Copper alloy electrical connector parts, coatings on copper alloy electrical connector parts, and methods for forming coatings on copper alloy electrical connector parts
Patent Information
- Application Number
- JP2024532819
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-02
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024544197000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to Copper alloy electrical connector parts,Copper alloy electrical connector parts coating and method for forming a coating on a copper alloy electrical connector component - Patents.com Regarding. [Background technology]
[0002] This section provides background information related to the present disclosure. It is not necessarily prior art.
[0003] Tin coatings have been used for many years by terminal and connector manufacturers to provide a stable separable contact interface over the life of the connector. Tin plating is relatively soft, allowing the mating contacts to break through the thin surface oxide that may form at fairly low loads, providing a good electrical path between the mating parts. Thinner tin coatings are generally more desirable because they generally provide lower normal force resistance and reduced coefficient of friction. However, the thickness of the tin layer must be sufficient so that the formation of tin-copper intermetallic compounds does not "use up" the available free tin and change the physical properties of the connector. Various barrier layers, such as Ni layers and Ni and Cu layers, have been introduced to reduce the formation of tin-copper intermetallic compounds and allow thinner tin layers to reduce friction. Efforts to improve tin coatings and reduce friction are ongoing. Summary of the Invention [Problem to be solved by the invention]
[0004] Books The disclosed embodiments include 、 Improved Tin Coating Copper alloy electrical connector component having a coating thereon, a coating on the copper alloy electrical connector component, and a method for forming a coating on the copper alloy electrical connector component provide. [Means for solving the problem]
[0005] The present invention relates to a copper alloy electrical connector component, comprising a nickel layer between about 5 μin and about 20 μin on said copper alloy, a copper layer between about 7 μin and about 18 μin on said nickel layer, one or more silver layers between about 5 μin and about 15 μin in total on said copper layer, and one or more tin layers between about 40 μin and about 80 μin in total, wherein the silver and tin layers are mixed to form between about 8 vol% and about 45 vol% Ag by reflow heating of said copper alloy electrical connector. 3 A coating is formed which induces the formation of Sn intermetallic compounds. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPIB at 100× magnification. [Diagram 2] FIG. 2 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPID at 100× magnification. [Diagram 3] FIG. 3 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPIA at 100× magnification. [Figure 4] FIG. 4 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPIC at 100× magnification. [Figure 5A] FIG. 5A is an SEM micrograph of sample PPIB at 10 kV. [Figure 5B] FIG. 5B is an EDS analysis of PPIB at the location identified in FIG. 5A. [Figure 6] FIG. 6 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPII at 100× magnification. [Figure 7] FIG. 7 is an optical micrograph of the post-reflow surfaces of sides A and B of sample PPIJ at 100× magnification. [Figure 8] FIG. 8 is a TEM image and EDS map of sample PPIA, showing the absence of a silver layer and the presence of a copper layer. [Figure 9] FIG. 9 is a TEM image and EDS map of sample PPIB, showing the absence of a silver layer and the presence of a copper layer. [Figure 10] Figure 10 shows the EDS line scan of sample PPIA. [Figure 11] Figure 11 shows the EDS line scan of sample PPIB. [Figure 12] FIG. 12 is a TEM image of sample PPIA, with the layers and phases identified. [Figure 13] FIG. 13 is a composite EDS map of PPIA, with crosshairs indicating the locations of layer thickness measurements. [Figure 14]FIG. 14 is a TEM image of sample PPIA, with the layers and phases identified. [Figure 15] FIG. 15 is a composite EDS map of the PPIA, with crosshairs indicating the locations of layer thickness measurements. [Figure 16] Figure 16 is a scatter plot of the individual R / N points versus the volume fraction of Ag3Sn intermetallic compounds in the surface coating, showing that the R / N decreases with increasing volume fraction of Ag3Sn intermetallic compounds in the surface coating, and the variance also decreases with increasing volume fraction of Ag3Sn. [Figure 17] FIG. 17 is a scatter plot of the average R / N versus the volume fraction of Ag3Sn intermetallic compounds in the surface coating. It shows that the average R / N decreases with increasing volume fraction of Ag3Sn intermetallic compounds in the surface coating. Corresponding reference characters indicate corresponding parts throughout the several views of the drawing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] This section provides a summary of the disclosure and is not an exhaustive disclosure of its complete scope or all of its features.
