Polyamide 56 resin and fiber, its preparation method and use
In-situ polymerization of titanium dioxide in polyamide 56 resin addresses compatibility issues, enhancing fiber strength and dyeability, and reducing breakages, thus improving the production efficiency and cost-effectiveness of polyamide 56 fibers.
Patent Information
- Application Number
- JP2024538129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current methods for producing polyamide 56 fibers face challenges such as monofilament breakage, filament breakage, strength loss, and poor dyeability due to the large difference in melting points between polyamide 6 and polyamide 56, and issues with uniform mixing of titanium dioxide, leading to phase separation and compatibility problems.
A method involving in-situ polymerization of titanium dioxide during the polymerization of polyamide 56 resin, ensuring uniform dispersion and avoiding the need for additional masterbatch addition equipment, with controlled particle size and distribution to enhance compatibility and dyeability.
The method reduces monofilament and filament breakages, improves fiber strength, and ensures good dyeability, while being simple to operate and lowering manufacturing costs, with reduced production investment.
Smart Images

Figure 2024544339000001 
Figure 2024544339000002 
Figure 2024544339000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to polyamides, specifically polyamide 56 resins, fibers, and methods for their preparation and uses. [Background technology]
[0002] Polyamide fiber is one of the world's earliest industrialized synthetic fibers and plays an important role in the field of synthetic fibers. There are many types of polyamide fiber. However, the most widely produced and industrially used at present are polyamide 6 and polyamide 66. The main applications are socks, lace underwear, corsets, athletic underwear, wedding dresses, casual jackets, sportswear, all-weather coats, outdoor jackets, quick-drying wear, padded jackets, outdoor tents, sleeping bags and mountaineering bags; industrial yarn is widely used in the fields of cord yarn, transmission belts, hoses, ropes, fishing nets, tires and parachutes.
[0003] Polyamide fibers are divided into two types, bright fiber and dull fiber, depending on whether they contain a matting agent or not. Bright fiber fabrics have a more pronounced gloss and waxy surface, making them difficult to use for casual clothing and high-end clothing with high demands. However, dull fiber fabrics have the advantages of a soft gloss close to natural, a soft touch, vivid colors, good drapeability and strong light blocking properties, and are increasingly in demand among consumers.
[0004] Titanium dioxide (TiO2) is widely used as a matte material in the field of artificial dull fiber. At present, the main production method of dull fiber is the online addition technology of dull masterbatch. In this method, firstly, the dull masterbatch is added during the spinning process, which requires the spinning factory to be equipped with masterbatch addition equipment, which increases the production investment; secondly, during the masterbatch addition process, the masterbatch addition ratio needs to be strictly controlled. If the mixing ratio is inappropriate or the mixing is uneven, it is easy to cause the deterioration of the compatibility between the dull masterbatch and the matrix resin, which is easy to cause problems such as monofilament breakage, filament breakage, strength reduction and poor dyeing during the spinning process.
[0005] A Chinese invention patent application (publication number: CN105986327A) discloses polyamide 56 fiber and its manufacturing method. The spinning process is carried out by melt-kneading a plurality of dull polyamide 6 resin particles and polyamide 56 resin particles that have been subjected to a viscosity adjustment process and a moisture adjustment process, and spinning the resulting kneaded material at a temperature in the range of 275°C to 285°C to obtain dull 56 fiber. In the above patent application, a polyamide 6 matrix material is used as a dull master batch. In this material, firstly, the melting point of polyamide 6 is about 220°C, while the melting point of polyamide 56 is about 256°C, and since the melting point difference between the two is large, it is difficult to appropriately control the spinning processing conditions. As a result, phase separation may occur, and the melt viscosity and fiber strength may decrease; secondly, in order to prepare polyamide 56 fiber with a high titanium dioxide content, it is necessary to add dull polyamide 6 resin particles with a content of more than 10% by weight to polyamide 56 resin particles. However, this leads to poor compatibility, which causes problems during the spinning process, such as increased filament breakage and end breakage, reduced fiber strength, uneven dyeing, and reduced M ratio.
[0006] China's invention patent application (publication number: CN110054891A) discloses a dull polyamide 56 masterbatch, dull fiber and its preparation method. It is necessary to first prepare a dull polyamide 56 masterbatch, and then mix and spin it with polyamide 56 to prepare dull fiber, which requires a relatively large production investment. This spinning method is carried out by adding the dull masterbatch by mixing, so it is necessary to add the masterbatch uniformly, otherwise it is easy to cause problems such as poor compatibility between the dull masterbatch and the matrix spinning raw material, monofilament breakage, poor dyeing and relative reduction of M rate. Summary of the Invention
[0007] One of the main objects of the present invention is to provide a polyamide 56 resin containing titanium dioxide in an amount of 0.2 to 5.0% by weight, in which 98% or more of the titanium dioxide has a dispersed particle size of 0.2 to 0.6 μm.
[0008] An embodiment of the present invention further provides a method for preparing a polyamide 56 resin, comprising the step of preparing a polyamide 56 resin from a monomer by a polymerization reaction, wherein the polyamide 56 resin comprises titanium dioxide, and the titanium dioxide is added during the polymerization reaction.
[0009] One embodiment of the present invention further provides polyamide 56 fibers prepared by melt spinning the aforementioned polyamide 56 resin or by directly spinning the melt produced during the preparation process of the polyamide 56 resin.
[0010] An embodiment of the present invention further provides a method for preparing the aforementioned polyamide 56 fibers, comprising the steps of: (a) heating a polyamide 56 resin to a molten state to obtain a polyamide 56 melt; (b) conveying the polyamide 56 melt to a spin box, injecting it into a spin pack, and extruding it through a spinneret to form as-spun fibers; (c) subjecting the as-spun fibers to a cooling, oiling, drawing, and winding process to obtain a pre-oriented yarn of polyamide 56; and (d) subjecting the pre-oriented yarn of polyamide 56 to a hot drawing process through a first roller, then cooling and setting, passing through a false twister, a second roller, an interlacer, and subjecting it to an oiling process and a winding process to obtain a polyamide 56 fiber.
