Method for preparing ultra-high molecular weight polyethylene nanocomposite products, molds and products

The preparation of UHMWPE nanocomposites through controlled injection of low molecular weight polyolefin nanocomposites with nanomaterials forms a uniform lubricating layer, addressing high friction in oil-free conditions and enhancing mechanical properties for stable performance.

JP2024544210AActive Publication Date: 2024-11-28SHANGHAI RES INST OF CHEM IND CO LTD +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024533254
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-10
Filing Date
2022-08-12
Publication Date
2024-11-28
Estimated Expiration
2042-08-12

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene (UHMWPE) materials exhibit high friction coefficients under oil-free lubrication conditions, limiting their application in such environments, and existing methods to reduce friction in water lubrication do not translate effectively to oil-free conditions.

Method used

A method involving the preparation of UHMWPE nanocomposites by injecting a low molecular weight polyolefin nanocomposite melt into a UHMWPE melt within a mold, using a specific mold structure and controlled injection process to form a uniform lubricating layer, incorporating nanomaterials like graphene or molybdenum disulfide to reduce friction.

Benefits of technology

The process results in UHMWPE products with ultra-low friction coefficients and improved mechanical properties, suitable for oil-free lubrication conditions, ensuring stable performance and reduced wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544210000001_ABST
    Figure 2024544210000001_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing an ultra-high molecular weight polyethylene nanocomposite product, which includes the steps of: S1: preparing an ultra-high molecular weight polyethylene base material into an ultra-high molecular weight polyethylene melt and injecting it into a mold; S2: cooling the ultra-high molecular weight polyethylene melt to a first temperature under a preset pressure; S3: injecting a low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature; and S4: cooling and molding to prepare the ultra-high molecular weight polyethylene nanocomposite product. The present invention ensures the mechanical performance and wear resistance of the UHMWPE product itself, the surface of the produced UHMWPE product has a uniform structure, and forms a lubricating layer through the surface structure, ensuring a stable ultra-low friction coefficient, the molding process is simple, one-time molding is achieved, the cost is low, and it has a good market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of polymer physical processing, and in particular to a method for preparing ultra-high molecular weight polyethylene nanocomposite products. [Background technology]

[0002] With the development of the economy and society, the prevalence of a series of problems caused by friction, such as wear, lubrication, material and energy consumption, has a significant impact on social and economic development and has attracted great attention from the scientific and technological community. According to statistics from the World Society of Friction, friction losses of more than one-third of the world's one-time energy losses are caused by an annual loss of about 1% of gross national product.

[0003] According to current market research, the main wear-resistant materials commonly used in the current market are ultra-high molecular weight polyethylene, nylon, and polytetrafluoroethylene materials. UHMWPE generally refers to the linear structure of polyethylene (PE) with a molecular weight of 1.5 million or more, and is a new type of thermoplastic engineering plastic. Polytetrafluoroethylene (PTFE) is a polymer compound made from tetrafluoroethylene by polymerization. Polyamide, commonly known as nylon, is a general term for thermoplastic resins that contain repeating amide groups -[NHCO]- on the main chain of the molecule.

[0004] UHMWPE performance characteristics: Ultra-high molecular weight polyethylene (UHMW-PE) is a thermoplastic engineering plastic with a linear structure and excellent comprehensive performance. It was first industrialized by Allied Chemical Company in the United States in 1957, and then industrial production was started by Hoechst in Germany, Hercules Company in the United States, and Mitsui Petrochemical Company in Japan. China first succeeded in industrialization in 1964. Under the conditions at that time, the molecular weight of the product was about 1.5 million, but with the advancement of process technology, the molecular weight of the current product is 1 to 9 million or more. The wear resistance of UHMWPE is the highest among plastics, several times higher than carbon steel and brass, and tens of times higher than ordinary polyethylene, the friction coefficient is close to polytetrafluoroethylene (PTFE), smaller than other plastics, water absorption is smaller than other engineering plastics, good anti-adhesion, very good impact resistance, high tensile strength, good corrosion resistance, good low temperature resistance, low density, and low cost.

