Method for producing nanopores
The track etching process using ion irradiation and low-toxicity etchants addresses the limitations of current nanoporous membrane production, enabling scalable and reproducible membranes with tunable nanopore geometries for advanced applications in sensing and filtration.
Patent Information
- Application Number
- JP2024534467
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-07
- Filing Date
- 2022-12-07
- Publication Date
- 2024-12-26
AI Technical Summary
Current methods for producing nanoporous membranes are limited by the use of toxic etchants and lack the ability to precisely tune nanopore geometry for specific applications, such as chemical and biological sensing, filtration, and ion transport.
A track etching process using high-energy ion irradiation followed by selective etching with low-toxicity etchants allows for the fabrication of nanopores with tunable geometry, including conical and biconical shapes, suitable for various applications by controlling parameters like etchant composition, concentration, temperature, and material composition.
The method enables the production of nanoporous membranes with high scalability, reproducibility, and compatibility with CMOS manufacturing, offering enhanced performance in sensing, filtration, and ion transport through customizable nanopore shapes and sizes.
Smart Images

Figure 2024546760000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing nanopores in materials, and in particular to membranes having nanopores produced by the method. [Background technology]
[0002] A nanopore is a hole or cavity with a size on the nanoscale. Nanopores are narrow channels in materials such as membranes, with one or more dimensions in the nanoscale range. Nanopores are also found in biological systems, for example in the lipid bilayer of cell membranes. Nanopores can also be engineered artificially and used for a number of applications. Summary of the Invention [Problem to be solved by the invention]
[0003] A membrane is a barrier that selectively allows some substances (such as molecules or ions) to pass while blocking others, depending on the properties of the membrane material and functional elements such as nanopores. Nanoporous membranes are membranes that have one or more nanopores and are currently used in many applications, including filtration, bio- and chemical sensing, size-selective ion transport, desalination, ion pumps, molecular sieves, protein detection, gas sensing, nanofluidics, DNA sequencing, and bioelectronics. Nanoporous membranes are also used in ionic current rectification (ICR), where the nanopores, when immersed in an electrolyte, behave like electronic diodes and effectively transport ions in different directions with different bias polarities across the membrane. Industrial applications of nanoporous membranes are also increasing. It should be noted that this specification focuses primarily on the fabrication of silicon-based nanoporous membranes, but the invention is not limited to membranes of such components. [Means for solving the problem]
[0004] The inventors have conducted research and development to fabricate nanopores in materials using a track etching process. In some embodiments, the material may comprise an inorganic material, particularly a silicon-based material. In other embodiments, the material may comprise an organic material. In the track etching process, a film is irradiated to create long, narrow damage tracks in the material. These damaged areas are often more sensitive to appropriate chemical etchants than the undamaged material. The difference in chemical etching rate between the damaged tracks and the undamaged material results in the formation of nanopores.
[0005] In a first aspect, a method for fabricating nanopores in a material is disclosed, the method comprising the steps of irradiating the material with radiation to create damage tracks in the material having nanometer scale sizes, and etching the damage tracks with an etchant to produce nanopores.
[0006] The irradiation step can include high energy irradiation. In an embodiment, the irradiation step can include ion irradiation. The ion irradiation can include swift heavy ion irradiation. The ion irradiation creates ion tracks along the material. These ion tracks are damage regions that are preferentially etched relative to undamaged material. The ion tracks range from about 3-15 nanometers in diameter and 10-100 micrometers in length.
[0007] The radiation exposure step determines the number of nanopores in the membrane. The number of ions that bombard the membrane translates to the number of nanopores. Heavy ions are ions heavier than silicon (Si). Heavy ions can have energies greater than 10 MeV. Heavy ions include xenon (Xe) ions and gold (Au) ions. In one embodiment, the material is irradiated with 200 MeV xenon ions. In another embodiment, the material is irradiated with 89 MeV gold ions. In yet another embodiment, the material is irradiated with 185 MeV gold ions. In another embodiment, the material is irradiated with 1.6 GeV gold ions.
[0008] In other embodiments, the irradiating step can include irradiating with laser radiation, which forms a laser track in the material.
[0009] The radiation exposure step determines the number of nanopores that are formed in the material. In the case of ion radiation exposure, the number of ions that bombard the material translates into the number of nanopores that are etched. The density of the nanopores can vary from a single nanopore to about 10 nanopores per square centimeter.