[0008] The present disclosure provides for a layer of silver under a layer of tin. The inventors have found that the frictional force of a tin-coated electrical connector is increased by the presence of tin-silver intermetallic compounds in the tin layer, particularly Ag in the tin layer. 3 It was observed that the Sn intermetallic compound volume fraction reduced the Sn content.
[0009] In one embodiment, the present disclosure provides a coating on a copper alloy electrical connector component. The coating may be formed by applying between about 5 μin and about 20 μin of nickel layer onto the copper alloy of the electrical connector component, and then applying between about 7 μin and about 18 μin of copper layer onto the nickel layer. This provides a barrier to diffusion and reduces the formation of tin-copper intermetallic compounds that may otherwise consume the available tin of the tin layer. Eventually, the copper of the barrier layer will form a tin-copper intermetallic compound with the tin, and the nickel layer and tin-copper intermetallic compound layer will retard further loss of tin to the formation of intermetallic compounds with the copper from the connector component. A layer of silver and tin is applied onto the copper layer, and the Ag layer is removed by a reflow process ... 3 This is followed by the formation of a silver-tin layer containing Sn intermetallic compounds.
[0010] Typically, between about 5 μin and about 15 μin of silver and between about 40 μin and about 80 μin of tin are applied. This may be a single layer of silver on a copper layer and a single layer of tin on a silver layer. Alternatively, this may be multiple layers of silver and tin stacked on top of each other on a copper layer. Coated copper alloy electrical connector components have a mixture of silver and tin layers and at least 8 vol. %, preferably between 8 vol. % and about 40 vol. %, Ag. 3 It is heated to cause the formation of Sn intermetallic compounds.
[0011] In another embodiment, the present disclosure provides a method of providing a coating on a copper alloy electrical connector component. The method includes applying a layer of nickel between about 5 μin and about 20 μin onto the copper alloy and applying a layer of copper between about 7 μin and about 18 μin onto the nickel layer. One or more layers of silver and tin are then applied onto the copper layer, followed by a reflow process and Ag+ ... 3 This is followed by the formation of a silver-tin layer containing Sn intermetallic compounds.
[0012] Typically, between about 5 μin and about 15 μin of silver and between about 40 μin and about 80 μin of tin are applied. This may be a single layer of silver on a copper layer and a single layer of tin on a silver layer. Alternatively, this may be multiple layers of silver and tin stacked on top of each other on a copper layer. Coated copper alloy electrical connector components contain a mixture of silver and tin layers and at least 8 vol. %, preferably between 8 vol. % and about 40 vol. %, Ag. 3 It is heated to cause the formation of Sn intermetallic compounds.
[0013] In another embodiment, the present disclosure provides a copper alloy electrical connector component having a coating. The coating is formed by applying between about 5 μin and about 20 μin of nickel layer onto the copper alloy of the electrical connector component, and then applying between about 7 μin and about 18 μin of copper layer onto the nickel layer. This provides a barrier to diffusion and reduces the formation of tin-copper intermetallic compounds that may otherwise consume the available tin of the tin layer. Eventually, the copper of the barrier layer will form a tin-copper intermetallic compound with the tin, and the nickel layer and tin-copper intermetallic compound layer will retard further loss of tin to the formation of intermetallic compounds with the copper from the connector component. A layer of silver and tin is applied onto the copper layer, and the Ag layer is removed by a reflow process ... 3 This is followed by the formation of a silver-tin layer containing Sn intermetallic compounds.
[0014] Typically, between about 5 μin and about 50 μin of silver and between about 40 μin and about 80 μin of tin are applied. This may be a single layer of silver on a copper layer and a single layer of tin on a silver layer. Alternatively, this may be multiple layers of silver and tin stacked on top of each other on a copper layer. Coated copper alloy electrical connector components may include a mixture of silver and tin layers and at least 8 vol.% Ag. 3 It is heated to cause the formation of Sn intermetallic compounds.
