Cold-rolled steel sheet and galvanized steel sheet with excellent press formability, and manufacturing method thereof

The cold-rolled steel sheet with controlled MnS and BN precipitates and optimized alloy content addresses press formability issues, ensuring high strength and minimal defects through a specific manufacturing process, enhancing the performance of appliance parts.

JP2024545506AInactive Publication Date: 2024-12-09POHANG IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024534504
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2022-12-16
Publication Date
2024-12-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cold-rolled and galvanized steel sheets used in appliance parts face issues with press formability, leading to defects like cracks and reduced strength due to complex forming methods and ultra-low carbon content complications.

Method used

A cold-rolled steel sheet composition of 0.010 to 0.025% C, 0.10 to 0.25% Mn, 0.002 to 0.011% S, 0.0006 to 0.0026% B, 0.0010 to 0.0034% N, 0.006 to 0.028% Al, with controlled precipitates of MnS and BN, and a yield strength of 150 to 220 MPa, along with a manufacturing process involving reheating, hot rolling, cold rolling, and annealing.

Benefits of technology

The solution ensures high strength and excellent press formability with minimized defects, achieving a yield strength of 150 to 220 MPa and an elongation rate of 35 to 48%, while optimizing alloy content for economic efficiency and preventing surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545506000001_ABST
    Figure 2024545506000001_ABST
Patent Text Reader

Abstract

A cold-rolled steel sheet according to one embodiment of the present invention may contain, by weight%, 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), the balance being Fe and unavoidable impurities, and may contain precipitates of at least one of MnS and BN, the average grain size of the precipitates being 40 to 250 nm, the area fraction of the precipitates in the cold-rolled steel sheet being 1 to 10%, and the yield strength being 150 to 220 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to steel sheets for use in components and frames of electronic products, and more particularly to a cold-rolled steel sheet and a galvanized steel sheet having excellent press workability, and a method for producing the same. [Background technology]

[0002] Materials used for home appliance parts, such as refrigerator doors, washing machine frames, and TV back panels, are low-carbon steels with a carbon content of 200 to 400 ppm, and are generally pressed to form embossed parts, bent parts, etc. The material thus formed must have a certain level of strength as it plays a role in supporting the product, and must have high formability for integral molding.

[0003] Recently, the materials for the parts of the home appliances have been made thinner, and more complicated forming methods are being applied compared to the past, which has raised forming problems such as cracks occurring during forming of the existing low carbon steel materials or distortion occurring after forming.To solve these problems, there is a need to develop steel materials with excellent formability.

[0004] One method proposed to meet the above requirements is to secure both strength and formability by using solid solution strengthening and precipitation strengthening of ultra-low carbon elements such as manganese (Mn), silicon (Si), phosphorus (P), and titanium (Ti) with a carbon content of 40ppm or less, but this complicates the manufacturing process, causing problems with the competitiveness of the material cost.In addition, various surface defects occur during product production, so there is a strong demand for a method to improve press formability using existing low carbon systems that are not ultra-low carbon systems. Summary of the Invention [Problem to be solved by the invention]

[0005] The technical problem to be solved by the present invention is to provide a cold-rolled steel sheet which is excellent in press workability, does not suffer from defects such as cracks during forming, and has high strength.

[0006] Another technical problem to be solved by the present invention is to provide a zinc-plated steel sheet having the above-mentioned advantages.

[0007] Another technical problem to be solved by the present invention is to provide a method for manufacturing the cold rolled steel sheet and the galvanized steel sheet having the above advantages. [Means for solving the problem]

[0008] A cold-rolled steel sheet according to one embodiment of the present invention may contain, by weight, 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), the balance being Fe and unavoidable impurities, and may contain precipitates of at least one of MnS and BN, the area fraction of the precipitates in the cold-rolled steel sheet being 1 to 10%, and the yield strength being 150 to 220 MPa.

[0009] In one embodiment, the cold rolled steel sheet may satisfy the following formula 1:

[0010] <Expression 1> 100,000×min([B] / 10.8, [N] / 14)>9.25 (In the above formula 1, min(a, b) means the smaller value of a and b, and [B] and [N] mean the contents (wt%) of B and N.)

[0011] In one embodiment, the cold rolled steel sheet may satisfy the following formula 2:

[0012] <Expression 2> ([N]-1.3×[B])×9.643<0.015 (In the above formula 2, [B] and [N] mean the contents (wt%) of B and N.)

[0013] In one embodiment, the cold rolled steel sheet may satisfy the following formula 3:

[0014] <Expression 3> 0 <T MnS -T BN <100 (In the above formula 3, T BN is 573,198 × min([B] / 10.8, [N] / 14) + 1142, where min(a, b) is the smaller of a and b, and T MnS means 15000 × [S] + 1170, and [B], [N], and [S] mean the contents of B, N, and S (wt%).