[0010] The material may include a membrane. The thickness of the membrane depends on the expected function and application of the nanopore membrane. For example, relatively thin nanopore membranes (<100 nm) are suitable for DNA and protein sensing applications, while relatively thick membranes are suitable for filtration purposes, since they need to withstand fluid pressure. In an embodiment, the membrane has a thickness of less than 50 nanometers, such as less than 30 nanometers. The membrane thickness can be as low as 1 nanometer, for example 1.5 nanometers or more. Relatively thin membranes are usually considered a prerequisite for obtaining high resolution measurements, since they have a higher signal-to-noise ratio (SNR) and a larger capture radius compared to relatively thick membranes. As nanopore technology is increasingly geared towards sequencing, the fabrication of thin films is ideal.
[0011] The thickness of the membrane can reach 10 micrometers. The thickness of the membrane is at least 10 nanometers. In some embodiments, the surface area of the membrane reaches 25 square millimeters. The minimum surface area is 0.0001 square millimeters.
[0012] The material components can include one or more amorphous inorganic materials. Amorphous solids / materials are amorphous solids, i.e. solids in which the atoms / molecules are not arranged according to a particular pattern. The material components can be silicon-based. The material components can include amorphous silicon. The material components can include one or more inorganic oxide materials. The material components can include one or more of silicon dioxide, silicon nitride, silicon oxynitride, hafnium oxide, hafnium silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, and tin oxide.
[0013] In some embodiments, the membrane material layer may include diamond.
[0014] The focus of the present invention is to form nanopores in silicon-based materials. In particular, silicon dioxide, silicon nitride, and silicon oxynitride are of interest. Silicon dioxide, silicon nitride, and silicon oxynitride are known as important inorganic materials used in silicon microelectronics due to their excellent mechanical performance. Silicon dioxide and silicon oxynitride films are excellent candidate materials for chemical and / or biological sensors due to their properties such as excellent mechanical and chemical resistance, high temperature resistance, high density, and negligible leakage current. Silicon oxynitride is also widely used in optical sensors.
[0015] When the film contains silicon nitride, it is nearly stoichiometric Si X N Y (X~3 and Y~4).
[0016] Silicon oxynitride is an amorphous material with a composition between silicon dioxide and silicon nitride. For many optical sensor applications this material is of interest and many of its properties can be altered by changing the oxygen and / or nitrogen content. By changing the oxygen and nitrogen content ratio, the refractive index of the film can be easily tuned from 1.45 to 2.1. This property makes it very useful for bio-optical sensors.
[0017] When the component of the material is silicon dioxide, the material can include a thermal oxide (i.e., silicon dioxide produced by thermal oxidation) or the material can be formed by plasma enhanced chemical vapor deposition (PECVD).
[0018] In some embodiments, the material is a single material. In other embodiments, the material is a composite material. A composite material is a material formed by combining two or more materials with different physical and / or chemical properties. The resulting composite material exhibits different physical and / or chemical properties than the individual material components.
[0019] In some embodiments, the material is a combination of different materials. By combining different materials, bipolar nanopores with better filtering performance can be fabricated. Furthermore, such bipolar nanopores can be used as nanofluidic diodes, create logic gates in solution phase, and mimic biological processes.
[0020] In some embodiments, the membrane material layer is a single layer formed from a single material component. In other embodiments, the membrane material layer is multi-layered. The membrane material layer can include two or more sub-layers with different components. The layers can include silicon, silicon dioxide, and / or silicon oxynitride. In some embodiments, the membrane material layer is formed from a combination of one or more amorphous inorganic materials and nanoparticles. The resulting films have many applications in optical and optoelectronic devices and can be used to manipulate light-matter interactions.
[0021] In some embodiments, the membrane material layer is formed from a combination of one or more silicon-based inorganic materials and nanoparticles. In some embodiments, the membrane material layer is formed from a combination of one or more inorganic oxide materials and nanoparticles. The nanoparticles can be inorganic nanoparticles. The nanoparticles can be metal nanoparticles. In some embodiments, the nanoparticles are gold nanoparticles. In other embodiments, the nanoparticles are silver nanoparticles. In yet other embodiments, the nanoparticles are copper nanoparticles.
[0022] The nanoparticles can be spherical and / or elongated. In some embodiments, the membrane material layer includes one type of metal nanoparticles. In other embodiments, the membrane material layer includes two or more types of metal nanoparticles. In some embodiments, the nanoparticles are dispersed in the membrane material layer. In other embodiments, the nanoparticles are provided (e.g., embedded) between two layers of any of the above materials.
[0023] In one embodiment, the membrane material layer comprises an inorganic oxide and gold nanoparticles. In another embodiment, the membrane material layer comprises silicon dioxide and gold nanoparticles. In yet another embodiment, the membrane material layer comprises silicon nitride and gold nanoparticles. In still another embodiment, the membrane material layer comprises silicon oxynitride and gold nanoparticles.
