Conductive particles, conductive materials and connection structures

The conductive particles with a single-layer polycrystalline structure address the issue of interlayer boundaries in conventional particles, ensuring low resistance and reliability in anisotropic conductive materials.

JP2024544440AActive Publication Date: 2024-12-03DUK SAN NEOLUX
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022562536
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2021-12-15
Publication Date
2024-12-03
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

Conventional conductive particles with multiple metal layers on an insulating core exhibit increased connection resistance due to interlayer boundaries, leading to reliability issues in anisotropic conductive materials.

Method used

The conductive particles feature a single-layer conductive layer with a polycrystalline structure, composed of multiple elements like Ni and others, without interlayer boundaries, ensuring low initial connection resistance and minimal resistance increase even under high temperature and humidity conditions.

Benefits of technology

The conductive particles maintain low initial connection resistance and resist significant resistance increase, enhancing the reliability of anisotropic conductive materials in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544440000001_ABST
    Figure 2024544440000001_ABST
Patent Text Reader

Abstract

The present invention is a conductive particle comprising an insulating core and a conductive layer on the insulating core, the conductive layer containing at least two elements, and is characterized in that a diffraction pattern obtained by analyzing the conductive layer using XRD forms at least two diffraction circles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive particle having a metal conductive layer on the surface of an insulating core, and more particularly to a conductive particle used as a core conductive material of an anisotropic conductive adhesive material for connecting fine pitch circuits. The present invention also relates to a conductive material and a connection structure using the conductive particle. [Background technology]

[0002] Anisotropic conductive materials are bonding materials that transmit electrical signals between upper and lower electrodes but do not transmit electrical signals between left and right electrodes. Anisotropic conductive materials are bonding materials that are mainly used to connect a large number of electrodes to a driving IC, especially in displays.

[0003] Conductive particles are generally used in anisotropic conductive materials in a dispersed form mixed with a hardener, an adhesive, a resin binder, and other additives, such as anisotropic conductive films, anisotropic conductive adhesives, anisotropic conductive pastes, anisotropic conductive inks, and anisotropic conductive sheets.

[0004] Anisotropic conductive materials are used in FOG (film on glass; flexible substrate - glass substrate), COF (chip on film; semiconductor chip - flexible substrate), COG (chip on glass; semiconductor chip - glass substrate), FOB (film on board; flexible substrate - glass epoxy substrate), etc.

[0005] For example, assuming that an anisotropic conductive material is used to join a semiconductor chip and a flexible substrate, the anisotropic conductive material can be placed on the flexible substrate, the semiconductor chip is stacked on top of the anisotropic conductive material, and the anisotropic conductive material is hardened under pressure / heat, thereby realizing a connection structure in which the conductive particles electrically connect the electrodes of the substrate and the electrodes of the semiconductor chip.

[0006] When the conductive particles are used in the anisotropic conductive material, they are mixed with additives such as hardeners, adhesives, resin binders, and fillers, and when a connection structure is formed after pressure / heating, the electrical connection between the upper and lower electrodes is maintained by the hardening / adhesion of the anisotropic conductive material.

[0007] However, in conventional conductive particles having a metal conductive layer on the surface of an insulating core, the conductive layer is formed in multiple layers to improve the conductivity of the conductive layer. In this case, some parts are formed amorphous or boundaries exist between each layer of the conductive layer, resulting in an increase in resistance at the boundaries, which increases the connection resistance of anisotropic conductive materials using the conductive particles, thereby causing an increase in reliability resistance. Summary of the Invention [Problem to be solved by the invention]

[0008] The technical problem that the embodiments of the present invention aim to solve is to provide conductive particles having high strength, low initial connection resistance and resistance increase rate while having a single conductive layer, an anisotropic conductive material containing the same, and an anisotropic connection structure, in order to solve the problems of the prior art described above. [Means for solving the problem]

[0009] One aspect of the present invention is a conductive particle, An insulating core; a conductive layer on the insulating core, the conductive layer comprising at least two elements; The diffraction pattern obtained by analyzing the conductive layer using XRD shows that at least two diffraction circles are formed, and the average length of the major axis of the crystal grains in the conductive layer is 8 nm to 13 nm.