[0011] An embodiment of the present invention further provides the use of the aforementioned polyamide 56 fibers in a knitted or woven fabric.
[0012] The method for preparing polyamide 56 resin according to one embodiment of the present invention can effectively avoid problems such as monofilament breakage and poor dyeability in the subsequent spinning process. In addition, the method is simple, easy to operate, and has low production costs.
[0013] Exemplary embodiments embodying the features and advantages of the present invention are described in detail in the following description. It should be understood that the present invention may have various modifications in different embodiments, all of which do not depart from the scope of the present invention, and the description therein is intended to be illustrative in nature, rather than limiting, the present invention.
[0014] One embodiment of the present invention provides a method for preparing a polyamide 56 resin, comprising the steps of preparing a polyamide 56 resin from monomers by a polymerization reaction, wherein the polyamide 56 resin comprises titanium dioxide, and the titanium dioxide is added during the polymerization reaction.
[0015] In the method of one embodiment of the present invention, titanium dioxide is added for in-situ polymerization during the polymerization reaction of polyamide 56. This allows the titanium dioxide to be uniformly dispersed in the polyamide 56 resin. This also effectively avoids problems such as monofilament breakage and poor dyeability in the subsequent spinning process. In addition, the preparation method is simple, easy to operate, and has low production costs.
[0016] In one embodiment of the present invention, TiO2 is added directly during polymerization for in-situ polymerization. The operation of this method is relatively simple, does not require additional masterbatch addition equipment, and is easy to control, so that production investment can be reduced. In addition, by adding TiO2 during polymerization, TiO2 and resin can be mixed for a longer time, and the dispersion of TiO2 in the matrix resin is more uniform, resulting in less monofilament breakage and filament breakage during the subsequent spinning process, higher fiber strength, and better dyeability.
[0017] In one embodiment, the titanium dioxide powder added during the polymerization of polyamide 56 may have a particle size of 0.15 to 0.5 μm, preferably 0.15 to 0.4 μm, more preferably 0.15 to 0.3 μm, for example 0.18 μm, 0.20 μm, 0.22 μm, 0.23 μm, 0.25 μm, 0.27 μm or 0.28 μm.
[0018] Here, the titanium dioxide can be added to the polyamide 56 polymerization system in the form of particles or in the form of a titanium dioxide slurry.
[0019] In one embodiment, titanium dioxide is added in an amount of 0.2 to 5.0% by weight, preferably 0.2 to 3.0% by weight, based on the total weight of the polyamide 56 resin.
[0020] In one embodiment, the raw materials for producing the polyamide 56 resin include at least 1,5-pentanediamine and adipic acid, or the polyamide 56 resin is obtained by polymerization of 1,5-pentanediamine and adipic acid as monomers.
[0021] In one embodiment, 1,5-pentanediamine is prepared from bio-based feedstocks by fermentation or enzymatic conversion.
[0022] In the method for preparing polyamide 56 resin according to one embodiment of the present invention, non-petroleum-origin materials, such as bio-based origin materials, are used as raw materials, which do not cause significant pollution and are beneficial to environmental protection.
[0023] In one embodiment, a method for preparing a polyamide 56 resin comprises the steps of: (1) preparing a polyamide 56 salt solution; (2) carrying out polymerization using a polyamide 56 salt solution as a raw material to obtain a polyamide 56 melt; and (3) A process of filtering the polyamide 56 melt through a melt filter, and finally pelletizing and drying the same to obtain a polyamide 56 resin.
[0024] In one embodiment, titanium dioxide may be added in any one or more of steps (1) and (2).
[0025] In one embodiment, step (1) comprises homogeneously mixing 1,5-pentanediamine, adipic acid and water under nitrogen conditions to obtain a polyamide 56 salt solution.
[0026] In one embodiment, the molar ratio of 1,5-pentanediamine to adipic acid may be (1-1.08):1, such as 1.02:1, 1.04:1, 1.05:1, or 1.06:1.
[0027] In one embodiment, step (2) includes heating a polyamide 56 salt solution to increase the pressure in the reaction system to 0.3 to 2.4 MPa (gauge pressure), maintaining the pressure for 0.2 to 2.5 hours by degassing, then reducing the pressure in the reaction system to 0 to 0.3 MPa (gauge pressure), and then evacuating the reaction system to a vacuum degree of -0.001 to -0.08 MPa (gauge pressure) to obtain a polyamide 56 melt.
[0028] In one embodiment, the reaction system has a temperature of 230 to 265°C, such as 235°C, 240°C, 245°C, 250°C, or 255°C, at the end of the pressure maintenance in step (2).
[0029] In one embodiment, in step (2), the pressure is maintained for 0.5 to 2 hours, preferably 0.5 to 1.5 hours, for example, 0.8 hours, 1 hour or 1.2 hours.
[0030] In one embodiment, the reaction system has a temperature of 240 to 275°C, for example, 245°C, 250°C, 255°C, 260°C, 265°C, or 270°C, at the end of the depressurization in step (2).
[0031] In one embodiment, the reaction system has a temperature of 250 to 285°C, such as 255°C, 260°C, 265°C, 270°C, 275°C, or 280°C, after the evacuation in step (2).
[0032] In one embodiment, after evacuation in step (2), the degree of vacuum is maintained for 10 to 50 minutes, preferably 15 to 45 minutes.
[0033] In one embodiment, a second additive can be added to the reaction system. The second additive can be added in one or more stages of either step (1) or step (2). The second additive may or may not be added simultaneously with titanium dioxide.