[0024] Processes are disclosed in which parameters such as temperature during the etching step, etchant composition, etchant concentration, material composition, density and morphology are controlled to tailor the geometry of the nanopores formed by the above methods. As used herein, "nanopore geometry" refers to the overall shape and size of the nanopore. Geometry includes parameters such as cone angle, radius and symmetry. Symmetry includes whether the nanopore is a combination of a cone and a cylinder, or a combination of two cones with different cone angles.
[0025] As used herein, "cone angle" or "cone opening angle" refers to the angle of the sidewall formed by a cross section along the apex and base center of the nanopore. "Half-cone angle" is half the cone angle, i.e., the angle between the cone axis and the nanopore sidewall. Compared to similar cylindrical pore membranes, conical nanopores enhance the transport rate of the membrane and provide higher sensitivity in biological and chemical sensing applications. Furthermore, with appropriate size, conical and hourglass-shaped (biconical) nanopores can exhibit nanofiltering and ionic current rectification properties. These nanopores allow selective charge ion transport through the pore. They can also reject different ions based on whether the solution flows in from the tip or base of the pore.
[0026] As used herein, "radius" refers to the maximum radius of the nanopore. If the nanopore has a conical (or truncated conical) shape, the radius refers to the base radius of the cone. If the nanopore has a conical or truncated conical shape, there are two radii: a maximum (or base) radius and a minimum (or tip) radius. However, unless otherwise specified, "radius" as used herein refers to the maximum (or base) radius of a conical or truncated conical nanopore.
[0027] The size and cone angle of the nanopore affect the sensing performance of the nanopore. As the cone angle increases, the effective pore length decreases (providing higher flux) and the capture radius increases, making these nanopores highly suitable for molecular sensing, protein detection and DNA sequencing. Numerical simulations have shown that by varying the cone angle and nanopore height, the performance such as ionic current rectification properties, impedance pulse sensing can be modified. Thus, by tuning the cone angle, nanopores can be fabricated to suit specific application requirements.
[0028] As used herein, "tunable" means that one or more parameters of the nanopore can be altered, in other words, tunable means that the shape and / or structure and / or size of the nanopore can be adjusted depending on the particular application.
[0029] In certain embodiments, adjusting the geometry of the nanopore comprises adjusting one or more of the cone angle, radius, and symmetry of the nanopore.
[0030] For a particular material composition, etchant composition, etchant concentration, and etching time, increasing the etching temperature decreases the cone angle of the nanopore and / or increases the radius of the nanopore.
[0031] For a particular material composition, etchant composition, temperature and etching time, increasing the etchant concentration increases the cone angle of the nanopore and / or increases the radius of the nanopore.
[0032] The composition of the material can also be varied. For example, by modifying the stoichiometry and density of the PECVD-grown silicon oxide film, the size of the nanopores can be tuned. Furthermore, if the film comprises silicon oxynitride, the refractive index of the film can be tuned from 1.45 to 2.1 by changing the oxygen to nitrogen content ratio, which also affects the geometry of the nanopores formed.
[0033] The above relationships can be used to tailor the nanopore geometry. For example, if a lower nanopore cone angle is desired, the etching step can be performed at a relatively higher etching temperature and / or a relatively lower etchant concentration. In another example, if a larger nanopore radius is desired, the etching step can be performed at a relatively higher etching temperature and / or a relatively higher etchant concentration.
[0034] The cone angle of the nanopore can be adjusted from about 3 degrees to about 110 degrees. In some embodiments, the cone angle of the nanopore can be adjusted from about 10 degrees to about 110 degrees. Thus, the half cone angle can be adjusted from about 1.5 degrees to about 55 degrees, such as from 5 degrees to about 55 degrees. In some embodiments, the half cone angle can be adjusted from about 25 degrees to about 55 degrees.
[0035] The radius and depth of the nanopore can also be tailored depending on the application requirements. The radius and depth of the nanopore can vary from about 20 nanometers to several micrometers. In some embodiments, the depth of the nanopore is up to 10 micrometers.
[0036] By using a combination of etchants, the overall geometry of the nanopore can be tailored. For example, a combination of wet hydrogen fluoride (HF) and vapor hydrogen fluoride can be used to fabricate a generally funnel-shaped nanopore. A wet hydrogen fluoride etch is used to fabricate the conical portion of the funnel-shaped nanopore, and a vapor hydrogen fluoride etch is used to fabricate the cylindrical portion of the nanopore. Notably, the conical portion of the funnel-shaped nanopore can also be fabricated using an alkaline hydroxide etchant, and the cylindrical portion can be fabricated using vapor hydrogen fluoride.
[0037] Some examples of applications of nanopores with different geometries are given.
