Pouch film laminate and battery case manufactured using the same
The pouch film laminate with tailored loop rigidity and layer composition addresses moldability issues, enabling deep cup formation and reduced curling, thus increasing the battery case's accommodation volume and energy density.
Patent Information
- Application Number
- JP2024536499
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-24
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-12-22
AI Technical Summary
Conventional pouch film laminates for battery cases have limitations in moldability, leading to restricted depth of the cup portion, increased dead space, and reduced energy efficiency due to curling and difficulty in forming sharp corners.
A pouch film laminate with specific loop rigidity in the MD direction of 750 mN to 1300 mN, combined with a ratio of TD to MD loop rigidity of 0.8 to 1.2, utilizing a base layer of polyethylene terephthalate and nylon films, a gas barrier layer of aluminum alloy, and a sealant layer of unoriented polypropylene, to enhance drawability and reduce curling.
The solution allows for deep cup formation with sharp corners, minimizing curling and increasing the accommodation volume for the electrode assembly, thereby enhancing energy density and reducing process defects.
Smart Images

Figure 2024544321000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0187275 filed on December 24, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a pouch film laminate and a battery case manufactured using the same, and more specifically, to a pouch film laminate that has excellent formability and is less prone to curling after molding, and a battery case manufactured using the same. [Background technology]
[0003] Secondary batteries are used not only in small products such as digital cameras, portable DVD players, MP3 players, mobile phones, PDAs, portable game devices, power tools, and e-bikes, but also in large products that require high output such as electric vehicles and hybrid cars, as well as in power storage devices and backup power storage devices that store surplus generated electricity and new renewable energy.
[0004] Generally, a secondary battery is manufactured by coating a positive electrode current collector and a negative electrode current collector with an electrode active material slurry to manufacture a positive electrode and a negative electrode, laminating them on both sides of a separator to form an electrode assembly of a predetermined shape, housing the electrode assembly in a battery case, injecting an electrolyte, and sealing the case.
[0005] Secondary batteries are divided into pouch type and can type depending on the material of the case that houses the electrode assembly. The pouch type houses the electrode assembly in a pouch made of a flexible polymer material, while the can type houses the electrode assembly in a case made of metal or plastic.
[0006] The pouch-type battery case is manufactured by pressing a flexible pouch film laminate to form a cup portion, and then, after the cup portion is formed, an electrode assembly is placed in the receiving space of the cup portion and the seal portion is sealed to manufacture a secondary battery.
[0007] Among such press processes, drawing molding is performed by inserting a pouch film into a press device and applying pressure to the pouch film laminate with a punch to stretch the pouch film laminate. The pouch film laminate is generally formed of multiple layers, with a polymer film such as polyethylene terephthalate laminated on one side of a gas barrier layer made of a metal material and a sealant layer laminated on the other side.
[0008] However, such conventional pouch film laminates have low formability, which limits how deep the cup can be formed, and when filleting is applied to the corners of the bottom and opening of the cup, there is also a limit to how much the filleting radius can be reduced. There is also a limit to how close the wall of the cup can be to a vertical shape. This increases the dead space of the secondary battery, reduces the size of the electrode assembly, and reduces the energy efficiency per volume. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made to solve the above-mentioned problems, and has an object to provide a pouch film laminate that has excellent draw formability, can form a deep cup portion, and is less likely to curl after forming, and a battery case manufactured using the same. [Means for solving the problem]
[0010] In one aspect, the present invention provides a pouch film laminate including a gas barrier layer, a base layer disposed on one side of the gas barrier layer, and a sealant layer disposed on the other side of the gas barrier layer, the pouch film laminate having a loop stiffness in the MD direction of 750 mN to 1300 mN.
[0011] Preferably, the loop stiffness in the TD direction of the pouch film laminate can be 750 mN to 1300 mN, and the ratio of the loop stiffness in the TD direction to the loop stiffness in the MD direction can be 0.8 to 1.2.
[0012] The base layer may have a breaking strength in the MD direction of 10 N / 15 mm to 18 N / 15 mm.
[0013] Also, according to one embodiment, the base layer may be a laminate of a polyethylene terephthalate film and a nylon film, wherein the polyethylene terephthalate film has a thickness of 5 μm to 20 μm, and the nylon film has a thickness of 10 μm to 30 μm.