[0005] Polytetrafluoroethylene (PTFE) performance properties: high chemical stability, good low and high temperature resistance, excellent anti-adhesion properties, very low coefficient of friction, the best lubrication properties even for plastics, good insulating properties, excellent ageing resistance and thermal stability, very low water absorption.

[0006] Wear-resistant materials should be considered primarily for wear resistance and good self-lubrication, and should also have good comprehensive mechanical properties.Compared with polytetrafluoroethylene and nylon materials, ultra-high molecular weight polyethylene has excellent mechanical properties, the best wear resistance, and a friction coefficient comparable to that of polytetrafluoroethylene, and has important comprehensive performance in wear resistance and lubrication, but the friction coefficient is still large under oil-free lubrication conditions, which limits the application of ultra-high molecular weight polyethylene in oil-free lubrication, so it is an important task to further reduce its friction coefficient.

[0007] At present, the method of reducing the wear resistance of ultra-high molecular weight polyethylene is mainly blending composite, and patent CN201710478676.5 discloses an ultra-high molecular weight polyethylene multifunctional nanocomposite material suitable for use under water lubrication conditions. In addition to adding reinforcing fibers to the ultra-high molecular weight polyethylene material, the present invention adds surface-modified tribohydrolyzable nanoparticles. The composite material of the present invention has good wear resistance under water lubrication conditions, and when the composite material is used in seawater medium, the boundary film at the friction interface can effectively protect the metal bi-layer surface while reducing the wear of the polymer composite material, and reduce the corrosive wear of the metal. This patent has good wear resistance under water lubrication conditions, but cannot be applied to oil-free lubrication conditions, so there is a need to develop UHMWPE products under oil-free lubrication conditions.

[0008] Li Huilin's group at Sichuan University, China (Journal of Friction Science 2004, 24(1):21-24) used compression molding to prepare polypropylene (PP) and MoS2-filled ultra-high molecular weight polyethylene (UHMWPE) composites. Research showed that adding MoS2 alone improves the wear resistance of UHMWPE, but increases the friction coefficient and reduces mechanical performance. Modification of UHMWPE with PP and MoS2 significantly improves the processing performance. The processing performance, load-bearing capacity and long-term wear resistance of the 72.7%UHMWPE / 18.2%PP / 9.1%MoS2 ternary composite are significantly better than UHMWPE, and UHMWPE mainly suffers from adhesive wear and fatigue wear. The 72.7%UHMW-PE / 18.2%PP / 9.1%MoS2 ternary composite only undergoes slight plastic deformation when rubbing against steel under the same test conditions. This result significantly improved the wear resistance of UHMWPE while reducing the friction coefficient of UHMWPE products from 0.19 to 0.16. However, this is still far from the friction coefficient of 0.05 to 0.08 under oil lubrication, and further improvement is needed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] China Patent Application Publication No. 107338094 [Non-patent literature]

[0010] [Non-Patent Document 1] Journal of Tribology 2004,24(1):21~24 Summary of the Invention [Means for solving the problem]

[0011] In order to solve the above technical problems, the present invention provides a method for preparing an ultra-high molecular weight polyethylene nanocomposite product, the method includes the steps of: S1: preparing an ultra-high molecular weight polyethylene substrate into an ultra-high molecular weight polyethylene melt and injecting it into a mold; S2: cooling the ultra-high molecular weight polyethylene melt to a first temperature under a preset pressure; S3: injecting a low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature; and S4: cooling and molding to prepare the ultra-high molecular weight polyethylene nanocomposite product.

[0012] Preferably, the first temperature is 80 to 100°C, and the second temperature is 90 to 100°C.

[0013] Preferably, the ultra-high molecular weight polyethylene substrate is an ultra-high molecular weight polyethylene powder, and the molecular weight of the ultra-high molecular weight polyethylene substrate is 1 to 9 million g / mol.