[0038] Single conical nanopores are used, for example, for electrically driven salt flux rectification, with applications in areas such as nanofiltering, energy generation, and ion pumps. Due to their inherent rectification properties, conical nanopores have many advantages over cylindrical nanopores. For example, restricted diffusion occurs throughout the entire length of the nanopore in cylindrical nanopores, whereas restricted diffusion occurs only at the tip of the pore in conical nanopores. Thus, conical nanopore membranes exhibit higher throughput / flow rates compared to cylindrical nanopore membranes, allowing for faster and more effective separation of proteins, biomolecules, and the like. These advantages of conical nanopores depend on the size of their cone angle, with the effect increasing as the cone angle increases. Thus, by tuning the cone angle and fabricating nanopores with large cone angles, nanopores can be fabricated with great potential advantages in all of the aforementioned applications.
[0039] Symmetric biconical nanopores are particularly suitable for filtration applications because they require a lower driving force for operational separation compared to a single-conical nanopore of the same length. Furthermore, by functionalizing part of the nanopore or fabricating a nanopore composed of two different oxides, biconical nanopores can be used as logic gates or nanofluidic diodes.
[0040] Funnel-shaped nanopores are biomimetic (e.g., similar nanopore shapes used for chloride transport in the human body) and can achieve higher asymmetric ion transport with high rectification ratios. These nanopores also improve light transmission efficiency. Funnel-shaped nanopores are particularly suitable for applications in the fields of materials, electronics, and life sciences.
[0041] Asymmetric biconical nanopores are particularly suitable for asymmetric ion transport. Due to their different cone angles and / or shapes, these nanopores can be used for asymmetric ion transport even without an external driving force. Even with a driving force, such as electrical power, these nanopores allow one ion to flow out of one side of the solution and the other ion to flow out of the other side of the solution.
[0042] In addition to the above mentioned application examples, all nanopores can be used as templates for the synthesis of nanowires of different shapes. Effect of the Invention
[0043] Thus, the present invention allows the production of nanoporous membranes and offers the following advantages: The use of toxic and dangerous etchants (e.g., hydrogen fluoride) is avoided or at least reduced. Using hydrogen fluoride as the sole etchant severely limits the geometric shape of the nanopores. For example, using hydrogen fluoride as the only etchant makes it possible to fabricate conical (or truncated conical) or funnel-shaped pores and not to alter the opening angle (also called the cone angle) of the conical / funnel-shaped nanopores. Low toxicity etchants can be used and their composition and / or concentration can be altered to tailor the nanopore geometry. By varying the material composition, etching temperature, and etchant composition and concentration, the nanopores can be highly tunable. Highly scalable. The ion bombardment process is highly scalable, and the bombardment area can be easily varied from a few micrometers to several meters. Also, the number of nanopores can be varied from a single nanopore to 1010 nanopores per square centimeter. The etching process is also highly scalable, and thousands of membranes can be etched at once. The process is compatible with CMOS (complementary metal-oxide-semiconductor) manufacturing processes, making it an industrially feasible process that can be integrated into a variety of devices. The process is highly reliable and reproducible. Many potential applications exist, including chemical and biological sensing, size and charge selective ion transport, water desalination, ion pumps, DNA sequencing, molecular sieves, water filtration, protein separation and detection, and health monitoring. [Brief description of the drawings]
[0044] [Figure 1a] FIG. 1 is a schematic diagram showing an embodiment of the fabrication process of the present invention, illustrating the fabrication process of tunable nanopores when potassium hydroxide (KOH), sodium hydroxide (NaOH) and a combination thereof are used as etching agents. [Figure 1b] FIG. 1 is a schematic diagram showing an embodiment of the fabrication process of the present invention, illustrating the process of fabricating actual funnel-shaped nanopores using a combination of wet and vapor hydrogen fluoride etching. [Diagram 2] 1A-1D are scanning electron microscope (SEM) images of examples of membranes of the invention. (a) shows an SEM image of a large number of nanopores in a thin silicon oxide membrane. (b) shows a top-view SEM image of a one-sided etched conical nanopore in a silicon oxynitride membrane. (c) shows a cross-sectional SEM image of a one-sided etched conical nanopore in a silicon oxide membrane. (d) shows a cross-sectional SEM image of a two-sided etched conical nanopore in a silicon oxide membrane. [Diagram 3](a) Etching time as a function of nanopore radius at temperatures of 70°C (squares), 80°C (circles), and 90°C (triangles), and (b) shows the effect of etching temperature on the half-cone angle of the nanopore. [Figure 4] 1 is a graph showing an Arrhenius plot of the radial etch rate for Example 1. The dotted line shows a linear fit of the data and indicates the activation energy for the etch. [Diagram 5] (a) Etch time as a function of nanopore radius at a constant 80° C. etch temperature and etchant concentrations of 1 M (squares), 3 M (circles), 6 M (triangles), and 9 M (inverted triangles). (b) Etch rate as a function of etchant concentration. [Figure 6] 13 is a graph showing the effect of etchant concentration on the half-cone angle of the nanopores of Example 2. [Figure 7] 13 is a graph showing the effect of refractive index of different silicon oxynitride films on nanopore radius of Example 4. [Figure 8] FIG. 1 shows SEM images of the top view (a) and cross-sectional view (b) of a funnel-shaped nanopore. [Figure 9] FIG. 1 is a schematic diagram showing the fabrication process of both symmetric and asymmetric conical-gate nanopores. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] The detailed description given below describes exemplary embodiments with reference to the drawings. The description of the exemplary embodiments and drawings, and the definitions set forth in the claims, are not intended to be limiting. The invention is available in other embodiments, and other modifications are possible without departing from the spirit and scope of the subject matter of the invention. Aspects of the invention can be arranged, substituted, combined, separated, and designed in the general manner described herein and in the specific manner shown in the drawings. Many different configurations are possible.