[0010] It is preferable that the conductive layer contains Ni and at least one element selected from the group consisting of B, P, N, Pd, Pt, W, Au, Ag, Mo, and Co, and that the radius of the innermost diffraction circle among the diffraction circles is 4.93 (l / nm) ± 0.2 (l / nm).

[0011] When the conductive layer is divided into a first region adjacent to the insulating core, a second region adjacent to the first region, and a third region adjacent to the second region and located outermost, it is preferable that the first region, the second region, and the third region are a single layer with no interlayer boundaries between the regions.

[0012] It is preferable that the conductive layer has an element content that varies depending on the region.

[0013] The conductive layer preferably contains at least two elements selected from the group consisting of B, P, N, Pd, Pt, W, Au, Ag, Mo and Co.

[0014] In this case, the conductive particles may further include protrusions on the surface of the conductive layer, and may further include an insulating layer or insulating particles on the surface of the conductive layer. It is preferable that the outermost surface of the conductive layer is subjected to an anti-rust treatment using a hydrophobic anti-rust agent.

[0015] Another aspect of the present invention provides an anisotropic conductive material comprising at least one type of conductive particle as described above.

[0016] Another aspect of the present invention provides a connection structure comprising at least one type of the conductive particles.

[0017] Another aspect of the present invention provides an electronic device comprising at least one type of conductive particle as described above. Effect of the Invention

[0018] The conductive particles according to the embodiments of the present invention have a single-layer structure in which the conductive layer contains a number of metal elements, and thus eliminates boundaries in the conductive layer, while providing crystallinity to the conductive layer, thereby providing excellent electrical conductivity and low resistance effects through the advantages of the crystal structure, and also providing an effect of increased hardness.

[0019] Therefore, by using the conductive particles according to the embodiments of the present invention, it is possible to provide an anisotropic conductive material and anisotropic connection structure that not only maintains a low resistance increase by keeping the initial connection resistance low, but also has a low resistance increase even after high temperature / high humidity reliability testing. [Brief description of the drawings]

[0020] [Figure 1] 1 is a 500,000x image of a conductive layer of conductive particles according to an embodiment of the present invention taken using a field emission transmission electron microscope (FETEM-JEM-2100F, 200 kV). [Diagram 2] 1 is a diffraction pattern measured by using an XRD (X-RAY DIFFRACTOMETER, product name: SmartLab, manufacturer: Rigaku Corporation, target: Cu, electromagnetic waves used: Kα) for a conductive layer of conductive particles according to an embodiment of the present invention. [Diagram 3] FIG. 13 is a diagram showing a method for determining the radius of a diffraction circle. [Figure 4] FIG. 2 is a diagram showing the positions where the conductive layer of the conductive particles was analyzed according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Before describing the present invention in detail below, it should be understood that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to limit the scope of the present invention, which is limited only by the appended claims. All technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art, unless otherwise defined.

[0022] Throughout this specification and the claims, unless otherwise indicated, the words comprise, comprise, and comprising are used to mean the inclusion of the stated object, step, group of objects, and group of steps, and are not used to mean the exclusion of any other object, step, group of objects, or group of steps.

[0023] On the contrary, the various embodiments of the invention may be combined with any other embodiment unless expressly stated to the contrary. Any feature indicated as being particularly preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.

[0024] The conductive particles according to the embodiment of the present invention are conductive particles that are included between electrodes to electrically connect the electrodes, and the electrodes may be oxide electrodes such as ITO (indium tin oxide) and ZnO (zinc oxide), metal electrodes made of metal, or metal powder. For example, the electrodes may be paste electrodes formed by mixing Ag or Cu powder with resin to make a paste. The electrodes may include at least one of the oxide electrodes, metal electrodes, and paste electrodes.

