Selective acid leaching of mixed hydroxide precipitates.
The use of peroxymonosulfuric acid in an acidic leaching solution effectively separates nickel and cobalt from mixed hydroxide precipitates, enhancing recovery rates and reducing impurity sensitivity.
Patent Information
- Application Number
- JP2024527260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-12
- Filing Date
- 2022-11-10
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for recovering nickel and cobalt from mixed hydroxide precipitates are energy-intensive, require multiple processing steps, and suffer from incomplete separation and cross-contamination, especially when dealing with impurities like iron and chromium.
A process involving the use of peroxymonosulfuric acid in an acidic leaching solution to selectively dissolve nickel from mixed hydroxide precipitates, allowing for at least 75% of nickel to be dissolved in the leachate and at least 90% of cobalt to be recovered in the solid phase.
Achieves high recovery rates of nickel and cobalt with minimal cross-contamination, eliminating the need for additional neutralizing agents and reducing the number of processing steps, while being less sensitive to impurities.
Smart Images

Figure 2024544881000005 
Figure 2024544881000006 
Figure 2024544881000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for the recovery of metals from raw materials, and in particular to the selective recovery of nickel directly from mixed hydroxide precipitates containing nickel, cobalt and optionally manganese. [Background technology]
[0002] Today, the number of electric vehicles (EVs) is increasing. The current main battery power storage technology for EVs is the lithium-ion battery (LIB). In LIBs, lithium ions move from the negative or anode (mainly made from carbon, e.g. graphite) through an electrolyte to the positive electrode (cathode) during discharge and reverse during charging. Chemistry, performance, cost and safety characteristics vary between different types of LIBs. Electronic games often use lithium cobalt oxide (LiCoO) as the cathode material, which provides high energy density but presents safety risks, especially if damaged. 2 ) (using polymer gel as electrolyte) is used. 4 ), Lithium-ion manganese oxide battery (LiMn 2 O 4 , Li 2 MnO 3 or LMO) and lithium nickel manganese cobalt oxide (LiNiMnCoO 2 Neutralized MC (Non-Metal Capacitor-Coated or NMC) offers lower energy density, but longer life span and lower chance of fire or explosion. In particular, NMC is leading the way in automotive applications, i.e. EVs. The cathode used in NMC batteries is, for example, a combination of nickel:manganese:cobalt in a weight ratio of 8:1:1 (hence the name NMC 811).
[0003] Although more nickel will be needed to meet the demand for LIBs in the near future, most of the nickel in the global supply chain is not actually suitable for battery production.
[0004] The predominant source of nickel is sulfide or laterite deposits. Large high-grade sulfide deposits are becoming increasingly rare, so that processing of laterite ores is predicted to become the major source of the metal.
[0005] A common method of processing laterite ores is to leach the solids in acid. Acid leaching is generally followed by impurity precipitation, which is generally accomplished by adding limestone. After impurity precipitation, both nickel and cobalt are usually recovered from the aqueous solution by mixed sulfide precipitation (MSP) or mixed hydroxide precipitation (MHP). MHP is a relatively recent large-scale industrial technique that is accomplished by adding basic chemicals such as magnesia, lime, limestone or sodium hydroxide to the leach solution. MHP consists mostly of nickel hydroxide, but also contains valuable cobalt hydroxide, possibly manganese and various other impurities. MHP represents a more valuable concentrated product, as the approximately 1% nickel and 0.1% cobalt present in the original laterite ore are significantly upgraded in terms of their relative amounts in MHP.
[0006] Because MHP has such high valuable metals content, it is increasingly viable to operate centralized nickel and cobalt smelters, as the shipping costs of the upgraded intermediate products would be a fraction of the cost of shipping the as-mined ore.
[0007] MHP can be further processed in several ways. For example, MHP can be added to the melt of an iron smelting furnace to alloy the nickel contained with the iron. This process is not suitable for MHP with significant cobalt content, as the valuable cobalt is not recovered and therefore economically unviable.
[0008] Another major processing route for refining MHP is by leaching the material in an ammonia / ammonium carbonate solution, as described, for example, in US 2007 / 0166214. Nickel and cobalt dissolve in the ammonia solution to form an ammonia complex. This solution is further processed in a Caron-type process to recover the nickel and cobalt. Using this process, several process steps are required to recover the nickel and / or cobalt.