[0034] In one embodiment, the second additive may include one or more of a flame retardant, an antioxidant, an end capping agent, an ultraviolet absorber, an infrared absorber, a nucleating agent, an optical brightener, and an antistatic agent.
[0035] In one embodiment, the second additive is added in an amount of 0-1%, such as 0.05%, 0.1%, 0.2%, 0.4%, 0.5%, 0.6% or 0.8%, based on the total weight of the raw materials for producing the polyamide 56 resin.
[0036] In one embodiment, after drying in step (3), the polyamide 56 resin has a moisture content of 300 to 1000 ppm, preferably 300 to 800 ppm, and more preferably 600 to 800 ppm.
[0037] In one embodiment, in step (3), drying may be carried out at a temperature of 80 to 130°C, preferably 100 to 110°C, such as 90°C, 95°C, 98°C, 102°C, 104°C, 105°C, 106°C, 108°C, 115°C, 120°C, or 125°C.
[0038] In one embodiment, in step (3), drying may be carried out for 10 to 30 hours, preferably 15 to 25 hours, such as 12 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, or 28 hours.
[0039] In one embodiment, in step (3), a melt filter is used for filtration before pelletization to remove large-sized particles caused by the aggregation of TiO2 during polymerization. This can lead to a smaller particle size and narrower size distribution of titanium dioxide in the polyamide 56 resin, and can further improve the uniformity of the polyamide 56 melt. This avoids the phenomenon of monofilament breakage and further filament breakage caused by excessive particle size during the drawing process, avoiding the influence on the mechanical properties and dyeability of the fiber, thus reducing monofilament breakage during the subsequent spinning process and improving dyeability.
[0040] In one embodiment, after filtration through a melt filter, the titanium dioxide in the dull polyamide 56 resin has a dispersed particle diameter of 0.2 to 1.0 μm, preferably 98% or more of the titanium dioxide particles have a dispersed particle diameter of 0.2 to 0.6 μm, and more preferably 95% or more of the titanium dioxide particles have a dispersed particle diameter of 0.2 to 0.35 μm.
[0041] In one embodiment, the melt filter has a mesh size of 5 to 15 μm.
[0042] In one embodiment of the present invention, a method for preparing polyamide 56 resin is used to prepare dull polyamide 56 resin by in-situ polymerization of TiO2. By strictly controlling the particle size and particle size distribution of TiO2 particles, agglomerated TiO2 particles can be avoided or removed, the particle size distribution can be narrowed, and the spinnability can be improved.
[0043] One embodiment of the present invention provides a polyamide 56 resin that can be prepared by the above-mentioned method.
[0044] One embodiment of the present invention provides a polyamide 56 resin having a relative viscosity of 2.3 to 3.0, preferably 2.5 to 2.8; an oligomer content of 1.5% by weight or less, preferably 1% by weight or less, more preferably 0.8% by weight or less, for example, 0.3 to 1.0% by weight, 0.3 to 0.8% by weight, etc.; a water content of 300 to 1000 ppm, preferably 300 to 800 ppm, more preferably 600 to 800 ppm; a number average molecular weight of 15000 to 42000, preferably 18000 to 35000; and a molecular weight distribution of 1.2 to 2.0, preferably 1.4 to 1.8. The oligomer according to the present invention has a degree of polymerization of 5 or less.
[0045] The polyamide 56 resin according to one embodiment of the present invention has a low oligomer content, a narrow polyamide resin molecular weight distribution, and a moderate viscosity.
[0046] In one embodiment, the polyamide 56 resin may have a relative viscosity of 2.4, 2.5, 2.6, 2.7, 2.8, or 2.9, etc.
[0047] In one embodiment, the polyamide 56 resin may have a moisture content of 350 ppm, 550 ppm, 650 ppm, 700 ppm, 750 ppm, 850 ppm, or 900 ppm, etc.
[0048] In one embodiment, the polyamide 56 resin may have a number average molecular weight of 16000, 20000, 22000, 25000, 28000, 30000, 32000, 34000, 38000, or 40000, etc.
[0049] In one embodiment, the polyamide 56 resin may have a molecular weight distribution of 1.3, 1.5, 1.6, 1.7, or 1.9, etc.
[0050] In one embodiment, the oligomer content of the polyamide 56 resin may be 0.3%, 0.6%, or 1.0%. The degree of polymerization of the oligomer described in this invention is less than or equal to 10. If the oligomer content in the resin is too high, the oligomer will precipitate and coagulate under the spinneret during spinning, and the excessive precipitation will affect the spinning process, cause monofilament breakage during spinning, and shorten the life of the spin pack.
[0051] In one embodiment, the polyamide 56 resin includes a titanium dioxide based matting agent.
[0052] In one embodiment, the polyamide 56 resin can be a semi-dull polyamide 56 resin, a dull polyamide 56 resin, or a full-dull polyamide 56 resin.
[0053] In one embodiment, the polyamide 56 resin is a semi-dull polyamide 56 resin having a titanium dioxide content of 0.2-0.4 wt %, preferably 0.25-0.35 wt %, for example 0.3 wt %.
[0054] In one embodiment, the polyamide 56 resin is a full-dull polyamide 56 resin having a titanium dioxide content of 1.2 to 2.0 wt %, preferably 1.4 to 1.8 wt %, for example 1.5 wt %, 1.6 wt %, or 1.7 wt %.
[0055] In one embodiment, the polyamide 56 resin is an ultradull polyamide 56 resin having a titanium dioxide content of 2.5 to 5.0 wt%, preferably 3.0 to 4.5 wt%, for example 2.8 wt%, 3.2 wt%, 3.5 wt%, 4.0 wt%, 4.2 wt%, 4.4 wt%, or 4.8 wt%.