[0015] In one embodiment, the precipitates may have an average grain size of 40 to 250 nm. In one embodiment, the ferrite may have an average grain size of 10 to 40 μm. In one embodiment, the cold rolled steel sheet may have an elongation of 35 to 48%.

[0016] A galvanized steel sheet according to another embodiment of the present invention may be obtained by subjecting the above-mentioned cold-rolled steel sheet to hot-dip galvanizing.

[0017] A method for producing a cold rolled steel sheet according to another embodiment of the present invention includes the steps of: (a) forming a slab containing, by weight, 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), the balance being Fe and unavoidable impurities, by 1 The method may include the steps of reheating the slab at a temperature of 100°C or more and less than 1,250°C, hot rolling the heated slab to produce a hot rolled steel sheet, coiling the hot rolled steel sheet at a coiling temperature in the range of 450 to 700°C, cold rolling the coiled hot rolled steel sheet to produce a cold rolled steel sheet, annealing the cold rolled steel sheet, and temper rolling the cold rolled steel sheet at a rolling reduction ratio of more than 0.5 and less than 1.5%. In one embodiment, the slab may be heated to 1,200°C or more in the step of heating the slab.

[0018] In one embodiment, in the step of producing the hot-rolled steel sheet, the finish rolling temperature is Ar 3 In one embodiment, the step of producing the cold-rolled steel sheet may include cold rolling at a rolling reduction of 50 to 95% to produce the cold-rolled steel sheet. In one embodiment, after the step of producing the cold-rolled steel sheet, the method may further include a step of plating a surface of the cold-rolled steel sheet with zinc. Effect of the Invention

[0019] According to an embodiment of the present invention, the cold-rolled steel sheet is obtained by minimizing the aluminum content in the steel and controlling the contents of essential components such as boron and nitrogen, thereby ensuring high strength and elongation, and at the same time, obtaining an extremely thin cold-rolled steel sheet with excellent workability and free of surface defects, and suppressing the occurrence of defects in bending portions during bending.

[0020] The galvanized steel sheet according to another embodiment of the present invention may have the above-mentioned advantages.

[0021] The method for manufacturing a cold-rolled steel sheet and a galvanized steel sheet according to another embodiment of the present invention can have the above-mentioned advantages. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 shows composite precipitates of MnS and BN according to one embodiment of the present invention. [Diagram 2] FIG. 2 shows the grain size with and without the compositional content range according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a graph showing changes in BN and MnS precipitation temperatures in response to changes in sulfur (S) content according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below can be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.

[0024] The terminology used herein is merely to refer to particular embodiments and is not intended to limit the invention. As used herein, the singular forms include the plural forms unless the text clearly indicates otherwise. As used herein, the meaning of "comprising" embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.

[0025] When an element is referred to as being "on" or "on" another element, it means that it is immediately on or above the other element, or there may be other elements in between. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.

[0026] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted as having a meaning consistent with the relevant technical literature and the currently disclosed content, and are not interpreted as ideal or very formal unless otherwise defined.

[0027] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.

[0028] In an embodiment of the present invention, the term "additionally contain an additional element" refers to the additional amount of the additional element replacing the remaining iron (Fe).

[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0030] A cold rolled steel sheet according to one embodiment of the present invention contains, by weight, 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), with the balance being Fe and unavoidable impurities.

[0031] The reasons for limiting the alloy components are explained below.

[0032] C: 0.010 to 0.025% by weight Carbon (C) is an element that dissolves in steel and advantageously improves strength. The carbon content is, for example, from 0.020% by weight onwards, carbides are precipitated in the steel. Therefore, as the C content increases in the range of 0.010 to 0.025% by weight, specifically, in the range of 0.011 to 0.024% by weight, a range is created in which the properties of the steel change.

[0033] If the carbon content is too low, the amount of C dissolved in the steel is small, which reduces the effect of solid solution strengthening and reduces the strength of the steel.If the carbon content is too high, solid solution strengthening restarts after the maximum precipitation of carbides, which increases the strength excessively and may increase the aging index.

[0034] Mn: 0.10 to 0.25% by weight Manganese (Mn) is an element that plays a role in improving the strength of steel through solid solution strengthening in steel and combines with sulfur (S) to form MnS precipitates. The manganese (Mn) content may be 0.10 to 0.25 wt %. Specifically, the manganese content may be 0.12 to 0.24 wt %.

[0035] In the present invention, the manganese is preferably added in an amount of 0.10% by weight or more in order to ensure strength due to the manganese. If the manganese content is excessively high, a central segregation zone is formed, which may cause defects during hot rolling, and excessively coarse MnS precipitates are formed, which makes it difficult to expect a composite precipitation effect with BN precipitates described later, and may result in a decrease in the strength of the steel material.