[0014] The gas barrier layer may have a thickness of 50 μm to 100 μm and may include an aluminum alloy thin film. Preferably, the aluminum alloy thin film may include 1.2 wt % to 1.7 wt % of iron and have a crystal grain size of 10 μm to 13 μm.
[0015] The sealant layer may have a thickness of 60 μm to 100 μm and may include unstretched polypropylene, acid-modified polypropylene, polypropylene-butylene-ethylene copolymer, or a combination thereof.
[0016] In another aspect, the present invention provides a battery case produced by drawing the above-mentioned pouch film laminate of the present invention, comprising a cup portion having a depth of 10 mm or more and a curl height of 25 mm or less. Effect of the Invention
[0017] When the loop stiffness of the pouch film laminate satisfies the range of the present invention, the limit forming depth during cup forming is large, the corners of the cup can be formed with a large gradient, and curling is reduced after the cup is formed. Therefore, by using the pouch film laminate according to the present invention, a battery case having a large storage volume for an electrode assembly and less curling can be manufactured. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a cross-sectional view of a pouch film laminate according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram illustrating a method for measuring loop stiffness. [Diagram 3] 1 is a diagram illustrating a battery case according to an embodiment of the present invention. [Figure 4] 13A and 13B are diagrams illustrating a battery case according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will now be described in more detail.
[0020] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0021] In the present invention, "MD direction (Machine Direction)" means the longitudinal direction of the pouch film laminate, and "TD direction (Transverse Direction)" means the width direction of the pouch film laminate.
[0022] The present inventors have conducted extensive research to manufacture a battery case that has a large storage space for a battery assembly, can realize a high energy density, and has little curling and few process defects after cup molding. As a result, they have found that the above-mentioned object can be achieved when a battery case is manufactured using a pouch film laminate having a loop rigidity that satisfies a specific range, and have thus completed the present invention.
[0023] <Pouch film laminate> An embodiment of the pouch film laminate according to the present invention is illustrated in Fig. 1. Hereinafter, the pouch film laminate according to the present invention will be described with reference to Fig. 1.
[0024] Referring to FIG. 1, a pouch film laminate 1 according to the present invention includes a gas barrier layer 20, a base layer 10 disposed on one side of the gas barrier layer, and a sealant layer 30 disposed on the other side of the gas barrier layer, and is characterized in that the MD direction loop stiffness of the pouch film laminate is 750 mN to 1300 mN, preferably 800 mN to 1200 mN, and more preferably 800 mN to 1000 mN.
[0025] When the loop stiffness of the pouch film laminate 1 in the MD direction is 750 mN to 1300 mN, it has excellent drawability and can form a deep cup part, and the clearance required during the formation of the cup part is small, so that the gradient of the wall surface can be formed sharply, and it has excellent curling resistance after formation. Specifically, when the loop stiffness of the pouch film laminate in the MD direction is less than 750 mN, the drawability is reduced and there is a limit to increasing the storage volume of the cup part, and when the loop stiffness in the MD direction is more than 1300 mN, curling may occur severely after the formation of the cup. If the volume of the cup part is small, the number of battery assemblies that can be accommodated is small, and high energy density cannot be achieved, and if curling occurs after the formation of the cup, problems such as vacuum destruction phenomenon during pouch transfer for the battery assembly process and / or wrinkles on the battery case during the degass sealing process may occur.
[0026] Furthermore, the pouch film laminate of the present invention may have a ratio of the loop rigidity in the TD direction to the loop rigidity in the MD direction of 0.8 to 1.2, preferably 0.9 to 1.1. When the ratio of the loop rigidity in the TD direction to the loop rigidity in the MD direction of the pouch film laminate satisfies the above range, damage and wrinkles can be suppressed during the cup forming process.
[0027] Specifically, the loop rigidity in the TD direction of the pouch film laminate of the present invention is preferably 750 mN to 1300 mN, preferably 800 mN to 1200 mN, and more preferably 800 mN to 1000 mN. When the loop rigidity in the TD direction satisfies the above range, the pouch film laminate has excellent draw formability, can effectively suppress the occurrence of curling after the molding of a cup, and has a small difference from the loop rigidity in the MD direction, so that the occurrence of damage and wrinkles after molding can be suppressed.