[0014] Preferably, the low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterials.

[0015] Preferably, the molecular weight of the low molecular weight polyolefin is 100 to 10,000 g / mol.

[0016] Preferably, the mass fraction of said nanomaterial is between 0.1% and 3.0%.

[0017] Preferably, the nanomaterial is a mixture of one or more of graphene, graphite or molybdenum disulfide.

[0018] Preferably, the ultra-high molecular weight polyethylene nanocomposite product is produced by the mold for preparing ultra-high molecular weight polyethylene nanocomposite product provided by the present invention, in which in step S1, the ultra-high molecular weight polyethylene melt is injected into the cavity formed by the first mold plate and the movable plate; in step S2, the first mold plate is moved to move the movable plate toward the substrate so as to maintain the ultra-high molecular weight polyethylene melt at a preset pressure; in step S3, the method of injecting low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature includes: moving the first mold plate back at a preset speed, controlling the switch to open the hot runner, injecting the low molecular weight polyolefin nanocomposite melt, and in step S4, controlling the switch to close the hot runner, followed by cooling and molding.

[0019] Preferably, the preset speed is between 0.1 mm / s and 2 mm / s.

[0020] The present invention further provides a mold for preparing an ultra-high molecular weight polyethylene nanocomposite product, which is composed of a first mold plate, a second mold plate and a switch, the second mold plate includes a substrate, a high pressure spring, a hot runner and a movable plate, the first mold plate and the movable plate form a cavity for receiving an ultra-high molecular weight polyethylene melt, the hot runner is fixed to the substrate, the hot runner is used to inject the low molecular weight polyolefin nanocomposite melt, the switch is used to control the opening and closing of the hot runner, the movable plate is supported on the substrate via a high pressure spring and can move horizontally relative to the substrate, a through hole is opened in the movable plate, the through hole is used for the hot runner to pass through, and when the gap between the movable plate and the substrate is minimum, the hot runner protrudes from the surface of the movable plate.

[0021] Preferably, the hot runner protrudes from the surface of the movable plate by 1 to 10 mm, and the hot runner has a diameter of 1 to 2 mm.

[0022] Preferably, the total surface area of ​​the hot runners accounts for 10% to 60% of the surface area of ​​the movable plate.

[0023] Preferably, the hot runner has a circular or polygonal shape.

[0024] The present invention further provides an ultra-high molecular weight polyethylene nanocomposite product, which is produced by the method for preparing an ultra-high molecular weight polyethylene nanocomposite product according to any one of the above.

[0025] Compared with the prior art, the present invention guarantees the mechanical performance and wear resistance of the UHMWPE product itself, the surface of the produced UHMWPE product has a uniform structure, and a lubricating layer is formed through the surface structure, ensuring a stable ultra-low friction coefficient, the molding process is simple, one-time molding is achieved, the cost is low, and it has a good market prospects. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic diagram showing the preparation method of the ultra-high molecular weight polyethylene nanocomposite product of Example 1. [Diagram 2] FIG. 1 is a schematic diagram of a mold for preparing the ultra-high molecular weight polyethylene nanocomposite products of Examples 2 to 9. [Diagram 3] FIG. 1 is a schematic diagram showing the steps of the preparation method of ultra-high molecular weight polyethylene nanocomposite products of Examples 3 to 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In order to facilitate the understanding of the present application, the present application will now be described more fully with reference to the accompanying drawings, in which preferred embodiments of the present application are illustrated. However, the present application may be embodied in various different forms and is not limited to the embodiments set forth herein. Rather, these embodiments are provided to make the disclosure of the present application more thorough and comprehensive.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs. In this specification, the terms used in the specification of this application are used only for the purpose of describing specific examples, and are not intended to limit this application.

