Anti-pollution items

The pollution prevention article with a specialized coating layer forms a removable salt dome to prevent and easily remove inorganic chloride contaminants, addressing fouling issues and maintaining equipment efficiency.

JP2024544618AActive Publication Date: 2024-12-03LG CHEM LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024531534
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-26
Filing Date
2023-09-26
Publication Date
2024-12-03
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

Existing anti-pollution coatings fail to effectively prevent and easily remove inorganic chloride contaminants like potassium chloride from adhering to the internal surfaces of processing equipment, leading to fouling and reduced operational efficiency.

Method used

A pollution prevention article with an inorganic chloride pollution prevention coating layer that satisfies specific contact angle conditions (80° < REC < 150°, REC/CAH ≥ 2.5, and CAH ≥ 25°) to form a removable salt dome during drying, minimizing surface adhesion and facilitating easy removal.

Benefits of technology

The coating effectively prevents fouling by forming a removable salt dome, ensuring easy detachment of inorganic chloride contaminants without residue, thus maintaining equipment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544618000001_ABST
    Figure 2024544618000001_ABST
Patent Text Reader

Abstract

The present invention relates to a pollution prevention article, and more particularly to a pollution prevention article capable of preventing fouling caused by inorganic chlorides.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [Cross-reference to related applications] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0121583 dated September 26, 2022 and Korean Patent Application No. 10-2023-0129096 dated September 26, 2023, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a pollution prevention article, and more particularly to a pollution prevention article capable of preventing fouling caused by inorganic chlorides. [Background technology]

[0003] Anti-fouling coatings are used industrially on a variety of equipment surfaces to prevent the adhesion or adsorption of contaminants to the surfaces.

[0004] During cement production, chlorine (Cl) dust is generated as a by-product in the process of recycling waste plastic, and recently, due to environmental concerns, a separate chlorine dust treatment facility is being used to extract additional potassium chloride (KCl) from the chlorine dust by-product.

[0005] However, during the chlorine dust treatment process, fouling due to potassium chloride often occurs on the inner surface of the equipment, and when fouling occurs, the process operation rate is significantly reduced.

[0006] Therefore, in order to ensure smooth operation of the process, it is necessary to prevent inorganic chloride contaminants such as potassium chloride from adhering to the inner surfaces of the treatment equipment.

[0007] However, the surface of stainless steel, which is generally used as the base material for such treatment equipment, has high wettability and is prone to adhesion of contaminants due to its characteristics, so it requires periodic cleaning. In addition, there are methods of using super-water-repellent coating or hydrophobic coating to prevent adhesion of contaminants, but even with such coating, it is not easy to prevent or remove inorganic chloride contaminants, and the durability of the coating layer is not high, so the effect does not last long.

[0008] Therefore, research is needed into anti-fouling coating layers that can prevent inorganic chloride contaminants from adhering to the inner surfaces of devices and can easily be removed even if they do adhere. Summary of the Invention [Problem to be solved by the invention]

[0009] In order to solve the above problems, the present invention provides a contamination prevention article including an inorganic chloride contamination prevention coating layer. [Means for solving the problem]

[0010] According to one embodiment of the present invention, there is provided a contamination prevention article comprising a substrate; and an inorganic chloride contamination prevention coating layer provided on at least one surface of the substrate, wherein the inorganic chloride contamination prevention coating layer satisfies the following formulas 1 to 3:

[0011] [Formula 1] 80° <REC<150° [Formula 2] REC / CAH≧2.5 [Formula 3] CAH≧25°

[0012] In the above formulas 1 to 3, REC is the receding contact angle with respect to water (unit: °), CAH is the Contact Angle Hysteresis, which is the difference between the advancing contact angle (unit: °) and the receding contact angle (unit: °) with respect to water. Effect of the Invention

[0013] According to the pollution-preventing article of the present invention, fouling caused by inorganic chlorides can be effectively prevented.

[0014] In particular, it can effectively prevent the fouling phenomenon in which potassium chloride generated in the chlorine dust treatment process, which extracts additional potassium chloride (KCl) from chlorine dust generated as a by-product in the process of recycling waste plastic during cement production, adheres to the inner walls of the treatment device. [Brief description of the drawings]

[0015] [Figure 1] 2 is a schematic diagram illustrating a process in which a salt dome is formed on a surface of an antifouling coating layer according to an embodiment of the present invention; FIG. [Diagram 2] FIG. 2 is a schematic diagram illustrating a cross section of a salt dome according to one embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic diagram showing a process in which a salt dome is not formed on the surface of a coating layer according to a comparative example of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing a process in which a salt dome is not formed on a substrate surface according to a comparative example of the present invention. [Diagram 5] 1 is a photograph of a salt dome according to one embodiment of the present invention (A) and comparative domes (B, C). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another.

[0017] Furthermore, the terminology used in this specification is used only to describe exemplary embodiments and is not intended to limit the present invention.