[0028] FIG. 2 illustrates the process of measuring the loop stiffness of the pouch film laminate of the present invention. As illustrated in FIG. 2(a), first, the pouch film laminate is cut to a width×length of 15 mm×150 mm to prepare a measurement sample. When measuring the loop stiffness in the MD (machine direction), the sample is cut so that the MD direction coincides with the width direction of the measurement sample, and when measuring the loop stiffness in the TD (transverse direction), the sample is cut so that the TD direction coincides with the width direction of the measurement sample. Then, as illustrated in FIG. 2(b), both ends of the measurement sample are clamped and fixed with clips of a measuring device, and as illustrated in FIG. 2(c), the clips are moved to deform the measurement sample into a loop shape. Then, as illustrated in FIG. 2(d), the loop is pressed in at a speed of 5 mm / min, and the maximum load value applied to the loop during deformation is measured, which is the loop stiffness value.
[0029] The loop rigidity of the pouch film laminate is affected by the thickness and material of each layer (i.e., base layer, gas barrier layer, sealant layer) constituting the pouch film laminate, so that the thickness and material of each layer constituting the pouch film laminate can be adjusted to produce a pouch film laminate having a desired loop rigidity. For example, the gas barrier layer is formed of a soft aluminum thin film (e.g., AA8021) having a high elongation rate, the gas barrier layer is formed to a thickness of 50 μm to 100 μm, and the base layer is formed of a film or film laminate having a MD breaking strength of 10 N / 15 mm to 18 N / 15 mm, so that the pouch film laminate satisfying the loop rigidity of the present invention can be produced. However, the method for producing the pouch film laminate satisfying the loop rigidity value of the present invention is not limited to this.
[0030] Each layer of the pouch film laminate according to the present invention will now be described in detail.
[0031] Base material layer The substrate layer 10 is disposed on the outermost layer of the battery case to protect the electrode assembly from external impacts and to provide electrical insulation.
[0032] The substrate layer 10 may be made of a polymer material, for example, one or more polymer materials selected from the group consisting of polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymers, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, polyparaphenylene benzobisoxazole, polyarylate, and Teflon (registered trademark).
[0033] The substrate layer 10 may have a single layer structure, or may have a multi-layer structure in which different polymer films 12 and 14 are laminated as shown in Fig. 1. When the substrate layer 10 has a multi-layer structure, an adhesive layer 16a may be interposed between the polymer films.
[0034] Meanwhile, the base layer 10 may have a total thickness of 5 μm to 60 μm, preferably 10 μm to 50 μm, and more preferably 20 μm to 50 μm. When the base layer has a multi-layer structure, the thickness includes the thickness of the adhesive layer interposed between the films. Here, the thickness of the adhesive layer may be 1 to 10 μm, preferably 1 to 7 μm, and more preferably 1 to 4 μm. When the thickness of the base layer 10 satisfies the above range, the durability, insulation, and formability are excellent. If the thickness of the base layer is too thin, the durability decreases and the base layer may be damaged during the forming process, and if the thickness is too thick, the formability may decrease, the total thickness of the pouch film laminate film may increase, the battery storage space may decrease, and the energy density may decrease.
[0035] In the present invention, the base layer may have a breaking strength in the MD direction of about 10 N / 15 mm to 18 N / 15 mm, preferably about 10 N / 15 mm to 15 N / 15 mm. When the breaking strength in the MD direction of the base layer satisfies the above range, the loop stiffness value in the MD direction required in the present invention can be easily realized. If the breaking strength in the MD direction of the base layer is too small, the loop stiffness in the MD direction of the pouch film laminate decreases, and if it is too large, the loop stiffness in the MD direction of the pouch film laminate becomes excessively large.
[0036] Meanwhile, the MD breaking strength of the base layer is the strength at which the base layer breaks when pulled in the MD, and can be measured by cutting a film or film laminate constituting the base layer so that the MD is the longitudinal direction to prepare a measurement sample, and then mounting the measurement sample in a UTM device and pulling it to measure the maximum strength at which break occurs.
[0037] The MD breaking strength of the substrate layer varies depending on the type of film constituting the substrate layer, the film thickness, and / or the thickness of the adhesive layer, etc., so that a substrate layer having the desired breaking strength can be formed by appropriately adjusting the type of film, the film thickness, and / or the adhesive layer thickness, etc.
[0038] According to one embodiment, the base layer 10 may have a laminated structure of a polyethylene terephthalate (PET) film and a nylon film. Here, it is preferable that the nylon film is disposed on the gas barrier layer 20 side, i.e., on the inside, and the polyethylene terephthalate film is disposed on the surface side of the battery case.