[0015] Further areas of applicability will become apparent from the description provided herein. The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.
[0016] The drawings described herein are for illustrative purposes of only selected embodiments rather than all possible implementations and are not intended to limit the scope of the present disclosure.
[0017] Example embodiments will now be described in more detail with reference to the accompanying drawings. EXAMPLES
[0018] Tin coatings were formed on copper alloy substrates with a nickel-copper barrier layer and a silver layer between the barrier layer and the tin layer, with two different thicknesses for the tin layer and two different thicknesses for the silver layer. The samples were subjected to a reflow process, and the friction (R / N) was measured and averaged on each side of the substrate. The results are shown in Table 1.
[0019] [Table 1]
[0020] The coefficient of friction for the values reported in this disclosure was determined using a linear reciprocating rider-on-flat method typical in the industry for evaluating electrical connector materials. The test was performed by sliding a 1 / 8" diameter hemispherical rider of the material over the flat of the material under a load of 2.5 N (250 gf) in dry conditions over a length of 3 mm at a speed of 3 mm / s for 10 cycles. One cycle was 3 mm forward and 3 mm backward. The contact speed portion of each cycle was 60% of the cycle. The duration of each test was 25 seconds.
[0021] The R / N values measured from this test represent the sliding friction coefficient, where R was the measured traction force and N was the applied normal force. The R / N value, which was considered the final result of each test, was calculated as the average R / N for 10 forward and 10 backward movements. The R / N of each movement was taken as the portion of the movement with the highest average R / N from a total length of five consecutive data points. This corresponded to approximately 0.5 mm of movement.
[0022] The coefficient of friction was generally lower for the thicker Ag-underplated samples PPIB and PPID. As can be seen from Table 1, the lowest sample average R / N(PPIB) had a combination of thick Ag and thin Sn (15 / 37) and the highest sample average R / N(PPIC) had a combination of thin Ag and thick Sn (5 / 75).
[0023] Figures 1 to 4 show optical micrographs of the reflowed surfaces of Samples A to D, presented in the same order as in Table 1, i.e., ascending R / N. These micrographs show a blue-grey second phase at the reflowed surface, the volume fraction of which visibly decreases from Figures 1 to 4. As can be seen from these figures, an increase in R / N is associated with a decrease in the amount of the second phase.
[0024] FIG. 5B shows an EDS analysis of the blue-gray phase of FIGS. 1-4. The composition of this phase, shown in the inset of the spectrum in FIG. 5B, indicates that this phase is Ag. 3 The inventors have shown that the dependence of R / N on Ag thickness is 3 We speculate that this is an incidental consequence of the R / N dependence on the Sn volume fraction.
[0025] If it is assumed that the Ag plated layer will completely dissolve in the Sn by reflow, then Ag 3 The volume fraction of Sn will depend solely on the Ag thickness relative to the Sn thickness before reflow. With some assumptions, the Ag volume fraction at the reflow surface 3The volume fraction of Sn can be calculated from the thicknesses of the Ag and Sn plated layers.
[0026] 1) The Ag-plated layer dissolves completely into the Sn by reflow.
[0027] 2) Ag 3 There is a sufficient thickness of Sn to consume all of the Ag to form Sn, i.e., Ag is the limiting factor.
[0028] 3) The thickness of Ag and Sn is constant per unit of surface area.
[0029] 4) The densities of the plated layers of Ag and Sn match their pure elemental values.
[0030] 5) Ag 3 The density of Sn is known and matches that of the compounds that form on the reflow surface.
[0031] Ag on reflow surface 3 Sn volume fraction φAg 3 Sn will be related to the volume fraction of Ag in the plated layer, φAg. The volume fraction of Ag per unit of surface area will be related to the plated layer thickness simply by φAg=tAg / (tAg+tSn), where tAg=Ag layer thickness and tSn=Sn layer thickness. After substituting the density and atomic weight values, φAg 3 Sn is φAg 3 It can be approximated by Sn≈1.5084*φAg.