[0009] WO 2010 / 118455 relates to a process in which MHP is treated with two acidic solutions to extract nickel and / or cobalt from the MHP. In this process, an additional solvent extraction step is required to remove impurities from the solution containing dissolved nickel and / or cobalt. Nickel and / or cobalt are then recovered from the solution by electrowinning or a hydrogen reduction step.
[0010] Such prior art approaches are generally relatively energy intensive, or do not result in optimal nickel and / or cobalt recovery, or require an excessive number of processing steps, or are sensitive to the presence of other impurities such as aluminum, iron and chromium. A need exists for improved methods of recovering nickel from nickel-containing ores. It would be desirable to provide a process for the direct separation of nickel from cobalt in MHP and that allows for the efficient recovery of both valuable products.
[0011] US 2016 / 0355906 relates to a process for selectively leaching nickel from MHP while retaining cobalt in the leach residue solids by using sodium persulfate or potassium permanganate as oxidants, but even in this process nickel-cobalt separation is not complete and there is significant cross-contamination of these two metals. Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention aims to overcome one or more of the problems or disadvantages identified in the prior art literature. [Means for solving the problem]
[0013] The present invention relates to a process for selectively leaching nickel from a mixed hydroxide precipitate (MHP) by contacting the MHP with an acidic leach solution and peroxymonosulfuric acid to dissolve at least 75% by weight of the nickel in the leach solution and recover at least 90% by weight of the cobalt in the solid phase, based on the total amounts of nickel and cobalt present in the MHP, respectively.
[0014] The present invention also relates to a process for selectively leaching nickel from a mixed hydroxide precipitate (MHP) by contacting the MHP with a composition consisting essentially of an acidic leach solution and peroxymonosulfuric acid at a temperature between 30°C and 80°C. [Brief description of the drawings]
[0015] [Figure 1] The results of Examples 1 and 2 are shown. [Diagram 2] When peroxymonosulfate (CA) is used as the oxidant (see Example 1), less cobalt is recovered in the acidic leach solution, i.e. more cobalt is recovered in the solid phase compared to the use of persulfate as the oxidant (see Example 2). [Diagram 3] The results of Examples 3 and 4 are shown. [Figure 4] The results of Examples 3 and 4 are shown. [Diagram 5] The results of Example 5 are shown. [Figure 6] The results of Example 5 are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Before describing the current formulations of the present invention, it is to be understood that the present invention is not limited to the particular formulations described, since such formulations may, of course, vary. It is also to be understood that the terminology used herein is not intended to be limiting, since the scope of the present invention is limited only by the appended claims.
[0017] As used herein, the terms "comprising", "including" and "composed" are synonymous with "including", "including" or "containing", "containing" and are inclusive or open-ended and do not exclude additional, unrecited elements, components or method steps. As used herein, the terms "comprising", "including" and "composed" are understood to include the terms "consisting of", "comprising" and "consisting of".
[0018] Throughout this application, the term "about" is used to indicate that a value includes the standard deviation of error for the device or method being employed to determine the value.
[0019] As used herein, the terms "weight-%", "wt.-%", "weight percentage" or "percent by weight" are used interchangeably.
[0020] The recitation of numerical ranges by endpoints includes all integers and, where appropriate, fractions subsumed within that range (e.g., "1 to 5" can include 1, 2, 3, 4, for example, when referring to the number of elements, and can also include 1.5, 2, 2.75, and 3.80, for example, when referring to measurements). The recitation of endpoints also includes the endpoint values themselves (e.g., 1.0 to 5.0 includes both 1.0 and 5.0). Any numerical range recited herein is intended to include all subranges subsumed therein.
[0021] All references cited herein are incorporated by reference in their entirety. Specifically, the teachings of all references mentioned individually herein are incorporated by reference.
[0022] Unless otherwise defined, all terms used in the disclosure of the present invention, including technical and scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. For further guidance, definitions of terms are included to better understand the teachings of the present invention.
[0023] In the following sections, various alternatives, embodiments and variants of the present invention are defined in more detail. Each alternative and embodiment thus defined may be combined with any other alternative and embodiment and each variant, unless expressly indicated otherwise or clearly indicated as incompatible when the ranges of values of the same parameter are in isolation. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.
[0024] Furthermore, in one or more embodiments, the particular features, structures or characteristics described herein may be combined in any suitable manner, as would be apparent to one of ordinary skill in the art from this disclosure. In addition, while some embodiments described herein include some features that are included in other embodiments but do not include other features, it is contemplated that combinations of features from different embodiments are within the scope of the invention and may result in different embodiments, as would be apparent to one of ordinary skill in the art.