[0029] <Example 1> As shown in FIG. 1, Example 1 provides a method for preparing an ultra-high molecular weight polyethylene nanocomposite product, the method includes the steps of: S1: preparing an ultra-high molecular weight polyethylene substrate into an ultra-high molecular weight polyethylene melt and injecting it into a mold; S2: cooling the ultra-high molecular weight polyethylene melt to a first temperature under a preset pressure; S3: injecting a low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature; and S4: cooling and molding to prepare the ultra-high molecular weight polyethylene nanocomposite product.

[0030] The first temperature is in the range of 80 to 100°C, and the second temperature is in the range of 90 to 100°C.

[0031] The ultra-high molecular weight polyethylene base material is an ultra-high molecular weight polyethylene powder, and the molecular weight of the ultra-high molecular weight polyethylene base material is 1 to 9 million g / mol. Preferably, the molecular weight is high, and a high molecular weight provides better wear resistance.

[0032] The low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 100-10000g / mol, and the mass fraction of the nanomaterial is 0.1%-3.0%. The nanomaterial is one or more mixtures of graphene, graphite or molybdenum disulfide. As the base material of the room temperature solid lubricant material, the main function of the low molecular weight polyolefin is to keep the whole lubricant material in a solid state and to compound with the UHMWPE product, while precipitating during the wear process to form a lubricant film, greatly reducing the friction coefficient, and at the same time forming a melt at high temperature to form wear protection for the product. The amount of the nanomaterial added is mainly set according to the requirements of reducing the friction coefficient of the lubricant layer, improving the heat resistance of the lubricant layer, and wear resistance.

[0033] <Example 2> As shown in FIG. 2, Example 2 provides a mold for preparing an ultra-high molecular weight polyethylene nanocomposite product, which includes: The mold is composed of a first mold plate 1, a second mold plate 2 and a switch 3. The second mold plate 2 includes a substrate 21, a high-pressure spring 22 and a movable plate 23. The first mold plate 1 and the movable plate 23 form a cavity 11 for accommodating ultra-high molecular weight polyethylene melt. The hot runner 24 is fixed to the substrate 21. The hot runner 24 is used to inject low molecular weight polyolefin nanocomposite melt. The switch 3 is used to control the opening and closing of the hot runner 24. The movable plate 23 is supported on the substrate 21 via the high-pressure spring 22 and moves horizontally relative to the substrate 21. A through hole is opened in the movable plate 23, and the through hole is used for the hot runner 24 to pass through. When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23. At this time, the protrusion amount of the hot runner 24 from the surface of the movable plate 23 is 1 to 10 mm. When the gap between the movable plate 23 and the substrate 21 is at its maximum, the hot runner 24 does not protrude from the surface of the movable plate 23 .

[0034] The diameter of the hot runner 24 is 1 to 2 mm. The total surface area of ​​the hot runner 24 accounts for 10% to 60% of the surface area of ​​the movable plate 23. The shape of the hot runner 24 is circular or polygonal. The surface area ratio of the hot runner affects the friction coefficient of the final product; the higher the ratio, the lower the friction coefficient, but if the ratio is too high, the wear rate of the product will decrease. To achieve a comprehensive balance between the friction coefficient and the wear rate, the surface area ratio is 10 to 60%.

[0035] <Example 3> Example 3 provides a more specific example by combining the mold of Example 2 based on the preparation method of Example 1.

[0036] As shown in FIG. 3, this embodiment provides a method for preparing an ultra-high molecular weight polyethylene nanocomposite product, which comprises applying the mold for preparing the ultra-high molecular weight polyethylene nanocomposite product described in Example 2; As shown in FIG. 3a, in step S1, the ultra-high molecular weight polyethylene melt is injected into the cavity 11 formed by the first mold plate 1 and the movable plate 23, and in step S2, the first mold plate 1 is moved to move the movable plate 23 toward the substrate 21, and after a preset pressure is reached, the movement of the first mold plate 1 is stopped, and the ultra-high molecular weight polyethylene melt is cooled to a first temperature under the action of the high pressure spring 22 while maintaining the preset pressure.

