageously the reduced pressure being generated by a vacuum pump.
40. 2. The method according to claim 1, wherein the powder suspended in the shielding gas and the carrier gas is introduced into the reactor under the effect of a reduced pressure in the reactor, the reduced pressure being generated by a vacuum pump or a venturi ejector, advantageously the reduced pressure being generated by a vacuum pump.
Citation Information
Patent Citations
Device and method for performing spheroidizing treatment on powder by using line-focus solar furnace
CN110052618A
Furnace apparatus for smashing to spherical pieces
JP1979065175A
Cited By
Method for producing fine particles and device for producing fine particles
WO2026126426A1