[0056] In one embodiment, the dispersed particle size of titanium dioxide in the polyamide 56 resin is 0.2 to 1.0 μm. Furthermore, titanium dioxide particles having a dispersed particle size of 0.2 to 0.6 μm account for 98% or more, and titanium dioxide particles having a dispersed particle size of 0.2 to 0.6 μm account for 98.5% or more. Furthermore, titanium dioxide particles having a dispersed particle size of 0.2 to 0.35 μm account for 95% or more, and titanium dioxide particles having a dispersed particle size of 0.2 to 0.35 μm account for 96% or more. Here, in this specification, the content of titanium dioxide refers to the content converted into the particle number of titanium dioxide particles.
[0057] One embodiment of the present invention provides a polyamide 56 fiber, which can be prepared by melt spinning the aforementioned polyamide 56 resin.
[0058] In one embodiment, the polyamide 56 fibers can be semi-dull, dull, and full-dull polyamide 56 fibers, among which the semi-dull, dull, and full-dull polyamide 56 fibers can be obtained by melt spinning semi-dull, dull, and full-dull polyamide 56 resins, respectively.
[0059] In one embodiment, polyamide 56 fibers include undrawn yarn (UDY), fully drawn yarn (FDY), pre-oriented yarn (POY), highly oriented yarn (HOY), fully oriented yarn (FOY), draw textured yarn (DTY), bulk continuous filament (BCF), monofilament, staple fiber, and industrial yarn, preferably pre-oriented yarn (POY) and draw textured yarn (DTY). Draw textured yarn is also known as drafting false twist yarn or stretcher strain yarn.
[0060] The polyamide 56 fiber of one embodiment of the present invention has advantages such as high strength, low temperature dyeability, moisture absorption, flexibility, abrasion resistance and high elasticity, and has broad development prospects in the fields of consumer yarns and industrial yarns.
[0061] In one embodiment, the polyamide 56 fibers may have a filament fineness of 0.5-5.0 dtex, preferably 0.8-4.0 dtex, more preferably 1.2-3.0 dtex, even more preferably 1.2-2.0 dtex, such as 1.0 dtex, 1.5 dtex, 1.8 dtex, 2.5 dtex, 3.5 dtex or 4.5 dtex.
[0062] In one embodiment, the polyamide 56 fibers may have a breaking strength of 3.3 to 5.5 cN / dtex, preferably 3.5 to 4.8 cN / dtex, more preferably 3.7 to 4.5 cN / dtex, and even more preferably 3.9 to 4.2 cN / dtex.
[0063] In one embodiment, the polyamide 56 fibers have a coefficient of variation in breaking strength less than or equal to 5.0%, preferably less than or equal to 3.0%, more preferably less than or equal to 2.5%, and even more preferably less than or equal to 2.0%.
[0064] In one embodiment, the polyamide 56 fibers have an initial modulus of 15-35 cN / dtex, preferably 22-33 cN / dtex, more preferably 24-30 cN / dtex, and even more preferably 26-28 cN / dtex.
[0065] In one embodiment, the polyamide 56 fibers may have a shrinkage in boiling water of 7% or less, preferably 6.8% or less, more preferably 6.5% or less, and even more preferably 6.0% or less.
[0066] In one embodiment, the polyamide 56 fibers may have a moisture regain of 4.0% or greater, preferably 4.5% or greater, more preferably 5.0% or greater, and even more preferably 5.5% or greater.
[0067] In one embodiment, the polyamide 56 fibers may have a crimp shrinkage of 35 to 60%, preferably 40 to 58%, and more preferably 45 to 55%.
[0068] In one embodiment, the polyamide 56 fibers may have a crimp stability of 38-58%, preferably 40-56%, more preferably 48-54%, for example 45%, 50% or 52%.
[0069] In one embodiment, the polyamide 56 fiber may have a dye uniformity (gray scale) of 3.5 grade or greater, preferably 4.0 grade or greater, more preferably 4.5 grade or greater, and even more preferably 5.0 grade or greater.
[0070] In one embodiment, the polyamide 56 fibers may have an M ratio of 92% or more, preferably 94% or more, more preferably 96% or more, and even more preferably 98% or more.
[0071] In one embodiment, the soap washing fastness of the polyamide 56 fiber: the fade fastness may be 3.5 grade or more, preferably 4.0 grade or more, more preferably 4.5 grade or more, even more preferably 5.0 grade or more; the color fastness may be 3.5 grade or more, preferably 4.0 grade or more, more preferably 4.5 grade or more, even more preferably 5.0 grade or more.
[0072] One embodiment of the present invention provides a method for preparing the aforementioned polyamide 56 fibers, comprising the steps of: (a) heating a polyamide 56 resin to a molten state to form a polyamide 56 melt; (b) The polyamide 56 melt is transported through a melt pipeline to a spinning box, and then precisely metered by a metering pump, and then injected into a spin pack and extruded through a spinneret under high pressure to obtain as-spun fibers; (c) subjecting the extruded as-spun fibers to a cooling process, an oiling process, a drawing process, and a winding process to obtain a pre-oriented yarn of polyamide 56; and (d) A process in which the pre-oriented yarn of polyamide 56 is passed through a yarn guide, through a first roller, through a twist stopper, and subjected to hot drawing in a first heat box, then cooled and set using a cooling plate, passed through a false twister, a second roller, and an interlacer, and then subjected to oiling and winding to obtain a stretch-textured yarn of polyamide 56.
[0073] In one embodiment, the heating in step (a) is carried out using a screw extruder, and the temperature in zone 1 may be from 245 to 265°C, preferably from 250 to 260°C; the temperature in zone 2 may be from 260 to 280°C, preferably from 265 to 275°C; the temperature in zone 3 may be from 275 to 285°C, preferably from 278 to 283°C; and the temperature in zone 4 may be from 280 to 290°C.
[0074] In one embodiment, the spin box of step (b) may have a temperature of 278-290°C, preferably 282-285°C; the spin pack may have a pressure of 13-22 MPa, preferably 15-18 MPa.