[0025] The conductive particle according to an embodiment of the present invention includes an insulating core particle and a conductive layer provided on the surface of the insulating core particle, and may have protrusions on the surface made of the same or different conductive material as the conductive layer.

[0026] The insulating core particles according to the embodiment of the present invention are not particularly limited, and may be, for example, resin fine particles or organic / inorganic hybrid particles.

[0027] The resin microparticles are copolymers obtained by polymerizing urethane-based, styrene-based, acrylate-based, benzene-based, epoxy-based, amine-based, imide-based, or other monomers, or modified monomers thereof, or mixed monomers thereof, by a method such as seed polymerization, dispersion polymerization, suspension polymerization, or emulsion polymerization.

[0028] When the organic / inorganic hybrid particles have a core-shell structure, the shell is inorganic when the core is organic, and the shell is organic when the core is inorganic. In the case of the organic used, the above-mentioned monomers, modified monomers, or mixed monomers are used, and in the case of the inorganic, oxides-SiO2, TiO2, Al2O3, ZrO2, etc., nitrides-AlN, Si3N4, TiN, BaN, etc., carbides-WC, TiC, SiC, etc. can be used. As a method for forming the shell, chemical coating method, Sol-Gel method, spray coating method, CVD (chemical vapor deposition), PVD (physical vapor deposition), plating method, etc. can be used. In addition, a form in which inorganic particles are dispersed in an organic matrix is ​​also possible, a form in which organic particles are dispersed in an inorganic matrix, and a form in which organic / inorganic are dispersed in each other at 50:50 are also possible.

[0029] The conductive layer of the conductive particles according to the embodiment of the present invention is a conductive layer containing at least two elements, where the conductive layer contains at least two elements selected from the group consisting of B, P, N, Ni, Pd, Pt, W, Au, Ag, Mo and Co.

[0030] Preferably, it contains nickel and at least one element selected from the group consisting of B, P, N, Pd, Pt, W, Au, Ag, Mo and Co.

[0031] For example, it can be made of two-metal alloys such as nickel-phosphorus, nickel-boron, nickel-tungsten, and nickel-nitrogen, or three-metal alloys such as nickel-phosphorus-tungsten, nickel-boron-tungsten, nickel-phosphorus-cobalt, nickel-phosphorus-palladium, and nickel-boron-palladium. It can also be made of four-metal alloys such as nickel-phosphorus-boron-tungsten, nickel-phosphorus-palladium-tungsten, and nickel-boron-tungsten-platinum. It can also be made of five or more metal alloys.

[0032] The reason why nickel is essentially contained as shown in the example is that nickel has good electrical conductivity, and since the insulating core used in the conductive particles mainly uses polymer beads, it has excellent adhesion to plastics.

[0033] The conductive layer according to the present embodiment is a single layer having no interlayer boundaries therein, and the content of elements in the conductive layer may vary depending on the region in the conductive layer, but the conductive layer is manufactured to be polycrystalline throughout the entire region. Manufacturing the conductive layer as polycrystalline with small grain boundaries is advantageous in terms of electrical conductivity.

[0034] Therefore, the conductive layer of the conductive particles according to one embodiment of the present invention is a single polycrystalline layer containing two or more elements, having fine crystal grains with an average major axis length of 8 to 13 nm, and having no interlayer boundaries.

[0035] In this case, it is preferable that, as a result of measuring the diffraction pattern of the entire region of the conductive layer by XRD, a plurality of diffraction circles are formed, and the radius of the innermost diffraction circle among the formed diffraction circles is 4.93±0.2 (l / nm). Meanwhile, when measuring the XRD diffraction pattern, the radius of the diffraction circle is measured by a reciprocal lattice, and the unit is conveniently used as l / nm.

[0036] The size of the crystal grains and the radius of the innermost diffraction circle are determined by the type, content, reaction rate, etc. of the elements used. Therefore, since the conductive layer of the present invention has different elements and their contents depending on the region, the size of the crystal grains and the radius of the innermost diffraction circle change in each region of the conductive layer as a result of measuring the diffraction pattern of the entire region of the conductive layer by XRD.