[0036] S: 0.002 to 0.011% by weight Sulfur (S) is an element that forms MnS precipitates together with manganese (Mn). It is contained in a relatively small amount compared to manganese, and in the precipitation of MnS, the S content can dominate the total MnS content. The manganese content may be 0.002 to 0.011 wt%. Specifically, the manganese content may be 0.003 to 0.010 wt% (30 to 100 ppm).

[0037] If the sulfur content is too low, the MnS precipitates cannot be sufficiently formed, making it difficult to expect a composite precipitation effect with the BN precipitates, and the precipitation temperature can be below 1,200° C., which is the average heating temperature of the present invention. If the sulfur content is too high, the precipitation start temperature becomes too high, making it difficult to expect a composite precipitation effect with the BN precipitates.

[0038] B: 0.0006 to 0.0026% by weight Boron (B) is an element that reacts with nitrogen (N) in steel to form BN precipitates, and has the effect of reducing the amount of dissolved nitrogen in steel and of forming coarse final crystal grains. The boron content may be 0.0006 to 0.0026 wt%. Specifically, the boron content may be 0.0011 to 0.0025 wt%.

[0039] If the boron content is too low, not only is the amount of BN precipitates formed very small, but the precipitation temperature of the BN precipitates is below 1,200°C, and the BN formed in the hot rolling step in the heating temperature section is redissolved, which may reduce the effect of reducing grain boundary pinning. If the boron content is too high, it is highly likely that boron will combine with N in the steel and segregate to the grain boundaries of the remaining B to exist as free boron, which may cause problems such as scabs during steelmaking and continuous casting, and may ultimately have the adverse effect of excessively increasing strength by segregating to the grain boundaries of the steel.

[0040] N: 0.0010 to 0.0034% by weight Nitrogen (N) is an element that reacts with boron (B) to form BN precipitates. The nitrogen content may be 0.0010 to 0.0034% by weight. Specifically, the nitrogen content may be 0.0014 to 0.0030% by weight.

[0041] If the nitrogen content is too low, the amount of BN that can precipitate decreases, which may make it difficult to achieve the coarse BN precipitation effect of the present invention, whereas if the nitrogen content is too high, BN precipitates are formed and the remaining nitrogen exists in a solid solution state, which may cause the strength of the steel to be excessively improved and increase the aging index.

[0042] Al: 0.006 to 0.028% by weight Aluminum (Al) is an element added for deoxidizing effect. The content of the aluminum may be 0.006 to 0.028 wt%. Specifically, the content of the aluminum may be 0.010 to 0.028 wt%. If the content of the aluminum is too low, the deoxidizing ability may decrease and inclusion defects may be formed by combining with compositions such as manganese (Mn) and calcium (Ca).

[0043] The aluminum is dissolved with nitrogen (N) and can be added for the purpose of inducing the formation of AlN at a low temperature to prevent aging. In the case of the nitrogen, in the present invention, since it is partially removed in the form of BN by utilizing the boron, it is not necessary to add a large amount of aluminum (Al) as in the case of general cold-rolled steel sheets. Even if only the aluminum within the aluminum content range is added, it is possible to minimize the amount of dissolved nitrogen that causes aging.

[0044] The present invention can reduce the yield strength of the steel material used in press forming, increase ductility, and ensure excellent press workability by eliminating expensive elements such as Nb, Ti, P, and Mn, and optimizing the contents of alloy elements such as B, Mn, and S, which are relatively low-valence elements. Specifically, Nb and Ti may each be contained at 0.01% by weight or less, P may be contained at 0.015% by weight or less, and Mn may be contained at 0.025% by weight or less.

[0045] In one embodiment, the cold rolled steel sheet includes iron (Fe) as the balance. Inevitable impurities may also be included. Inevitable impurities refer to impurities that are inevitably mixed in during the steelmaking and manufacturing process of the cold rolled steel sheet. Since unavoidable impurities are widely known, a detailed description will be omitted. In one embodiment of the present invention, the addition of elements other than the above-mentioned alloy components is not excluded, and various elements may be included within a range that does not impair the technical concept of the present invention. When an additional element is further included, the remaining Fe is replaced with the additional element.

[0046] A cold-rolled steel sheet according to one embodiment of the present invention satisfies the following formula 1.

[0047] <Expression 1> 100,000×min([B] / 10.8, [N] / 14)>9.25 (In the above formula 1, min(a, b) means the smaller value of a and b.)