[0025] The present invention relates to a process by which nickel can be directly and selectively leached from mixed hydroxide precipitates (MHPs).
[0026] The term "mixed hydroxide precipitate" or "MHP" as used herein refers to a mixed nickel-cobalt hydroxide precipitate, preferably solid. Such precipitates are commonly known as intermediate products in the commercial processing of nickel-containing ores. The precipitates typically contain various nickel, cobalt and optionally manganese compounds, including oxides and hydroxides. It is to be understood that references herein to "nickel", "cobalt" or "manganese" with respect to the separation may be taken as references to one or more of these compounds, including oxides and hydroxides of the metals. Nickel and cobalt are generally at higher concentrations in MHP than in the original mined ore corresponding to the source material. Typically, MHPs used in the present invention contain 34-55% nickel, 1-4.5% cobalt and optionally 1-7% manganese by weight based on the total weight of the anhydrous MHP.
[0027] Surprisingly, it has been found that by treating MHP with an acidic leach solution and peroxymonosulfuric acid according to the invention, nickel dissolves in the acidic solution, and cobalt and, if present, manganese can be almost completely recovered in the solid phase as precipitates. The recovery of cobalt in the solid phase by using the process of the invention is stable, i.e. does not result in dissolution of the precipitated cobalt, as opposed to nickel, after treatment of MHP with an acidic leach solution and peroxymonosulfuric acid. The solid phase generally contains Co as the main constituent. 3 O 4 , Co 2 O 3 and CoOOH. The solid phase contains unreacted Ni(OH) 2 and NiOOH. When manganese is present in the MHP, it can also be almost completely recovered in the solid phase, which contains manganese oxide MnO as the main manganese constituent. 2 Also contains
[0028] According to the invention, the MHP is contacted with an acidic leach solution and peroxymonosulfuric acid such that at least 75% by weight of the nickel is dissolved in the leach solution and at least 90% by weight of the cobalt is recovered in the solid phase, based on the total amount of nickel and cobalt present in the MHP, respectively. It is preferred that the MHP is contacted with an acidic leach solution and peroxymonosulfuric acid such that at least 80% by weight of the nickel is dissolved in the acidic leach solution, more preferably at least 85% by weight, and even more preferably at least 90% by weight, based on the total amount of nickel present in the MHP. It is further preferred that at least 95% by weight, at least 98% by weight, and more preferably 99% by weight, of the cobalt can be recovered in the solid phase, based on the total amount of cobalt present in the MHP.
[0029] According to another embodiment of the invention, nickel is selectively leached from the MHP by contacting the MHP with a composition consisting essentially of an acidic leach solution and peroxymonosulfuric acid at a temperature between 30° C. and 80° C.
[0030] The acidic leach solution used in the process of the present invention is an aqueous acidic leach solution. Preferably, the acid of the acidic leach solution is sulfuric acid (H 2 SO 4 ) or any suitable strong acid capable of achieving adequate dissolution of nickel. Further examples of acids that may be suitable include nitric acid, hydrochloric acid and other strong mineral acids. Alternatively, the acid of the acidic leach solution may be peroxymonosulfuric acid. Best results are obtained when the acid is sulfuric acid or peroxymonosulfuric acid.
[0031] In the process of the invention, the mixed hydroxide precipitate contains nickel, cobalt and optionally manganese. Typically, the nickel is dissolved and the cobalt is recovered in the solid phase, and if manganese is present in the MHP, the manganese is also recovered in the solid phase.
[0032] It is further preferred that the acidic leach solution has an initial acid concentration (preferably initial sulfuric acid concentration) in the process of about 0.5 wt%, about 1.0 wt% or more, preferably about 5.0 wt% or more, more preferably about 10 wt% or more. The acidic leach solution generally has an initial acid concentration (preferably initial sulfuric acid concentration) of about 30 wt% or less, preferably about 20 wt% or less. Preferably, the acidic leach solution used in the process of the present invention has an initial acid concentration (preferably initial sulfuric acid concentration) of 1.0 wt% to 20 wt%, 2.0 to 15.0 wt%, more preferably 3.0 to 10.0 wt% or even more preferably 5.5 to 7.0 wt%.