[0037] As shown in FIG. 3b, in step S3, the method of injecting the low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature includes: moving the first mold plate 1 backward at a preset speed, controlling the switch 3 to open the hot runner 24, and injecting the low molecular weight polyolefin nanocomposite melt, the preset speed being 0.1mm / s-2mm / s; If the preset speed is too high, it will affect the pressure retention of the product, so it is preferably less than 2 mm / s. Retracting at a low speed will keep the pressure basically unchanged, flattening the product and at the same time preventing the injected molten material from spilling out of the product surface.

[0038] As shown in Fig. 3c, in step S4, the switch 3 is controlled to close the hot runner 24, followed by cooling and molding. As shown in Fig. 3d, after cooling and molding, the mold is opened to take out the ultra-high molecular weight polyethylene nanocomposite product.

[0039] The following Examples 4 to 9 provide more specific and illustrative examples further formed based on Examples 1 to 3.

[0040] <Example 4> First, an ultra-high molecular weight polyethylene substrate is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 1 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene melt is cooled. After cooling to 80°C, the first mold plate 1 is controllably retreated, and the retreating speed is 0.1 mm / s. The movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreating process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 90-100°C.

[0041] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 1 mm, the diameter of the hot runner 24 is 1 mm, the shape is circular, and the total surface area of ​​the hot runner 24 accounts for 10% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 1000 g / mol, the nanomaterial is graphene, and the mass fraction of the nanomaterial is 0.2%. After finally cooling completely and molding, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0042] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.098, tensile strength 32.3Mpa, wear index 159. The wear index is used to characterize the wear resistance performance of UHMWPE products, the test standard is based on ISO 15527-2007, the exemplary test method is to subject the UHMWPE product to mortar wear under a rotation speed of 1300r / min and a water temperature of 5℃, the comparative sample is SLL-4 with a molecular weight of 5 million g / mol, and the wear time is 3h.

[0043] <Example 5> First, an ultra-high molecular weight polyethylene base material is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 3 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene melt is cooled. After cooling to 90°C, the first mold plate 1 is controllably retreated, with a retreat speed of 1 mm / s, the movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreat process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 90°C.

[0044] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 2 mm, the diameter of the hot runner 24 is 2 mm, the shape is hexagonal, and the total surface area of ​​the hot runner 24 accounts for 20% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 337.58 g / mol, the nanomaterial is molybdenum disulfide, and the mass fraction of the nanomaterial is 0.5%. Finally, after complete cooling and molding, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0045] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.086, tensile strength 33.6 Mpa, wear index 139.

[0046] <Example 6> First, an ultra-high molecular weight polyethylene base material is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 5 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene product melt is cooled. After cooling to 90°C, the first mold plate 1 is controllably retreated, with a retreat speed of 2 mm / s, the movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreat process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 95°C.

[0047] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 10 mm, the diameter of the hot runner 24 is 1 mm, the shape is a parallelepiped, and the total surface area of ​​the hot runner 24 accounts for 30% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 3000 g / mol, the nanomaterial is graphite, and the mass fraction of the nanomaterial is 0.8%. Finally, after complete cooling and molding, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0048] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.080, tensile strength 35.0 Mpa, wear index 115.

[0049] <Example 7> First, an ultra-high molecular weight polyethylene base material is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 6 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene product melt is cooled. After cooling to 100°C, the first mold plate 1 is controllably retreated, with a retreat speed of 2 mm / s, the movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreat process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 100°C.

[0050] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 1 mm, the diameter of the hot runner 24 is 1 mm, the shape is circular, and the total surface area of ​​the hot runner 24 accounts for 40% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 6000 g / mol, the nanomaterial is graphite, and the mass fraction of the nanomaterial is 0.8%. Finally, after complete cooling and molding, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0051] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.075, tensile strength 38.9Mpa, wear index 109.