[0032] Table 2 shows the Ag and Ag for samples PPIA to PPID, sorted in ascending order of R / N. 3 The calculated volume fraction of Sn is given. The thickness values in Table 2 are measurements reported by sample number. The calculated values are Ag / Sn ... 3 These calculations show that the decrease in the volume fraction of Sn correlates with the decrease in the Ag 3The decrease in Sn supports the dependence of R / N on Ag thickness.
[0033] [Table 2]
[0034] This analysis of R / N should include consideration of the thickness of the Sn layer, since a thicker Sn layer is usually associated with a higher R / N. Samples PPII and PPIJ have an outer layer of 97:3 Sn:Ag on a Cu / Ni barrier. Therefore, the Ag content at the reflow surface of these two samples would have been constant at approximately 3 wt.% regardless of plating thickness. These two samples differed only in the thickness of the SnAg layer.
[0035] Indeed, the thickness effect mentioned above was evident for PPII and J as shown in Table 3. R / N was higher for the thicker layer sample (PPIJ) than for the thinner layer sample (PPII). This thickness effect was evidenced between the same two thicknesses of 37 and 75 μin in the set of samples PPIA to PPID.
[0036] [Table 3]
[0037] Both PPII and PPIJ had statistically significantly lower R / N than conventional tin coatings such as STAR, indicating that the cause of the lower R / N was Ag in the plating. In samples PPIA to PPID, Ag was deposited on the reflow surface. 3 Appears as Sn and Ag 3 The dependence of R / N on the volume fraction of Sn was observed and calculated.
[0038] Figures 5 and 6 are micrographs of the reflowed surfaces of PPII and PPIJ, respectively. These micrographs show a small volume fraction of finely dispersed second phase. However, the micrograph of side B of PPII shows areas of large second phase that are unexplained.
[0039] Ag on SnAg reflow surface 3 The volume fraction of Sn is given by the equation TIFF2024544197000035.tif37131 and will be related to the weight fraction of Ag in the plated layer, wAg.
[0040] This equation and the relationship between Ag, Sn, and Ag 3 Using the density and atomic weight of Sn, the Ag content in the reflow layer of 97 / 3 SnAg plating (wAg=0.03) was 3 The volume fraction of Sn is φAg 3 Sn=0.0304. Ag in the 97 / 3SnAg layer 3 With the calculated volume fraction of Sn, PIII and J are compared with samples PPIA to PIID in Table 4. The samples in this table are grouped by thickness to clarify the effect, and they are sorted in ascending order of R / N within each group. The table shows Ag 3 The effect of Sn volume fraction is evident. The low volume fraction SnAg sample had the highest R / N in each group. In both groups of samples, the R / N was significantly higher than that of Ag. 3 It increases with decreasing Sn volume fraction.
[0041] Ag 3 The main assumption in the calculation of the Sn volume fraction was that the Ag layer would be completely dissolved in the Sn upon reflow. This assumption is supported by the cross sections of the reflowed surfaces of samples A and B, which show that the Ag underlayer was completely dissolved upon reflow.
[0042] Cross sections of the reflowed surfaces of PPIA and PPIB were prepared by focused ion beam (FIB) machining and examined by transmission electron microscopy (TEM). FIB cross sectioning had the advantage that deformation and heat introduced into the sample would be negligible, while TEM examination allowed high resolution magnification to accurately determine the morphology, composition, and thickness of the individual layers and phases. Figures 8 and 9 show TEM images and EDS maps from the FIB cross sections. The Ag maps showed that no Ag layer remained on either sample, and the Ag layer was completely dissolved into the Sn upon reflow. 3 The assumptions in the Sn calculations are further confirmed.
[0043] Ni, Cu, Cu 3 Sn, Cu 6 Sn 5 , and clear layers of Sn are seen in the TEM images of both PPIA and PPIB, whereas Ag 3 Areas of Sn were found on the surface of the PPIB. The FIB lamellae of the PPIA were either Ag 3 The inventors believe that this is the reason for the Ag phase in this sample. 3 This is believed to be due to the lower volume fraction of Sn, which may have ensured that the lamellae did not accidentally contain any of this phase.