[0033] According to the invention, the MHP can be contacted with a pre-prepared acid leach solution as defined above, or in a first step, water is added to the MHP and then an acid is added to this mixture of MHP and water to form an acid leach solution in an amount to obtain an acid leach solution having the initial concentration in the process of the invention as defined above. The acid added to the mixture of MHP and water can be a highly concentrated acid, i.e. the acid is an aqueous acid solution having an acid concentration of 93-98%, preferably 95-98%, or an aqueous acid solution having an acid concentration high enough to obtain an acid leach solution having the initial concentration in the process of the invention as defined above.
[0034] The term "acid leach solution" as used herein refers to a prepared acid leach solution or a solution obtained by adding water to MHP and then adding acid to the mixture of water and MHP. This is typically an aqueous acid leach solution.
[0035] The term "leachate" as used herein refers to the solution obtained after contacting MHP with an acidic leach solution and peroxymonosulfuric acid. The leachate solution contains dissolved nickel, unconsumed acid, if present, unconsumed peroxymonosulfuric acid, if present, and in most cases water.
[0036] Peroxymonosulfate (H2 SO 5 ) is also known as persulfuric acid, peroxysulfuric acid or Caro's acid. The IUPAC name for peroxymonosulfuric acid is (dioxidanido)hydroxydioxidosulfur.
[0037] Peroxymonosulfuric acid, preferably the peroxymonosulfuric acid solution used in the process of the present invention, contains hydrogen peroxide (H 2 O 2 ) to sulfuric acid (H 2 SO 5 ) H 2 O 2 +H 2 SO 4 ⇔H 2 SO 5 +H 2 O formula 1
[0038] According to the invention, the peroxymonosulfuric acid (solution) used in the process preferably contains not more than 1 mole of hydrogen peroxide per 8 moles of peroxymonosulfuric acid. Preferably, the molar ratio of peroxymonosulfuric acid to hydrogen peroxide is greater than 8:1, more preferably 10:1, even more preferably 12:1.
[0039] Sulfuric acid (H) to generate peroxymonosulfuric acid 2 SO 4 ) and hydrogen (H 2 O 2 ) is more preferably from 3:1 to 8:1, more preferably from 4:1 to 6:1. Preferably, the peroxymonosulfuric acid solution used in the process of the present invention has a concentration of from 5 to 20% by weight, preferably from 8 to 12% by weight, based on the total amount of peroxymonosulfuric acid solution used in the process.
[0040] Peroxymonosulfuric acid acts as an oxidizing agent in this process, i.e., it is a reagent that can increase the oxidation state of a substrate, e.g., lose electrons (thereby reducing itself in this process). 2+) and cobalt (Co 2+ ) and optionally manganese (Mn 2+ The divalent ions of cobalt (Co(II)) have different abilities to be oxidized. According to the present invention, peroxymonosulfuric acid oxidizes dissolved divalent cobalt (Co(II)) to trivalent cobalt (Co(III)), which precipitates (see Equation 2). H 2 SO 5 +2Co 2+ 5H 2 O → 2Co(OH) 3 +H 2 SO 4 +4H + formula 2 H 2 SO 5 +Mn 2 +H 2 O→MnO 2 +H 2 SO 4 +2H + formula 3
[0041] The process of the invention may be carried out such that the MHP is contacted first with an acidic leach solution and subsequently with peroxymonosulfuric acid to at least partially dissolve the nickel, at least partially dissolve and then precipitate the cobalt, and at least partially oxidize and precipitate manganese, if present, to a solid phase. The term "subsequently" as used in this context means after the entire amount of the acidic leach solution has been contacted with the MHP or after a portion of the total amount of the acidic leach solution used in the process of the invention has been added to the MHP.
[0042] Alternatively, the MHP may be contacted with an acidic leach solution and peroxymonosulfuric acid simultaneously to at least partially dissolve the nickel and at least partially dissolve the cobalt, e.g., Co. 3 O 4 , Co 2 O 3 or CoOOH, and manganese, if present, is at least partially oxidized and precipitated, for example, in MnO 2In a first embodiment of this alternative, the acidic leach solution is different from the peroxymonosulfate solution. In a second embodiment, the acidic leach solution is the same as the peroxymonosulfate solution. In this case, all of the acid is present in the peroxymonosulfate solution as sulfuric acid and no acid is added separately.
[0043] In yet another alternative, the MHP is contacted first with peroxymonosulfuric acid and subsequently with an acidic leach solution to at least partially dissolve the nickel and leave the cobalt and manganese, if present, in the solid phase.
