Sintered stone hot bending furnace and sintered stone hot bending processing method

The sintered stone hot bending furnace and method address fitting and energy efficiency issues by using local reheating and airflow for rapid cooling, resulting in cost-effective, precise, and aesthetically superior sintered stone products.

JP2024544226AActive Publication Date: 2024-11-28MONALISA GRP CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024534105
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2022-12-15
Publication Date
2024-11-28
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing sintered stone manufacturing methods face issues such as imperfect fitting with molds, high energy consumption, and high production costs due to uniform heating and slow cooling processes, leading to defects like discoloration and inaccurate bending arcs.

Method used

A sintered stone hot bending furnace and method that utilizes local reheating and directional airflow for rapid cooling, allowing precise control over heating and cooling to ensure accurate bending and reduce energy consumption.

Benefits of technology

The solution achieves reduced manufacturing time and costs while ensuring the sintered stone accurately fits the mold design, maintaining surface flatness and color integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544226000001_ABST
    Figure 2024544226000001_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of sintered stone processing, and discloses a sintered stone hot bending furnace and a sintered stone hot bending processing method. The sintered stone hot bending furnace includes a furnace cover configured as an insulating plate, the insulating plate having a gas passage communicating with the furnace chamber, a blower unit installed outside the furnace body and communicating with the gas passage of the furnace cover to supply air flow into the furnace chamber, a heating device including a first heating device fixedly installed on the inner wall of the furnace body to adjust the environmental temperature of the furnace chamber, and a second heating device moving vertically and / or horizontally on the furnace body to adjust the local heating temperature of the sintered stone to be hot bent. The sintered stone hot bending furnace not only reduces energy consumption and shortens cooling time, but also ensures that the bending radius of the hot-bent sintered stone manufactured meets the design requirements, has a high degree of conformity with the mold, and does not affect the surface flatness or color decoration of the sintered stone.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of ceramic slab processing, and in particular to a sintered stone hot bending furnace and a sintered stone hot bending method. [Background technology]

[0002] Flat sintered stone has a single structure and its range of use is limited, which restricts the development of sintered stone production capacity. Sintered stone tea tables, sintered stone hand washing basins, etc. currently on the market are all made by cutting sintered stone and gluing it with adhesive, and the corners are right angles. When used for a long time, the glued parts tend to turn yellow or black, affecting the aesthetics. In Patent Document 1, cut sintered stone is placed in a mold and heated to its softening temperature, and then molded into a heat-processed sintered stone that fits the shape of the mold by gravity alone. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] China Patent Application Publication No. 111960653 [Patent Document 1] China Patent Application Publication No. 114646218 [Patent Document 2] China Patent Application Publication No. 102372423 [Patent Document 3] China Utility Model Registration Publication No. 209259924 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the method of Patent Document 1 has the defect that the hot-bent sintered stone and the mold are not completely compatible, and the bending radius does not meet the design requirements. In addition, in the processing process, the hot-bending furnace needs to be heated to the softening temperature of the sintered stone as a whole, and then the temperature needs to be lowered by natural cooling before the hot-bent sintered stone is taken out, which results in a long manufacturing period, high energy consumption, and high production costs. [Means for solving the problem]

[0005] In response to the above problems, the present invention provides a sintered stone hot bending furnace and a sintered stone hot bending processing method, which adopts local reheating and introduces directional air flow for rapid cooling, thereby reducing energy consumption, shortening cooling time, shortening production period, and reducing production costs. Not only that, the bending radius of the produced hot-bent sintered stone meets the design requirements, has a high degree of compatibility with the mold, and does not affect the surface flatness and color decoration of the sintered stone.

[0006] In a first aspect, the present invention provides a sintered stone hot bending furnace, the sintered stone hot bending furnace comprising: A furnace body, a die disposed in the furnace chamber for placing the sintered stone to be hot-bent; a furnace cover configured as an insulating plate, the insulating plate being provided with a gas passage communicating with the furnace chamber; A blower unit is installed outside the furnace body and communicates with the gas passage of the furnace cover to supply air flow into the furnace chamber; A first heating device fixedly installed on the inner wall of the furnace body to adjust the environmental temperature of the furnace chamber; A heating device including a second heating device that moves vertically and / or horizontally in the furnace body to adjust the local heating temperature of the sintered stone at the location to be hot-bent; a temperature control device installed on the outer wall of the furnace body, which displays the ambient temperature of the furnace chamber and the local temperature of the sintered stone at the location to be hot-bent; a temperature sensing device interconnected with the temperature control device and the heating device, for adjusting the heating power of the heating device by adjusting the temperature control device; It is installed on the outer wall of the furnace body and includes an observation port for observing the hot bending condition of the sintered stone inside the furnace chamber.

