Resin composition and printed circuit board containing same

A resin composition with a specific cyanate ester resin and phenolic resin ratio, combined with an imidazole and metal compound accelerator, addresses the issue of surface roughness and adhesion in multilayer printed circuit boards, enhancing their performance.

JP2024544322AActive Publication Date: 2024-11-28LG CHEM LTD
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2024536501
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-07
Filing Date
2023-10-19
Publication Date
2024-11-28
Estimated Expiration
2043-10-19

AI Technical Summary

Technical Problem

Existing resin compositions for multilayer printed circuit boards fail to achieve desired surface roughness during desmear processing, leading to poor adhesion and chemical resistance, particularly when using cyanate ester resins alone.

Method used

A resin composition comprising a specific weight ratio of cyanate ester resin and phenolic resin, along with a curing accelerator containing both imidazole and metal compounds, is used to enhance adhesion and surface roughness.

Benefits of technology

The composition achieves excellent cured physical properties, including appropriate surface roughness and copper foil adhesion, resulting in improved multilayer printed circuit boards with enhanced wiring adhesion and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544322000001
    Figure 2024544322000001
  • Figure 2024544322000002
    Figure 2024544322000002
  • Figure 2024544322000003
    Figure 2024544322000003
Patent Text Reader

Abstract

A resin composition according to one embodiment of the present application comprises an epoxy resin; a curing agent including a cyanate ester resin and a phenolic resin; inorganic particles including silica particles; and a curing accelerator, the weight ratio of the cyanate ester resin to the phenolic resin being 95:5 to 40:60, and the curing accelerator simultaneously including an imidazole compound and a metal compound.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0147208, filed with the Korean Intellectual Property Office on November 7, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a resin composition and a printed circuit board containing the same. [Background technology]

[0003] Generally, double-sided printed circuit boards are based on CCL (Copper Clad Laminate), which is made by laminating copper foil on both sides of an insulating material. To connect electrical signals, holes are drilled in the copper foil on both sides, and the copper foil on both sides is connected with a plating layer using electrolytic copper plating. After that, a UV photosensitive dry film is applied to form a circuit, and a pattern is selectively formed by irradiating UV light. After that, the circuit pattern is formed on the copper foil on both sides by etching, and then a PSR (Photoimagable Solder Resist) is applied for insulation, and the surface on which the final components are mounted is subjected to surface treatment such as gold plating, through which the double-sided printed circuit board can be manufactured.

[0004] Also, the multi-layer printed circuit board is the same up to the circuit formation stage of the double-sided board, but after forming the circuit pattern, instead of applying PSR on it, it can be manufactured by stacking one prepreg and one copper foil on top of the other, and then heating and pressing them. Therefore, the multi-layer printed circuit board means a build-up board in which PCB is formed in multiple layers.

[0005] In this case, the multilayer printed circuit board can be manufactured by forming via holes that electrically connect the inner layer circuit pattern and the outer layer circuit pattern through laser processing, and forming a plating layer on the inner surface of the via hole. Thereafter, if necessary, a solder resist layer can be further formed as a protective layer on the plating layer, or a larger number of outer layers can be further formed.

[0006] In this technical field, in order to improve the quality of multilayer printed circuit boards, there is a demand for insulating layers that not only have excellent adhesion to the conductor wiring that constitutes the conductive layer, but also have excellent chemical resistance and the like. Summary of the Invention [Problem to be solved by the invention]

[0007] The present application seeks to provide a resin composition and a printed circuit board comprising the same. [Means for solving the problem]

[0008] One embodiment of the present application comprises: Epoxy resins; A hardener comprising a cyanate ester resin and a phenolic resin; Inorganic particles, including silica particles; and Contains a curing accelerator, the weight ratio of the cyanate ester resin to the phenolic resin is 95:5 to 40:60; The curing accelerator simultaneously contains an imidazole compound and a metal compound, and the resin composition is provided.

[0009] Further, another embodiment of the present application provides a printed circuit board comprising the above-mentioned resin composition or a cured product thereof. Effect of the Invention

[0010] The resin composition according to one embodiment of the present application can have excellent cured properties by applying a cyanate ester resin and a phenolic resin having a specific weight ratio as a curing agent and applying a curing accelerator containing an imidazole compound and a metal compound at the same time. In addition, an insulating film manufactured using the resin composition according to one embodiment of the present application can have an appropriate surface roughness by desmearing, and is therefore characterized by excellent copper foil adhesion.