[0046] First, reference is made to Figures 1a and 1b. Shown is a schematic diagram of a process for fabricating tunable nanopores using potassium hydroxide, sodium hydroxide, and combinations thereof as etchants. Figure 1a illustrates the process and shows various nanopore shapes that can be fabricated in this manner. The membranes are composed of silicon oxide or silicon oxynitride, and each membrane is supported on a silicon frame. The membranes are bombarded with swift heavy ions to form ion tracks in each membrane. Each membrane is then etched with a different etchant and / or under different etching conditions. Depending on the particular etchant or etching conditions, various nanopore geometries can be fabricated, including single cone, funnel, symmetric bicone, and asymmetric bicone.
[0047] Figure 1b illustrates the process of fabricating funnel-shaped nanopores in these membranes using a combination of wet and vapor hydrogen fluoride etches. Wet hydrogen fluoride etches are used to fabricate the conical portion of the funnel-shaped nanopores, and vapor hydrogen fluoride etches are used to fabricate the cylindrical portion of the nanopores. Of note, the conical portion of the nanopores can also be fabricated using an alkaline hydroxide etchant, while the cylindrical portion can be fabricated using vapor hydrogen fluoride.
[0048] 1a and 1b illustrate the fabrication of various nanopore geometries including single-cone, double-cone, funnel-shaped, symmetric and asymmetric nanopores. Each different nanopore shape may have different applications. For example, single-cone nanopores are used for electrically driven salt flux rectification, with applications in areas such as nanofiltering, energy generation, and ion pumps. Due to their inherent rectification properties, conical nanopores have many advantages over cylindrical nanopores. For example, restricted diffusion occurs throughout the entire length of the nanopore in cylindrical nanopores, whereas restricted diffusion occurs only at the tip of the pore in conical nanopores. Thus, conical nanopore membranes exhibit higher throughput / flow rates compared to cylindrical nanopore membranes, allowing for faster and more effective separation of proteins, biomolecules, and the like. These advantages of conical nanopores depend on the size of their cone angle, with the effect increasing as the cone angle increases. Thus, by tuning the cone angle and fabricating nanopores with large cone angles, nanopores can be fabricated with great potential advantages in all the aforementioned applications.
[0049] Symmetric biconical nanopores are particularly suitable for filtration applications because they require a lower driving force for operational separation compared to a single-conical nanopore of the same length. Furthermore, by functionalizing part of the nanopore or fabricating a nanopore composed of two different oxides, biconical nanopores can be used as logic gates or nanofluidic diodes.
[0050] Funnel-shaped nanopores are biomimetic (e.g., similar nanopore shapes used for chloride transport in the human body) and can achieve higher asymmetric ion transport with high rectification ratios. These nanopores also improve light transmission efficiency. Funnel-shaped nanopores are particularly suitable for applications in the fields of materials, electronics, and life sciences.
[0051] Asymmetric biconical nanopores are particularly suitable for asymmetric ion transport. Due to their different cone angles and / or shapes, these nanopores can be used for asymmetric ion transport even without an external driving force. Even with a driving force, such as electrical power, these nanopores allow one ion to flow out of one side of the solution and the other ion to flow out of the other side of the solution.
[0052] In addition to the above mentioned application examples, all nanopores can be used as templates for the synthesis of nanowires of different shapes.
[0053] Figure 2 shows scanning electron microscope (SEM) images of various membrane samples produced according to the method of the present invention. Figure 2(a) shows a side view of multiple holes in a thin silicon oxide membrane, and the scale bar is 1 micron in length. Figure 2(b) shows a top view SEM image of a one-sided etched conical nanohole in a silicon oxynitride membrane, and the scale bar is 4 microns in length. Figure 2(c) and (d) show cross-sectional SEM images of one-sided and two-sided etched conical nanoholes in a silicon oxide membrane, respectively, and the scale bar is 200 nanometers in length. EXAMPLES
[0054] Here we describe non-limiting examples of methods for producing nanopores in materials.