[0007] Preferably, the flow direction of the air flow coincides with the molding direction of the sintered stone toward the arc of the mold, so that the sintered stone conforms toward the mold by the force of the air flow.

[0008] Preferably, the insulating plate has one or more holes formed therein to form a gas passageway, which communicates with an external blower unit.

[0009] Preferably, the insulating plate includes a first insulating plate and a second insulating plate fitted into the first insulating plate, the second insulating plate being made of a porous material, the first insulating plate having one or more air holes formed therein to form a gas passage, and the gas passage and the porous structure of the second insulating plate being connected to a blowing unit to supply air flow into the furnace chamber.

[0010] Preferably, the second heat insulating board is made of honeycomb ceramics having a porous structure distributed on the surface and inside.

[0011] Preferably, an expansion bracket to which a second heating device is attached is disposed on the insulating plate of the furnace roof, and the movement of the second heating device is adjusted by controlling the expansion bracket.

[0012] Preferably, the temperature sensing device includes a first temperature sensing device installed on the inner wall of the furnace body to sense the environmental temperature in the furnace chamber, and a second temperature sensing device arranged perpendicular to and spaced apart from the second heating device.

[0013] Preferably, the expansion bracket is fitted with a second temperature sensing device connected to the second heating device for sensing the local temperature at the location of the sintered stone to be hot bent.

[0014] In a second aspect, the present invention provides a method for hot bending sintered stone using any one of the sintered stone hot bending furnaces described above. The method includes: Step S1: placing the sintered stone to be hot-bent in a mold and closing the furnace chamber; Step S2: turning on a first heating device to preheat the furnace chamber; Step S3 of increasing the heating power of the first heating device, reheating the sintered stone until it softens, and promoting the initial molding of the sintered stone by its own gravity; Step S4: moving the second heating device to adjust the distance between the second heating device and the portion of the sintered stone to be hot-bent, and turning on the second heating device to locally heat the sintered stone to improve the fit between the sintered stone and the die; Step S5: turning off the first heating device and the second heating device and turning on the blower unit to introduce air flow into the furnace chamber to rapidly cool the sintered stone, and making the flow direction of the air flow coincide with the molding direction of the sintered stone toward the circular arc of the mold, so that the sintered stone is further fitted to the mold by the force of the air flow; Step S6 includes turning off the blower unit, allowing the furnace chamber to cool naturally to room temperature, and removing the hot-bent sintered stones.

[0015] Preferably, the local heating temperature is 1200 to 1300°C. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a flow chart of a method for hot bending sintered stone using a sintered stone hot bending furnace of the present invention. [Diagram 2] 2 is a perspective view of the sintered stone hot bending furnace of the present invention (some components are not shown). 1 is a gas passage, 2 is a heat insulating plate, 3 is a furnace body, 4 is a temperature sensor, 5 is a temperature control device, and 6 is an observation port. [Diagram 3] Fig. 3 is a cross-sectional view of the sintered stone hot bending furnace of the present invention. 1 is a gas passage, 2-1 is a first insulating plate, 2-2 is a second insulating plate, 3 is a furnace body, 4-1 is a first temperature sensor, 4-2 is a second temperature sensor, 7 is a first heating device, 8 is a second heating device, 9 is sintered stone, 10 is a mold, and 11 is an expansion bracket. [Figure 4] Figure 4 shows the discoloration defects of dark-colored hot-bent sintered stone produced using existing sintered stone thermal processing equipment. [Diagram 5] FIG. 5 is a diagram showing the arc error defects of hot-bent sintered stones of different lots manufactured using existing sintered stone thermal processing equipment. [Figure 6] FIG. 6 is a schematic diagram of the arc degree error of hot-bent sintered stones of different lots manufactured in Example 1. [Figure 7] FIG. 7 is an image of the dark-colored hot-bent sintered stone produced in Example 1. [Figure 8] FIG. 8 is an image of the hot-bent sintered stone tea table manufactured in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In order to make the objectives, technical solutions and technical effects of the present invention clearer, the present invention will be further described in detail below in conjunction with the brief description of the drawings and the detailed description of the invention.