[0037] In this case, in the present invention, the conductive layer has a crystal grain size with an average major axis length of 8 to 13 nm throughout the entire region of the conductive layer, regardless of the change in content depending on the region, and the radius of the innermost diffraction circle among the diffraction circles in the XRD analysis diffraction pattern is set to within 4.93 (l / nm) ± 0.2 (l / nm), because this allows the formation of a single layer with high adhesive strength with the insulating core and no interlayer boundary within the conductive layer.

[0038] For example, the conductive layer can be divided into a first region adjacent to the insulating core, a second region adjacent to the first region, and a third region adjacent to the second region and located outermost, and the conductive layer can be further divided into a fourth region formed with a first content, a fifth region formed with a second content, and a sixth region formed with a third content, based on content.

[0039] In this case, the conductive layer according to the embodiment of the present invention satisfies the above-mentioned range of the average major axis length and the radius of the innermost diffraction circle in all of the first region, the second region, the third region, the fourth region, the fifth region, and the sixth region.

[0040] The conductive layer according to the embodiment of the present invention is crystalline having the above-mentioned grain boundaries, as confirmed by a FETEM image of the conductive layer of the conductive particles according to one embodiment of the present invention shown in FIG. 1 taken at a magnification of 500,000 and a diffraction pattern obtained by XRD analysis of the conductive layer shown in FIG. 2, which shows a polycrystalline conductive layer.

[0041] As shown in Figure 1, the grain boundaries with different crystal orientations are observed, confirming the presence of a polycrystalline conductive layer. It is also confirmed that the grain size of the conductive particles is 5.13 to 12.76 nm based on the long axis, with an average of approximately 9.76 nm.

[0042] In addition, Figure 2 shows multiple diffraction circles, which confirm the crystallinity. In this case, the radius of the innermost diffraction circle is within the aforementioned range.

[0043] Meanwhile, according to an embodiment of the present invention, a polycrystalline conductive layer having a small grain size while being a single layer having no interlayer interface containing two or more elements can be achieved by electroless plating in which the element content and reaction rate in the plating layer are adjusted, although the method is not limited thereto.

[0044] For example, in electroless Ni plating, a conductive layer can be formed by Ni-P plating using sodium hypophosphite, Ni-B plating using sodium borohydride (SHB), dimethyl amine borane (DMAB), diethyl amine borane (DEAB), etc., or Ni-N plating using hydrazine, depending on the type of reducing agent. Furthermore, by adding metal salts containing Pd, Pt, W, Au, Ag, Mo, Co, etc., it is possible to perform electroless plating of alloys such as Ni-PW, Ni-BW, Ni-P-Co-W, Ni-B-Co-W, Ni-W, Ni-Co, Ni-Pd, and Ni-P-Pd.

[0045] In the case of electroless plating mainly composed of Ni-P, if the P content is high, an amorphous layer is formed and has excellent corrosion resistance, but the strength is weak and there are problems with high resistance in terms of electrical conductivity (10 μΩcm@20℃ for P, 6.97 μΩcm@20℃ for Ni). Therefore, keeping the P content below 3% is advantageous for the formation of a crystalline material.

[0046] In addition, in the case of electroless plating mainly composed of Ni-B, the resistivity of B (1.5×10^12μΩcm@20℃) is very high, so even if the B content is only a few percent, an amorphous plating layer is formed, so it is advantageous to keep the B content below 0.5% in order to form a crystalline layer.

[0047] Electroless plating with Ni-N as the main component is less corrosion resistant than Ni-P and Ni-B, but when the N content is 2% or less, a conductive layer can be formed in a crystalline state.

[0048] Meanwhile, the conductive layer made of Ni-P, Ni-B, or Ni-N may be used as described above. However, when strength or corrosion resistance is particularly required or other physical properties are required, elements such as Pd, Pt, W, Au, Ag, Mo, and Co may be further included to form a single crystalline plating layer using an alloy electroless plating method.