[0044] It is further preferred that the amount of acidic leach solution and / or peroxymonosulfuric acid used in the process of the present invention is added continuously to the MHP. The continuous addition of the acidic leach solution can be carried out such that in a first step water is added to the MHP and then to this mixture an acid is added to form the acidic leach solution, resulting in an acidic leach solution as defined above. In another embodiment, a pre-prepared acidic leach solution as defined above is added continuously to the MHP. In a further preferred embodiment, peroxymonosulfuric acid is added continuously to the mixture of the MHP and the acidic leach solution.
[0045] The term "continuously" or "continuously" as used herein means that the total amount of acidic leach solution and / or peroxymonosulfuric acid is added to the MHP in small portions (preferably at most 1% or less than 1% by weight, respectively, of the total amount of acidic leach solution and / or peroxymonosulfuric acid used in the process), preferably at equally spaced times throughout a given period or in a continuous stream. Typically, the period during which the acidic leach solution and / or peroxymonosulfuric acid is continuously added to the MHP is at least 30 minutes, specifically at least 1 hour. Typically, this period is at most 8 hours, specifically at most 6 hours, more specifically at most 4 hours, sometimes at most 3 hours, and sometimes at most 2 hours. A preferred period is between 30 minutes and 4 hours.
[0046] When the components, i.e., the acidic leach solution and / or peroxymonosulfuric acid, are added to the MHP in small amounts at equally spaced times throughout a given period of time, the components are preferably added to the MHP in about 5 to about 12 portions, about 6 to about 10 portions, or more preferably about 6 to about 8 portions, at intervals of about 5 to about 40 minutes, more preferably about 10 to about 30 minutes.
[0047] In a further preferred embodiment of the invention, the components are added to the MHP in a continuous infusion rate, preferably 0.1-1.0 ml / min at laboratory scale, 0.2-0.9 ml / min at laboratory scale or 0.3-0.8 ml / min at laboratory scale, more preferably 0.4-0.6 ml / min at laboratory scale. For industrial scale, as known in the art, this infusion rate has to be adjusted accordingly.
[0048] In a more preferred embodiment, the total amount of peroxymonosulfuric acid used in the process is added to the mixture of MHP and acidic leach solution at a laboratory scale continuous injection rate of 0.7-0.9 ml / min. Further, it is preferred that the peroxymonosulfuric acid is added to the mixture of MHP and acidic leach solution over a period of 1.0-2.5 hours, more preferably 1.5-2.0 hours.
[0049] It has been found that in many cases, the cobalt is first leached by the acid of the acid leach solution and begins to precipitate as the peroxymonosulfuric acid is injected, while the nickel dissolves continuously as the peroxymonosulfuric acid is injected.
[0050] The total amount of acidic leach solution and peroxymonosulfuric acid used in the process depends on the amount of nickel, cobalt and optionally manganese present in the MHP, in other words, the amount of metal dissolution and precipitation can be controlled by the amount of acidic leach solution and peroxymonosulfuric acid used in the process, respectively.
[0051] It is preferred that the molar ratio of the acid, i.e. the acid of the acidic leach solution in combination with the sulfuric acid generated during this process, in particular by the reaction of the cobalt ions and, if present, the manganese ions with peroxymonosulfuric acid (see equations 2 and 3), to the dissolved nickel is between 0.6 and 0.9, more preferably between 0.7 and 0.85.
[0052] In this process, the nickel hydroxide (Ni(OH)) present in MHP is reduced by using a smaller stoichiometric amount of acid. 2 ) acts as a neutralizing agent. In that case, no additional neutralizing agent needs to be used in the process to control the pH of the contacting step of the process.
[0053] In the present invention, the molar ratio of peroxymonosulfuric acid to the cobalt recovered is preferably at least 0.7, particularly at least 1.0, more particularly at least 1.5. This molar ratio is usually at most 6.0, often at most 5.0, particularly at most 4.0, more particularly at most 3.0. Good results are obtained with a ratio between 0.7 and 3.0.
[0054] Furthermore, the process of the present invention should be carried out at an appropriate pH to ensure that nickel is dissolved in the acidic leach solution and that cobalt and optionally manganese are recovered in the solid phase in the desired amounts. Preferably, according to the present invention, the pH during the contacting step is between 2 and 7, specifically between 3 and 6, more specifically between 3.5 and 5. The pH value of the liquid present during the contacting step is determined by methods commonly used in the art. One possible method is to use a VWR, pHenomenal® 111 pH electrode, a 3-in-1 pH probe equipped with sensors for pH and ORP.