[0018] A singular expression includes a plural expression unless the context clearly indicates otherwise.

[0019] As used herein, terms such as "comprises," "comprising," or "having" are intended to describe embodied features, numbers, steps, components, or combinations thereof, and do not exclude the presence of one or more other features, numbers, steps, components, combinations thereof, or additional possibilities.

[0020] Additionally, in this specification, when a layer or element is referred to as being formed "on" or "on" another layer or element, this means that the layer or element is formed directly on the layer or element, or that other layers or elements may be additionally formed between layers, on the object, or on the substrate.

[0021] The present invention can be modified in various ways and can have various forms, and the specific embodiments are exemplified and described in detail below. However, it should be understood that the present invention is not limited to the specific disclosed forms, but includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0022] Hereinafter, a contamination prevention article according to one embodiment of the present invention will be described in detail.

[0023] A contamination prevention article according to one embodiment of the present invention includes a substrate; and an inorganic chloride contamination prevention coating layer provided on at least one surface of the substrate, wherein the inorganic chloride contamination prevention coating layer satisfies the following formulas 1 to 3:

[0024] [Formula 1] 80° <REC<150° [Formula 2] REC / CAH≧2.5 [Formula 3] CAH≧25°

[0025] In the above formulas 1 to 3, REC is the receding contact angle with respect to water (unit: °), CAH is the Contact Angle Hysteresis, which is the difference between the advancing contact angle (unit: °) and the receding contact angle (unit: °) with respect to water.

[0026] The term "contact angle" as used herein refers to the angle between the gas / liquid interface of a liquid droplet placed on a solid surface and the solid surface. Such contact angles can be measured by various methods, and in this specification, the contact angle of a liquid droplet was measured by the Sessile Drop Method using a commercial contact angle measuring device (KRUSS, model: DSA-100).

[0027] The contact angle is a measure of the wettability of a surface, with a low contact angle indicating high wettability and a high contact angle indicating low wettability.

[0028] In addition, the term "advancing contact angle" as used herein refers to the maximum contact angle that can be formed without the contact line between the droplet and the surface moving. In actual measurements, it is defined as the contact angle at which the contact line of the droplet starts to move while continuously adding small amounts of water.

[0029] In addition, the term "receding contact angle" as used herein refers to the minimum contact angle that can be formed without the contact line between the droplet and the surface moving. In actual measurement, it can be measured as the angle just before the three-phase (solid / liquid / gas) interface moves as the amount of water is gradually reduced through the needle of the syringe into which the water has been injected.

[0030] In the present specification, the advancing contact angle and the receding contact angle were measured using a water droplet at atmospheric pressure (1 atm) and 25°C.

[0031] In addition, the term "CAH" used herein means contact angle hysteresis, which is the difference between the advancing contact angle and the receding contact angle measured as described above.

[0032] The present inventors have been researching methods for preventing the adhesion of contaminants, particularly inorganic chlorides, to the surface of a substrate or coating layer, and have discovered that when the contact angle of the surface satisfies certain conditions, it is possible to effectively prevent the adhesion of inorganic chloride contaminants while maintaining excellent coating durability, which led to the completion of the present invention.

[0033] More specifically, it was confirmed that when the surface of the coating layer satisfies the contact angle condition of one embodiment of the present invention, even if a solution containing an inorganic chloride such as potassium chloride (KCl) is applied to the surface of the coating layer, it dries in a dome-like shape that is hollow and has a minimized contact area with the surface of the coating layer. This makes it possible to prevent fouling due to inorganic chlorides, and since the dome shape is maintained even after drying, it can be removed as it is, making it very easy to remove contaminants.

[0034] In addition, it was confirmed that a dome is not formed or maintained simply because the coating layer surface is hydrophobic or the contact angle is high, but rather, a dome is formed during drying only when the backward contact angle, contact angle history, and ratio of the backward contact angle to the contact angle history in Equations 1 to 3 according to one embodiment of the present invention satisfy certain conditions.

[0035] As an example, the inorganic chloride stain-preventing coating layer of the present invention satisfies all of the following formulas 1 to 3.

[0036] [Formula 1] 80° <REC<150° [Formula 2] REC / CAH≧2.5 [Formula 3] CAH≧25°

[0037] In the above formulas 1 to 3, REC is the receding contact angle with respect to water (unit: °), CAH is the Contact Angle Hysteresis, which is the difference between the advancing contact angle (unit: °) and the receding contact angle (unit: °) with respect to water.

[0038] The inorganic chloride antifouling coating layer according to one embodiment of the present invention satisfies the above formula 1. That is, the receding contact angle (REC) may be more than 80°, or 85° or more, or 90° or more, 95° or more, or 100° or more, but less than 150°, or 145° or less, or 140° or less, or 135° or less, or 130° or less.