[0052] <Example 8> First, an ultra-high molecular weight polyethylene base material is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 9 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene product melt is cooled. After cooling to 80°C, the first mold plate 1 is controllably retreated, with a retreat speed of 0.1 mm / s, the movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreat process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 90°C.

[0053] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 1 mm, the diameter of the hot runner 24 is 1 mm, the shape is circular, and the total surface area of ​​the hot runner 24 accounts for 50% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 8000 g / mol, the nanomaterial is graphene, and the mass fraction of the nanomaterial is 1.8%. Finally, after being completely cooled and molded, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0054] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.070, tensile strength 38.6 Mpa, wear index 90.

[0055] <Example 9> First, an ultra-high molecular weight polyethylene base material is prepared by melt molding, and the molecular weight of the ultra-high molecular weight polyethylene resin is 8 million. After the pressure is maintained (i.e., after the preset pressure is reached), the ultra-high molecular weight polyethylene product melt is cooled. After cooling to 80°C, the first mold plate 1 is controllably retreated, with a retreat speed of 1 mm / s, the movable plate 23 moves following the first mold plate 1 under the action of the high pressure spring 22, and the switch 3 is controlled to open the hot runner 24. During the retreat process, low molecular weight polyolefin composite melt is injected, and the injection temperature is 90°C.

[0056] When the gap between the movable plate 23 and the substrate 21 is minimum, the hot runner 24 protrudes from the surface of the movable plate 23 by 1 mm, the diameter of the hot runner 24 is 2 mm, the shape is hexagonal, and the total surface area of ​​the hot runner 24 accounts for 60% of the surface area of ​​the movable plate 23. The injected low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial. The molecular weight of the low molecular weight polyolefin is 9000 g / mol, the nanomaterial is molybdenum disulfide, and the mass fraction of the nanomaterial is 3.0%. Finally, after complete cooling and molding, an ultra-low friction coefficient ultra-high molecular weight polyethylene super nanocomposite product is prepared.

[0057] The friction coefficient and mechanical properties of the prepared product are as follows: friction coefficient 0.068, tensile strength 38.0 Mpa, wear index 98.

[0058] <Example 10> Example 10 provides an ultra-high molecular weight polyethylene nanocomposite product, which is produced by the preparation method of the ultra-high molecular weight polyethylene nanocomposite product of Example 1 or Examples 3-9.

[0059] The product can be used to manufacture friction parts under oil-free conditions, such as the boot lining of the sliding guide shoe of a lift. In the prior art, in order to maintain a low friction coefficient, lubricating oil needs to be added between the boot lining and the guide rail, which leads to oil pollution and makes maintenance complicated, and the lack of lubrication leads to rapid wear of the boot lining, resulting in high energy consumption and low comfort. The boot lining made of this product does not need to add lubricating oil during use, does not generate oil pollution, reduces the complexity of maintenance, and ensures low energy consumption and high comfort of the lift product.

[0060] The product can also be used in other sliding friction parts, such as the guide parts of moving platforms, and has a wide range of application value.

[0061] The above description is merely a preferred embodiment of the present invention, and does not limit the embodiments and protection scope of the present invention. It should be understood that those skilled in the art can make equivalent replacements and obvious modifications based on the contents of the specification and accompanying drawings of the present invention and that they are all within the protection scope of the present invention. [Explanation of symbols]

[0062] 1 first mold plate, 11 cavity, 2 second mold plate, 21 substrate, 22 high pressure spring, 23 movable plate, 24 hot runner, 3 switch.

Claims

1. S1: preparing an ultra-high molecular weight polyethylene substrate into an ultra-high molecular weight polyethylene melt and injecting it into a mold; S2: cooling the ultra-high molecular weight polyethylene melt to a first temperature under a preset pressure; S3: injecting a low molecular weight polyolefin nanocomposite melt into the ultra high molecular weight polyethylene melt at a second temperature; S4: Cooling and molding to prepare an ultra-high molecular weight polyethylene nanocomposite product; 1. A method for preparing an ultra-high molecular weight polyethylene nanocomposite product, comprising:

2. The first temperature is 80 to 100° C., and the second temperature is 90 to 100° C.; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 1 .