[0055] Examples 1 to 3 Silicon oxide membrane samples are used to fabricate nanopores. The membranes have a surface area of 300 μm × 300 μm and a thickness of 1 μm. The membranes include thermal oxide (i.e., silicon oxide produced by thermal oxidation) and membranes produced by plasma-enhanced chemical vapor deposition (PECVD).
[0056] Some samples were irradiated with 200 MeV xenon ions at the Synchrocyclotron U-150M of the Kazakhstan Institute of Nuclear Physics, some with 1.6 GeV gold ions at the UNILAC linear accelerator at the GSI Helmholtz Centre for Heavy Ion Research in Germany, and some with 185 MeV and 89 MeV gold ions at the 14UD accelerator at the Australian National University. The fast heavy ion irradiation produces long and narrow damage tracks that form ion tracks along the membrane. These damaged areas, called "ion tracks", are about 3-15 nanometers in diameter and range from 10-100 micrometers in length, and are more sensitive than the undamaged material to appropriate chemical etchants. Chemical etching of the ion tracks results in the formation of nanopores.
[0057] The samples are then etched using different etchants at different concentrations and temperatures, and the following examples illustrate the effect of these parameters.
[0058] Example 1: Effect of temperature Thermal silicon oxide membranes are irradiated with 1.6 GeV gold ions at a dose of 108 ions per square centimeter. 6 M potassium hydroxide is used as the etchant to etch the damaged areas (ion tracks) in the membrane into nanopores. The etchant concentration is kept constant and samples are etched at different temperatures to investigate the effect of temperature on the etching kinetics of nanopore membranes. The etched samples are then observed by SEM and the radius and half cone angle of the nanopores are measured through cross-sectional SEM imaging.
[0059] Figure 3(a) shows the radius of the nanopores as a function of etching time as observed by SEM. The samples were etched at three different temperatures, 70 °C, 80 °C, and 90 °C, while the etchant concentration was kept constant. A linear fit of the data gives the radial etch rate of the nanoporous membrane. It was found that the radial etch rate increases with increasing temperature.
[0060] Figure 3(b) shows the effect of etching temperature on the half-cone angle. As can be seen, as the temperature increases, the half-cone angle decreases. This directly indicates that as the temperature increases, the axial etch rate increases faster than the radial etch rate.
[0061] The measurements show that the radial etching rate with increasing temperature can be described by the Arrhenius law (see Figure 4). The activation energy obtained from this graph is Ea = (1.25 ± 0.14) eV for etching with 6 M potassium hydroxide.
[0062] These results indicate that the activation energies for the track and radial etch rates are different, which leads to different cone angles at different temperatures. This suggests that the cone angle of the fabricated nanopores can be tuned by changing the processing temperature. Thus, high tunability of the nanopore shape is achieved by modifying the processing temperature.
[0063] Example 2: Effect of Etchant Concentration Four different etchant concentrations are used to fabricate the nanopores. The etchants used are 1 M, 3 M, 6 M, and 9 M potassium hydroxide solutions. The silicon oxide membrane is etched while the etching temperature is kept constant at 80±1°C.
[0064] Figure 5(a) shows the radius of the nanopore as a function of time. A linear fit of the data gives the etch rate, which is plotted as a function of etchant concentration in Figure 5(b). The etch rate increases from (0.99 ± 0.03) nm / min at 1 M potassium hydroxide to (1.97 ± 0.06) nm / min at 3 M potassium hydroxide. For 6 M potassium hydroxide, the etch rate decreases to (1.57 ± 0.03) nm / min, then increases to (3.77 ± 0.11) nm / min at 9 M potassium hydroxide. Figure 6 shows the effect of etchant concentration on the half cone angle. As shown in the figure, with increasing etchant concentration, the half cone angle increases. Thus, altering the etchant concentration provides another way to tune the shape and size of the nanopore. This is important, as the effects of temperature and etchant concentration can be combined to fine-tune the cone angle, increase or decrease the etch rate, and adjust the size of the cone.
[0065] Example 3: Effect of membrane components and manufacturing method Both thermal oxides and oxides grown by PECVD are used to fabricate nanoporous membranes. Thermal oxides have high quality (low defects, low water content, high density, good dielectric properties, etc.) while PECVD oxides allow control over the film properties (stoichiometry, density, refractive index, generated stress, etc.). PECVD oxides can also be integrated into multilayer structures.
[0066] The PECVD film is deposited at 650°C.