[0048] In one embodiment, the value of the formula 1 may be greater than 9.25. Specifically, the value of the formula 1 may be greater than 9.8 and less than 19.3. In one embodiment, the formula 1 may mean the minimum boron (B) and nitrogen (N) contents at which the precipitates become coarse and the precipitation temperature is higher than the heating temperature. The formula 1 relates to the minimum boron (B) and nitrogen (N) contents at which BN precipitates are formed to form coarse precipitates and thereby control the yield strength low. The boron and the nitrogen are in contact in an atomic state, so the atomic ratio may be, for example, 1:1. However, when some of the atoms are present in greater amounts, some of the other atoms present in smaller amounts may determine the amount of BN precipitates and the precipitation temperature.

[0049] A cold rolled steel sheet according to one embodiment of the present invention satisfies the following formula 2.

[0050] <Expression 2> ([N]-1.3×[B])×9.643<0.015 (In the above formula 2, [B] and [N] mean the contents (wt%) of B and N.)

[0051] In one embodiment, the value of the formula 2 may be less than 0.015. Specifically, the value of the formula 2 may be less than 0.009. More specifically, the value of the formula 2 may be greater than -0.02 and less than 0.006. The formula 2 ([N]-1.3 x [B]) x 9.643 relates to the minimum Al content required for nitrogen (N) scavenging. Specifically, when the nitrogen is not scavenged (e.g., cannot be removed) by boron (B) and the atomic ratio of the nitrogen is higher, the aluminum is designed not to exceed 0.015 wt%, which is the minimum lower limit for the aluminum to act as a deoxidizer. In one embodiment, the cold-rolled steel sheet satisfies the formula 2, and the aluminum (Al) content can be controlled to be low, thereby providing an economical cold-rolled steel sheet.

[0052] The cold rolled steel sheet according to one embodiment of the present invention satisfies the following formula 3.

[0053] <Expression 3> 0 <T MnS -T BN <100 (In the above formula 3, T BN is 573,198 × min([B] / 10.8, [N] / 14) + 1142, where min(a, b) is the smaller of a and b, and T MnS means 15000 × [S] + 1170, and [B], [N], and [S] mean the contents of B, N, and S (wt%).

[0054] In the above equation 3, T BN is the precipitation temperature of BN, T MnS indicates the precipitation temperature of MnS, and the principle of the formation of the coarse precipitates contained in the cold rolled steel sheet is based on the fact that the precipitation temperature of MnS and the onset point of the precipitation temperature of BN are similar, so that the MnS precipitates and the precipitated MnS acts as a precipitation nucleus for the BN.

[0055] In one embodiment, the T MnS -T BN If the value of T is smaller than the lower limit, a re-solid solution phenomenon occurs, and it may be difficult to expect the effect of complex precipitation of MnS and BN. MnS -T BN If the value of is larger than the upper limit, MnS is formed in a coarse state, and the coarse MnS cannot act as a nucleus for the BN precipitation, so that it may be difficult to expect the composite precipitation effect.

[0056] Referring to Fig. 1, in one embodiment, the cold rolled steel sheet may include at least one precipitate of MnS and BN, and the area fraction of the precipitate may be 1 to 10%. Specifically, the area fraction may be 1.5 to 7%. If the area fraction is smaller than the lower limit, there is a problem that precipitation strengthening occurs due to the fineness of the precipitates formed, making it difficult to ensure the desired strength and workability. If the area fraction is larger than the upper limit, there is a problem that the strength increase effect due to precipitation strengthening occurs more than the effect of coarsening crystal grains due to coarse precipitates.

[0057] In one embodiment, the average grain size of the precipitates may be 40 to 250 nm. Specifically, the average grain size of the precipitates may be 50 to 200 nm. If the average grain size of the precipitates is too small, the grain coarsening effect intended in the present invention may not be obtained due to the formation of fine precipitates, and if the average grain size of the precipitates is too large, the total number of MnS generated is small, and it may not be able to function as precipitation nuclei for BN, which may reduce the formability of the steel.

[0058] In one embodiment, the cold-rolled steel sheet may have a yield strength of 150 to 220 MPa. Specifically, the cold-rolled steel sheet may have a yield strength of 160 to 220 MPa. The yield strength of the cold-rolled steel sheet is based on a 0.2% offset method. If the yield strength of the cold-rolled steel sheet is too low, the strength is too low, and there is a problem that the performance of supporting the product is reduced when used for the intended purpose of the present invention. If the yield strength of the cold-rolled steel sheet is too high, there is a problem that the product may twist and cracks may occur at embossed or bent parts.

[0059] In one embodiment, the elongation of the cold-rolled steel sheet may be 35 to 48%. Specifically, the elongation of the cold-rolled steel sheet may be 39 to 46%. If the elongation of the cold-rolled steel sheet is too small, there is a high possibility that cracks will occur during forming. However, if the elongation of the cold-rolled steel sheet is too high, there is a problem of reduced rigidity because the strength is excessively reduced.