[0018] The present invention provides a sintered stone hot bending furnace. The furnace body of the sintered stone hot bending furnace has a heat retention function. Preferably, the furnace body is made of a refractory heat-insulating material. The composition of the refractory heat-insulating material is not limited, and any refractory heat-insulating material commonly used in the field may be adopted. The shape and size of the furnace body can be adaptively adjusted according to demand. In some embodiments, the furnace body is a rectangular parallelepiped structure.

[0019] The mold is disposed in the furnace chamber. It is used to place the sintered stone to be hot-bent. The mold may adopt a graphite mold having the characteristics of fast heat conduction and high temperature resistance. The mold manufacturing process and mold structure are common in the field, and detailed description is omitted here. In practice, the graphite mold is formed based on the design drawing of the hot-bent sintered stone, and the shape, size and bending effect of the mold are consistent with the design drawing of the hot-bent sintered stone. The mold may be placed on a base on the opposite side of the furnace cover. Preferably, the upper surface of the base is fixedly connected to the lower surface of the mold.

[0020] The cover of the sintered stone hot bending furnace has a shape and size adapted to the furnace body. For example, if the furnace body has a rectangular parallelepiped structure, the cover is also constructed in a corresponding rectangular parallelepiped shape. The cover is placed over the furnace body to form a space (furnace chamber) that is relatively closed except for a specially designed gas passage. The cover is constructed as an insulating plate. The insulating plate may be one-piece, two-piece, or of course multi-piece design. The insulating plate is provided with a gas passage communicating with the furnace chamber.

[0021] The blower unit is installed outside the furnace body and communicates with the gas passage of the furnace cover to supply air flow into the furnace chamber. The blower unit may be an electric blower. The flow direction of the air flow coincides with the direction of change (i.e., molding) of the sintered stone (which may have a flat surface) into the arc of the mold, and the force of the air flow makes the sintered stone conform to the mold direction.

[0022] In some embodiments, the furnace cover is an integrally molded insulation plate. The insulation plate has one or more holes to form a gas passage and communicate with an external blower unit. During quenching, the airflow supplied by the blower unit is blown directly into the furnace chamber through the gas passage. When the flow direction of the airflow coincides with the change direction of the sintered stone according to the arc of the mold, the force of the airflow causes the sintered stone to be shaped toward the mold. Since the mold is placed on a base opposite to the furnace cover, the sintered stone placed on the mold can also correspond to the holes of the furnace cover, and the direction and strength of the force of the airflow can be maintained to the maximum extent possible from external factors.

[0023] In some embodiments, the furnace cover is an insulating plate formed as a two-piece. The insulating plate includes a first insulating plate and a second insulating plate fitted into the first insulating plate. The second insulating plate has a shape that matches the first insulating plate. The first insulating plate and the second insulating plate may have one or more through holes as a gas passage. Preferably, the second insulating plate is made of a porous material, and the first insulating plate has one or more holes opened therein to form a gas passage. In this way, the gas passage and the porous structure of the second insulating plate communicate with the blowing unit to supply an air flow into the furnace chamber. In this way, the air flow supplied by the blowing unit during quenching is blown directly into the furnace chamber through this gas passage, and when the flow direction of the air flow coincides with the change direction of the sintered stone along the arc of the mold, the force of the air flow makes the sintered stone conform toward the mold.

[0024] Preferably, the second insulation plate is made of honeycomb ceramics having a porous structure distributed on the surface and inside. The air flow delivered by the blower unit passes through the gas passage of the first insulation plate, enters the inside of the second insulation plate, passes through the pores, and enters the furnace chamber, and then acts on the sintered stones.

[0025] The heating device includes a first heating device and a second heating device. The first heating device is fixedly installed on the inner wall of the furnace body and functions to adjust the overall environmental temperature of the furnace chamber. The first heating device may adopt ordinary electric heating components in this field. Including but not limited to electric heating wire (wire heating furnace), electric heating tube, electric heating plate. For example, it may be a wire heating furnace. The number of heating components of the first heating device can be adaptively adjusted according to the actual situation. In some embodiments, one or more wire heating furnaces are respectively arranged on the inner walls of the opposite sides of the furnace body. The environmental temperature of the furnace chamber can be changed by adjusting the heating power of the first heating device.

[0026] The second heating device is placed in the furnace chamber and can be moved vertically and / or horizontally in the furnace body. The second heating device is placed at or near the location where the sintered stone is to be hot-bent. By moving the second heating device, the distance between the second heating device and the location where the sintered stone is to be hot-bent is adjusted, and the local heating temperature of the sintered stone at that location is changed. The second heating device may adopt a mobile heating component commonly used in this field. For example, it may be a mobile siliconite. The number of second heating devices can be adaptively adjusted according to the actual situation. The local heating temperature can be changed by adjusting the heating power of the second heating device.