[0067] Differences are observed between nanopores fabricated in thermal oxide and PECVD silicon oxide films. When etched with 3M potassium hydroxide at 80°C, the half-cone angle in the PECVD silicon oxide film is more than twice that in the thermal oxide film. Furthermore, the etching rate of the PECVD film is higher. These results provide the potential to manipulate these observations to further tune the shape and size of the nanopores. Thus, the geometry of the nanopores can be further tuned by manipulating and controlling the composition, purity, and / or microstructural properties of the materials.
[0068] Example 4: Formation of nanopores in silicon oxynitride Silicon oxynitride is an amorphous material whose composition varies between silicon dioxide and silicon nitride. For many optical sensor applications this material is interesting, and many of its properties can be varied by changing the oxygen and / or nitrogen content. By changing the oxygen and nitrogen content ratio, the refractive index of the film can be easily tuned from 1.45 to 2.1. This property is very useful for bio-optical sensors. Using PECVD, silicon oxynitride films with different refractive indices and compositions were produced (see Table 1). The refractive index of the film was obtained by fitting the ellipsometric reflectance data to the Tauc-Lorentz model.
[0069] [Table 1]
[0070] The samples were irradiated with 200 MeV xenon ions at the Synchrocyclotron U-150M of the Kazakhstan Institute of Nuclear Physics. Afterwards, the different silicon oxynitride membranes were etched at 90 °C for 90 min using 3 M potassium hydroxide as an etchant. Figure 7 shows the radius of the nanopores as a function of the refractive index. The etching rate first increases with increasing nitrogen content and then decreases. Also, the cone angle changes with the change in the membrane composition. The cone angle decreases as the nitrogen content in the membrane increases. This allows further tuning of the pore structure. These results and the membrane properties can be used to integrate optical waveguides in multilayer systems or for optical trapping of biomolecules.
[0071] Example 5: Fabrication of nanopores using combined etchants Potassium hydroxide and sodium hydroxide are used as etchants used to etch the ion tracks. As mentioned before, the effect of potassium hydroxide etch concentration and temperature was discussed. Similar results were observed for sodium hydroxide etching. For example, the thermal silicon sample etched using 3M sodium hydroxide at 90 °C has an etch rate of (4.87 ± 0.14) nm / min and a half cone angle of (32.84 ± 1.93) degrees. The presented results show that by using different etchant combinations, different concentrations of etchants, and different etching temperatures, nanopores of different shapes and sizes can be fabricated. These shapes include near funnel-shaped pores and asymmetric biconical nanopores. Figure 8 shows an example of such a situation. (a) shows a top-view SEM image of a funnel-shaped nanopore, and (b) shows a cross-sectional SEM image. These nanopores were fabricated by first etching using 3M potassium hydroxide at 90 °C for 45 min, followed by etching using 2.5% hydrogen fluoride at room temperature for 10 min.
[0072] Similarly, different etchant combinations can be used to fabricate and fine-tune the shape and size of the nanopores to meet application requirements. As mentioned above, actual funnel-shaped nanopores can be fabricated using combinations of wet and vapor hydrogen fluoride etchants, as well as combinations of wet and vapor hydrogen fluoride etchants. The approximate funnel-shaped nanopores fabricated with a combination of potassium hydroxide and hydrogen fluoride and the actual funnel-shaped nanopores fabricated with a combination of wet and vapor hydrogen fluoride etchants exhibit better current rectification properties and isotope selectivity than cone-shaped nanopores. By modifying the cylindrical portion of the funnel-shaped nanopore, the current rectification factor can be increased by more than 100%.
[0073] Example 6: Fabrication of gated nanopores A multilayer is formed with highly doped silicon between silicon oxide and / or silicon oxynitride layers. The thickness of the doped silicon layers on both sides of the silicon oxide and / or silicon oxynitride layers can be tailored. Ion tracks are formed in the multilayer by ion bombardment, and then the ion tracks are etched to form nanopores, as shown in Figure 9. Potassium hydroxide or sodium hydroxide is used to etch the gate nanopores. These etchants etch damaged areas in the silicon oxide / silicon oxynitride layers and the intermediate silicon layer, and therefore these nanopore structures can be etched. Figure 9 shows the formation of symmetric and asymmetric biconical nanopores. After the nanopores are formed, a rapid thermal anneal is used to grow a thermal oxide layer on the exposed silicon in the pores. The thermal oxide layer acts as an insulating layer and prevents current leakage from the doped silicon into the solution / electrolyte during experiments (e.g., sensing, ion rejection, molecular sieving, etc.). Alternatively, a thin silicon oxide layer can be deposited on the pore surface using deposition techniques such as atomic layer deposition to prevent current flow through the gate.
[0074] Although a number of specific method and apparatus embodiments have been described, it should be understood that these methods and apparatus can be embodied in many other forms.