[0075] In one embodiment, the cooling in step (c) includes cooling with quench air and cooling with cross air blowing, preferably cooling with cross air blowing; the air speed may be 0.3 to 0.8 m / sec, preferably 0.45 to 0.6 m / sec; the air temperature may be 18 to 23° C.; and the air humidity may be 50% to 85%, preferably 55% to 70%.
[0076] In one embodiment, the oiling in step (c) is performed by nozzle oiling; the oiling rate may be 0.4-0.6% by weight, preferably 0.45-0.55% by weight; the oiling height may be 80-150 cm, preferably 90-130 cm, more preferably 95-110 cm.
[0077] In one embodiment, the winding speed during winding in step (c) may be 4000-5000 m / min, preferably 4200-4800 m / min, more preferably 4300-4500 m / min; the overfeed speed may be 10-100 m / min, more preferably 20-80 m / min.
[0078] In one embodiment, the stretch ratio in the hot stretching in step (d) may be 1.1 to 1.4, preferably 1.15 to 1.35; the hot stretching temperature may be 160 to 210°C, preferably 170 to 205°C, more preferably 180 to 195°C.
[0079] In one embodiment, the speed ratio D / Y of the false twisting machine in step (d) may be 1.3 to 2.2, preferably 1.5 to 2.0; the pressure of the compressed air in the interlacer may be 0.3 to 1.5 MPa, preferably 0.4 to 1.2 MPa, more preferably 0.5 to 1.0 MPa.
[0080] In one embodiment, the oiling in step (d) is carried out by nozzle oiling; the oiling rate may be 2.2-2.8% by weight, preferably 2.3-2.6% by weight.
[0081] In one embodiment, the winding speed during winding in step (d) may be 300-800 m / min, preferably 400-700 m / min; the winding overfeed rate during winding is 1-8%, preferably 1.5-6%, more preferably 2-5%.
[0082] In one embodiment of the present invention, the raw materials for producing polyamide 56 fiber can be prepared by biological methods, which is a green material that does not depend on petroleum resources and does not cause serious environmental pollution, while at the same time reducing carbon dioxide emissions and reducing the occurrence of the greenhouse effect.
[0083] The polyamide 56 fiber of one embodiment of the present invention can be produced using conventional spinning equipment for polyamide 6 and polyamide 66 without modification of the spinning equipment. The production yield can be improved by optimizing the quality of the polyamide 56 fiber resin and the spinning process.
[0084] The polyamide 56 fiber of one embodiment of the present invention has good mechanical properties, dimensional stability, moisture absorption and dyeability, and has a good matte effect when applied to knitted or woven fabrics.
[0085] One embodiment of the present invention provides the use of the aforementioned polyamide 56 fiber in a knitted or woven fabric, wherein the polyamide 56 fabric may have a light transmittance of 50% or less, preferably 48% or less, more preferably 35% or less, even more preferably 30% or less.
[0086] In one embodiment, polyamide 56 fiber has high strength, softness, moisture absorption, bulkiness (shrinkage stability), good dyeability and matt performance, and is suitable for use in knitwear and consumer apparel. Non-limiting examples of knit and woven applications include underwear, shirts, suits, yoga wear, down jackets, outdoor jackets, socks, suitcases and bags, curtains, shoe materials, embroidery threads, trademarks, sofa cloths, workwear, sportswear, and rubber bands, etc.
[0087] The fabric prepared from the polyamide 56 fiber of one embodiment of the present invention has good matt performance, and when it contains the same content of TiO2, the matt effect is better than that of polyamide 6 fiber and polyamide 66 fiber. Moreover, the content of TiO2 that needs to be added when preparing polyamide 56 fiber with the same matt effect is less, which can reduce the production cost.
[0088] In one embodiment of the present invention, the light transmittance of a semi-dull polyamide 56 fabric may be 48% or less, the light transmittance of a fully-dull polyamide 56 fabric may be 33% or less, and the light transmittance of an ultra-dull polyamide 56 fabric may be 25% or less. EXAMPLES
[0089] The polyamide 56 resin, polyamide 56 fiber and preparation method thereof according to one embodiment of the present invention will be further described below with specific examples.Unless otherwise specified, all raw materials used are commercially available, and the relevant test details are as follows; furthermore, all parameters related to the present invention are measured according to the following methods.
[0090] 1)Fineness: The fineness is measured according to GB / T 14343.
[0091] 2) Breaking strength and modulus: The breaking strength can be measured under the conditions of 0.05±0.005cN / dtex pretension, 500mm clamping distance, and 500mm / min stretching speed; modulus = breaking strength at 1% elongation × 100.
[0092] 3) The method for measuring the moisture content includes: placing the washed fiber in an oven in an unraveled state to dry, placing the oven-dried fiber sample in the standard atmosphere specified in GB / T6529 to adjust the humidity until it reaches equilibrium; and measuring the moisture content in an oven at an oven drying temperature of 105°C using the moisture content measuring method specified in GB / T6503.
[0093] 4) Shrinkage rate in boiling water The shrinkage in boiling water is measured according to GB / 6505, with a pretension of 0.05±0.005cN / dtex.
[0094] 5) Dyeing uniformity (gray scale) / grade: Dye uniformity is judged in accordance with FZ / T 50008 "Test method for dye uniformity of polyamide filament yarn" at 98°C for 30 minutes.
[0095] 6) Moisture content of resin: The moisture content is measured by a Karl Fischer titrator.
[0096] 7) Crimp shrinkage rate and crimp stability: Measured according to GB / T 6506-2001 "Test method for crimp shrinkage properties of textured filament yarn".
[0097] 8) Soap washing fastness: Soap wash fastness is measured according to GB / T 3921.1-1997.