[0027] A telescopic bracket is arranged on the insulating plate of the furnace cover, on which the second heating device is attached. The movement of the second heating device is adjusted by controlling the telescopic bracket. For example, the distance between the second heating device and the hot bending sintered stone is adjusted by adjusting the length of the telescopic bracket. In this way, the second heating device and the mold are located on opposite sides, and the hot bending process can be controlled more conveniently.

[0028] The second heating device is movably arranged in the sintered stone hot bending furnace to locally heat the portion of the sintered stone to be hot bent, so that the portion of the sintered stone to be hot bent can be closely and quickly fitted into the mold to achieve the design standard.

[0029] The temperature control device is installed on the outer wall of the furnace body and displays the ambient temperature of the furnace chamber and the local temperature of the sintered stone to be hot-bent. In some embodiments, the temperature control device includes a panel that displays the temperature.

[0030] The temperature sensing device is interconnected with the temperature control device and the heating device, and adjusts the heating power of the heating device by controlling the temperature control device. In some embodiments, the temperature sensing device includes a first temperature sensing device installed on the inner wall of the furnace body to sense the environmental temperature of the furnace chamber, and a second temperature sensing device disposed perpendicular to and spaced apart from the second heating device.

[0031] The temperature sensing device may be a thermocouple for measuring temperature. For the first temperature sensing device, one or more thermocouples may be provided on the inner walls of both opposing sides of the furnace body, respectively, to detect the environmental temperature in each area of ​​the furnace chamber. For the second temperature sensing device, the distance from the second heating device is preferably 3 to 6 cm, and this distance can satisfactorily reflect the local temperature of the portion of the sintered stone to be hot-bent. Preferably, the second temperature sensing device connected to the second heating device is attached to the expansion bracket to sense the local temperature of the portion of the sintered stone to be hot-bent.

[0032] The observation port is installed on the outer wall of the furnace body to observe the hot bending state of the sintered stone in the furnace chamber. The observation port is one or more observation holes or observation windows.

[0033] In the existing sintered stone hot bending furnace, the entire sintered stone is heated in the production process of hot bending sintered stone, which causes the flat surface of the sintered stone to overheat and warp or change color, and the parts to be hot bent are insufficiently or unevenly heated, which is also prone to color change and cannot be precisely fitted to the mold. The sintered stone hot bending furnace of the present invention overcomes the above problems, and the obtained hot-bent sintered stone has a high degree of consistency with the mold, meets the design requirements, and does not affect the surface flatness or color decoration of the sintered stone.

[0034] Hereinafter, a method for hot bending sintered stone using the above-mentioned sintered stone hot bending furnace will be described as an example.

[0035] Select the sintered stone to be hot bent. The composition of the sintered stone is not limited, and the composition of the sintered stone commonly used in this field is adopted. The specification of the sintered stone is not limited, but the specification of the sintered stone needs to be compatible with the dimensions of the furnace chamber. In a specific embodiment, the sintered stone manufactured by Monalisa Group Co., Ltd. is used.

[0036] The sintered stone to be hot-bent is placed on the surface of the die, and the furnace chamber is closed. For example, the sintered stone to be hot-bent is placed on the die in the furnace chamber, and the furnace chamber is closed by placing a furnace lid on it.

[0037] Preheating. Sintered stones are porcelain slabs made with advanced technology and are brittle materials, and cracks often occur during heating due to the influence of thermal stress. In addition, sintered stones are poor conductors of heat, and the heat transfer rate is relatively slow. In the first heating process, the temperature is low, the heat radiation is small, and the surface of the sintered stone is heated first, and at the same time, the temperature of the mold in the furnace chamber is low, and there is a large temperature difference in the thickness direction of the sintered stone, so the sintered stone is heated unevenly, and the thermal expansion of the sintered stone does not match, and stress occurs. If the thermal stress exceeds the strength of the sintered stone, the sintered stone will explode. Within a certain range, the faster the heating rate, the larger the temperature difference and the larger the thermal stress. Therefore, it is necessary to preheat and heat the sintered stone uniformly in the thickness direction to prevent the sintered stone from exploding in the process from room temperature to reheating. Preheating is performed using the first heating device. The preheating is performed by uniformly heating the furnace chamber to 800-900 ° C within 25-50 minutes.

