Method and system for producing doped carbon nanomaterials

Molten carbonate electrolysis with doping elements produces doped carbon nanomaterials efficiently, addressing scalability and cost issues, resulting in materials with enhanced properties for various applications.

JP7551165B2Active Publication Date: 2024-09-17C2CNT LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022193507
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-02-21
Filing Date
2022-12-02
Publication Date
2024-09-17
Estimated Expiration
2038-02-21

AI Technical Summary

Technical Problem

Current methods for producing doped carbon nanomaterials, such as carbon nanotubes, graphene, and carbon nano-onions, are expensive, difficult to scale, and lack the ability to produce doped forms efficiently, limiting their applications in electronic wires, catalysts, and oxygen or charge storage materials.

Method used

A method involving molten carbonate electrolysis is used to produce doped carbon nanomaterials by adding doping elements like lithium sulfate or sulfur dioxide to the electrolyte, with controlled electrolysis conditions to achieve specific morphologies and doping, such as carbon nanotubes, graphene, or hollow carbon nanospheres.

Benefits of technology

This approach allows for the production of doped carbon nanomaterials with enhanced properties, including high conductivity and catalytic properties, in a cost-effective and scalable manner, suitable for diverse applications including electronic wires, catalysts, and improved oxygen or charge storage materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551165000007
    Figure 0007551165000007
  • Figure 0007551165000001
    Figure 0007551165000001
  • Figure 0007551165000014
    Figure 0007551165000014
Patent Text Reader

Abstract

A method for producing carbon nano-onions is provided. [Solution] A method for producing carbon nanomaterials including carbon nano-onions includes the steps of heating a carbonate electrolyte to obtain a molten carbonate electrolyte, placing the molten carbonate electrolyte between an anode and a cathode in a cell, including a nano-onion selective component in the cell, removing a nucleating agent from within the cell, passing a current between the cathode and the anode in the cell, and collecting carbon nano-onion growths from the cathode in the cell.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Copyright A portion of the disclosure of this application contains material that is subject to copyright protection. The copyright owner has no objection to the ability of anyone to copy the patent disclosure, if it appears in the Patent and Trademark Office patent file or records, but otherwise reserves all copyright rights whatsoever.

[0002] Priority This application claims priority to U.S. Provisional Patent Application No. 62 / 461,641, filed February 27, 2017, the entirety of which is incorporated by reference herein.

[0003] The present invention relates to the production of doped carbon nanomaterials (carbon nanomaterials to which small amounts of impurities have been added), and in particular to the production of doped carbon nanomaterials from molten carbonate electrolytes (electrolytic solutions). [Background technology]

[0004] Prior to the recognition of various unique carbon nanoscale structures such as fullerenes, nanotubes, and nanofibers beginning in 1985, the reduction of hydroxides and carbonates from barium chloride / carbonate melts to carbon (macroscopic, visible, macroscopic) in inorganic molten electrolytes was recognized as early as the late 1800s. Today, the primary methods for producing carbon-doped nanomaterials are arc discharge, laser ablation of carbon substrates, and catalytic thermal chemical vapor deposition (CVD). The doping of these carbon nanomaterials provides favorable properties, which were first found in carbon nanotube products. These techniques are expensive and difficult to implement on a large scale, resulting in the current high cost of doped carbon nanotubes. The related graphene and carbon nano-onion structures are even more expensive to synthesize by these techniques.

[0005] Some CVD doped carbon nanotubes have extraordinary and useful properties, including high electrical conductivity, catalysis, heavy metal removal, enhanced oxygen reaction rates, and improved charge storage. Sulfur doped carbon has certain potential applications, including heterogeneous catalysis, adsorption, and energy conversion and storage. However, to date, few approaches have been developed to essentially incorporate sulfur into the carbon matrix. N-type doped carbon has a range of potential applications, including oxygen oxidation and reduction, fuel cell catalysts, supercapacitors, and sensors. Boron doping is well known to create metallic carbon nanotubes and enhance the conductivity of carbon nanotubes. Similarly, P-type doping of carbon can greatly affect their properties and applications, including lowering elongational breakage, as an aerobic oxidation catalyst, in batteries, and in ultrasensitive sensors. Boron and nitrogen are the most studied carbon dopants (impurities added to carbon) due to their close size (and atomic number) to carbon.

[0006] Carbon nanomaterials have great potential as a material resource, and their applications range from reinforced composites, capacitors, lithium-ion batteries, nanoelectronics, and catalysts to the main components of lightweight and strong building materials due to their excellent properties of strength, electrical and thermal conductivity, flexibility, and durability. Chemical vapor deposition or organometallic reactions using arc discharge are one of the major valuable, but expensive, methods for producing carbon nanomaterials. When doping of carbon nanomaterials is attempted by these production methods, it is generally achieved as a post-synthesis treatment following these expensive synthesis steps. One of the recent innovations is the use of melt electrolysis for carbon nanomaterial production. In this process, a molten carbonate electrolyte is placed between a cathode and an anode, a transition metal nucleating agent is added, and an electric current is applied to the cathode. This process produces a carbon residue on the cathode in one step and with low energy, which may contain carbon nanomaterials. The cathode in the melt electrolytic production of carbon nanotubes is the electrode on which the carbon products are deposited.