[0044] The Cu maps show that each sample contained a significant thickness of Cu layer after reflow. This is noteworthy because existing tin coatings such as STAR and ATB would have no or very little Cu layer after reflow, so Cu would not be available for inhibitor-free intermetallic growth by thermal aging.
[0045] Figure 10 presents a line scan analysis of PPIA. In this line scan, Cu 6 Sn 5 (54.5at%Cu, 45.5at%Sn) and Cu 3The atomic composition of Sn (75at%Cu, 25at%Sn) is clearly visible. This scan shows that there was a layer of pure Sn on the surface. Cu 6 Sn 5 The Cu phase appears as a single large grain adjacent to the pure Sn layer. 3 The Sn phase is Cu 6 Sn 5 and Cu layers, it is seen as a very fine-grained layer with a grain size of approximately 130 µm.
[0046] Figure 11 presents a line scan analysis of PPIB. In this scan, Ag 3 The atomic composition of Sn (75 at% Ag, 25 at% Sn) is clearly seen in the large Ag-containing phase at the surface. The EDS map of this sample in Figure 9 shows the Ag line scan. 3 It shows that just below the Sn phase there is a small region of pure Sn. On the line scan this region is detected starting at approximately 0.98 μm. The scan of this small region of pure Sn shows that it is adjacent to the Cu phase where the Cu x-rays were detected. 6 Sn 5 The line scan was located close enough to and directly passing along the edge of the Sn line at about 1 μm that the Sn line on the graph only reached 80 at% Sn and why the Sn content steadily decreased as the scan progressed over this region, which would explain why Cu was detected in this area. The line scan showed that below this small region of Sn, from about 1.20 to 1.35 μm along the scan, the composition of Cu and Sn was roughly constant, with the Cu 6 Sn 5 This shows that the composition is consistent with the Cu content (54.5at%Cu, 45.5at%Sn). 6 Sn 5 The area along the line scan between the and Cu layers is 3It contained a very small layer of Sn, as seen by the fine grain morphology similar to PPIA, and as seen in the EDS map of FIG. 9 which showed higher levels of Cu and lower levels of Sn in this layer. However, the line scan passed right along the edge of this thin layer of fine grains, so the EDS did not detect any Cu. 3 The composition of Sn could not be elucidated.
[0047] The plated layer thicknesses of Ni, Cu, Ag, and Sn before reflow are given in Table 5 for Samples A through D, as measured by XRF and reported by PPI.
[0048] [Table 5]
[0049] The layer and phase thicknesses of the PPIA and PPIB reflowed samples were measured from the TEM images and EDS maps given in Figures 12-15. These images and maps show the total thickness of the Ni layer along with the outer plated surface on the same image. Thickness measurements were taken sequentially at 10 equally spaced locations on each image as shown in the EDS maps in Figures 13 and 15. Location 1 is the left-most location. The thickness measurements are given in Tables 6 and 7.
[0050] [Table 6]
[0051] [Table 7]
[0052] The parameters for calculating the thickness of the plating consumed and the thickness of the intermetallic compound (IMC) formed are presented in Table 8. The parameters a and b allow the calculation of the thickness of elements A and B consumed to form a given IMC thickness of AxBy. The reciprocals of these parameters a-1 and b-1 allow the calculation of the thickness of the IMC formed by the reaction of A or B of a given thickness. The ratio of parameters a and b allows the calculation of the thickness consumed for the reactant elements. For example, for a given thickness of element A consumed to form AxBy, the b / a ratio gives the thickness of B that will be consumed in the reaction, and vice versa for the a / b ratio for a given thickness consumed of element B.
[0053] [Table 8]
[0054] With these parameters, the thicknesses of the plated layers of Ag, Cu, and Sn before reflow can be back-calculated from the measurements in Tables 6 and 7. The results of these calculations are shown in Table 9 and compared with the results reported by sample number.