[0038] Reheating. The power of the first heating device is increased to reheat and soften the sintered stone, which is then initially molded by gravity. The shape of the initial molded stone almost matches the shape of the mold. The reheating raises the environmental temperature of the furnace from 800-900°C to 1000-1100°C within 30-40 minutes.

[0039] The fitting process is performed locally at high temperature. The second heating device is moved to adjust the distance between the second heating device and the part of the sintered stone to be hot-bent. At the same time, the second heating device is turned on to locally heat the part of the sintered stone to be hot-bent, and promote the fitting (heat retention) between the part of the sintered stone to be hot-bent and the mold. The movement of the second heating device can be controlled by a computer program. The distance between the second heating device and the part of the sintered stone to be hot-bent is preferably 1 to 3 cm. If the distance between the second heating device and the part of the sintered stone to be hot-bent is too close, the local temperature of the sintered stone will be too high and defects such as hot-bending holes will occur, and if the distance is too far, the part of the sintered stone to be hot-bent cannot be effectively locally heated, which will affect the bending effect. The local heating temperature may be 1200 to 1300 ° C. The sintering temperature range of the sintered stone is 1250 to 1270 ° C, and the above local heating temperature can further soften the part of the sintered stone to be hot-bent and completely fit the mold.

[0040] The first and second heating devices are turned off, and air is introduced into the furnace chamber to perform quenching, and the (downward) action force generated by the introduced air in the furnace chamber makes the sintered stone more conform to the mold. Specifically, air flow is introduced into the furnace chamber to quench the sintered stone, and the flow direction of the air flow coincides with the direction in which the sintered stone changes to the mold arc, so that the force of the air flow makes the sintered stone more conform to the mold. In the conventional technology, the sintered stone is slowly cooled by high-temperature annealing through temperature control or by natural cooling, but since there is no wind force, the sintered stone cannot be further molded to fit the mold. The speed of quenching can be controlled by controlling the output of the blower unit and adjusting the air volume of the blower unit. When the air volume is large, a lot of air enters the furnace body, and the quenching speed is fast, and when the air volume is small, the air enters the furnace body, and the quenching speed is slow.

[0041] Preferably, the rapid cooling is performed by lowering the temperature of the furnace chamber to 800-900°C within 30-50 minutes. For example, the rapid cooling is performed by lowering the temperature of the furnace chamber to 850°C within 30-50 minutes. By introducing a directional air flow into the furnace chamber to rapidly cool the sintered stone, the temperature drop rate is increased, the production period of the product is shortened, and the softened sintered stone is further molded by fitting it to a mold by the wind force.

[0042] In some embodiments, the blower unit is turned on, and the air enters the furnace chamber from the gas passage of the first insulating plate through the pores of the second insulating plate, and a certain downward force is formed after the gas enters, which acts on the softened sintered stone, so that the softened sintered stone is further adapted to the mold by the wind force. At the same time, the air can also achieve the purpose of rapid cooling.

[0043] Cool naturally. Turn off the blower unit and allow the furnace chamber to cool naturally to room temperature to obtain a hot-bent sintered stone that fits the mold and meets the bending radius design requirements.

[0044] The hot-bent sintered stone includes, but is not limited to, convex-arc sintered stone, concave-arc sintered stone, wave-shaped sintered stone, folded-plate sintered stone, etc. The hot-bent sintered stone also includes, but is not limited to, inner-bent sintered stone or outer-bent sintered stone, and the bending angle is not limited to a fixed angle.

[0045] The hot bending method of the present invention uses a first heating device to raise the environmental temperature in the furnace chamber to 1000-1100°C, and forms the sintered stone into a basic shape that fits the mold by its own gravity, and uses a second heating device to locally heat the area of ​​the sintered stone to be hot bent, so that the area of ​​the sintered stone to be hot bent fits tightly and quickly to the mold, thereby achieving the design standard.

[0046] When manufacturing a dark-colored hot-bent product using the thermal processing device and method of Patent Document 1, localized discoloration is observed in the hot-bent portion of the sintered stone as shown in Figure 4, and a large arc degree error occurs when manufacturing an arc-shaped hot-bent product. As shown in Figure 5, the deviation in arc coincidence between arc-shaped hot-bent products of different lots reaches 10 mm.