[0039] Polyethylene terephthalate (PET) has excellent durability and electrical insulation, and when a PET film is placed on the surface side, it has excellent durability and insulation. However, in the case of a PET film, the adhesion to the aluminum alloy thin film constituting the gas barrier layer 20 is weak, and the stretching behavior is also different, so when a PET film is placed on the gas barrier layer side, peeling between the base layer and the gas barrier layer may occur during the molding process, and the gas barrier layer may not be stretched uniformly, resulting in a problem of reduced moldability. In contrast, since the stretching behavior of a nylon film is similar to that of the aluminum alloy thin film constituting the gas barrier layer 20, when a nylon film is placed between the polyethylene terephthalate and the gas barrier layer, it is possible to obtain an effect of improving moldability.
[0040] The polyethylene terephthalate film may have a thickness of 5 μm to 20 μm, preferably 5 μm to 15 μm, and more preferably 7 μm to 15 μm, and the nylon film may have a thickness of 10 μm to 40 μm, preferably 15 μm to 35 μm, and more preferably 15 μm to 25 μm. When the thicknesses of the polyethylene terephthalate film and the nylon film satisfy the above ranges, the formability, flexibility, and durability are improved, and the loop stiffness value required in the present invention can be easily achieved.
[0041] Gas Barrier Layer The gas barrier layer 20 is intended to ensure the mechanical strength of the battery case, to block the entry and exit of gas or moisture from the outside of the secondary battery, and to prevent electrolyte leakage.
[0042] The thickness of the gas barrier layer can be 50 μm to 100 μm, preferably 55 μm to 90 μm, and more preferably 55 μm to 80 μm. When the thickness of the gas barrier layer satisfies the above range, it is easy to realize a desired loop stiffness value, and the moldability is increased, so that the cup part can be formed deep and sharp. Conventionally, it has been common to form a gas barrier layer using an aluminum alloy thin film having a thickness of 40 μm. However, when the thickness of the gas barrier layer is at the level of 40 μm, the flexibility of the pouch film laminate is reduced, making it difficult to realize a desired loop stiffness value, and the moldability is reduced, limiting the increase in the molding depth, and it is also difficult to form a sharp corner of the cup part.
[0043] On the other hand, the gas barrier layer may be made of a metal material, specifically, an aluminum alloy thin film.
[0044] The aluminum alloy thin film may contain aluminum and one or more metal elements other than aluminum, such as iron (Fe), copper (Cu), chromium (Cr), manganese (Mn), nickel (Ni), magnesium (Mg), silicon (Si), and zinc (Zn).
[0045] Preferably, the aluminum alloy thin film has an iron (Fe) content of 1.2wt% to 1.7wt%, preferably 1.3wt% to 1.7wt%, more preferably 1.3wt% to 1.45wt%. If the iron (Fe) content in the aluminum alloy thin film is less than 1.2wt%, the strength of the aluminum alloy thin film is reduced, and cracks and pinholes may occur during forming, and if it exceeds 1.7wt%, the flexibility of the aluminum alloy thin film is reduced, and there is a limit to the improvement of formability and bendability.
[0046] The aluminum alloy thin film includes an aluminum alloy thin film having a crystal grain size of 10 μm to 13 μm, preferably 10.5 μm to 12.5 μm, and more preferably 11 μm to 12 μm. When the crystal grain size of the aluminum alloy thin film satisfies the above range, the forming depth can be increased without the occurrence of pinholes or cracks during cup forming. When the crystal grain size of the aluminum alloy thin film exceeds 13 μm, the strength of the aluminum alloy thin film decreases and the occurrence of cracks and pinholes increases due to the difficulty in dispersing internal stress during stretching, while when the crystal grain size is less than 10 μm, the flexibility of the aluminum alloy thin film decreases, limiting the improvement of formability and bendability.
[0047] The grain size varies depending on the composition of the aluminum alloy thin film and the processing method of the aluminum alloy thin film, and can be measured by observing a cross section of the aluminum alloy thin film in the thickness direction with a scanning electron microscope (SEM). Specifically, in the present invention, a cross section SEM image of the aluminum alloy thin film in the thickness direction is obtained using a scanning electron microscope, and the maximum diameters of any 30 crystal grains among the crystal grains observed in the SEM image are measured, and the average value of these is evaluated as the grain size.