[0060] In one embodiment, the cold-rolled steel sheet may include a part of carbides in a ferrite single-phase structure as a microstructure. The carbide fraction may be, for example, 5% or less in terms of area fraction. If the carbide fraction is out of the above range, it may become a starting point for cracks to occur in the steel material, and deterioration of the steel material may occur during heat treatment. In one embodiment of the present invention, the ferrite single-phase structure means a structure consisting of ferrite structure in addition to precipitates and carbides. In other words, the ferrite structure may be 85% or more in terms of area fraction with respect to the entire steel sheet. More specifically, it may be 85 to 99%.

[0061] Referring to Fig. 2, in one embodiment, the ferrite grain size may be 10 to 40 µm. In Fig. 2, the grain sizes can be seen when the cold rolled steel sheet satisfies the composition range of the present invention (A, Example 1 in Table 1 below) and when it does not (B and C, Comparative Examples 6 and 8 in Table 1 below, respectively). If the grain size is too small, there is a problem that the strength of the steel material is excessively high compared to the intended strength of the present invention. If the grain size is too large, defects such as orange peel may occur at the processed area after processing.

[0062] In one embodiment of the present invention, the cold-rolled steel sheet may be galvanized to obtain a galvanized steel sheet, which will be described in detail later in the description of a method for manufacturing a cold-rolled steel sheet.

[0063] A method for producing a cold-rolled steel sheet according to an embodiment of the present invention includes the steps of reheating a slab containing 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), the remainder Fe, and unavoidable impurities, hot rolling the heated slab to produce a hot-rolled steel sheet, coiling the hot-rolled steel sheet at a coiling temperature in the range of 450 to 700°C, cold rolling the coiled hot-rolled steel sheet to produce a cold-rolled steel sheet, and annealing the cold-rolled steel sheet. The alloy composition of the slab is the same as that of the cold-rolled steel sheet described above, so a duplicated description will be omitted. Since the alloy composition does not change during the manufacturing process of the cold-rolled steel sheet, the alloy composition of the slab and the cold-rolled steel sheet is substantially the same.

[0064] The step of reheating the slab is a step of heating the slab at a low temperature at which the precipitates, for example at least one of BN and MnS, cannot be redissolved. In one embodiment, the step of reheating the slab can be reheated at a temperature of 1,150°C or more. A temperature of 1,150°C or more is required because most of the precipitates present in the steel must be redissolved. Specifically, the slab can be heated at a temperature of 1,200°C or more, more specifically, at a temperature of 1,200°C or more and less than 1,250°C in order to dissolve the precipitates well. By heating within the above temperature range, the hot rolling temperature can be sufficiently secured. If the temperature is outside the upper limit of the above temperature range, the fraction of precipitates in the cold rolled steel sheet is excessively small and the grain size of the precipitates is small, so that the precipitates cannot be redissolved.

[0065] The step of hot rolling the slab to produce a hot-rolled steel sheet is carried out by rolling the slowly cooled slab with Ar 3 The slab is hot-rolled at the above temperature to produce a hot-rolled steel sheet. 3 The temperature at which iron transforms from ferrite or cementite to austenite is the third transformation temperature, and Ar3 can be calculated by the following formula:

[0066] Ar 3 Temperature = 914.57 - 95.24 x wt% C - 43.5 x wt% Mn - 21.15 x wt% C x wt% Mn - 128.6 x wt% C 1 / 2 It can be defined as:

[0067] The hot rolling finishing temperature is Ar 3 The reason for limiting the above is to perform rolling in the single phase region. Specifically, the finishing temperature of the hot rolling is Ar 3 or 1,200°C, specifically, Ar 3 The Ar 3 The temperature may be, for example, 880 to 900°C.

[0068] The step of hot rolling a slab to produce a hot rolled steel sheet may include coiling the produced hot rolled steel sheet. In one embodiment, the hot rolled steel sheet may be coiled at a temperature range of 500 to 700° C. Specifically, the temperature range may be 600 to 700° C.

[0069] If the hot-rolled steel sheet is coiled at a temperature lower than the above range, the hot-rolled structure becomes coarse and it is difficult to ensure cold rolling properties after hot rolling. If the hot-rolled steel sheet is coiled at a temperature higher than the above range, oxygen in the scale formed on the steel surface during coiling reacts with carbon in the steel, resulting in scale that does not easily undergo pickling, which may ultimately affect the crystal orientation during galvanization. In one embodiment, the coiled hot-rolled steel sheet may have a thickness of 2.0 to 5.0 mm, as a non-limiting example.