[0055] The process according to the invention is preferably carried out at a temperature of 30 to 80° C., particularly 35 to 65° C., more particularly 40 to 55° C. Depending on the reaction conditions, the heat of reaction may be sufficient to reach the required temperature range without additional heating.
[0056] It is further preferred that the MHP is present in a stoichiometric (%) amount of from 100% to about 40%, from about 90% to about 50%, and more preferably from about 85% to about 60% compared to the amount of acid in the acidic acid solution.
[0057] Preferably, the solutions, i.e. the acidic acid solution in contact with the MHP and the acidic acid and peroxymonosulphuric acid solutions, are stirred during the process of the present invention or are agitated separately under mechanical conditions in vessels / reactors normally used in metal leaching processes. One advantage of doing this is to minimise as much as possible local differences in temperature due to the introduction of the acidic leach solution and peroxymonosulphuric acid to the MHP, as such differences would result in reduced performance manifested by increased peroxymonosulphuric acid or higher residual levels of undissolved nickel.
[0058] The process is preferably carried out at atmospheric pressure.
[0059] The MHP used in the process of the invention may contain, in addition to nickel and cobalt, a manganese compound. The process of the invention may have the same effect on manganese as described for cobalt.
[0060] According to the invention, the nickel dissolved in the acidic leach solution can be recovered directly from said solution. Alternatively, after the contacting step, in a first further step, the leach solution containing a high concentration of dissolved nickel is separated from a solid phase containing precipitated cobalt and optionally manganese, in a second further step, the cobalt and / or manganese, if present, is separated from the solid phase, and in a third further step, the nickel is recovered from the leach solution by various suitable means known in the art. In particular, nickel can be recovered from the leach solution by means including electrowinning of nickel metal, hydrogen reduction to nickel metal or crystallization to nickel sulfate hydrate. The process may further comprise a step of separating cobalt and manganese solids, if present in the MHP, by selective dissolution of cobalt or manganese in an acidic or alkaline ammonia-containing solution, as described, for example, in US Patent Publication No. 2016 / 0355906.
[0061] In the process according to the invention, the solid phase recovered at the end of the process may be subjected to at least one further contact with a leach fluid in order to recover the nickel remaining in the solid phase. The leach fluid used in this further contact step may be the same as the acidic leach solution and peroxymonosulphuric acid used in the first contact step. It may also be different or any kind of known leach fluid. The operating conditions of the further contact step may be the same or different from those of the first contact step.
[0062] By using the process of the present invention and / or by using an oxidizing agent other than peroxymonosulfuric acid, separation of nickel from cobalt and optionally manganese in MHP is surprisingly effective and offers distinct advantages over certain prior art approaches which instead attempt to selectively precipitate cobalt and optionally manganese from a solution containing both nickel and cobalt and optionally manganese.
[0063] The present invention is further illustrated by the following examples. It should be understood that the following examples are for illustrative purposes only and are not used to limit the present invention thereto. EXAMPLES
[0064] Example 1 (according to the invention) In Example 1, Ni(OH) 2 , Co(OH) 2 Peroxymonosulfuric acid was continuously injected into the reactor containing sulfuric acid at a laboratory scale continuous flow injection rate of 0.8 ml / min.
[0065] Ni(OH) 2 was present in the reactor in an amount of 38 g, and the molar ratio of nickel to cobalt (Ni:Co) was 1:0.05. The slurry concentration present in the reactor was 10 wt.%. The molar ratio of sulfuric acid to hydrogen peroxide (H ) to produce peroxymonosulfuric acid was 1:0.05. 2 SO 4 :H 2 O 2 ) was 5:1, and the concentration of peroxymonosulfuric acid in the solution used in this reaction was 10%. Taking into account the additional sulfuric acid produced during the reaction according to Equation 2, the molar ratio of peroxymonosulfuric acid to cobalt was 3, and the molar ratio of sulfuric acid to nickel was 0.85.
[0066] The mixture present in the reactor was stirred at 300 rpm, the reaction temperature was 45° C. and the pH was greater than 4. No neutralizing agent was used to control the pH of the solution during the reaction, utilizing a VWR, pHenomenal® 111 pH electrode, 3-in-1 pH measurement probe equipped with sensors for pH and ORP.
[0067] Example 2 (Comparative Example) In Example 2, MHP was first treated with persulfate (Na 2 S 2 O 8 After 30 minutes of reaction, the sulfuric acid solution was then injected.