[0048] Specifically, the aluminum alloy thin film may be an aluminum alloy having alloy number AA8021, but is not limited thereto.
[0049] Sealant Layer The sealant layer 30 is bonded by thermocompression to seal the battery case, and is located as the innermost layer of the pouch film laminate 1.
[0050] The sealant layer 30 is the surface that comes into contact with the electrolyte and the electrode assembly after being molded into a battery case, and therefore must have insulating properties and corrosion resistance. It must also have high sealing properties since it must completely seal the inside and prevent material transfer between the inside and the outside.
[0051] The sealant layer 30 may be made of a polymer material, for example, one or more selected from the group consisting of polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymers, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, polyparaphenylene benzobisoxazole, polyarylate, and Teflon (registered trademark), and among them, it is particularly preferable to include polypropylene (PP), which has excellent mechanical properties such as tensile strength, rigidity, surface hardness, abrasion resistance, and heat resistance, and chemical properties such as corrosion resistance.
[0052] More specifically, the sealant layer 30 may include polypropylene, cast polypropylene (CPP), acid modified polypropylene, polypropylene-butylene-ethylene copolymer, or a combination thereof.
[0053] The sealant layer 30 may be a single layer structure or a multi-layer structure including two or more layers of different polymeric materials.
[0054] The sealant layer may have a total thickness of 60 μm to 100 μm, preferably 60 μm to 90 μm, and more preferably 70 μm to 90 μm. If the thickness of the sealant layer is too thin, the seal durability and insulation properties may decrease, and if the thickness is too thick, the flexibility may decrease, the total thickness of the pouch film laminate may increase, and the energy density relative to the volume may decrease.
[0055] The pouch film laminate of the present invention as described above may be manufactured by a method for manufacturing a pouch film laminate well known in the art. For example, the pouch film laminate of the present invention may be manufactured by a method in which a base layer 10 is attached to an upper surface of a gas barrier layer 20 by an adhesive, and a sealant layer 30 is formed on a lower surface of the gas barrier layer 20 by coextrusion or an adhesive layer, but is not limited thereto.
[0056] The pouch film laminate according to the present invention may have a total thickness of 160 μm to 200 μm, preferably 180 μm to 200 μm. When the thickness of the pouch film laminate satisfies the above range, it is possible to minimize the reduction in battery accommodating space and the deterioration of sealing durability due to the increase in the thickness of the pouch laminate, and to increase the molding depth.
[0057] <Battery case> An embodiment of a battery case according to the present invention is shown in Figures 3 and 4. Hereinafter, the battery case according to the present invention will be described with reference to Figures 3 and 4.
[0058] As shown in Figs. 3 and 4, the battery case 100 according to the present invention is manufactured by drawing and forming the above-mentioned pouch film laminate 1 according to the present invention, and includes at least one cup portion 110a, 110b.
[0059] The pouch film laminate 1 is as described above, and therefore a detailed description thereof will be omitted.
[0060] The cup parts 110a and 110b are spaces 112 for accommodating an electrode assembly (not shown) and an electrolyte (not shown), and are manufactured by drawing the pouch film laminate 1 using a punch or the like. Here, the drawing can be performed by applying pressure to the sealant layer side of the pouch film laminate 1 with a punch.
[0061] Meanwhile, the battery case 100 according to the present invention may include one cup portion 110a as shown in FIG. 3, or may include two cup portions 110a and 110b as shown in FIG.
[0062] Meanwhile, the battery case 100 according to the present invention includes a lower case 110 and an upper case 120, and the cup parts 110a and 110b may be formed in only one or both of the lower case 110 and the upper case 120. When the pouch film laminate 1 is molded using a one-cup molding device, a battery case having one cup part can be manufactured as shown in Fig. 3, and when the pouch film laminate 1 is molded using a two-cup molding device, a battery case having cup parts formed in both the lower case 110 and the upper case 120 can be manufactured as shown in Fig. 4.
[0063] After the electrode assembly is accommodated in the cup parts 110a and 110b and an electrolyte is injected, the upper case 120 is folded to contact the upper end of the lower case 110, thereby isolating the electrode assembly and the electrolyte from the outside.
[0064] Thereafter, the corners of the upper case 120 and the lower case 110 are heat-pressurized to perform a sealing process.