[0047] The present invention will be described in more detail through the following examples. Similarly, the following examples are provided to further illustrate the present invention and do not limit the scope of the present invention. Non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention are both within the scope of the present invention. Specific process variables in the following examples are merely examples within the applicable range, that is, those skilled in the art can select within an appropriate range based on the description of the present invention, and are not limited to the specific numerical values ​​in the following examples.

[0048] As shown in FIG. 2 and FIG. 3, the hot bending furnace includes a furnace body 3 made of a fireproof heat-insulating material. An insulating plate 2 is designed on the upper part of the furnace body 3. The insulating plate 2 is an insulating plate formed like a two-piece, and includes a first insulating plate 2-1 and a second insulating plate 2-2. The second insulating plate 2-2 is fitted inside the first insulating plate 2-1. The second insulating plate 2-2 is made of honeycomb ceramics with porosity distributed on the surface and inside. The first insulating plate 2-1 is provided with a gas passage 1. The gas passage, the pores of the porous structure of the second insulating plate, and the external blower unit communicate with each other to supply air flow into the furnace chamber. A mold 10 is placed on the bottom of the furnace chamber of the furnace body 3. A sintered stone 9 to be hot-bent is placed on the upper surface of the mold 10. A first heating device 7 and a second heating device 8 are installed in the furnace chamber of the furnace body 3. The first heating device is a wire heating furnace, which is fixed to the inner wall of the furnace chamber. The second heating device is a mobile siliconite, which is installed in the furnace chamber, and the mobile siliconite can move vertically and horizontally in the furnace body, thereby adjusting the distance between the mobile siliconite and the part of the sintered stone to be hot-bent. A first temperature sensor 4-1 for temperature measurement is installed on the side wall of the furnace body 3. An expansion bracket 11 on which a second temperature sensor 4-2 is installed is arranged on the heat insulating plate 2 of the furnace cover. A temperature control device 5 is installed on the outer wall of the furnace body 3. The temperature control device 5 is connected to the first heating device 7, the second heating device 8, the expansion bracket 11, the first temperature sensor 4-1, and the second temperature sensor 4-2. By adjusting the temperature control device 5, the adjustment of the environmental temperature in the sintered stone hot bending furnace during the hot bending process is realized. Moreover, the movement of the second heating device is controlled by adjusting the temperature control device 5, specifically, the distance between the second heating device 8 and the sintered stone 9 is controlled by adjusting the extension length of the extension bracket 11. The outer wall of the furnace body 3 is further provided with observation ports (three observation holes) 6 for observing the hot bending state of the sintered stone inside the furnace.

[0049] Example 1 The sintered stone is pre-treated. The sintered stone to be treated is cut to a thickness of 5.5 mm, and the edges on all four sides are polished, after which it is washed and dried. The dimensional deviation of the sintered stone after cutting is controlled to ±0.3 mm.

[0050] Hot bending is performed. The graphite mold is placed on the base and the mold is fixed. The sintered stone to be hot bent is placed on the mold, the sintered stone is parallel to the four sides of the mold, the furnace cover is placed, and the hot bending furnace is closed. The first heating device is turned on to preheat the heating furnace, and the preheating is performed by uniformly increasing the temperature of the furnace chamber to 800°C within 25 minutes.

[0051] Then, the sintered stone is softened under high temperature conditions and initially molded according to the shape of the mold by its own gravity. The reheating is carried out by slowly increasing the temperature of the furnace chamber to 1000℃ within 30 minutes.

[0052] A high temperature fitting process is performed locally. The second heating device is moved to control the distance between the second heating device and the part of the sintered stone to be hot-bent to 3 cm, and the power of the second heating device is turned on to locally heat the part to be hot-bent to 1200°C. The fitting condition of the sintered stone and the mold in the furnace chamber is observed through the observation hole until the sintered stone fits into the mold under its own gravity.

[0053] The first and second heating devices are turned off, and the blower unit is turned on, so that the air flows from the gas passage of the first insulating plate through the pores of the second insulating plate into the furnace chamber, and a certain downward force is formed after the gas enters, which acts on the softened sintered stone, so that the sintered stone is further molded to fit the mold under the influence of the wind force, and the purpose of rapid cooling is also achieved. The rapid cooling reduces the temperature of the furnace chamber to 850℃ within 30 minutes.

[0054] The blower unit is turned off and the stone is allowed to cool naturally to room temperature, after which it is processed into hot-bent sintered stone with an inward bending angle of 125°.

[0055] 6 is a schematic diagram of the arc degree error of different lots of sintered stones manufactured in Example 1. It can be seen that the arc degree error is significantly reduced. The maximum deviation of the arc conformity of the hot-bent sintered stones of different lots was only 3 mm.