[0049] In order to form a polycrystalline material with no interlayer boundaries and small crystal grain size, it is necessary to control the reaction rate as well as the element content. The reaction rate is controlled by the amount of reducing agent, the temperature of the plating solution, and the pH.

[0050] If the reaction rate is too slow, an amorphous conductive layer is formed, whereas if the reaction rate is too fast, the balance of the plating solution is lost, making plating unstable or resulting in poor plating quality and making it impossible to commercialize the product.

[0051] The shape of the protrusions of the conductive particles of the present invention is not particularly limited. Spherical, needle-like, polygonal, and other shapes are also possible. The size of the protrusions of the present invention is not particularly limited. The protrusions are preferably convex with a size of 50 nm to 500 nm, and more preferably have a size of 100 to 300 nm.

[0052] The method for forming the protrusions of the conductive particles of the present invention is not particularly limited. For example, a catalytic substance can be applied to the surface of the insulating core particles, and a conductive layer and protrusions can be formed through electroless plating. Small metal or inorganic particles can also be attached to the insulating core particles, and a conductive layer and protrusions can be formed through electroless plating.

[0053] The conductive particles of the present invention preferably have an insulating layer on their outermost surface. As electronic products become smaller and more integrated, the pitch of electrodes becomes smaller, and if there are no insulating particles on the outermost surface, electrical conduction between adjacent electrodes occurs. Methods for forming an insulating layer include a method of chemically attaching insulating particles to the outermost surface of conductive particles using a functional group, a method of dissolving an insulating solution in a solvent and coating by spraying or depositing, and a method of attaching insulating particles to the outermost surface of conductive particles and coating by applying hot air and impact.

[0054] It is preferable to apply an anti-rust treatment to the conductive particle conductive layer of the present invention. This is because the anti-rust treatment increases the contact angle with water to improve reliability in a high humidity environment and reduces the performance degradation of the connection member due to impurities dissolving in water. Therefore, a rust inhibitor having hydrophobic properties is generally used. The coating method can be a method of dissolving the rust inhibitor in a solvent and then depositing or spraying the solution.

[0055] The conductive particles of the present invention can be dispersed in a binder resin to produce an anisotropic conductive material, such as an anisotropic conductive paste, an anisotropic conductive film, or an anisotropic conductive sheet.

[0056] The resin binder is not particularly limited. For example, vinyl resins such as styrene, acrylic, and vinyl acetate, thermoplastic resins such as polyolefin and polyamide, and curable resins such as urethane and epoxy. The above resins can be used alone or in combination of two or more. Radical initiators such as BPO (Benzoyl Peroxide), photoinitiators such as TPO (Trimethylbenzoyl Phenylphosphinate), and epoxy latent curing agents such as HX3941HP can be used alone or in combination with the resin for the purpose of polymerization or curing. In addition, other substances can be added to the anisotropic conductive material binder resin within a range that does not hinder the achievement of the object of the present invention. For example, colorants, softeners, heat stabilizers, light stabilizers, antioxidants, inorganic particles, etc.

[0057] The method for producing the anisotropic conductive material is not particularly limited. For example, the conductive particles can be uniformly dispersed in a resin binder to be used as an anisotropic conductive paste, or the anisotropic conductive material can be thinly applied to a release paper to be used as an anisotropic film.

[0058] The connection structure of the present invention is a structure in which circuit boards are connected using conductive particles using the insulating core of the present invention or the anisotropic conductive material of the present invention. For example, it can be used as a method for connecting a display semiconductor chip of a smartphone to a glass substrate that configures a circuit, or a method for connecting μ-LEDs or mini-LEDs to a circuit board. EXAMPLES