[0039] In addition, the inorganic chloride contamination prevention coating layer according to an embodiment of the present invention satisfies the above formula 2. That is, the ratio of the backward contact angle to the contact angle hysteresis (REC / CAH) may be 2.5 or more, or 2.8 or more, or 3.0 or more, or 3.1 or more, or 3.2 or more, and may be 10 or less, or 9 or less, or 8 or less, or 7 or less, or 6 or less, or 5 or less, or 4 or less, or 3.5 or less.

[0040] In addition, the inorganic chloride contamination prevention coating layer according to one embodiment of the present invention satisfies the above formula 3. That is, the contact angle history (CAH) may be 25° or more, or 26° or more, or 28° or more, and 60° or less, or 50° or less, or 40° or less, or 35° or less, or 32° or less.

[0041] In one embodiment of the present invention, the substrate may be, but is not limited to, stainless steel such as SUS or STS, or glass.

[0042] FIG. 1 is a schematic diagram illustrating a process in which a salt dome is formed on a surface of a coating layer according to an embodiment of the present invention.

[0043] According to one embodiment of the present invention, when the backward contact angle, the contact angle history, and the ratio of the backward contact angle to the contact angle history satisfy the conditions of Equations 1 to 3, an inorganic chloride solution is applied to the surface of a coating layer to form droplets, which are then dried.

[0044] More specifically, referring to Fig. 1, first, as the droplets of inorganic chloride solution attached to the surface of the coating layer are dried, solid salt is generated from the edge along the boundary between the droplet and the air. As the droplets continue to dry, the salt continues to grow along the boundary of the droplet, and the droplets remaining inside are absorbed into the salt dome and evaporated to the outside, eventually forming a salt dome shape that is hollow inside and made of salt.

[0045] On the other hand, when certain conditions of Equations 1 to 3 according to an embodiment of the present invention are satisfied, the formed salt dome maintains its shape on a flat surface, but when the surface is tilted, for example at about 45 degrees, it easily falls off without a strong external force and leaves no residue, making it very easy to remove.

[0046] The inorganic chloride contamination-preventing coating layer of the present invention is not limited to a coating layer of a specific component, and as long as the coating layer simultaneously satisfies the formulas 1 to 3, it can exhibit the effect of being easily removed by forming a salt dome on the coating layer surface during the adhesion and drying process of chlorides, regardless of the structure, components, manufacturing method, etc. of the coating layer.

[0047] If the backward contact angle (REC) with respect to water is less than 80°, the salt or solution inside the droplet tends to remain in contact with the coating layer rather than moving to the outer periphery, and in this process, salt components may remain on the surface of the coating layer when drying. On the other hand, if the REC is too high, over 150°, the droplet dries in an almost spherical shape, and the solution inside the droplet rather than the solution near the surface continues to move to the outer periphery, and the solution near the surface evaporates in the latter half of drying. As a result, salt remains in the part of the droplet that contacts the surface, and a salt dome may not form.

[0048] In addition, if the contact angle hysteresis (CAH) is less than 25°, the interface between the droplet and the surface in the salt dome is not fixed and is prone to moving freely, which allows the droplet interface to gradually move into the salt dome as the droplet dries. As a result, the size of the dome itself gradually decreases during the drying process and becomes solidified, making it impossible to maintain the shape of the salt dome.

[0049] Therefore, in order for the salt dome shape to be maintained without any residual salt on the coating layer surface, the REC and CAH must each be high above a certain level. However, if the ratio of CAH to REC is too high, the salt dome shape may collapse during the drying process, and ultimately it becomes difficult to maintain the salt dome shape after drying.

[0050] Therefore, the ratio of REC to CAH is also important for the formation and maintenance of the salt dome. When the conditions of Equations 1 to 3 are simultaneously satisfied, the salt dome shape can be maintained during the drying process of the droplets while no salt components remain on the surface of the coating layer.

[0051] Figure 2 is a schematic diagram of a cross-section of a salt dome according to one embodiment of the present invention, where Ro is the outer radius of the salt dome, Ri is the inner radius of the salt dome, and h is the height of the salt dome.

[0052] Referring to Figure 2, the ratio of the dome height to the outer radius (Ro) of the salt dome is 0.5 or more (h / Ro≧0.5), and the free space area at the contact surface between the salt dome and the surface is 50% or more (Ri 2 / Ro 2 ≧0.5), it can be considered that a salt dome as defined in the present invention has been formed.

[0053] In contrast, FIG. 3 is a schematic diagram showing a process in which a salt dome is not formed on the surface of a coating layer according to a comparative example of the present invention, and FIG. 4 is a schematic diagram showing a process in which a salt dome is not formed on the surface of a substrate according to a comparative example of the present invention.