[0055] [Table 9]
[0056] Considering that the back-calculated values are based on a very small statistical sample of single cross sections from FIB cuts covering a very small area of the plated surface, the back-calculated results are in good agreement with the results reported by the sample.
[0057] The idea of existing tin coating systems with barriers such as ATB and STAR is that the Cu / Ni barrier retards the growth of Cu-Sn IMCs by retarding the diffusion of Cu from the substrate material. However, if the plated Cu thickness is large, excess Cu may be present after reflow. For this, there will be no barrier against diffusion by thermal aging. Thus, a high rate of growth of Cu-Sn IMCs will occur until the excess Cu is consumed. If the plated Cu is too large, it could consume all of the Sn in a short amount of time of thermal aging. For a given thickness of Ag and Cu, the calculation of the amount of Sn consumed after a short time of thermal aging such as 150°C / 1wk can be made straightforward using the a and b parameters in Table 8. The equation for the amount of Sn consumed is: tSn.cons.=(b / a)Ag 3 SntAg+(b / a)Cu 6 Sn 5 tCu where tSn.cons.=thickness of Sn consumed as IMC, tAg and tCu=thickness of Ag and Cu plating that will be completely consumed as IMC after short time heat aging, respectively. From Table 8, (b / a)Ag 3 Sn=0.52968, (b / a)Cu 6 Sn 5 =1.91995.
[0058] Table 10 shows the results of calculations made for PPI samples A through D. The results of the calculations for samples A and B indicate that there will be little or no free Sn remaining in these samples. PPIA will have 2-3 μin of free Sn, PPIB will have no free Sn, and PPIC and D will each have approximately 40 μin of free Sn.
[0059] [Table 10]
[0060] Table 11 shows the calculated amount of Sn that will be consumed as IMC upon short aging for various combinations of Ag and Cu thickness. For the standard ATB, the Cu specification is 7 to 18 μin. The minimum Sn thickness for the standard ATB is 40 μin and there is no Ag plating. Table 11 shows that a minimum of 5 μin of free Sn will be present after short aging with the standard ATB. That is, at the maximum Cu thickness of 18 μin, 34.6 μin of Sn will be consumed as IMC leaving 5.4 μin of free Sn.
[0061] [Table 11]
[0062] To apply silver additions according to the principles of the present disclosure to a conventional ATB, either the maximum Cu specification would need to be decreased or the minimum Sn specification would need to be increased relative to a standard ATB to ensure that 5 μin of free Sn would be available after a short time aging, i.e., to ensure the same amount of free Sn as a standard ATB. For example, as shown in Table 10, with 15 μin of Ag and 18 μin of Cu, after a short time aging, 42.5 μin of Sn would be consumed as IMC. To ensure 5 μin of free Sn in these Ag and Cu thicknesses, the minimum specification for Sn would need to be 48 μin.
[0063] Considered another way, with a minimum Sn thickness of 40 μin and a maximum Ag thickness of 15 μin, to guarantee 5 μin of free Sn after short aging, the maximum Cu thickness would need to be 14 μin or less. Other combinations of thicknesses may be possible. The point here is that because silver is applied to the ATB, the Cu and / or Sn specifications would need to be different than the standard ATB to guarantee that free Sn is available after short aging.
[0064] In a particularly preferred embodiment, Ag at the reflow surface 3 To help ensure the presence of Sn intermetallics, the thickness of the Cu layer is reduced and / or the thickness of the Sn layer is increased to ensure that free Sn remains available after short-term aging. In this particularly preferred embodiment, there is preferably between about 5 and 15 μin of Ag and a Cu / Ni thickness that will ensure at least 5 μin of free Sn after short-term aging. One possible configuration that focuses on reducing the Cu thickness is 40-80 μin Sn / 5-15 μin Ag / 7-14 μin Cu / 5-20 μin Ni. Another possible configuration that focuses on increasing the Sn is 50-80 μin Sn / 5-15 μin Ag / 7-18 μin Cu / 5-20 μin Ni.
[0065] Table 12 provides additional data with sample 7 illustrating the low copper preferred embodiment.