[0056] 7 is an image of the dark-colored hot-bent sintered stone produced in Example 1. No localized discoloration occurs in the dark-colored hot-bent sintered stone.

[0057] Example 2 The sintered stone is pre-treated. The sintered stone to be treated is cut to a thickness of 15.5 mm, and the edges on all four sides are polished, after which it is washed and dried. The dimensional deviation of the sintered stone after cutting is controlled to ±0.3 mm.

[0058] Hot bending is performed. The graphite mold is placed on the base and the mold is fixed. The sintered stone to be hot bent is placed on the mold, the sintered stone is parallel to the four sides of the mold, the furnace cover is placed, and the hot bending furnace is closed. The first heating device is turned on to preheat the heating furnace, and the preheating is performed by uniformly increasing the temperature of the furnace chamber to 850°C within 50 minutes.

[0059] Then, the sintered stone is softened under high temperature conditions and initially molded according to the shape of the mold by its own gravity. The reheating is carried out by slowly increasing the temperature of the furnace chamber to 1100℃ within 40 minutes.

[0060] A high temperature fitting process is performed locally. The second heating device is moved to control the distance between the second heating device and the part of the sintered stone to be hot-bent to 1.5 cm, and the power of the second heating device is turned on to locally heat the part to be hot-bent to 1300°C. The fitting condition of the sintered stone and the mold in the furnace chamber is observed through the observation hole until the sintered stone fits into the mold under its own gravity.

[0061] The first and second heating devices are turned off, and the blower unit is turned on, so that the air flows from the gas passage of the first insulating plate through the pores of the second insulating plate into the furnace chamber, and a certain downward force is formed after the gas enters, which acts on the softened sintered stone, so that the sintered stone can be further molded to fit the mold under the influence of the wind force, and the purpose of rapid cooling is achieved. The rapid cooling reduces the temperature of the furnace chamber to 850℃ within 50 minutes.

[0062] The fan unit is turned off and the stone is allowed to cool naturally to room temperature, after which it is processed into a hot-bent sintered stone tea table with a 90° bending angle.

[0063] 8 is an image of the hot-bent sintered stone tea table manufactured in Example 2. The bending radius of the hot-bent sintered stone tea table meets the design requirements.

[0064] Example 3 The sintered stone is pre-treated. The sintered stone to be treated is cut to a thickness of 10.5 mm, and the edges on all four sides are polished, after which it is washed and dried. The dimensional deviation of the sintered stone after cutting is controlled to ±0.3 mm.

[0065] Hot bending is performed. The graphite mold is placed on the base and the mold is fixed. The sintered stone to be hot bent is placed on the mold, the sintered stone is parallel to the four sides of the mold, the furnace cover is placed, and the hot bending furnace is closed. The first heating device is turned on to preheat the heating furnace, and the preheating is performed by uniformly increasing the temperature of the furnace chamber to 900°C within 40 minutes.

[0066] The sintered stone is then softened under high temperature conditions and initially shaped according to the mold shape by its own gravity. The reheating is carried out by slowly increasing the temperature of the furnace chamber to 1050°C within 45 minutes.

[0067] The fitting process is carried out at a local high temperature. The second heating device is moved to control the distance between the second heating device and the part of the sintered stone to be hot-bent to 1.0 cm, and the power of the second heating device is turned on to locally heat the part to be hot-bent to 1250°C. The fitting status of the sintered stone and the mold in the furnace chamber is observed through the observation hole until the sintered stone fits into the mold under its own gravity.

[0068] The first and second heating devices are turned off, and the blower unit is turned on, so that the air flows from the gas passage of the first insulating plate through the pores of the second insulating plate into the furnace chamber, and a certain downward force is formed after the gas enters, which acts on the softened sintered stone, so that the sintered stone can be further molded to fit the mold under the influence of the wind force, and the purpose of rapid cooling is also achieved. The rapid cooling reduces the temperature of the furnace chamber to 850℃ within 45 minutes.

[0069] The blower unit is turned off and the basin is allowed to cool naturally to room temperature, after which it is processed into a hot-bent sintered stone hand washing basin.