[0054] 3, initially, as in the present invention, a droplet of inorganic chloride solution attached to the surface of a coating layer is dried, salt is generated from the edge along the boundary between the droplet and air. However, if any one or more of the conditions of formulas 1 to 3 according to an embodiment of the present invention is not satisfied, as the droplet continues to dry, a salt dome shape is not formed and an incomplete dome is formed, or the dome shape collapses and salt components remain in a shape that is irregularly attached to the surface.

[0055] Referring to FIG. 4, when droplets of an inorganic chloride solution are applied to a surface with a low contact angle such as SUS, the salt generated during the drying process does not form a dome shape but spreads over the entire surface and adheres strongly, making it difficult to remove and causing fouling.

[0056] FIG. 5 is a photograph of a salt dome according to one embodiment of the present invention (A) and comparative domes (B, C).

[0057] In FIG. 5, (A) is a photograph of a perfectly formed salt dome peeled off from a surface according to one embodiment of the present invention, (B) is a photograph of an incompletely formed dome, and (C) is a photograph of chloride that has spread and adhered to the surface without the dome forming.

[0058] An inorganic chloride contamination prevention coating layer satisfying the above-mentioned characteristics may include, but is not limited to, a first coating layer including a cured product of alkyl-trialkoxysilane and tetraalkoxysilane; and a second coating layer formed on the first coating layer and including a cured product of fluorinated polyether silane.

[0059] The alkyl-trialkoxysilane may be a compound represented by the following formula 1:

[0060] [Chemical formula 1] R 11 -Si(R 12 )(R 13 )(R14 )

[0061] In the above chemical formula 1, R 11 is an alkyl group having 1 to 5 carbon atoms, R 12 ~R 14 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0062] According to one embodiment of the present invention, the tetraalkoxysilane may be a compound represented by the following formula 2:

[0063] [Chemical formula 2] Si(R 21 )(R 22 )(R 23 )(R 24 )

[0064] In the above chemical formula 2, R 21 ~R 24 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0065] According to one embodiment of the invention, the first coating liquid may contain 1 to 50 parts by weight of tetraalkoxysilane based on 100 parts by weight of alkyl-trialkoxysilane.

[0066] According to one embodiment of the invention, the first coating liquid may contain 1 to 10 parts by weight of an organic acid based on 100 parts by weight of an alkyl-trialkoxysilane.

[0067] According to one embodiment of the present invention, the fluorinated polyether silane may be a compound containing a moiety represented by the following chemical formulas 3-1 to 3-4.

[0068] [Chemical formula 3-1] CF3- [Chemical formula 3-2] -CF2-CF2-O- [Chemical formula 3-3] -CF2-CF2-CF2-O- [Chemical formula 3-4] -Si(R 31 )(R 32 )(R 33 )

[0069] In the above chemical formula 3-4, R 31 ~R 33 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0070] According to one embodiment of the invention, the curing of the first coating liquid and the curing of the second coating liquid can be carried out independently at a temperature condition of 100 to 150°C.

[0071] According to one embodiment of the invention, the cured thickness of the first coating layer may be about 0.1 to about 100 μm, more preferably about 1 to about 50 μm, or about 2 to about 10 μm. When the cured thickness of the first coating layer is within the above range, it is possible to prevent cracks from occurring while exhibiting an appropriate coating hardness.

[0072] The cured thickness of the second coating layer may be about 1 to about 100 nm, or about 5 to about 50 nm. Specifically, the second coating layer may be in a state where the fluorinated polyether silane contained in the second coating liquid is applied almost as a mono-molecule layer. When the cured thickness of the second coating layer is in the above range, a uniform coating layer and an appropriate surface energy level can be maintained.

[0073] According to one aspect of the present invention, the optical film can be formed by a method including the steps of: applying a first coating liquid containing an alkyl-trialkoxysilane, a tetraalkoxysilane, and an organic acid; curing the applied first coating liquid to form a first coating layer; applying a second coating liquid containing a fluorinated polyether silane on the first coating layer; and curing the applied second coating liquid to form a second coating layer.

[0074] In a method according to one embodiment of the present invention, a first coating liquid containing an alkyl-trialkoxysilane, a tetraalkoxysilane, and an organic acid is first applied to a surface of a substrate.

[0075] According to one embodiment of the present invention, the alkyl-trialkoxysilane may be a compound represented by the following formula 1:

[0076] [Chemical formula 1] R 11 -Si(R 12 )(R 13 )(R 14 )

[0077] In the above chemical formula 1, R 11 is an alkyl group having 1 to 5 carbon atoms, R 12 ~R 14 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0078] More specifically, the R 11 may be methyl, ethyl, propyl, butyl, or pentyl and may be straight or branched chain.

[0079] R 12 ~R 14 Each may independently be methoxy, ethoxy, propoxy, butoxy, or pentoxy and may be straight or branched chain.