[0066] [Table 12]
[0067] Ag in the tin layer 3 Although the presence of Sn intermetallics contributes to the reduction in friction, the inventors have determined that a total of 5-10 μin of silver layer provides sufficient Ag to provide a beneficial reduction in friction (R / N) while reducing metal costs compared to other preferred embodiments of the present disclosure. 3 In particular, these embodiments can achieve friction (R / N) of 0.2 or less, more preferably 0.18 or less, with a total of 10 μin of silver layers.
[0068] These embodiments also provide a free tin layer of at least 5 μin after heat aging at 150° C. in accordance with SAE's USCAR 2-8(2022), the entire contents of which are incorporated herein by reference, indicating that desirable frictional and electrical properties of a connector having the coating will remain over the useful life of the connector.
[0069] The foregoing description of the embodiments is provided for purposes of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, are interchangeable where applicable, and may be used in selected embodiments even if not specifically shown or described. They may also be modified in many ways. Such modifications should not be considered as departures from the present disclosure, and all such modifications are intended to be included within the scope of the present disclosure.
Claims
1. A copper alloy electrical connector component having thereon a coating including applying a nickel layer of between about 5 μin and about 20 μin on said copper alloy, a copper layer of between about 7 μin and about 18 μin on said nickel layer, one or more silver layers totaling between about 5 μin and about 15 μin on said copper layer, and one or more tin layers totaling between about 40 μin and about 80 μin, wherein subsequent reflow heating of said connector results in a mixture of said silver and tin layers and between about 8 vol% and about 45 vol% Ag. 3 Copper alloy electrical connector parts, causing the formation of Sn intermetallic compounds.
2. 2. The copper alloy electrical connector component of claim 1, wherein said one or more silver layers are applied as a single layer over said copper layer and said one or more tin layers are applied as a single layer over said silver layer.
3. 2. The copper alloy electrical connector component of claim 1, wherein said one or more silver layers and said one or more tin layers are applied as multiple alternating layers of silver and tin.
4. 2. The copper alloy electrical connector component of claim 1, wherein said coating imparts an R / N to said connector component after reflow heating of between about 0.20 and about 0.
13.
5. 5. The copper alloy electrical connector component of claim 4, wherein said coating imparts an R / N to said connector component after reflow heating of between about 0.19 and about 0.
135.
6. 10. The copper alloy electrical connector component of claim 1, wherein there are one or more silver layers totaling between about 5 .mu.in and about 10 .mu.in.
7. 1. A copper alloy electrical connector component comprising: applying a nickel layer between about 5 μin and about 20 μin on the copper alloy; applying a copper layer between about 7 μin and about 18 μin on the nickel layer; applying a silver layer between about 5 μin and about 15 μin; applying tin between about 40 μin and about 80 μin; and heating the coated copper alloy electrical connector component to mix the silver and tin layers and to deposit between about 8 vol % and about 45 vol % Ag. 3 causing the formation of Sn intermetallic compounds.
8. 8. The copper alloy electrical connector component of claim 7, wherein said coating imparts an R / N to said connector component of between about 0.20 and about 0.
13.
9. 9. The copper alloy electrical connector component of claim 8, wherein said coating imparts an R / N to said connector component after reflow heating of between about 0.19 and about 0.
135.
10. 8. The copper alloy electrical connector component of claim 7, wherein there is one or more silver layers totaling between about 5 .mu.in and about 10 .mu.in applied prior to reflow heating.
11. 1. A coating on a copper alloy electrical connector component, the coating comprising: applying a nickel layer between about 5 μin and about 20 μin on the copper alloy; applying a copper layer between about 7 μin and about 18 μin on the nickel layer; applying a silver layer between about 5 μin and about 15 μin and a tin layer between about 40 μin and about 80 μin total on the copper layer; and heating the coated copper alloy electrical connector component to mix the silver and tin layers and to deposit between 8 vol% and 45 vol% Ag. 3 causing the formation of Sn intermetallic compounds.