Claims

1. A furnace body, a die disposed in the furnace chamber for placing the sintered stone to be hot-bent; a furnace cover configured as an insulating plate, the insulating plate being provided with a gas passage communicating with the furnace chamber; A blower unit is installed outside the furnace body and communicates with the gas passage of the furnace cover to supply air flow into the furnace chamber; A heating device including a first heating device fixedly installed on the inner wall of the furnace body to adjust the environmental temperature of the furnace chamber, and a second heating device moving vertically and / or horizontally of the furnace body to adjust the local heating temperature of the sintered stone at the location to be hot-bent; a temperature control device installed on the outer wall of the furnace body, which displays the ambient temperature of the furnace chamber and the local temperature of the sintered stone at the location to be hot-bent; a temperature sensing device interconnected with the temperature control device and the heating device, for adjusting the heating power of the heating device by adjusting the temperature control device; An observation port is installed on the outer wall of the furnace body for observing the hot bending state of the sintered stone in the furnace chamber; A sintered stone hot bending furnace for hot bending sintered stone, in which the heating power of a first heating device is increased to reheat the sintered stone until it softens, thereby promoting the initial shaping of the sintered stone by its own gravity, the second heating device is moved to adjust the distance between the second heating device and the portion of the initially shaped sintered stone to be hot bent, and the second heating device is turned on to locally heat the sintered stone so as to improve the fit between the sintered stone and the mold, the first heating device and the second heating device are turned off and the blower unit is turned on to introduce air flow into the furnace chamber, and the flow direction of the air flow is made to coincide with the shaping direction of the sintered stone toward the arc of the mold, so that the sintered stone is further fitted to the mold by the force of the air flow.

2. The sintered stone hot bending furnace according to claim 1 , wherein the insulating plate is provided with one or more holes to form a gas passage, which communicates with an external blowing unit.

3. 2. The sintered stone hot bending furnace according to claim 1, wherein the insulating plate includes a first insulating plate and a second insulating plate fitted into the first insulating plate, the second insulating plate is made of a porous material, the first insulating plate has one or more air holes formed therein to form a gas passage, and the gas passage and the porous structure of the second insulating plate communicate with a blowing unit to supply air flow into the furnace chamber.

4. The sintered stone hot bending furnace according to claim 3, wherein the second insulating plate is made of honeycomb ceramics having a porous structure distributed on the surface and inside.

5. The sintered stone hot bending furnace according to claim 1, wherein an expansion bracket to which a second heating device is attached is arranged on the insulating plate of the furnace cover, and the movement of the second heating device is adjusted by controlling the expansion bracket.

6. 2. The sintered stone hot bending furnace according to claim 1, wherein the temperature sensing device includes a first temperature sensing device installed on the inner wall of the furnace body to sense the environmental temperature in the furnace chamber, and a second temperature sensing device arranged perpendicular to and spaced apart from the second heating device.

7. 7. The sintered stone hot bending furnace according to claim 6, wherein the expansion bracket is provided with a second temperature sensing device connected to the second heating device for sensing the local temperature of the portion of the sintered stone to be hot bent.

8. A method for hot bending sintered stone using the sintered stone hot bending furnace according to any one of claims 1 to 7, Step S1: placing the sintered stone to be hot-bent in a mold and closing the furnace chamber; Step S2: turning on the first heating device to preheat the furnace chamber; Step S3: increasing the heating power of the first heating device, reheating the sintered stone until it is softened, and promoting the initial molding of the sintered stone by its own gravity; Step S4: moving the second heating device to adjust the distance between the second heating device and the portion of the sintered stone to be hot-bent, and turning on the second heating device to locally heat the sintered stone so as to improve the fit between the sintered stone and the die; Step S5: turn off the first heating device and the second heating device and turn on the blower unit to introduce air flow into the furnace chamber to rapidly cool the sintered stone, and make the flow direction of the air flow coincide with the molding direction of the sintered stone toward the circular arc of the mold, so that the sintered stone is further fitted to the mold by the force of the air flow; A method for hot bending sintered stones, comprising step S6 of turning off the blower unit, allowing the furnace chamber to cool naturally to room temperature, and removing the hot-bent sintered stones.

9. The method according to claim 8, wherein the localized heating temperature is 1200 to 1300°C.

Citation Information

Patent Citations

  • Hot bending furnace for colored glazing glass, method for preparing colored glazing toughened hot-bent glass and colored glazing toughened hot-bent glass

    CN102372423A

  • Hot working device and method for rock plates in different shapes

    CN111960653A

  • Positive-pressure curved glass forming mold and heating equipment thereof

    CN209259924U

  • Manufacture of bent tempered glass plate

    JP1984013639A

  • Bending apparatus and bending method of glass plate

    JP2010030859A