[0059] 1) Synthesis of insulating core particles A 3L glass beaker was charged with 1100 g of monomer TMMT (Tetramethylol Methane Tetaacrylate), 400 g of DVB, 15 g of HDDA, and 30 g of Styrene, and then 5 g of initiator BPO was added, followed by treating in a 40 kHz ultrasonic bath for 10 minutes to prepare a first solution. A 5L PP beaker was charged with 3,000 g of deionized water, to which 500 g of a dispersion stabilizer PVP (Polyvinylpyrrolidone)-30K and 200 g of a surfactant Solusol (Dioctyl sulfosuccinate sodium salt) were added and dissolved to prepare a second solution. The first solution and the second solution were placed in a 50 L reactor, and 40,000 g of deionized water was added. The solution was treated with an ultrasonic homogenizer (20 kHz, 600 W) for 90 minutes. The solution was rotated at 120 rpm and heated to 35° C., maintained for 3 hours, and then heated again to 85° C. After the solution reached 85° C., the solution was maintained for 16 hours to perform a polymerization process. The polymerized particles were filtered, washed, classified, and dried to obtain core resin particles. The average diameter of the produced core resin particles was measured using a mode value measured using a Particle Size Analyzer (BECKMAN MULTISIZER TM3). The number of core particles measured was 75,000. The average diameter was 3.51 μm.

[0060] 2) Formation of an insulating core particle outer conductive layer (1) Catalyst treatment process 30 g of the prepared insulating core particles were placed in a solution of 800 g of deionized water, 0.5 g of surfactant Triton X100, and 10 g of sulfuric acid, and treated in an ultrasonic bath for 1 hour to perform a washing and degreasing process to remove excess unreacted monomers and oil components present in the insulating core particles. At the end of the washing and degreasing process, a water washing process was performed three times using deionized water at 45°C. The insulating core particles that had been through the degreasing and water washing processes were placed in a solution of 150 g of stannous chloride and 300 g of 35-37% hydrochloric acid dissolved in 600 g of deionized water, and were subjected to sensitization treatment by immersion and stirring for 30 minutes at 30°C, and then washed three times with water. The sensitized insulating core was placed in 1 g of palladium chloride, 200 g of 35-37% hydrochloric acid, and 600 g of deionized water, and activated at 40°C for 1 hour. During the activation, ultrasonic waves were applied using an ultrasonic bath. After the activation, the core was washed with water three times. The activated insulating core was placed in a solution of 100 g of 35-37% hydrochloric acid and 600 g of deionized water, and stirred at room temperature for 10 minutes to perform an accelerated treatment. After the accelerated treatment, the core was washed with water three times to obtain a catalytically treated insulating core for electroless plating. (2) Plating process A 5L reactor was charged with 3500g of deionized water, and 70g of nickel sulfate as Ni salt, 5g of sodium acetate as a complexing agent, 2g of lactic acid, 0.001g of Pb-acetate as a stabilizer, 0.001g of sodium thiosulfate, and 1g of PEG-600 as a surfactant were dissolved in this order to produce solution (a). The catalyst-treated insulating core was added to the produced (a) solution, and a dispersion treatment was carried out for 10 minutes using an ultrasonic homogenizer. After the dispersion treatment, the solution pH was adjusted to 8.0 using ammonia water - solution (b). A solution (c) was prepared by dissolving 300 g of deionized water, 33 g of DMAB as a reducing agent, and 0.002 g of sodium thiosulfate as a stabilizer in a 1 L beaker. A solution (d) was prepared by dissolving 500 g of deionized water, 155 g of nickel sulfate, and 10 g of sodium hydroxide in a 1 L beaker. While maintaining the temperature of the solution (b) in the 5 L reactor at 20° C., the solution (c) was added at a rate of 5 g per minute using a metering pump, and the temperature of the reactor was heated to reach and maintained at 35° C. at a heating rate of 0.33° C. / min. The pH of the solution (b) in the 5 L reactor was adjusted to 8.0 by further adding aqueous ammonia until the solution temperature reached 35°C, and no aqueous ammonia was added after 75°C. The solution (c) was added, and 5 minutes later, solution (d) was added to the 5 L reactor at a rate of 20 g per minute using a metering pump. After the addition of the solution (c) was completed, the solution was maintained for 30 minutes to obtain Ni-plated conductive particles. EXAMPLES