[0011] Therefore, by using the resin composition according to one embodiment of the present application, a multi-layer printed circuit board having excellent wiring adhesion, chemical resistance, and the like can be manufactured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present application will now be described in more detail.

[0013] In this application, when a member is said to be located "on" another member, this includes not only the case where the member is in contact with the other member, but also the case where there is another member between the two members.

[0014] In this application, when a part is said to "comprise" a certain component, this means that it can further include other components, but not excluding other components, unless specifically stated to the contrary.

[0015] A method of laminating conductor layers and insulating films alternately has been developed as a method for manufacturing multilayer printed circuit boards, and is currently used for semiconductor packaging. The manufacturing process of the multilayer printed circuit board is as follows: first, a build-up insulating film is vacuum-laminated on an inner layer circuit, and then the process of precure → drilling → desmear → electroless plating → electrolytic plating → postcure → outer layer circuit formation is performed. Here, the desmear process removes smears with an acidic solution and also erodes the surface of the insulating film to a certain extent to form surface roughness, which serves to increase adhesion with the copper foil layer formed in the subsequent process.

[0016] As the resin composition for the build-up insulating film, a composition in which an epoxy resin and a phenol-based hardener were filled with silica particles as an inorganic filler was used in the initial products, but in response to the increasing demand for low dielectric properties and low CTE, products using a cyanate ester-based hardener in an epoxy resin were developed.

[0017] Although the cured products of the epoxy resin and the cyanate ester resin have advantages such as low CTE and high heat resistance, when used alone, there is a problem that desired surface roughness cannot be formed through a desmear process.

[0018] Therefore, the present application aims to provide a resin composition which not only has excellent curing properties but also can form a desired surface roughness even after a desmear process, and a printed circuit board including the same.

[0019] A resin composition according to one embodiment of the present application comprises an epoxy resin; a curing agent including a cyanate ester resin and a phenolic resin; inorganic particles including silica particles; and a curing accelerator, the weight ratio of the cyanate ester resin to the phenolic resin being 95:5 to 40:60, and the curing accelerator simultaneously including an imidazole compound and a metal compound.

[0020] In one embodiment of the present application, the epoxy resin preferably has two or more epoxy groups in one molecule. More specifically, the epoxy resin may include one or more of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, biphenyl type epoxy resin, tetramethylbiphenyl type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol S novolac type epoxy resin, biphenyl novolac type epoxy resin, naphthol novolac type epoxy resin, naphthol phenol co-condensed novolac type epoxy resin, naphthol cresol co-condensed novolac type epoxy resin, aromatic hydrocarbon formaldehyde resin, modified phenol resin type epoxy resin, triphenylmethane type epoxy resin, tetraphenylethane type epoxy resin, dicyclopentadiene phenol addition reaction type epoxy resin, phenol aralkyl type epoxy resin, naphthol aralkyl type epoxy resin, etc.

[0021] Among these, from the viewpoints of heat resistance, insulation reliability, and adhesion, it is more preferable that the epoxy resin contains one or more of bisphenol A type epoxy resin, naphthol type epoxy resin, naphthalene type epoxy resin, biphenyl type epoxy resin, epoxy resin having a butadiene structure, and the like.

[0022] In one embodiment of the present application, the curing agent includes a cyanate ester-based resin and a phenolic-based resin.

[0023] The cyanate ester resin may include at least one selected from novolac type (phenol novolac type, alkylphenol novolac type, etc.) cyanate ester resins, dicyclopentadiene type cyanate ester resins, bisphenol type (bisphenol A type, bisphenol F type, bisphenol S type, bisphenol M type, etc.) cyanate ester resins, and prepolymers of these partially converted to triazine.

[0024] More specifically, the cyanate ester resin is bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethyl and polyfunctional cyanate resins derived from phenol novolac, cresol novolac, dicyclopentadiene structure-containing phenolic resins, and the like; and prepolymers in which these cyanate resins are partially triazine-converted.

[0025] The weight average molecular weight of the cyanate ester resin may be, but is not limited to, 500 g / mol to 4,500 g / mol, or 600 g / mol to 3,000 g / mol.

[0026] In the present application, the weight average molecular weight can be measured by gel permeation chromatography (GPC) method (polystyrene equivalent).