[0098] 9) The relative viscosity of the resin is determined by the concentrated sulfuric acid method using an Ubbelohde viscometer: 0.25±0.0002 g of dry polyamide resin chips are accurately weighed, and 50 mL of concentrated sulfuric acid (96% by weight) is added to dissolve the chips. The flow time of the concentrated sulfuric acid (t0) and the flow time of the polyamide sample solution (t) are measured and recorded in a thermostatic water bath at 25°C.
[0099] Viscosity value calculation formula: Relative viscosity = t / t0; t - flow time of the solution; t0 - solvent flow time.
[0100] 10) The number average molecular weight and molecular weight distribution of the resin are measured by gel permeation chromatography (GPC).
[0101] 11) The dispersed particle size of titanium dioxide is measured and counted from a transmission electron microscope image of the polyamide resin chip.
[0102] 12) M rate: M rate = ((weight of fiber with dyeing uniformity of 4.5 grade or higher) / total weight of all dyed fibers) x 100%.
[0103] 13) Matte performance: The fibers obtained in the examples and comparative examples are woven on the same air jet loom, washed with an open soaper, and dyed with a liquid jet dyeing machine to produce woven fabrics of uniform specifications. A special inspection group (10 panelists) is organized to visually evaluate the matte performance of the woven fabrics and calculate the average value. That is, the matte surface performance of the woven fabrics is compared under conditions of a halogen lamp simulating sunlight and a temperature of 25°C, and the matte performance is divided into 1st, 2nd, 3rd, 4th, and 5th grades, from low to very high, and rated.
[0104] 14) The light transmittance is measured by an ultraviolet-visible spectrophotometer with a scanning wavelength of 300-800 nm, and the light transmittance of the fabric refers to the light transmittance at a wavelength of 550 nm.
[0105] 15) Fiber production yield: Production yield = (weight of fiber product obtained / total weight of resin input) x 100%.
[0106] 16) Test for oligomer content in resin: The polyamide sample is dried in a blast oven at 130 ° C for 7 hours, then placed in an aluminum plastic bag, sealed and cooled in a dryer, 2 g of the polyamide sample is accurately weighed and placed in a 250 mL round-bottom flask, and 100 mL of water is added. The resulting mixture is heated to reflux at 100 ° C for 24 hours using a heating jacket, and the polyamide sample is taken out and washed three times with pure water. The polyamide sample is dried in a blast oven at 130 ° C for 7 hours, then transferred to a pre-weighed aluminum plastic bag, sealed, and cooled in a dryer. The total weight of the aluminum plastic bag and the polyamide sample and the weight of the aluminum plastic bag are weighed, respectively, and the latter is subtracted from the former to obtain the weight of the polyamide sample after boiling with water, and the oligomer content is calculated from the difference in weight of the polyamide sample before and after boiling with water. Two samples are taken from each sample for testing.
[0107] 17) The test for titanium dioxide content in resin is carried out by the calcination method: 10 g of sample is placed in a crucible and calcined in a muffle furnace at 480°C for 10 hours, and the weight of the residue in the crucible is measured.
[0108] 18) The coefficient of variation (CV) test of breaking strength is carried out according to GB / T 14344-2008 "Method of tensile test for artificial filament yarn". When titanium dioxide is uniformly dispersed in the fiber, different numbers of fibers will break simultaneously during the drawing process, and the breaking strength corresponding to the break will be constant, reflecting the small coefficient of variation.
[0109] 19) Number of filament breaks: During the process of preparing polyamide fiber from as-spun fiber, the number of filament breaks is manually counted.
[0110] Example 1 [Preparation of polyamide 56 resin] (1) Under a nitrogen atmosphere, 1,5-pentanediamine, adipic acid, and water were uniformly mixed to prepare a polyamide 56 salt solution in which the molar ratio of 1,5-pentanediamine to adipic acid was 1.05:1.
[0111] (2) Titanium dioxide with a particle size of 0.2 μm was added to the polyamide 56 salt solution, and the salt solution system was heated to raise the pressure in the reaction system to 2.4 MPa, followed by degassing and maintaining the pressure for 1.2 hours, and then the pressure in the reaction system was reduced to 0 MPa (gauge pressure), and then evacuated to a vacuum of -0.04 MPa. The above vacuum was maintained for 35 minutes to obtain a polyamide 56 melt, and the amount of titanium dioxide added was 0.27% by weight based on the mass of the resin prepared under the same conditions without adding titanium dioxide. The temperature of the reaction system at the end of maintaining the pressure was 260°C, the temperature of the reaction system after the reduction in pressure was 275°C, and the temperature of the reaction system after evacuation was 280°C.
[0112] (3) The polyamide 56 melt was filtered through a melt filter with a mesh size of 10 μm, pelletized, and dried to obtain a polyamide 56 resin. The drying process was carried out at 110° C. for 20 hours.
[0113] [Preparation of polyamide 56 fiber] (a) The polyamide 56 resin prepared above was heated to a molten state in a screw extruder to form a polyamide 56 melt, where the temperature in zone 1 was 253°C, the temperature in zone 2 was 266°C, the temperature in zone 3 was 278°C, and the temperature in zone 4 was 288°C.
[0114] (b) The polyamide 56 melt was transported to the spinning box through the melt pipeline, and after being accurately metered by the metering pump, it was injected into the spinning pack and extruded through the spinneret under high pressure, where the temperature of the spinning box was 285°C and the pressure of the spinning pack was 16.2 MPa.
[0115] (c) The extruded as-spun fibers were subjected to cooling, oiling, drawing, and winding processes to obtain pre-oriented yarn of polyamide 56; here, cooling was carried out using cross air blow at an air speed of 0.48 m / s, air temperature of 20° C., and air humidity of 80%; oiling was carried out by nozzle oiling with an oiling rate of 0.5 wt.% and an oiling height of 110 cm; the winding speed during the winding process was 4300 m / min, and the overfeed speed was 60 m / min.