[0061] The preparation was carried out in the same manner as in Example 1, except that 3 g of potassium gold cyanide was added to solution (d). EXAMPLES

[0062] A 5L reactor was charged with 2500g of deionized water, and 70g of nickel sulfate as Ni salt, 5g of sodium acetate as a complexing agent, 2g of lactic acid, 0.001g of Pb-acetate as a stabilizer, 0.001g of sodium thiosulfate, and 1g of PEG-600 as a surfactant were dissolved in that order to prepare solution (a). The catalyst-treated insulating core was added to the prepared solution (a) and subjected to a dispersion treatment for 10 minutes using an ultrasonic homogenizer. After the dispersion treatment, the solution pH was adjusted to 5.5 using ammonia water - solution (b). A solution (c) was prepared by dissolving 500 g of deionized water, 280 g of sodium hypophosphite as a reducing agent, and 0.002 g of sodium thiosulfate as a stabilizer in a 1 L beaker. A solution (d) was prepared by dissolving 500 g of deionized water, 155 g of nickel sulfate, and 5 g of sodium hydroxide in a 1 L beaker. While maintaining the temperature of the solution (b) in the 5 L reactor at 65° C., the solution (c) was added at a rate of 5 g per minute using a metering pump, and the temperature of the reactor was heated to reach 75° C. at a heating rate of 0.33° C. and maintained at that temperature. Ammonia water was further added to adjust the pH of the solution (b) in the 5 L reactor to 5.5 until the solution temperature reached 75°C, after which no ammonia water was added. The solution (c) was added, and 5 minutes later, solution (d) was added to the 5 L reactor at a rate of 20 g per minute using a metering pump. After the addition of the solution (c) was completed, the solution was maintained for 30 minutes to obtain conductive particles having a crystalline Ni-P plating layer formed thereon. EXAMPLES

[0063] The procedure of Example 1 was repeated except that solution (d) was prepared by dissolving 500 g of deionized water, 155 g of nickel sulfate, 10 g of hydrochloric acid, and 0.5 g of palladium chloride (PdCl2). <Experimental Example>

[0064] The conductive particles obtained in Examples 1 to 4 were evaluated. 1) Size measurement of insulating core particles The average diameter of the insulating core particles is a mode value measured using a particle size analyzer (BECKMAN MULTISIZER TM3). At this time, the number of measured conductive particles is 75,000. 2)XRD analysis Table 1 summarizes the radii of the first to fourth diffraction circles measured from the diffraction pattern obtained by XRD (X-ray diffraction-SmatLab) analysis using a Cu target for the conductive layer of the conductive particles. The radius of the diffraction circle was measured by using Digital Micrograph (ver3.42.3048.0) to obtain four diameters passing through the center of one diffraction circle as shown in Figure 3, and then dividing the average of the four diameters by two to obtain the radius (r). The measurement sites of the conductive layer were the first region adjacent to the insulating core, the second region adjacent to the first region, and the third region adjacent to the second region and located on the outermost side. [Table 1] 3) By grain boundary analysis, the lengths of the major axes of the grain boundaries of the above-mentioned Examples 1 to 3 were measured, and the results are summarized in Table 2. [Table 2] 4) Measurement of connection resistance (1) Manufacturing of anisotropic conductive film 2g of naphthalene epoxy resin HP4032D (DIC, product name), 20g of phenoxy resin YP-50 (Tohto Kasei, product name), 25g of acrylic epoxy resin VR-60 (Showa Denko, product name), 22g of heat curing agent HXA-3922HP (Asahi Chemical, product name), and 5g of epoxy silane coupling agent A-187 (Momentive, product name) were thoroughly mixed, and then a mixture with a solid content of 50% was made using toluene as a solvent. The conductive particles were added to the mixture so that the weight ratio was 10%, and then the mixture was mixed for 5 minutes using a rotating mixer under conditions of 400 rpm revolution and 150 rpm rotation to produce an anisotropic conductive paste. The anisotropic conductive paste was used to make a film with a thickness of 20 μm on a release film, and then the film was dried in the air using a hot air drying oven at 75° C. for minutes to produce an anisotropic conductive film with a final thickness of 12 μm. (2) Electrode for resistance measurement The electrodes for resistance measurement were prepared by depositing ITO (Indium Tin Oxide) on a glass substrate to form transparent electrodes, and an FPCB with an electrode width of 20 μm and an electrode interval of 50 μm was prepared. (3) Joining The anisotropic conductive film was cut to a width of 3 mm, and using a bonding jig with a width of 1 mm and a length of 30 mm, it was pressed onto a glass substrate with ITO at 0.2 MPa, 120°C, and 10 seconds, and then an FPCB was placed on top and bonded at 45 MPa, 200°C, and 20 seconds to produce a connection structure. (4) Measurement of initial connection resistance The resistance was measured using the electrodes of the FPCB of the connection structure using an ADCMT 6871E Digital Multimeter 2 probe. (5) Measurement of reliability resistance Reliability Resistance was measured after leaving the device under 85°C and humid conditions for 100 hours. In order to measure the resistance, the connector that had been left for 100 hours was placed in a dry oven at 100° C. for 24 hours to remove residual moisture, and the resistance was measured using an ADCMT 6871E Digital Multimeter 2 probe. The results are summarized in Table 3. The criteria for the initial connection resistance are as follows: OOO: 2Ω or less OO: More than 2Ω but less than 3Ω O: More than 3Ω and less than 5Ω X: Exceeding 5Ω The criteria for the increase in connection resistance after 100 hours of reliability at 85°C are as follows: OOO: 2Ω or less rise OO: Over 2Ω to 4Ω or less O: Over 4Ω to 6Ω or less X: Over 6Ω rise [Table 3]