[0027] The phenolic resin may include a novolac type phenolic resin, which is a compound containing a phenol skeleton or a naphthol skeleton and has excellent heat resistance, water resistance, etc. More specifically, the phenolic resin may include novolac resins such as phenol novolac resin, bisphenol A novolac resin, cresol novolac resin, phenol-modified xylene resin, alkylphenol resin, and phenol-modified melamine resin.

[0028] In one embodiment of the present application, the weight ratio of the cyanate ester resin to the phenol resin may be 95:5 to 40:60, 90:10 to 40:60, or 88:12 to 45:55. If the content of the cyanate ester resin is less than 40 wt% based on the total weight of the cyanate ester resin and the phenol resin, it is not preferable because the cyanate ester resin cannot provide the advantages of cured physical properties such as low dielectric tangent (low Df), low CTE, and high heat resistance. In addition, if the content of the phenol resin is less than 5 wt%, it is not preferable because it may be difficult to realize a desired surface shape through a desmear process.

[0029] In one embodiment of the present application, the weight ratio of the epoxy resin to the curing agent may be 60:40 to 20:80, 60:40 to 30:70, or 55:45 to 35:65. When the weight ratio of the epoxy resin to the curing agent is satisfied, excellent heat resistance and mechanical properties can be obtained while having low dielectric tangent and low CTE characteristics. When the content of the epoxy resin exceeds 60 wt% based on the total weight of the epoxy resin and the curing agent, it is not preferable because a high degree of curing cannot be obtained through heat treatment, and excellent dielectric properties and desired curing properties cannot be obtained. In addition, when the content of the curing agent exceeds 80 wt%, it is not preferable because self-crosslinking in which the cyanate ester resin is linked to each other through a triazine structure may occur excessively, which may cause brittle fracture, making the film more likely to crack after curing.

[0030] In one embodiment of the present application, the inorganic particles include silica particles.

[0031] In one embodiment of the present application, the inorganic particles include only silica particles, and do not include any other inorganic particles other than the silica particles.

[0032] The average particle size of the silica particles may be 0.3 μm or less, 0.2 μm or less, or 0.05 μm or more.

[0033] When silica having an average particle size of 0.3 μm or less or 0.2 μm or less is used as the inorganic particles, it has been difficult to obtain a desired surface roughness by desmearing in the past. However, according to one embodiment of the present application, by satisfying the specific weight ratio of the cyanate ester resin:phenol resin described above, it is possible to form a desired surface roughness by desmearing.

[0034] Conventionally, the resin composition of the surface layer is etched to a certain thickness by wet desmearing, and the shape of the inorganic particle part protruding or the shape of the dent caused by the inorganic particle falling off is formed. At this time, the degree of hardening of the resin composition and the size of the inorganic particle are important factors that determine the surface roughness. In general, when a product having an average particle size of more than 0.3 μm is used as the inorganic particle, the degree of hardening of the resin composition can be appropriately adjusted so that the surface layer is well etched by the desmearing, and thus a surface roughness of Ra 200 nm or more can be easily obtained. However, when silica having an average particle size of 0.3 μm or less or 0.2 μm or less is used, even if the resin composition is well etched, the size of the inorganic particle is small, and it is difficult to obtain a surface roughness of Ra 200 nm or more.

[0035] Meanwhile, when a cyanate ester-based resin and a phenol-based resin are mixed and used in a specific weight ratio as in one embodiment of the present application, the etching rates of the two resins with respect to the desmear solution are different due to differences in curing speed and chemical resistance of the two resins with respect to the epoxy. As a result, non-uniform etching of the surface layer is induced during the desmear process, and a surface roughness of 200 nm or more can be formed regardless of the size of the inorganic particles.

[0036] In one embodiment of the present application, the resin composition may further contain a thermoplastic resin in order to improve the mechanical strength, film formability, etc. of the cured product. The thermoplastic resin may contain one or more selected from a phenoxy resin, a polyimide resin, a polyamideimide resin, a polyetherimide resin, a polysulfone resin, a polyethersulfone resin, a polyphenylene ether resin, a polycarbonate resin, a polyvinyl acetal resin, a polyvinyl butyral resin, a polyether ether ketone resin, and a polyester resin. It is more preferable that the thermoplastic resin contains a phenoxy resin.

[0037] The weight average molecular weight of the thermoplastic resin may be, but is not limited to, 5,000 g / mol to 200,000 g / mol.