[0065] As described above, the battery case according to the present invention is manufactured using a pouch film laminate 1 having a high loop rigidity in the MD direction of 750 mN to 1,300 mN. This gives the battery case excellent flexibility, a large limit forming depth when forming the cup portion, and allows the corners of the cup portion to have a large gradient, minimizing the occurrence of curling after the cup is formed.
[0066] Therefore, the battery case of the present invention can increase the storage volume within the cup portion compared to conventional battery cases, and as a result, the volume of the electrode assembly that can be stored is increased, thereby achieving a high energy density and minimizing defects due to curling after molding.
[0067] Specifically, the battery case according to the present invention has a cup depth of 10 mm or more, preferably 10 to 30 mm, and a curl height of 25 mm or less, preferably 20 mm or less, more preferably 15 mm or less.
[0068] Meanwhile, when the battery case has two cup parts, the depth of the cup parts refers to the total depth of the cup parts of the upper case and the lower case.
[0069] The curl height of the battery case was evaluated by measuring the height to which each corner of the battery case curled up with a steel ruler when the cup portion of the battery case was fixed to the bottom with double-sided tape, and the maximum value among these was taken as the curl height.
[0070] The present invention will now be described in more detail with reference to specific examples.
[0071] Example 1 A 25 μm-thick nylon film (product name: Nylon 6, manufacturer: HYOSUNG) and a 12 μm-thick polyethylene terephthalate (PET) film (manufacturer: HYOSUNG) were laminated on one side of a 60 μm-thick AA8021 aluminum (Al) alloy thin film (manufacturer: SAMA Aluminum) by dry lamination using a urethane adhesive to form a base layer. Here, the urethane adhesive was applied so that the adhesive layer was 3 μm thick. Next, molten non-oriented polypropylene (CPP) was co-extruded on the other side of the aluminum alloy thin film to form an 80 μm-thick sealant layer, thereby producing a pouch film laminate.
[0072] Example 2 A pouch film laminate was produced in the same manner as in Example 1, except that an AA8021 aluminum (Al) alloy thin film having a thickness of 80 μm was used.
[0073] Example 3 A pouch film laminate was manufactured in the same manner as in Example 1, except that a 15 μm-thick nylon film (product name: Nylon 6, manufacturer: HYOSUNG) and a 12 μm-thick polyethylene terephthalate (PET) film (manufacturer: HYOSUNG) were laminated by dry lamination using a urethane adhesive to form a base layer.
[0074] Comparative Example 1 A pouch film laminate was produced in the same manner as in Example 3, except that a 40 μm-thick AA8021 aluminum (Al) alloy thin film (manufacturer: SAMA Aluminum) was used.
[0075] Comparative Example 2 A pouch film laminate was produced in the same manner as in Example 1, except that when the base layer was formed, a urethane adhesive was applied so that the adhesive layer had a thickness of 5 μm.
[0076] Experimental example 1: Loop stiffness measurement Each of the pouch film laminates produced in Examples 1 to 3 and Comparative Examples 1 and 2 was cut into a first sample having a length of 15 mm in the MD direction and a length of 150 mm in the TD direction.
[0077] Further, each of the pouch film laminates produced in Examples 1 to 3 and Comparative Examples 1 and 2 was cut to a length of 15 mm in the TD direction and 150 mm in the MD direction to produce a second sample.
[0078] The first and second samples were each deformed into a loop with a radius of 16 mm and a circumference of 100 mm, and then a force was applied at a rate of 5 mm / min to measure the maximum strength required to deform the loop, which was evaluated as the loop rigidity. The measurement results are shown in Table 1 below.
[0079] Experimental Example 2: Measurement of the breaking strength of the base layer film in the MD direction The base layer film (nylon film / adhesive layer / polyethylene terephthalate film laminate) used in Examples 1 to 3 and Comparative Examples 1 and 2 was cut to a width x length of 15 mm x 80 mm to prepare a sample. Here, the sample was cut so that the longitudinal direction of the sample coincided with the MD direction of the pouch film laminate. The sample was fixed to a UTM device with a grip gap of 30 mm, and then pulled at a pulling speed of 50 mm / min to measure the strength at which the sample broke. The measurement results are shown in Table 1 below.