[0065] The features, structures, effects, etc. exemplified in each of the above-mentioned embodiments can be combined or modified in other embodiments by a person having ordinary skill in the art to which the embodiments belong. Therefore, the contents related to such combinations and modifications should be interpreted as being included in the scope of the present invention.

Claims

1. An insulating core; a conductive layer on the insulating core, the conductive layer comprising at least two elements; Conductive particles, wherein a diffraction pattern obtained by analyzing the conductive layer using XRD shows at least two diffraction circles, and the average length of the major axis of the crystal grains of the conductive layer is 8 nm to 13 nm.

2. The conductive particle according to claim 1 , wherein the conductive layer comprises Ni and at least one element selected from the group consisting of B, P, N, Pd, Pt, W, Au, Ag, Mo and Co.

3. The conductive particle according to claim 1 , wherein the radius of the innermost diffraction circle among the diffraction circles is 4.93 (l / nm)±0.2 (l / nm).

4. 2. The conductive particle according to claim 1, wherein when the conductive layer is divided into a first region adjacent to the insulating core, a second region adjacent to the first region, and a third region adjacent to the second region and located outermost, the conductive layer is a single layer with no boundaries between the first region, the second region, and the third region.

5. The conductive particle according to claim 1 , wherein the conductive layer has a content of an element that varies depending on the region.

6. The conductive particle according to claim 2 , wherein the conductive layer contains at least two elements selected from the group consisting of B, P, N, Pd, Pt, W, Au, Ag, Mo and Co.

7. The conductive particle according to any one of claims 1 to 6, further comprising an insulating layer or insulating particles on a surface of the conductive layer.

8. The conductive particle according to any one of claims 1 to 6, wherein an outermost surface of the conductive layer is subjected to an anti-rust treatment using a hydrophobic anti-rust agent.

9. An anisotropic conductive material comprising the conductive particles according to any one of claims 1 to 8.

10. A connection structure comprising the conductive particles according to any one of claims 1 to 8.

11. An electronic device comprising the conductive particles according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Electroconductive particle, electroconductive material, and connection structure

    JP2021027027A

  • Conductive particles, conducting material, and connection structure

    WO2015037711A1