[0038] In one embodiment of the present application, the resin composition includes a curing accelerator for efficiently curing an epoxy resin, a curing agent, etc., and the curing accelerator includes an imidazole compound and a metal compound at the same time. In addition, the curing accelerator may further include one or more selected from an amine compound and an organic phosphine compound in addition to the imidazole compound and the metal compound.

[0039] The imidazole-based compound can promote the curing reaction of the phenol-based resin in the curing agent, and the metal-based compound can promote the curing reaction of the cyanate ester-based resin in the curing agent. That is, since the resin composition according to one embodiment of the present application contains a cyanate ester-based resin and a phenol-based resin as a curing agent, if the resin composition does not contain any one of the imidazole-based compound and the metal-based compound as the curing accelerator, the desired surface roughness effect cannot be obtained.

[0040] When the curing accelerator contains both an imidazole-based compound and a metal-based compound, the etching rates of the imidazole-based compound and the metal-based compound with respect to the epoxy resin are different from each other due to differences in curing speed, chemical resistance, etc. As a result, non-uniform etching of the surface layer is induced during the desmear process, and a surface roughness of 200 nm or more can be formed regardless of the size of the inorganic particles.

[0041] However, when the curing accelerator contains only one of the imidazole-based compound and the metal-based compound, the film may be easily cracked after curing, and the surface may be over-etched during desmear treatment, causing whitening, which is not preferable.

[0042] The imidazole compounds include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2' -Methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2- These may include one or more of phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and the like.

[0043] The metal compounds include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. The organometallic complexes may include one or more of cobalt(II) acetylacetonate, cobalt(III) acetylacetonate, copper(II) acetylacetonate, zinc(II) acetylacetonate, iron(III) acetylacetonate, nickel(II) acetylacetonate, and manganese(II) acetylacetonate. The organometallic salts may include one or more of zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0044] Examples of the amine compounds include triethylamine, tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylamino-methyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.

[0045] The content of the curing accelerator may be 0.01% by weight to 5% by weight based on the total weight of the nonvolatile content of the resin composition.

[0046] In one embodiment of the present application, the resin composition may further include additives known in the art, which may include, but are not limited to, one or more additives selected from a leveling agent, a wetting agent, and an antistatic agent.

[0047] In one embodiment of the present application, the resin composition can be applied to a printed circuit board. More specifically, the resin composition can be applied to an insulating film of a printed circuit board. The insulating film can be used as an interlayer insulating material of a multi-layer printed circuit board.

[0048] Another embodiment of the present application provides a printed circuit board comprising the above-mentioned resin composition or a cured product thereof.

[0049] The printed circuit board may be a multi-layer printed circuit board, and the number of layers included in the multi-layer printed circuit board is not limited. For example, the multi-layer printed circuit board may include a structure of 2 to 20 layers depending on the purpose and application of the multi-layer printed circuit board. EXAMPLES

[0050] In the following, the present application will be described in detail with reference to examples in order to specifically explain the present application. However, the examples of the present application may be modified in various different forms, and the scope of the present application is not to be construed as being limited to the examples described below. The examples of the present application are provided to more completely explain the present application to those having average knowledge in the art.

[0051] <Example>

[0052] <Example 1> 70 parts by weight of bisphenol epoxy resin (YD-128, KUKDO Chemical), 30 parts by weight of phenol novolac epoxy resin (YDPN-639, KUKDO Chemical), 84 parts by weight of dicyclopentadiene bisphenol cyanate ester resin (75% non-volatile MEK solution, C03CS, TECHIA), 24 parts by weight of biphenyl phenol resin (GPH-65, Nippon Kayaku), 360 parts by weight of silica slurry (60% non-volatile MEK solution, K180SX-CM3, ADMATECHS) having an average particle size of 0.18 μm, 20 parts by weight of phenoxy resin (YP-50, KUKDO Chemical), and 110 parts by weight of MEK (methyl ethyl ketone) were mixed and stirred at 250 rpm for 3 hours using a mechanical stirrer.

[0053] Then, 1.0 part by weight of an imidazole-based hardening accelerator (2PHZ-PW, Shikoku Chemical Industry Co., Ltd.) and 0.05 part by weight of a metal-based hardening accelerator, cobalt (II) acetylacetonate (TCI), were diluted to a concentration of 10% in MEK and added, and the mixture was uniformly dispersed in a high-speed rotating mixer to prepare a coating liquid.