[0068] Ni(OH) 2 was present in the reactor in an amount of 38 g, and the molar ratio of nickel to cobalt (Ni:Co) was 1:0.05. The slurry concentration present in the reactor was 10 wt. %. Considering that additional sulfuric acid is produced during the reaction of sodium persulfate with cobalt, the molar ratio of sodium persulfate to cobalt (Na 2 S 2 O 8 The molar ratio of sulfuric acid to nickel (H 2 SO 4 :Ni) was 0.83.
[0069] The mixture present in the reactor was stirred at 300 rpm and the reaction temperature was 60°C.
[0070] result As can be seen from Figure 1, in Example 1, cobalt is first leached by sulfuric acid and starts to precipitate when peroxymonosulfuric acid (Caro's acid, CA) is injected. Nickel dissolves continuously with the injection of Caro's acid.
[0071] In Example 2, the sulfuric acid leached out the nickel while keeping the cobalt in the precipitation (see Figure 1).
[0072] The graph in Figure 2 shows that when peroxymonosulfate (CA) is used as the oxidant (see Example 1), less cobalt is recovered in the acidic leach solution, i.e. more cobalt is recovered in the solid phase compared to the use of persulfate as the oxidant (see Example 2).
[0073] [Table 1]
[0074] Thus, the use of peroxymonosulfuric acid results in selective acid leaching of MHP to produce a cobalt-free nickel sulfate solution without the addition of neutralizing agents.
[0075] Examples 3 and 4 (Nickel / Cobalt / Manganese) In Example 3, Ni(OH) suspended in water 2 , Co(OH) 2 and MnSO 4 Peroxymonosulfuric acid was continuously injected into the reactor containing the above in a continuous flow at an injection rate of 0.8 ml / min.
[0076] Ni(OH) 2 was present in the reactor in an amount of 38 g, the molar ratio of nickel to cobalt (Ni:Co) was 1:0.05, and the molar ratio of nickel to manganese (Ni:Mn) was 1:0.05. The slurry concentration present in the reactor was 10 wt. %. The molar ratio of sulfuric acid to hydrogen peroxide (H ) to produce peroxymonosulfuric acid was 10 wt. %. 2 SO 4 :H 2 O 2 The molar ratio of peroxymonosulfuric acid to cobalt and manganese (H 2 SO 5 :Co+Mn) was 3 and no addition of sulfuric acid was performed.
[0077] The mixture present in the reactor was stirred at 300 rpm, the reaction temperature was 70° C., and the pH was greater than 4. No neutralizing agent was used to control the pH of the solution during the reaction. A VWR, pHenomenal® 111 pH electrode, 3-in-1 pH measurement probe equipped with sensors for pH and ORP was utilized.
[0078] Example 4 was exactly like Example 3, with the addition of sulfuric acid starting 30 minutes after the last drop of peroxymonosulfuric acid was added, while maintaining the pH above 4.
[0079] The results of Examples 3 and 4 are shown in Figure 3. As can be seen from Figure 3, in Example 3, manganese dissolved in water and precipitated with the addition of peroxymonosulfuric acid. Cobalt partially dissolved and then precipitated with the addition of peroxymonosulfuric acid. Nickel dissolved continuously with the injection of peroxymonosulfuric acid. In Example 4, the dropwise addition of sulfuric acid while maintaining a pH above 4 (Figure 4) allowed for additional dissolution of nickel while maintaining cobalt and manganese in the solid phase.
[0080] [Table 2]
[0081] Example 5 (MHP sample) In Example 5, peroxymonosulfuric acid was continuously injected into a reactor containing a sample of MHP suspended in water at a continuous flow injection rate of 0.8 ml / min.
[0082] The MHP sample contained 47% moisture by weight and the following composition (by weight):
[0083] [Table 3]
[0084] The MHP sample was present in the reactor in an amount of 60 g, and the slurry concentration present in the reactor was 10 wt%. The molar ratio of sulfuric acid to hydrogen peroxide to produce peroxymonosulfuric acid (H 2 SO 4 :H 2 O 2 ) was 5:1, the peroxymonosulfuric acid concentration of the solution used in this reaction was 10% by weight, and the sulfuric acid concentration of the solution used in this reaction was 42% by weight.