[0080] Specifically, for example, the alkyl-trialkoxysilane may be one or more selected from the group consisting of methyl-trimethoxysilane, methyl-triethoxysilane, methyl-tripropoxysilane, methyl-tributoxysilane, methyl-tripentoxysilane, ethyl-trimethoxysilane, ethyl-triethoxysilane, ethyl-trippropoxysilane, ethyl-tributoxysilane, ethyl-tripentoxysilane, propyl-trimethoxysilane, propyl-triethoxysilane, propyl-trippropoxysilane, propyl-tributoxysilane, propyl-tripentoxysilane, butyl-trimethoxysilane, butyl-triethoxysilane, butyl-trippropoxysilane, butyl-tributoxysilane, butyl-tripentoxysilane, pentyl-trimethoxysilane, pentyl-triethoxysilane, pentyl-trippropoxysilane, and pentyl-tributoxysilane and pentyl-tripentoxysilane.

[0081] The alkyl-trialkoxysilane is a component that forms the main network of the inorganic coating film through a sol-gel reaction within the composition. At this time, the alkyl group increases the flexibility of the network structure and can relieve stress that occurs during the reaction between silanols or between silanols and the metal oxide layer on the substrate surface. When only alkylsilane is used, the number of silanols participating in the reaction is small, which is disadvantageous in lowering the surface energy during subsequent fluorine coating, and when only alkoxysilane is used, it may be difficult to achieve the above-mentioned stress relief effect.

[0082] According to one embodiment of the present invention, the tetraalkoxysilane may be a compound represented by the following formula 2:

[0083] [Chemical formula 2] Si(R 21 )(R 22 )(R 23 )(R 24 )

[0084] In the above chemical formula 2, R 21 ~R 24 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0085] More specifically, R 21 ~R 24 Each may independently be methoxy, ethoxy, propoxy, butoxy, or pentoxy and may be straight or branched chain.

[0086] Specifically, for example, the tetraalkoxysilane may be one or more selected from the group consisting of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and tetrapentoxysilane.

[0087] The tetraalkoxysilane can increase the number of silanol groups that can participate in the reaction between the silanols or between the silanols and the metal oxide layer on the substrate surface in the composition, which subsequently increases the reactivity with the fluorosilane and helps to realize a surface with low surface energy.

[0088] By mixing alkyl-trialkoxysilane and tetraalkoxysilane in the right ratio, it is possible to prevent the problem of cracks occurring in the entire coating layer network and to provide an appropriate amount of silanol reactive groups on the surface.

[0089] According to one embodiment of the invention, the organic acid may be a carboxylic acid having 1 to 5 carbon atoms.

[0090] Specifically, for example, the organic acid may be one or more selected from the group consisting of formic acid, acetic acid, and propionic acid.

[0091] The organic acids mentioned above act as catalysts to promote the hydrolysis of silane groups within the composition and can play a role in determining the overall network structure. Under low pH acidic conditions, the hydrolysis rate is more rapid than the condensation reaction rate, resulting in the formation of a linear structure through silane bonds. On the other hand, under basic conditions, the condensation reaction rate is faster, resulting in the formation of a particulate structure. Although inorganic acids such as hydrochloric acid can also be used instead of organic acids, organic acids are more useful in controlling the gel time.

[0092] According to one embodiment of the invention, the first coating liquid may contain about 1 to about 50 parts by weight of tetraalkoxysilane based on 100 parts by weight of alkyl-trialkoxysilane.

[0093] The use of tetraalkoxysilanes in the parts by weight as described above can be advantageous in achieving suitable surface energy and excellent adhesion.

[0094] According to one embodiment of the invention, the first coating liquid may contain about 1 to about 10 parts by weight of an organic acid based on 100 parts by weight of an alkyl-trialkoxysilane.

[0095] By using the organic acid in the above-mentioned parts by weight, a linear network structure can be obtained at an appropriate hydrolysis rate, and the mechanical properties of the coating layer can be maintained.

[0096] The pH of the first coating liquid may be about 7 or less, or about 5 or less, or about 3 or less, and may be about 1 or more, or about 2 or more.

[0097] The pH can affect the hydrolysis rate and the condensation reaction rate, and the difference in the rates of these two reactions determines the structure of the coating film and affects the storage stability of the coating solution.

[0098] From this perspective, a stable inorganic coating film can be obtained under acidic conditions having a pH in the aforementioned range.

[0099] The first coating liquid may further include an organic solvent in addition to the above-mentioned components. The organic solvent may specifically include, for example, alcohols or ethers, and the amount of the organic solvent may be appropriately selected in consideration of the coating property and drying after coating.

[0100] When the first coating solution is applied to the surface of the substrate, the coating thickness may be about 0.1 to about 100 μm, more preferably about 1 to about 50 μm, or about 2 to about 10 μm, based on the thickness after drying and curing. When the cured thickness of the first coating layer is within the above range, it is possible to prevent cracks from occurring while exhibiting an appropriate coating hardness.