[0075] In the following claims and the foregoing description, unless the context otherwise requires, the terms "comprises" and variations thereof (such as "comprises" or "includes") are used inclusively to specify the presence of described features but do not exclude the presence or addition of additional features in the various embodiments disclosed herein.
[0076] Further patent applications may be filed in Australia or overseas based on or claiming priority to this application. The following claims are provided by way of example only and are not intended to limit the scope of the invention. Features may be added or omitted to further define or redefine the invention or inventive subject matter in future applications.
Claims
1. 1. A method for producing nanopores in a material, comprising: a radiation exposure step of irradiating the material with radiation to create one or more damage tracks in the material having nanometer scale sizes; an etching step using an etchant to etch the damage track to create nanopores; The method includes:
2. The method of claim 1 , wherein the step of irradiating comprises ion irradiation.
3. The method of claim 1 , wherein the step of irradiating comprises ion irradiation, which is swift heavy ion irradiation, and the damage track comprises an ion track.
4. The method of any one of claims 1 to 3, wherein the material is a membrane.
5. The method of claim 4, wherein the thickness of the film reaches 10 micrometers.
6. The method of claim 4 or 5, wherein the film has a thickness of at least 10 nanometers.
7. The method according to any one of claims 4 to 6, wherein the area of the membrane reaches 25 square millimeters.
8. The method of any one of claims 4 to 7, wherein the membrane has an area of at least 0.0001 square millimeters.
9. The method of any one of claims 1 to 8, wherein the material components comprise one or more amorphous inorganic materials.
10. The method according to any one of claims 1 to 9, wherein the material component is silicon-based.
11. A method according to any preceding claim, wherein the component of the material comprises amorphous silicon.
12. The method of any one of claims 1 to 10, wherein the material components comprise one or more inorganic oxide materials.
13. 10. The method of any one of claims 1 to 9, wherein the components of the material include one or more of silicon oxide, silicon nitride, silicon oxynitride, hafnium oxide, hafnium silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, and tin oxide.
14. The method of any one of claims 1 to 13, wherein the etching agent comprises a water-soluble alkali hydroxide.
15. 15. The method of claim 14, wherein the etchant is selected from potassium hydroxide, sodium hydroxide, barium hydroxide, lithium hydroxide, calcium hydroxide, ammonium hydroxide, and cesium hydroxide.
16. The method according to any one of claims 1 to 14, wherein the etching agent is selected from hydrazine and difluoroxenon.
17. The method of any one of claims 1 to 16, wherein the etching agent further comprises hydrogen fluoride.
18. A process for tailoring the geometry of a nanopore formed by the method of any one of claims 1 to 17, comprising the steps of: (1) controlling the composition of the material and the refractive index of the material; and / or (2) controlling one or more parameters of the etching step: etching temperature, etchant composition, and etchant concentration; A process for tailoring the geometry of the nanopore, comprising:
19. 20. The process of claim 18, wherein the nanopore geometry comprises one or more of a cone angle, a radius, and a symmetry.
20. 20. The process of claim 19, wherein increasing the etching temperature selectively reduces the cone angle of the nanopores.
21. 20. The process of claim 19, wherein increasing the etchant concentration selectively increases the cone angle of the nanopores.
22. 20. The process of claim 19, wherein increasing the etching temperature selectively increases the radius of the nanopores.
23. 20. The process of claim 19, wherein increasing the concentration of the etchant selectively increases the radius of the nanopores.
24. A membrane comprising one or more nanopores produced using the method of any one of claims 1 to 17.
25. A membrane comprising one or more nanopores prepared using the process of any one of claims 18 to 23.
26. A membrane having one or more nanopores, The film components include one or more of the following materials: amorphous silicon, silicon oxide, silicon nitride, silicon oxynitride, hafnium oxide, hafnium silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, and tin oxide; A membrane wherein the geometric shape of said one or more nanopores is conical.
27. 27. The membrane of any one of claims 24 to 26, wherein the density of the nanopores is ≥ 1 and ≤ 10 nanopores per square centimeter.
28. 28. The membrane of any one of claims 24 to 27, wherein the geometric shape of the one or more nanopores is simple conical, funnel-shaped, symmetric biconical or asymmetric biconical.
29. The film according to any one of claims 24 to 28, wherein the thickness of the film is 20 nanometers or more and 10,000 nanometers or less.
30. The membrane according to any one of claims 24 to 29, wherein the area of the membrane is 0.0001 mm2 or more and 25 mm2 or less.
31. The method of claim 4 , wherein the film is multi-layered.
32. 32. The method of claim 31 , wherein the film comprises a semiconductor comprising a doped silicon layer between silicon oxide and / or silicon oxynitride layers.
33. 33. The method of claim 32, wherein the nanopore is a gated nanopore.