[0085] The mixture present in the reactor was stirred at 300 rpm, the reaction temperature was 70° C., and peroxymonosulfuric acid was continuously injected until the pH was 2 (FIG. 6). No neutralizing agent was used to control the pH of the solution during the reaction. A VWR, pHenomenal® 111 pH electrode, 3-in-1 pH measurement probe equipped with sensors for pH and ORP was used.
[0086] The results of Example 5 are shown in Figure 5, which demonstrates the dissolution of nickel from MHP into solution over time and with the addition of peroxymonosulfuric acid.
[0087] [Table 4]
Claims
1. 1. A process for selectively leaching nickel from a mixed hydroxide precipitate by contacting the mixed hydroxide precipitate with an acidic leach solution and peroxymonosulfuric acid to dissolve at least 75% by weight of the nickel in the leach solution and to recover at least 90% by weight of the cobalt in a solid phase, based on the total amounts of nickel and cobalt present in the mixed hydroxide precipitate, respectively.
2. A process for selectively leaching nickel from a mixed hydroxide precipitate by contacting said mixed hydroxide precipitate with a composition consisting essentially of an acidic leach solution and peroxymonosulfuric acid at a temperature between 30°C and 80°C.
3. 3. The process of claim 1 or 2, wherein the mixed hydroxide precipitate contains nickel, cobalt and optionally manganese, the nickel being dissolved and the cobalt being recovered in a solid phase, and manganese, if present in the mixed hydroxide precipitate, also being recovered in the solid phase.
4. 4. The process of any one of claims 1 to 3, wherein the mixed hydroxide precipitate is contacted first with the acidic leach solution and subsequently with the peroxymonosulphuric acid to at least partially dissolve nickel, at least partially dissolve and then precipitate cobalt, and at least partially oxidize and precipitate manganese, if present; or the mixed hydroxide precipitate is contacted simultaneously with the acidic leach solution and peroxymonosulphuric acid to at least partially dissolve nickel, at least partially oxidize and precipitate cobalt, and at least partially oxidize and precipitate manganese, if present; or the mixed hydroxide precipitate is contacted first with the peroxymonosulphuric acid and subsequently with the acidic leach solution to at least partially dissolve nickel and leave cobalt and manganese, if present, in the solid phase.
5. 5. The process according to any one of claims 1 to 4, wherein the solid phase recovered at the end of the process is subjected to at least one further contact with a leach fluid in order to recover the nickel remaining in the solid phase.
6. The process according to any one of claims 1 to 5, wherein the acid in the acidic leach solution is peroxymonosulfuric acid or sulfuric acid.
7. A process as claimed in any one of claims 1 to 6, wherein the acidic leach solution and / or the peroxymonosulfuric acid are added to the mixed hydroxide precipitate during a period of from 30 minutes to 4 hours.
8. The process according to any one of claims 1 to 7, wherein the contacting step of the process is carried out at a pH of from 2 to 7, preferably from 3.5 to 5.
9. 9. The process of any one of claims 1 to 8, wherein no additional neutralizing agent is used to control the pH of the contacting step of the process.
10. 10. The process of any one of claims 1 to 9, wherein the peroxymonosulfuric acid contains no more than 1 mole of hydrogen peroxide per 8 moles of peroxymonosulfuric acid.
11. 11. A process as claimed in any one of the preceding claims, wherein the molar ratio of the total amount of acid in the acidic leach solution and the additional sulphuric acid produced during the process to the nickel dissolved in the process by reaction of peroxymonosulphuric acid with cobalt ions is from 0.6 to 0.
9.
12. 12. The process of any one of claims 1 to 11, wherein the molar ratio of peroxymonosulfuric acid to recovered cobalt is from 0.7 to 3.
13. The process according to any one of claims 1 to 12, carried out at a temperature of from 30 to 80°C.
14. 14. The process according to any one of claims 1 to 13, wherein after the contacting step, in a first further step, the solid phase is separated from the leach solution containing dissolved nickel, in a second further step the cobalt and / or the manganese, if present, are separated from the solid phase, and in a third further step the nickel is recovered from the leach solution.
15. A process as claimed in any one of the preceding claims, wherein the nickel is recovered from the leach solution by electrowinning, hydrogen reduction or crystallisation.
Citation Information
Patent Citations
Method for recovering nickel, cobalt, iron, manganese and magnesium from oxidized nickel ore
CN102041381A
Improved methods for processing ore
JP2014504677A
Methods for producing cobalt and related oxides from various raw materials
JP2020523482A
How to recycle Li-ion batteries
JP2022552492A
Nickel-cobalt separation
US2977221A