[0054] The prepared coating solution was coated on a PET film having a thickness of 38 μm using an applicator, and then dried at 100° C. for 8 minutes to prepare an insulating film having a thickness of 25 μm.

[0055] <Example 2> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that 98 parts by weight of a novolac-type cyanate ester resin (MEK solution with 75% non-volatile components, C05CS, TECHIA) and 12 parts by weight of a biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) were added as the cyanate ester resin in Example 1.

[0056] <Example 3> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that 56 parts by weight of dicyclopentadiene bisphenol-based cyanate ester resin (MEK solution with 75% non-volatile components, C03CS, TECHIA) and 48 parts by weight of biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) were added.

[0057] <Example 4> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that 153 parts by weight of dicyclopentadiene bisphenol-based cyanate ester resin (MEK solution with 75% non-volatile components, C03CS, TECHIA) and 24 parts by weight of biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) were added.

[0058] <Comparative Example 1> In the above Example 1, 112 parts by weight of a novolac-type cyanate ester resin (MEK solution with 75% non-volatile components, C05CS, TECHIA) was added as the cyanate ester resin, and no biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) was added. An insulating film was produced using the same content ratio and manufacturing method as in Example 1, except that the cyanate ester resin was not added.

[0059] <Comparative Example 2> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that 28 parts by weight of dicyclopentadiene bisphenol-based cyanate ester resin (MEK solution with 75% non-volatile components, C03CS, TECHIA) and 72 parts by weight of biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) were added.

[0060] <Comparative Example 3> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that the dicyclopentadiene bisphenol-based cyanate ester resin was not added and 97 parts by weight of a biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) was added.

[0061] <Comparative Example 4> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that 94 parts by weight of dicyclopentadiene bisphenol-based cyanate ester resin (MEK solution with 75% non-volatile components, C03CS, TECHIA) and 4 parts by weight of biphenyl-based phenolic resin (GPH-65, Nippon Kayaku) were added.

[0062] <Comparative Example 5> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that the imidazole-based hardening accelerator was not added and only a metal-based hardening accelerator was added as the hardening accelerator.

[0063] <Comparative Example 6> An insulating film was manufactured using the same content ratio and manufacturing method as in Example 1, except that no metal-based hardening accelerator was added as the hardening accelerator, and only an imidazole-based hardening accelerator was added.

[0064] <Experimental Example 1> The properties of the insulating films produced in the above Examples and Comparative Examples were evaluated and are shown in the following Table 1. The evaluation methods for the properties shown in the following Table 1 are as follows.

[0065] <Coefficient of thermal expansion (CTE)> The insulating film was thermally cured at 190°C for 90 minutes, and then the thermal expansion coefficient was measured in the range of 25°C to 120°C using a TMA (thermos mechanical analyzer).

[0066] <Surface roughness (Ra, nm)> 1) Desmearing The insulating film was laminated on a CCL (copper clad laminate) substrate using a vacuum pressure laminator at a temperature of 100°C and a pressure of 0.7Mpa for 30 seconds, and then pre-cured in a hot air oven at 100°C for 30 minutes and then at 170°C for 30 minutes.

[0067] Next, the support film (PET film) of the insulator was peeled off to expose the insulating layer, and then the desmear treatment was carried out in three steps using Atotech's Securiganth MV series treatment solution: swelling solution treatment (60°C, 5 minutes), oxidation solution treatment (80°C, 20 minutes), and neutralization solution treatment (50°C, 4 minutes).

[0068] 2) Measurement of surface roughness (Ra, nm) The surface of the desmeared insulating layer was measured five times per sample using an optical profiler (Nanoview 3D surface profiler NV-2700, Nanosystem), and the arithmetic mean roughness (Ra) was calculated as the average value.

[0069] <Copper foil adhesion> 1) Copper plating Copper plating was carried out in two stages: electroless chemical copper plating and electrolytic copper plating. Electroless chemical copper plating was carried out using Atotech's Printoganth MV product, with the plating thickness being 0.5μm to 1.0μm, and the plate was then dried in a hot air oven at 150℃ for 30 minutes.

[0070] The copper electroplating was carried out using Atotech's Expt Inpro SAP6 chemicals so that the plating thickness was about 20 μm, and after the plating, the plate was heat-treated in a hot air oven at 190° C. for 1 hour.