[0116] (d) the polyamide 56 pre-oriented yarn is guided through a yarn guide to a first roller, passed through a twist stopper and subjected to hot drawing in a first heat box, then cooled and set using a cooling plate, passed through a false twister, a second roller and an interlacer, then subjected to nozzle oiling and wound up to obtain a polyamide 56 draw-textured yarn; Here, the draw ratio of the hot drawing was 1.3 times, and the hot drawing temperature was 185°C; the speed ratio D / Y of the false twister was 1.8; the pressure of the compressed air in the interlacer was 0.8 MPa; the oiling was carried out by nozzle oiling with an oiling rate of 2.5 wt%; the winding speed during winding was 600 m / min, and the overfeed speed of the winding during winding was 2.5%.
[0117] Example 2 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 0.34 wt %.
[0118] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0119] Example 3 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using basically the same raw materials as in Example 1, with the only differences being that in step (2), the vacuum degree was -0.07 MPa, the maintenance time was 10 minutes, and the amount of titanium dioxide added in step (2) was 0.35 wt %.
[0120] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0121] Example 4 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and process as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 1.23 wt % and the mesh size of the melt filter in step (3) was 5 μm.
[0122] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0123] Example 5 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and process as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 1.56 wt % and the mesh size of the melt filter in step (3) was 15 μm.
[0124] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0125] Example 6 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 1.84 wt %.
[0126] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0127] Example 7 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 2.56 wt %.
[0128] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0129] Example 8 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 3.05% by weight.
[0130] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0131] Example 9 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 1, with the only difference being that the amount of titanium dioxide added in step (2) was 4.05 wt %.
[0132] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0133] Example 10 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using basically the same raw materials and process as in Example 1. The only differences were that the amount of titanium dioxide added in step (2) was 0.34% by weight, the reaction system was evacuated to a vacuum degree of -0.06 MPa, and the temperature of the reaction system after evacuation was 285°C.
[0134] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0135] Example 11 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 10, with the only difference being that the amount of titanium dioxide added in step (2) was 1.54 wt %.
[0136] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0137] Example 12 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and process as in Example 10, with the only difference being that the amount of titanium dioxide added in step (2) was 2.53 wt %.
[0138] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0139] Example 13 [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared in Example 10 was used as the spinning raw material, and the specific spinning process was basically the same as that in Example 1, with the only difference being that the spinning pack contained a nonwoven filter screen with a mesh size of 10 μm.
[0140] Example 14 [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared in Example 11 was used as the spinning raw material, and the specific spinning process was basically the same as that in Example 1, with the only difference being that the spinning pack contained a nonwoven filter screen with a mesh size of 15 μm.
[0141] Example 15 [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared in Example 11 was used as the spinning raw material, and the specific spinning process was basically the same as that in Example 1, with the only difference being that the spinning pack contained a nonwoven filter screen with a mesh size of 20 μm.
[0142] Comparative Example 1 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 2, with the only difference being that in step (3), no melt filter was used for filtration, and the polyamide 56 resin was directly obtained by pelletization.
[0143] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0144] Comparative Example 2 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 5, with the only difference being that in step (3), no melt filter was used for filtration, and the polyamide 56 resin was directly obtained by pelletization.
[0145] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0146] Comparative Example 3 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and steps as in Example 7, with the only difference being that in step (3), no melt filter was used for filtration, and the polyamide 56 resin was directly obtained by pelletization.
[0147] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0148] Comparative Example 4 [Preparation of polyamide 6 fibers] Polyamide 6 resin (viscosity 2.7, molecular weight distribution 1.59, oligomer content 0.61%, water content 612 ppm) was mixed with 0.33 wt% titanium dioxide (particle diameter 0.2 μm), and this mixture was used as a spinning raw material and spun in the same manner as in Example 1 to obtain polyamide 6 fiber; here, the titanium dioxide content was based on the mass of the polyamide 6 resin.
[0149] Comparative Example 5 [Preparation of polyamide 66 fibers] Polyamide 66 resin (viscosity 2.68, molecular weight distribution 1.61, oligomer content 0.62%, water content 605 ppm) was mixed with 0.32 wt% titanium dioxide (particle diameter 0.2 μm), and this mixture was used as a spinning raw material and spun in the same manner as in Example 1 to obtain polyamide 66 fiber; the titanium dioxide content here was based on the mass of the polyamide 66 resin.
[0150] Comparative Example 6 [Preparation of polyamide 56 fiber] Polyamide 56 resin (viscosity 2.68, molecular weight distribution 1.61, oligomer content 0.61%, water content 607 ppm) was mixed with 0.26 wt% titanium dioxide (particle diameter 0.2 μm), and this mixture was used as a spinning raw material and spun in the same manner as in Example 1 to obtain polyamide 56 fiber; the titanium dioxide content here was based on the mass of the polyamide 56 resin.
[0151] Comparative Example 7 [Preparation of polyamide 56 resin] The polyamide 56 resin was prepared using essentially the same raw materials and process as in Example 5, with the only difference being that the mesh size of the melt filter in step (3) was 20 μm.
[0152] [Preparation of polyamide 56 fiber] The polyamide 56 resin prepared above was used as a spinning raw material, and the specific spinning process was the same as in Example 1.
[0153] Relevant performance tests were carried out on the polyamide 56 resins prepared in Examples 1 to 12 and Comparative Examples 1 to 3. The results are shown in Table 1.
[0154] [Table 1] Relevant performance tests were carried out on the polyamide fibers prepared in Examples 1 to 15 and Comparative Examples 1 to 7. The results are shown in Tables 2 and 3. [Table 2]
[0155] [Table 3] Unless specifically limited, the terms used herein have the meanings that are commonly understood by those skilled in the art.
[0156] The embodiments described in the present invention are for illustrative purposes only and do not limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, modifications and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above-described embodiments, but is limited only by the claims.