[0101] The coating method is not particularly limited, and may be selected from methods commonly used in the technical field to which the present invention pertains, such as directly coating with a tool such as a brush, spraying after appropriately adjusting the viscosity, or coating with a bar.

[0102] After coating, drying can be performed at room temperature for about 10 minutes to about 1 hour. Such drying conditions can vary depending on the type and amount of the solvent used.

[0103] After drying, curing can be carried out at a temperature of about 100 to about 150° C. for about 30 minutes to about 2 hours.

[0104] In the curing process, a sol-gel reaction of the alkyl-trialkoxysilane and silane groups in the tetraalkoxysilane compound in the first coating liquid occurs to form the first coating layer.

[0105] According to one embodiment of the present invention, the fluorinated polyether silane may be a compound containing a moiety represented by the following chemical formulas 3-1 to 3-4.

[0106] [Chemical formula 3-1] CF3- [Chemical formula 3-2] -CF2-CF2-O- [Chemical formula 3-3] -CF2-CF2-CF2-O- [Chemical formula 3-4] -Si(R 31 )(R 32 )(R 33 )

[0107] In the above chemical formula 3-4, R 31 ~R 33 each independently represents an alkoxy group having 1 to 5 carbon atoms.

[0108] The fluorinated polyether silane is a compound having a fluorinated carbon at one end, an alkoxysilane group at the other end, and a fluorinated ethoxy or fluorinated propoxy group in the middle, and can form a hard coating layer by directly forming a covalent bond with the first coating layer, and can drastically reduce the surface energy of the coating layer due to the large amount of fluorine chains.

[0109] In the second coating liquid, the fluorinated polyether silane can be used together with an alkoxy fluorinated alkyl solvent.

[0110] The alkoxy fluorinated alkyl solvent used herein may be an ether compound represented by the following chemical formula 4:

[0111] CF3-(CF2) n -O-(CH2) m -CH3

[0112] In the above chemical formula, n and m may each independently be an integer of 1-5.

[0113] The ether compound has an alkyl group that is not substituted with fluorine attached to one side of an oxygen atom at the center, and an alkyl group in which all hydrogen atoms are substituted with fluorine attached to the other side.

[0114] Such an ether compound has excellent compatibility with the above-mentioned fluorinated polyether silane compound, and can disperse the fluorinated polyether silane compound uniformly in the second coating liquid.

[0115] When the second coating liquid is applied to the substrate surface on which the first coating layer is formed, the coating thickness may be about 1 to about 100 nm based on the thickness after drying and curing. Specifically, the second coating layer may be in a state in which the fluorinated polyether silane contained in the second coating liquid is applied almost as a mono-molecule layer. When the cured thickness of the second coating layer is in the above range, a uniform coating layer and an appropriate surface energy level can be maintained.

[0116] The coating method is not particularly limited, and may be selected from methods commonly used in the technical field to which the present invention pertains, such as directly coating with a tool such as a brush, spraying after appropriately adjusting the viscosity, or coating with a bar.

[0117] After coating, drying can be performed at room temperature for about 10 minutes to about 1 hour. Such drying conditions can vary depending on the type and amount of the solvent used.

[0118] After drying, curing can be carried out at a temperature of about 100 to about 150° C. for about 30 minutes to about 2 hours.

[0119] In the curing process, the fluorinated polyether silane in the second coating liquid can form a second coating layer through interaction with the functional groups contained in the first coating layer.

[0120] According to one embodiment of the invention, the first coating layer may have a cured thickness of about 0.1 to about 100 μm.

[0121] The second coating layer may have a cured thickness of about 1 to about 100 nm.

[0122] The inorganic chloride contamination-preventing coating layer provided according to one embodiment of the present invention satisfies the above-mentioned formulas 1 to 3, and when droplets of an inorganic chloride solution are attached, a salt dome shape is formed. Such a salt dome is easy to remove and can prevent surface contamination and fouling caused by inorganic chlorides, thereby providing various articles with excellent contamination prevention effects.

[0123] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention. However, these examples are presented only as examples of the present invention and do not define the scope of the invention. EXAMPLES

[0124] <Example> Example 1 First coating liquid Five parts by weight of methyl-trimethoxysilane was used as the alkyl-trialkoxysilane component, one part by weight of tetraethoxysilane was used as the tetraalkoxysilane component, and four parts by weight of a 6 wt% acetic acid solution diluted in water was used as the organic acid component, and these were mixed together (pH about 2.3).

[0125] 100 parts by weight of the coating liquid was diluted with about 50 parts by weight of isopropyl alcohol as a solvent to prepare a first coating liquid.

[0126] Second coating liquid As the fluorinated polyether silane component, Optool-DSX, a perfluoropolyether silane from Daikin, was used by dissolving it in the solvent Novec-7200 from 3M at a concentration of 1 wt %.