[0071] 2) Evaluation of copper foil adhesion The 90 degree peel strength of the copper plating layer was measured using a Texture Analyzer (TA-XT Plus) manufactured by Stable Micro Systems, Inc. When the measured peel strength was 0.45 kgf / cm or more, the copper foil adhesion was judged to be good, and when it was less than 0.45 kgf / cm, the copper foil adhesion was judged to be poor.

[0072] [Table 1]

[0073] As shown in the above results, Examples 1 to 4 showed a low thermal expansion coefficient of 40 ppm / °C or less and good copper foil adhesion. However, Comparative Examples 1 and 4 showed a low thermal expansion coefficient of 33 to 34 ppm / °C, but the surface roughness (Ra) due to desmear treatment was 200 nm or less and the copper foil adhesion was poor. Moreover, Comparative Examples 2 and 3 showed a relatively high thermal expansion coefficient and poor copper foil adhesion.

[0074] In addition, when only a metal-based compound was included as a curing accelerator as in Comparative Example 5, the film was easily cracked after curing, making it impossible to prepare a sample, and the surface was over-etched during desmear treatment, resulting in whitening. In addition, when only an imidazole-based compound was included as a curing accelerator as in Comparative Example 6, the thermal expansion coefficient was relatively high, and the surface was over-etched during desmear treatment, resulting in whitening.

[0075] Therefore, the resin composition according to one embodiment of the present application can have excellent cured properties by applying a cyanate ester resin and a phenolic resin having a specific weight ratio as a curing agent and applying a curing accelerator containing an imidazole compound and a metal compound at the same time. In addition, the insulating film manufactured using the resin composition according to one embodiment of the present application can have an appropriate surface roughness by desmearing, and is therefore characterized by excellent copper foil adhesion.

[0076] Moreover, by using the resin composition according to one embodiment of the present application, a multi-layer printed circuit board having excellent wiring adhesion, chemical resistance, and the like can be produced.

Claims

1. Epoxy resin; a curing agent comprising a cyanate ester resin and a phenolic resin; Inorganic particles including silica particles; and Contains a curing accelerator, the weight ratio of the cyanate ester resin to the phenolic resin (cyanate ester resin:phenolic resin) is 95:5 to 40:60; The curing accelerator of the resin composition contains both an imidazole compound and a metal compound.

2. 2. The resin composition according to claim 1, wherein a weight ratio of the epoxy resin to the curing agent (epoxy resin:curing agent) is 60:40 to 20:

80.

3. 2. The resin composition according to claim 1, wherein the cyanate ester-based resin comprises at least one selected from the group consisting of novolac-type cyanate ester-based resins, dicyclopentadiene-type cyanate ester-based resins, bisphenol-type cyanate ester-based resins, and prepolymers of these resins partially converted to triazine.

4. The resin composition according to claim 1 , wherein the phenolic resin comprises a novolac phenolic resin.

5. The resin composition according to claim 1 , wherein the silica particles have an average particle size of 0.3 μm or less.

6. The resin composition according to claim 1, wherein the metal-based compound comprises one or more selected from the group consisting of cobalt (II) acetylacetonate, cobalt (III) acetylacetonate, copper (II) acetylacetonate, zinc (II) acetylacetonate, iron (III) acetylacetonate, nickel (II) acetylacetonate, manganese (II) acetylacetonate, zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

7. The resin composition according to claim 1, further comprising one or more thermoplastic resins selected from a phenoxy resin, a polyimide resin, a polyamideimide resin, a polyetherimide resin, a polysulfone resin, a polyethersulfone resin, a polyphenylene ether resin, a polycarbonate resin, a polyetheretherketone resin, a polyester resin, a polyvinyl acetal resin, and a polyvinyl butyral resin.

8. The resin composition according to claim 1 , further comprising at least one selected from the group consisting of a leveling agent, a wetting agent, and an antistatic agent.

9. The resin composition according to claim 1, which is for use in a printed circuit board.

10. A printed circuit board comprising the resin composition according to any one of claims 1 to 9 or a cured product thereof.

Citation Information

Patent Citations

  • Halogen-free thermosetting resin composition and prepreg and printed circuit laminate employing halogen-free thermosetting resin composition

    CN107177030A

  • Thermosetting resin composition and prepreg, laminate and high-frequency circuit substrate containing same

    CN109337289A

  • Thermosetting resin composition and copper-clad laminate

    JP1996034832A

  • Underfill material for liquid injection sealing

    JP1999106480A

  • Underfill material for liquid injection sealing

    JP1999106481A