Claims
1. The titanium dioxide is contained in an amount of 0.2 to 5.0% by weight, and 98% or more of the titanium dioxide has a dispersed particle size of 0.2 to 0.6 μm. Polyamide 56 resin.
2. 95% or more of the titanium dioxide has a dispersed particle size of 0.2 to 0.35 μm; The polyamide 56 resin according to claim 1.
3. The titanium dioxide is contained in an amount of 0.2 to 0.4 wt %, 1.2 to 2.0 wt %, or 2.5 to 5.0 wt %. The polyamide 56 resin according to claim 1.
4. The polyamide 56 resin has a relative viscosity of 2.3 to 3.0; and / or The polyamide 56 resin has a moisture content of 300 to 1000 ppm; and / or The polyamide 56 resin has a molecular weight distribution of 1.2 to 2.0; and / or The polyamide 56 resin has an oligomer content of 1.5% by weight or less. The polyamide 56 resin according to claim 1.
5. preparing a polyamide 56 resin from the monomers by a polymerization reaction; The polyamide 56 resin contains titanium dioxide, and the titanium dioxide is added during the polymerization reaction. Method for preparing polyamide 56 resin.
6. The monomers include 1,5-pentanediamine and adipic acid, and the polymerization reaction comprises: (1) preparing a polyamide 56 salt solution; and (2) carrying out polymerization using the polyamide 56 salt solution as a raw material to obtain a polyamide 56 melt; Titanium dioxide is added in step (1) and / or step (2); The method according to claim 5.
7. Step (2) comprises heating the polyamide 56 salt solution to increase the pressure of the reaction system of the polyamide 56 salt solution to 0.3 to 2.4 MPa, maintaining the pressure for 0.2 to 2.5 hours by degassing, then reducing the pressure of the reaction system to 0 to 0.3 MPa, and then evacuating the reaction system to a vacuum degree of −0.001 to −0.08 MPa. The method according to claim 6.
8. the reaction system has a temperature of 230-265° C. at the end of the pressure hold; and / or The reaction system has a temperature of 240-275° C. at the end of depressurization; and / or The reaction system has a temperature of 250-285° C. at the end of the vacuum; and / or The vacuum is maintained for 10 to 50 minutes after evacuation. The method of claim 7.
9. filtering, pelletizing and drying the polyamide 56 melt to obtain the polyamide 56 resin. The method according to claim 6.
10. A polyamide 56 resin prepared by the method according to any one of claims 5 to 9 or a polyamide 56 resin according to any one of claims 1 to 4, or a polyamide 56 melt prepared by the method according to any one of claims 5 to 8, Polyamide 56 fiber.
11. The polyamide 56 fiber is a filament fineness of 0.5 to 5.0 dtex; and / or A breaking strength of 3.3 to 5.5 cN / dtex; and / or An initial modulus of 15 to 35 cN / dtex; and / or Shrinkage in boiling water of 7% or less; and / or A moisture content of 4.0% or more; and / or A crimp shrinkage of 35-60% and a crimp stability of 38-58%; and / or Dye uniformity of 3.5 or better; and / or M rate of 92% or more and color fastness rating of 3.5 or more; and / or Has a color fastness of 3.5 or higher.
11. The polyamide 56 fiber of claim 10.
12. including one or more of undrawn yarns, fully drawn yarns, pre-oriented yarns, highly oriented yarns, fully oriented yarns, draw-textured yarns, bulk continuous filaments, staple fibers, monofilaments, and industrial yarns, more preferably including pre-oriented yarns and draw-textured yarns; 12. The polyamide 56 fiber of claim 11.
13. (a) heating the polyamide 56 resin to a molten state to obtain a polyamide 56 melt; (b) conveying the polyamide 56 melt to a spin box, injecting it into a spin pack, and extruding it through a spinneret to form as-spun fibers; (c) subjecting the as-spun fibers to a cooling process, an oiling process, a drawing process, and a winding process to obtain a pre-oriented yarn of polyamide 56; and (d) subjecting the pre-oriented yarn of polyamide 56 to a hot drawing process through a first roller, then cooling and setting, passing through a false twister, a second roller, an interlacer, and subjecting it to an oiling process and a winding process to obtain the polyamide 56 fiber. A method for preparing the polyamide 56 fibers according to any one of claims 10 to 12.
14. In step (a), the heating is carried out using a screw extruder, wherein zone 1 has a temperature of 245-265°C; zone 2 has a temperature of 260-280°C; zone 3 has a temperature of 275-285°C; and zone 4 has a temperature of 280-290°C; and / or In step (b), the spin box has a temperature of 278-290° C. and the spin pack has a pressure of 13-22 MPa. The method of claim 13.
15. In step (c), the cooling treatment is carried out by quench air cooling or cross air blow cooling at an air temperature of 18-23° C. and an air humidity of 50-85%; and / or The oiling treatment is carried out by nozzle oiling with an oiling rate of 0.4 to 0.6% by weight; and / or The winding process is carried out at a winding speed of 4200 to 5000 m / min and an overfeed speed of 10 to 100 m / min; The method of claim 13.
16. In step (d), the hot drawing process is carried out with a draw ratio of 1.1-1.4, the hot drawing process is carried out at a temperature of 160-210°C; the false twister has a speed ratio D / Y of 1.3-2.2; the compressed air in the interlacer has a pressure of 0.3-1.5 MPa; the oiling process is carried out by nozzle oiling with an oiling rate of 2.2-2.8% by weight; and further, the winding process is carried out with a winding speed of 300-800 m / min and an overfeed rate of winding during winding of 1-8%. The method of claim 13.
17. Use of the polyamide 56 fibers according to any one of claims 10 to 12 or prepared by the method according to any one of claims 13 to 16 in knitted or woven fabrics.
Citation Information
Patent Citations
Polyamide 56 resin, fiber and preparation method and application thereof
CN113736249A