3. The ultra-high molecular weight polyethylene base material is an ultra-high molecular weight polyethylene powder, and the molecular weight of the ultra-high molecular weight polyethylene base material is 1 to 9 million g / mol; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 1 .

4. The low molecular weight polyolefin nanocomposite melt is a composite product of low molecular weight polyolefin and nanomaterial; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 1 .

5. The molecular weight of the low molecular weight polyolefin is 100 to 10,000 g / mol; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 4 .

6. The mass fraction of the nanomaterial is 0.1% to 3.0%; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 4 .

7. The nanomaterial is a mixture of one or more of graphene, graphite, or molybdenum disulfide; The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 4 .

8. The device is composed of a first mold plate, a second mold plate, and a switch; The second mold plate includes a substrate, a high pressure spring, a hot runner and a movable plate; the first mold plate and the movable plate form a cavity for receiving ultra-high molecular weight polyethylene melt; The hot runner is fixed to a substrate, and the hot runner is used to inject a low molecular weight polyolefin nanocomposite melt; the switch is used to control opening and closing of the hot runner; the movable plate is supported on the substrate via a high-pressure spring and is movable in a horizontal direction relative to the substrate; a through hole is formed in the movable plate, the through hole is used for passing a hot runner, and when the gap between the movable plate and the substrate is minimum, the hot runner protrudes from the surface of the movable plate; A mold for preparing an ultra-high molecular weight polyethylene nanocomposite product, comprising:

9. The amount by which the hot runner protrudes from the surface of the movable plate is 1 to 10 mm. A mold for preparing the ultra-high molecular weight polyethylene nanocomposite product according to claim 8.

10. The diameter of the hot runner is 1 to 2 mm; A mold for preparing the ultra-high molecular weight polyethylene nanocomposite product according to claim 9.

11. The total surface area of ​​the hot runners accounts for 10% to 60% of the surface area of ​​the movable platen; A mold for preparing the ultra-high molecular weight polyethylene nanocomposite product according to claim 9.

12. The shape of the hot runner is circular or polygonal. A mold for preparing the ultra-high molecular weight polyethylene nanocomposite product according to claim 9.

13. The ultra-high molecular weight polyethylene nanocomposite product is produced by applying the mold for preparing the ultra-high molecular weight polyethylene nanocomposite product according to claim 8, In step S1, the ultra-high molecular weight polyethylene melt is injected into a cavity formed by the first mold plate and the movable plate; In step S2, the first mold plate is moved to move the movable plate toward the substrate so as to maintain the ultra-high molecular weight polyethylene melt at a preset pressure; In step S3, the method of injecting the low molecular weight polyolefin nanocomposite melt into the ultra-high molecular weight polyethylene melt at a second temperature includes: retracting the first mold plate at a preset speed; controlling the switch to open the hot runner; and injecting the low molecular weight polyolefin nanocomposite melt; In step S4, the switch is controlled to close the hot runner, followed by cooling and molding. The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 1 .

14. The preset speed is between 0.1 mm / s and 2 mm / s. The method for preparing ultra-high molecular weight polyethylene nanocomposite product according to claim 13, characterized in that:

15. Produced by the method for preparing an ultra-high molecular weight polyethylene nanocomposite product according to any one of claims 1 to 7, 13 and 14.

1. An ultra-high molecular weight polyethylene nanocomposite product comprising:

Citation Information

Patent Citations

  • Ultrahigh molecular weight polyethylene injection moulding method and mould thereof

    CN1579740A

  • Method of injection molding synthetic resin

    JP1978026855A

  • JP1987121912U

  • Impeller made of polyolefin

    JP1989163499A

  • Improved hot runner mold assembly and its use

    JP1993507445A