[0080] Experimental example 3: Measurement of limit forming depth Each of the pouch film laminates manufactured in Examples 1 to 3 and Comparative Examples 1 to 2 was cut to a size of 240 mm x 200 mm, and then molded in a battery case molding device having one cup molding part with a size of 160 mm wide x 90 mm long and a battery case molding device having two cup molding parts with a size of 160 mm wide x 61 mm long, while changing the molding depth, and the maximum molding depth (limit molding depth) just before cracks were generated was measured. Here, the punch and molding part of the battery case molding device were filleted (filleted, chamfered) at the corners and edges, the corners of the punch had a curvature of 2 mm and the corners had a curvature of 0.5 mm, and the corners of the molding part had a curvature of 2.5 mm and the corners had a curvature of 0.5 mm. In addition, the clearance between the punch and the molding part was 0.5 mm. In the battery case molding device having two cup molding parts, the distance between the two molding parts was 1 mm. The measurement results are shown in [Table 1] below.
[0081] Experimental Example 4: Measurement of curl characteristics In the third experimental example, the cup of the battery case molded to the maximum molding depth was fixed to the bottom with double-sided tape, and the height at which each corner of the battery case curled up was measured with a steel ruler, and the maximum value among these values was evaluated as the curl height. The measurement results are shown in Table 1 below.
[0082] [Table 1]
[0083] As shown in Table 1, when a battery case was manufactured using a pouch film laminate whose MD loop rigidity fell within the range of the present invention, a battery case with a deep limit forming depth and little curling could be manufactured. In contrast, when the pouch film laminate of Comparative Example 1, whose MD loop rigidity was less than 730 mN, was used, the limit forming depth was small, and when the pouch film laminate of Comparative Example 2, whose loop rigidity was 1300 mN or more, was used, it was confirmed that although the moldability was excellent, severe curling occurred after cup molding. [Explanation of symbols]
[0084] 1 Pouch film laminate 10 Base material layer 20 Gas barrier layer 30 Sealant Layer 16a, 16b adhesive layer 100 Battery case 110 Lower case 120 Upper Case 110a, 110b Cup part 130 Bridge
Claims
1. A gas barrier layer; a base layer disposed on one surface of the gas barrier layer; A pouch film laminate comprising: The pouch film laminate has a loop stiffness in the MD direction of 750 mN to 1300 mN.
2. The pouch film laminate according to claim 1, wherein the pouch film laminate has a loop stiffness in the TD direction of 750 mN to 1300 mN.
3. 2. The pouch film laminate according to claim 1, wherein the ratio of loop stiffness in the TD direction to loop stiffness in the MD direction of the pouch film laminate is 0.8 to 1.
2.
4. The pouch film laminate according to claim 1, wherein the base layer has a breaking strength in the MD direction of 10 N / 15 mm to 18 N / 15 mm.
5. The pouch film laminate according to claim 1 , wherein the base layer has a laminated structure of a polyethylene terephthalate film and a nylon film.
6. The thickness of the polyethylene terephthalate film is 5 μm to 20 μm, The pouch film laminate according to claim 5, wherein the nylon film has a thickness of 10 μm to 30 μm.
7. 2. The pouch film laminate according to claim 1, wherein the gas barrier layer has a thickness of 50 μm to 100 μm.
8. The pouch film laminate of claim 1 , wherein the gas barrier layer comprises an aluminum alloy thin film.
9. The pouch film laminate according to claim 8, wherein the aluminum alloy thin film contains 1.2 wt % to 1.7 wt % iron.
10. The pouch film laminate according to claim 8, wherein the aluminum alloy thin film has a grain size of 10 μm to 13 μm.
11. 2. The pouch film laminate according to claim 1, wherein the sealant layer has a thickness of 60 μm to 100 μm.
12. 10. The pouch film laminate of claim 1, wherein the sealant layer comprises unoriented polypropylene, acid modified polypropylene, polypropylene-butylene-ethylene copolymer, or a combination thereof.
13. A battery case manufactured by drawing the pouch film laminate according to claim 1, The battery case includes at least one cup portion, The battery case has a cup portion having a depth of 10 mm or more and a curl height of 25 mm or less.
Citation Information
Patent Citations
Packaging material
JP2000340186A
Packing material for battery
JP2008053133A
Lithium ion battery and battery pack having the same
JP2008251342A
plastic laminate film
JP2009544492A
Laminated material for secondary battery container and secondary battery container
JP2012014998A