[0070] In the step of cold rolling the hot rolled sheet to produce a cold rolled steel sheet, the coiled hot rolled steel sheet may be cold rolled at a reduction of 50% or more, specifically, at a reduction of 50 to 90% to produce a cold rolled steel sheet. If the reduction is less than the lower limit, it is difficult to ensure a target thickness of the cold rolled steel sheet. If the reduction is greater than the upper limit, the steel becomes excessively hard, resulting in reduced rollability.

[0071] The step of annealing the cold-rolled steel sheet includes annealing the cold-rolled steel sheet in an annealing line by batch annealing or continuous annealing, and may be performed, for example, by continuous annealing at a temperature range of 600 to 800° C. If the temperature is below the lower limit of the temperature range, recrystallization of the steel material may not occur sufficiently, and strength and ductility may be deteriorated due to high potential density. If the temperature is above the upper limit of the temperature range, problems such as heat buckle may easily occur during rolling of thin sheets.

[0072] After annealing, the steel is subjected to temper rolling. In one embodiment, the rolling reduction ratio in the temper rolling step may be in the range of 0.5 to 1.5%. The final steel has a problem that the yield strength increases when the yield point elongation phenomenon occurs due to the presence of solute C and N. Therefore, the occurrence of the yield point elongation phenomenon can be suppressed by controlling the rolling reduction ratio.

[0073] If the rolling reduction is too low, the material may harden due to the yield point elongation phenomenon, whereas if the rolling reduction is too high, the material may harden due to work hardening and the elongation may decrease. In one embodiment, the final thickness of the temper rolled steel may be in the range of 0.5 to 3.0 mm.

[0074] In one embodiment, the cold-rolled steel sheet manufacturing method may include a step of performing a plating process after the step of cold-rolling the hot-rolled sheet to manufacture a cold-rolled steel sheet. The step of performing a cold rolling process may be a step after the cold rolling process and before the annealing process, a step after the cold rolling and annealing process and before the temper rolling process, or a step after the temper rolling process. Specifically, the plating process may be performed after the temper rolling process.

[0075] The plating step may utilize various plating methods, such as hot-dip galvanizing or electrolytic galvanizing.

[0076] In one embodiment, the hot dip galvanizing may be performed in a coating bath having a temperature range of 400 to 500° C., specifically, 420 to 480° C. If the hot dip galvanizing is performed at a temperature lower than the lower limit of the range, zinc may not melt sufficiently and the coating may not be uniform. If the hot dip galvanizing is performed at a temperature higher than the upper limit of the range, the coating bath may volatilize, preventing the coating bath from sufficiently bonding with the steel sheet during cooling to form a sound structure, and causing the steel sheet to melt during the coating process.

[0077] In one embodiment, the electrolytic zinc plating may be followed by a fingerprint-resistant resin coating. The coating may be performed at a temperature in the range of 100 to 200° C. For example, if the temperature is below the lower limit of the range, the drying of the coated resin may be non-uniform. If the temperature is above the upper limit of the range, an aging phenomenon may occur during the drying process, resulting in an increase in yield point due to yield point elongation.

[0078] Hereinafter, specific examples of the present invention will be described. However, the following examples are merely specific examples of the present invention, and the present invention is not limited to the following examples. EXAMPLES

[0079] Slab steel having the composition shown in Table 1 below and the balance containing Fe and unavoidable impurities was produced, and the components are shown as actual values.

[0080] [Table 1]

[0081] Among the steel slabs having the composition in Table 1, the invention steel 1 was used as a reference, and was reheated at 1,200°C and hot-rolled at 920°C. The hot-rolled hot steel sheet was coiled and the cold reduction ratio was controlled. The cold-rolled cold-rolled steel sheet was annealed and then the temper rolling ratio was controlled. The precipitates, grain size, material properties, and defects of the steel material as shown in Table 2 below were confirmed.

[0082] [Table 2]

[0083] From Table 2, the precipitate fraction and grain size, hot-rolled grain size, cold-rolled grain size, yield strength, elongation, and the presence or absence of surface defects and processing defects of the inventive steel and comparative steel can be confirmed. The surface defects were determined based on the presence or absence of surface defects of the steel material with a length of 5 mm or more, and the processing defects were determined based on the presence or absence of cracks with a length of 2 mm or more at the processing site after the V-bending processing test. The V-bending processing test was performed under normal conditions, with the steel material placed in a V-shaped die and the moving speed of the die controlled within 5 mm / min.

[0084] From Table 2, it can be seen that in the cases of Examples 1 to 13, the upper and lower limit of the material were confirmed, and the yield strength was 220 MPa or less, and no surface defects or processing defects were generated. In the case of Comparative Example 1, it can be seen that the yield strength increases when the carbon (C) content is increased.