[0127] Formation of inorganic chloride anti-fouling coating layer The first coating liquid was applied to the surface of a stainless steel substrate (Stainless steel 316, 10 cm x 10 cm) using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130°C for about 1 hour to form a first coating layer with a thickness of about 5 μm.

[0128] The second coating solution was again applied thereto using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130° C. for about 1 hour to form a second coating layer with a thickness of about 10 nm.

[0129] Example 2 An inorganic chloride contamination prevention coating layer was formed in the same manner as in Example 1, except that the second coating solution in Example 1 was prepared by dissolving Optool-DSX, a perfluoropolyether-silane manufactured by Daikin, in a solvent, Novec-7200 manufactured by 3M, at a concentration of 0.1 wt%.

[0130] Comparative Example 1 Comparative Example 1 was prepared by using only the substrate made of the same stainless steel material as in Example 1.

[0131] Comparative Example 2 After thoroughly washing the slide glass with isopropyl alcohol and acetone, the slide glass was completely dried, and then 20 cst silicone oil (DMS-T12, Gelest) was applied to the front of the slide glass using a brush. The slide glass was then stood vertically for about an hour to remove excess oil on the surface, and then reacted at 130°C for 24 hours. The silicone oil remaining after the reaction was washed away with isopropyl alcohol and acetone.

[0132] Comparative Example 3 Using Sylgard 184 Elastomer Kit (Dow Corning), 10 parts by weight of base and 1 part by weight of hardener were mixed, and air bubbles were removed.The mixture was poured into a Petri dish to a thickness of 5 mm and then cured in an oven at 70°C for 3 hours.

[0133] Comparative Example 4 A super water-repellent coating was produced using Neverwet Spray (Rust-Oleum Corporation), a commercial super water-repellent coating product. Neverwet Base Coating was applied to the SUS substrate as a first coat and then dried at room temperature for 1 hour. Neverwet Top Coating was applied on top of the first coat and then dried at 70℃ for 1 hour.

[0134] Comparative Example 5 The S.PDMS1 solution according to Example 7 of Korean Patent Publication No. 2015-0033725 was prepared and coated onto a stainless steel substrate (Stainless steel 316, 10 cm x 10 cm), and then cured at 120°C for 3 hours.

[0135] Comparative Example 6 90.9 parts by weight of Dow's Sylgard 184 silicone elastomer kit base resin and 9.1 parts by weight of Dow's Sylgard 184 silicone elastomer kit crosslinker were mixed to remove air bubbles, and the mixture was applied to the surface of a stainless steel substrate (Stainless steel 316, 10 cm x 10 cm) and cured at 120°C for 3 hours.

[0136] Comparative Example 7 45 parts by weight of Dow's Sylgard 184 silicone elastomer kit base resin, 4.5 parts by weight of Dow's Sylgard 184 silicone elastomer kit crosslinker, and 50.5 parts by weight of silicone oil (Gelest, product name: DMS-T11) were mixed to remove air bubbles. This was applied to the surface of a stainless steel substrate (Stainless steel 316, 10 cm x 10 cm) and cured at 120°C for 3 hours.

[0137] Comparative Example 8 The sample prepared in Comparative Example 7 was immersed in DMS-T11 (Mw: 1,250 g / mol) silicone oil at room temperature for 24 hours, and then removed and stood upright for 30 minutes to remove residual oil from the surface.

[0138] [Table 1]

[0139] In Table 1, ADV is the advancing contact angle (unit: °) with water at a temperature of 25°C, REC is the receding contact angle (unit: °) with water at a temperature of 25°C, and CAH is the contact angle hysteresis, which is the difference between the advancing contact angle (unit: °) and the receding contact angle (unit: °) with water at a temperature of 25°C.

[0140] <Experimental Example> (1) Presence or absence of salt dome formation 400g of KCl (99.0%, Tokuyama Pharmaceutical Co., Ltd.) was completely dissolved in 1kg of distilled water at 80℃, then cooled to room temperature of 25℃, and the remaining solution after KCl precipitation was used as KCl saturated solution. For KCl salt dome evaluation, 50μL of KCl saturated solution was dropped onto 10 different points on the sample surface with a pipette. After drying in an oven at 60℃ for 12 hours, the salt dome morphology was confirmed.

[0141] After drying, the ratio of the dome height to the outer radius (Ro) must be 0.5 or more (h / Ro ≥ 0.5) and the area of ​​open space at the contact surface between the salt dome and the surface must be 50% or more (Ri 2 / Ro 2 We observed whether a salt dome with a mean surface area of ​​0.5 or greater was formed.

[0142] Cases where a salt dome that satisfied the above conditions was formed were rated as O, and cases where a dome was formed but an incomplete salt dome that did not satisfy the above conditions was formed, or where chlorides were spread and attached to the surface without a dome shape were rated as X.