12. 12. The coating on a copper alloy electrical connector component of claim 11, wherein said coating imparts an R / N to said connector component of between about 0.20 and about 0.
13.
13. 13. The coating on a copper alloy electrical connector component of claim 12, wherein after reflow heating, said coating imparts an R / N to said connector component of between about 0.19 and about 0.
135.
14. 10. The coating on a copper alloy electrical connector component of claim 1, wherein there is a total of about 5 .mu.in and about 10 .mu.in of the one or more silver layers applied prior to reflow heating.
15. 1. A method of forming a coating on a copper alloy electrical connector component, the method comprising: applying a nickel layer of between about 5 μin and about 20 μin onto the copper alloy; applying a copper layer of between about 7 μin and about 18 μin onto the nickel layer; applying a silver layer of between about 5 μin and about 15 μin total and a tin layer of between about 40 μin and about 80 μin total onto the copper layer; and reflow heating the coating to intermix the silver and tin layers and to obtain a silver-tin layer of between 8 vol % and about 45 vol % Ag in the resulting silver-tin layer. 3 causing the formation of a Sn intermetallic compound.
16. 16. The method of claim 15, wherein the silver layer is applied as a single layer onto the copper layer and a tin layer is applied as a single layer onto the silver layer.
17. The method of claim 15 , wherein the silver and tin layers are applied as multiple alternating layers of silver and tin.
18. The method of claim 15 , wherein the coating imparts an R / N of between about 0.20 and about 0.13 to the connector component.
19. 20. The method of claim 18, wherein after reflow heating, the coating imparts an R / N to the connector component of between about 0.19 and about 0.
135.
20. 20. The method of claim 18, wherein a total of between about 5 μin and about 10 μin of the one or more silver layers are applied prior to reflow heating.
21. 1. A method of forming a coating on a copper alloy electrical connector component, the method comprising: applying a nickel layer between about 5 μin and about 20 μin onto the copper alloy; applying a copper layer between about 7 μin and about 18 μin onto the nickel layer; applying a silver layer between about 5 μin and about 15 μin; applying tin between about 40 μin and about 80 μin; and heating the coated copper alloy electrical connector component to mix the silver and tin layers and to deposit between about 25 vol % and about 45 vol % Ag. 3 causing the formation of a Sn intermetallic compound.
22. A copper alloy electrical connector component having thereon a coating formed by applying between about 5 μin and about 20 μin of nickel onto said copper alloy, applying between about 7 μin and about 18 μin of copper onto said nickel layer, and applying a total of between about 5 μin and about 15 μin of silver and between about 40 μin and about 80 μin of tin onto said copper layer, wherein at least 8 vol. % Ag is removed by reflow heating of said layers. 3 A copper alloy electrical connector component, wherein the Cu and Ni thicknesses are selected to ensure that there is sufficient tin to form Sn intermetallic compounds, and further that at least 5 μin of free Sn remains after short time aging.
23. 23. The copper alloy electrical connector of claim 22, wherein said copper layer is between 7 and 14 μin.
24. 23. The copper alloy electrical connector of claim 22, wherein said tin layer totals at least 50 .mu.in.
25. 1. A method of forming a coating on a copper alloy electrical connector component, the method comprising: applying a nickel layer of between about 5 μin and about 20 μin on the copper alloy; applying a copper layer of between about 7 μin and about 18 μin on the nickel layer; applying a silver layer of between about 5 μin and about 15 μin; and applying tin of between about 40 μin and about 80 μin, wherein the Cu and Ni thicknesses are further selected to ensure that at least 5 μin of free Sn remains after short time aging in accordance with SAE USCAR 2-8.
Citation Information
Patent Citations
Electric contact material and its manufacture
JP1992370613A
Material for electrical and electronic parts, its production and electrical and electronic parts using the material
JP1999350189A
Coating material, electric / electronic component using the same, rubber contact component using the same, and coating material manufacturing method
JP2005126763A
Continuous layer for manufacture of composite for electronic mechanic component, its composite material, manufacturing method and use method
JP2005199699A
Apparatus and method for coating with fretting and whisker resistance
JP2007520053A