[0085] The influence of the manganese (Mn) content was examined in Comparative Examples 2 and 3. When the manganese (Mn) content is too low as in Comparative Example 2, the yield strength is reduced due to a decrease in the solid solution strengthening effect of the manganese, and when the manganese content is too high as in Comparative Example 3, the yield strength is too high, resulting in a problem of the occurrence of a twisting phenomenon in the steel material.

[0086] Comparative Examples 4 and 5 are used to examine the influence of the aluminum (Al) content. When the aluminum content is too low as in Comparative Example 4, the aluminum does not have sufficient deoxidizing ability, and calcium (Ca) and manganese (Mn)-based inclusions occur frequently in the steel, causing cracks. When the aluminum content is too high as in Comparative Example 5, it causes problems in terms of economy. In the present invention, it is only necessary to secure the aluminum content up to the deoxidizing level, so there is no need to add the aluminum excessively. Therefore, this does not match the direction of the present invention, which aims to secure economy by lowering the aluminum content to a required range level, and to provide an extremely thin steel material that has excellent press workability, is free from defects such as cracks during forming, and has high strength.

[0087] Comparative Examples 6 and 7 were used to examine the influence of the sulfur (S) content. When the amount of sulfur added is too small as in Comparative Example 6, not only is the amount of MnS precipitation low, but the precipitation temperature is lower than that of BN, so that a composite precipitation effect does not occur, and therefore no grain refinement and strength reduction effects occur. When the amount of sulfur added is too large as in Comparative Example 7, the MnS precipitation temperature increases, MnS precipitates coarsely, and composite precipitation with BN does not occur, so that there is no strength reduction effect. Also, referring to FIG. 3, it can be seen that the change in BN and MnS precipitation temperature due to the change in S content is shown in 0.015wt%C-0.15wt%Mn-0.02wt%Al-20ppm B,N base calculated through the Thermocalc. program. Therefore, it can be seen that in the base of the above composition system, the calculation result shows that the precipitation temperature of BN and MnS is reversed when the S content is 0.003%.

[0088] Comparative Examples 8 to 11 are for investigating the influence of the boron (B) and nitrogen (N) contents, which are the main factors in BN precipitation. Since the boron and nitrogen contents are present at similar levels, precipitation is controlled by the component having the lower content of the two in atomic ratio. It is important to have the minimum atomic weight of the boron and nitrogen as shown in Formula 1, and the boron and nitrogen contents are such that the precipitation temperature difference between MnS and BN is 0 to 100°C or less as shown in Formula 3. When the boron content is too low as in Comparative Example 8, the precipitation temperature of BN is low and it is redissolved in the heating furnace, so the precipitation strengthening effect is not generated. When the boron content is too high as in Comparative Example 9, the boron segregates to free B at the grain boundary, causing a pinning effect and possibly increasing the strength by making the hot rolling property poor.

[0089] When the nitrogen content is too low as in Comparative Example 10, the BN precipitation temperature is lowered and no coarsening effect is generated, similar to the boron content. When the nitrogen content is too high as in Comparative Example 11, AlN cannot be sufficiently formed together with the nitrogen within the aluminum content range according to an embodiment of the present invention, which may lead to an increase in strength due to aging.

[0090] Tables 3 and 4 below show the change in steel properties depending on the manufacturing conditions of the steel slabs having the composition in Table 1, based on the composition system in Example 1. In Table 3 below, the reheating temperature, finish rolling temperature, coiling temperature, cold reduction rate, annealing temperature, and temper rolling rate among the manufacturing conditions are changed, and in Table 4 below, the precipitate fraction, grain size, crystal grain size, yield strength, elongation rate, and defects such as surface defects and processing defects of the steel manufactured under the conditions in Table 3 below can be confirmed.

[0091] [Table 3]

[0092] [Table 4]

[0093] In Tables 3 and 4, Comparative Example 12 is an example of investigating the influence of the slab reheating temperature (SRT). When the slab reheating temperature is high at 1,250°C, precipitates such as BN and MnS can be redissolved, but at a cooling rate at the hot rolling level, it is difficult to form coarse precipitates such as BN and MnS, and there is a problem that there is no effect of reducing strength.

[0094] Comparative Examples 13 and 14 are used to examine the influence of the coiling temperature. When the coiling temperature is excessively high as in Comparative Example 13, the grains are coarsened at the high coiling temperature, which has the effect of reducing strength, but it can be seen that surface defects are generated on the surface due to oxidation of carbon (C). When the coiling temperature is excessively low as in Comparative Example 14, there is a problem that it is difficult to ensure the strength reduction effect due to the reduction in hot-rolled grain size and the reduction in cold-rolled grain size.