[0143] (2) Presence or absence of salt dome or chloride deposits (1) After observing the formation of salt domes, the surface was tilted so that the angle between the surface and the ground was 45°, and the number of salt domes (or chloride deposits if no salt domes were formed) that fell off from the surface was counted and evaluated as follows:

[0144] O: Four or more salt domes or deposits △: Salt dome or deposits are present (1-3 or less). X: The salt dome or all of the deposits fall off.

[0145] (3)Residues (2) After evaluating the presence or absence of salt dome adhesion, if there was no residue visible to the naked eye on the surface of the salt dome or the area where the adhesion had fallen off, it was rated as X, and if there was residue remaining, it was rated as O.

[0146] (4) Scratch resistance For the coating layer surfaces of the Examples and Comparative Examples, potassium chloride was applied between the two substrate surfaces by unit area (cm 2 After increasing the load by 0.1g, the load becomes 1000N / m 2 The load was applied and the sample was subjected to 100 reciprocating movements of 1 cm. After the scratch test, if no scratches were observed on the surface by the naked eye, the sample was rated as O, and if scratches were observed, the sample was rated as X.

[0147] [Table 2]

[0148] Referring to Table 2, in Examples 1 and 2, which satisfy all of the prescribed formulas 1 to 3 for the coating layer surface, salt domes were formed as the chlorides attached to the surface dried, and the formed salt domes easily fell off without excessive external force, leaving no residue, and it was evaluated that the effect of preventing contamination by chlorides was very excellent.

[0149] On the other hand, in the comparative examples that did not satisfy any one or more of the formulas 1 to 3, no salt dome was formed under the same conditions as in the examples (Comparative Examples 1 to 8), or deposits remained on the surface (Comparative Examples 1, 4 to 8), and there was almost no effect in preventing contamination by chlorides.

Claims

1. A substrate; and an inorganic chloride fouling prevention coating layer provided on at least one surface of the substrate; The inorganic chloride anti-fouling coating layer satisfies the following formulas 1 to 3, the anti-fouling article: [Formula 1] 80°<REC<150° [Formula 2] REC / CAH≧2.5 [Formula 3] CAH≧25° In the above formulas 1 to 3, REC is the receding contact angle (unit: °) with respect to water; CAH is the contact angle hysteresis, which is the difference between the advancing contact angle (unit: °) and the receding contact angle (unit: °) with respect to water.

2. 2. The contamination prevention article according to claim 1, wherein REC / CAH in formula 2 is 10 or less.

3. 2. The contamination prevention article of claim 1, wherein REC in Formula 1 is 85° or greater.

4. 2. The contamination prevention article of claim 1, wherein the CAH in formula 3 is 60° or less.

5. The contamination control article of claim 1 , wherein the inorganic chloride comprises potassium chloride (KCl).

6. The inorganic chloride antifouling coating layer is a first coating layer comprising a cured product of an alkyl-trialkoxysilane and a tetraalkoxysilane; and The contamination control article of claim 1 , further comprising a second coating layer formed on the first coating layer, the second coating layer comprising a cured product of a fluorinated polyether silane.

7. The contamination prevention article according to claim 6, wherein the alkyl-trialkoxysilane is a compound represented by the following chemical formula 1: [Chemical formula 1] R 11 -Si(R 12 )(R 13 )(R 14 ) In the above chemical formula 1, R 11 is an alkyl group having 1 to 5 carbon atoms, R 12 ~R 14 each independently represents an alkoxy group having 1 to 5 carbon atoms.

8. The contamination prevention article according to claim 6, wherein the tetraalkoxysilane is a compound represented by the following chemical formula 2: [Chemical formula 2] Si(R 21 )(R 22 )(R 23 )(R 24 ) In the above chemical formula 2, R 21 ~R 24 each independently represents an alkoxy group having 1 to 5 carbon atoms.

9. The contamination prevention article according to claim 6, wherein the fluorinated polyether silane is a compound having a group represented by the following chemical formulas 3-1 to 3-4: [Chemical formula 3-1] CF 3 - [Chemical formula 3-2] -CF 2 -CF 2 -O- [Chemical formula 3-3] -CF 2 -CF 2 -CF 2 -O- [Chemical formula 3-4] -Si(R 31 )(R 32 )(R 33 ) In the above chemical formula 3-4, R 31 ~R 33 each independently represents an alkoxy group having 1 to 5 carbon atoms.

10. The contamination control article of claim 1 , wherein the substrate is stainless steel.

Citation Information

Patent Citations

  • Perfluoropolyether benzotriazole derivatives and their use as coatings

    JP2007523894A

  • Perfluoropolyether coating composition for hard surfaces

    JP2013506750A

  • Surface treatment process for optical devices and antifouling articles manufactured thereby

    JP2014502210A

  • Hydrophobic hydrocarbon coatings

    JP2014522744A

  • Easy-to-clean article with stainless steel surface and method of making the same

    US20100129672A1