[0095] Comparative Examples 15 and 16 are used to investigate the degree of influence due to differences in temper rolling reduction ratios. Since the steel material of the present invention contains C content, it is possible to prevent aging by forming a movable potential through elongation through a skin pass mill (SPM). When the temper rolling reduction ratio is too small as in Comparative Example 15, the elongation of the steel material may increase due to the occurrence of aging. When the temper rolling reduction ratio is too high as in Comparative Example 16, there is a problem that the elongation increases due to work hardening, so the temper rolling reduction ratio of the present invention is limited to within ±0.5% of the thickness.

[0096] The present invention is not limited to the above-mentioned embodiment and / or examples, and can be manufactured in various different forms, and a person skilled in the art to which the present invention belongs should understand that the present invention can be embodied in other specific forms without changing the technical idea or essential characteristics of the present invention. Therefore, the above-described embodiment and / or examples should be understood to be illustrative in all respects and not limiting.

Claims

1. In weight percent, carbon (C): 0.010 to 0.025%, manganese (Mn): 0.10 to 0.25%, sulfur (S): 0.002 to 0.011%, boron (B): 0.0006 to 0.0026%, nitrogen (N): 0.0010 to 0.0034%, aluminum (Al): 0.006 to 0.028%, the balance being Fe and unavoidable impurities; Contains at least one precipitate of MnS and BN; The area fraction of the precipitates in the cold-rolled steel sheet is 1 to 10%, A cold-rolled steel sheet having a yield strength of 150 to 220 MPa.

2. The cold rolled steel sheet according to claim 1, which satisfies the following formula 1: <Formula 1> 100,000×min([B] / 10.8, [N] / 14)>9.25 (In the above formula 1, min(a, b) means the smaller value of a and b, and [B] and [N] mean the contents (wt%) of B and N.)

3. The cold rolled steel sheet according to claim 1, which satisfies the following formula 2. <Formula 2> ([N]-1.3×[B])×9.643<0.015 (In the above formula 2, [B] and [N] mean the contents (wt%) of B and N.)

4. The cold rolled steel sheet according to claim 1, which satisfies the following formula 3. <Formula 3> 0<T MnS -T BN <100 (In the above formula 3, T BN is 573,198 × min([B] / 10.8, [N] / 14) + 1142, where min(a, b) is the smaller value of a and b, and T MnS means 15000×[S]+1170, and [B], [N], and [S] mean the contents (wt%) of B, N, and S.

5. The cold-rolled steel sheet according to claim 1, wherein the average grain size of the precipitates is 40 to 250 nm.

6. 2. The cold rolled steel sheet according to claim 1, wherein the average grain size of ferrite is 10 to 40 μm.

7. 2. The cold rolled steel sheet according to claim 1, wherein the elongation of the cold rolled steel sheet is 35 to 48%.

8. A galvanized steel sheet obtained by subjecting the cold rolled steel sheet according to any one of claims 1 to 7 to a hot dip galvanizing treatment.

9. A step of reheating the slab containing, in weight percent, 0.010 to 0.025% carbon (C), 0.10 to 0.25% manganese (Mn), 0.002 to 0.011% sulfur (S), 0.0006 to 0.0026% boron (B), 0.0010 to 0.0034% nitrogen (N), 0.006 to 0.028% aluminum (Al), the balance being Fe and unavoidable impurities, at 1,100°C or higher and lower than 1,250°C; hot rolling the heated slab to produce a hot rolled steel sheet; Coiling the hot-rolled steel sheet at a coiling temperature in the range of 450 to 700°C; cold rolling the coiled hot-rolled steel sheet to produce a cold-rolled steel sheet; Annealing the cold-rolled steel sheet; and subjecting the cold-rolled steel sheet to temper rolling at a rolling reduction ratio of more than 0.5% and less than 1.5%.

10. Heating the slab, The method for producing a cold-rolled steel sheet according to claim 9, wherein the slab is heated to 1,200°C or more.

11. In the step of manufacturing the hot-rolled steel sheet, The finishing rolling temperature was Ar 3 The method for producing a cold-rolled steel sheet according to claim 9 .

12. The step of manufacturing the cold-rolled steel sheet includes: The method for producing a cold-rolled steel sheet according to claim 9, wherein the cold-rolled steel sheet is produced by cold rolling at a rolling reduction of 50 to 95%.

13. After the step of manufacturing the cold-rolled steel sheet, The method for producing a cold-rolled steel sheet according to claim 9, further comprising the step of plating a surface of the cold-rolled steel sheet with zinc.

Citation Information

Patent Citations

  • Hot rolled steel sheet and method of producing hot rolled steel sheet and cold rolled steel sheet

    JP2003293083A

  • Cold-rolled steel sheet with excellent press formability, galvanized steel sheet, and manufacturing method thereof

    KR1020150031118A

  • Low-carbon cold rolled steel sheet having excellent press formability and manufacturing method the same

    KR1020150072751A