[0007] Previously, it was the understanding of the prior art that carbon nanomaterials produced by molten carbonate electrolysis are undoped. It has not been anticipated or even considered to produce doped carbon nanomaterials in a simple one-step synthesis by adding a doping material during electrolysis. The reasoning behind the hypothesis was that both the control of doping and the control of electrolyte deposition are highly orchestrated and complex activities. Hence, it has never been considered before that both doping and electrolyte growth of carbon nanomaterials can occur synergistically at the same time in a molten medium at 700-800°C.

[0008] Thus, there is a limit to the types of carbon nanotubes that can generally be produced on a substrate by melt electrolysis. The inherent challenge with the use of undoped carbon nanomaterials is that while they retain excellent qualities of strength, thermal conductivity, and flexibility, they are not differentiated with respect to the target qualities as electronic wire replacements, specialty catalysts, heavy metal adsorbents, or improved oxygen or charge storage materials. These undoped carbon nanomaterials alone would not be candidates to expand the demands of the current carbon nanomaterial market. The low-cost, high-strength doped carbon nanomaterials constitute a large potential market for these materials as lighter weight replacements for wires, catalysts, and electrodes.

[0009] Thus, there is a demand for the production of doped carbon nanomaterials, including carbon nanotubes, graphene, carbon nanoonions, and hollow carbon nanospheres, which may further enhance the utility of carbon nanomaterials. Lack of uniformity is a challenge in the deployment of doped carbon nanomaterials produced by molten carbonate electrolysis. Previous barriers to doped carbon nanomaterials produced from molten carbonate carbon nanotube synthesis from carbon dioxide are being overcome, allowing doped carbon nanomaterials in one-pot molten electrolyte production. These materials are suitable for differentiated qualities as electronic wire replacements, specialty catalysts, heavy metal adsorbents, or improved oxygen or charge storage materials. However, doping elements that enable the production of doped carbonate electrosynthesized carbon nanomaterials have not been found.

[0010] The electrolytic process for producing carbon nanotube products is premised on the assumption that there is no effect of doping additives to the electrolyte, or to the cathode where carbon nanomaterials are formed, or to the anode where oxygen is produced in the electrolyte separation of molten carbonate into carbon and oxygen. In the electrolytic process, the cathode serves to provide nucleation sites but is not considered a source of dopants, and the anode is considered to provide a stable oxygen layer effective as an electrocatalyst to produce oxygen during electrolysis but is not considered a source of dopants during synthesis.

[0011] For example, it was previously thought that only the most dominant electrolyte additives affect the growth rate of carbon nanomaterials and are related to their morphology, and thus the only additives of importance to the electrolyte are transition metal salts, which are reduced on the cathode and act as nucleating agents, producing oxides that are tangled rather than straight carbon nanotubes. No salt or gas additives in the electrolyte were considered as potential sources of dopants during the growth of carbon nanomaterials. Summary of the Invention [Problem to be solved by the invention]

[0012] Thus, there is a need for an effective method to produce doped carbon nanomaterials from molten carbonate materials. There is also a need to selectively produce different morphologies of doped carbon nanomaterials, such as carbon nanotubes, carbon nano-onions, graphene, or hollow carbon nanospheres, each of which includes unique utilities such as high strength, electrical conductivity, lubricity, high surface catalytic properties, and ion storage in batteries. There is also a need to control both the morphology and doping of carbon nanomaterials during molten carbonate electrolysis. [Means for solving the problem]

[0013] In one aspect, a method for producing a doped carbon nanomaterial is disclosed. A carbonate electrolyte is heated to obtain a molten carbonate electrolyte. The molten carbonate electrolyte is placed between an anode and a cathode in a cell. A nanomaterial doping element, such as lithium sulfate or a sulfur dioxide (SO2) gas anode, is included in the electrolyte of the cell. An electric current is passed through the anode and cathode in the cell. Doped or undoped carbon nanomaterial growth is collected from the cathode of the cell.

[0014] Another example is a method for producing undoped carbon nano-onions. Graphene or hollow carbon nanospheres are disclosed. A carbonate electrolyte is heated to obtain a molten carbonate electrolyte. The molten carbonate electrolyte is placed between an anode and a cathode in a cell. The transition metals that promote carbon nanotube growth are removed and nanomaterial morphology selection factors are included, such as adding zinc oxide or applying an alternating current. An electric current is passed through the cathode and anode in the cell. Undoped carbon nanomaterial growth, including primarily carbon nano-onions, graphene platelets, or hollow carbon nanospheres, is collected.

[0015] Another example is a system for producing carbon nanomaterials. The system includes a current source. The system includes a cell that holds a molten carbonate electrolyte between a cathode and an anode. A carbon nanomaterial doping component is located within the cell. The current source is capable of passing a current through the cathode and the anode within the cell, producing a doped carbon nanomaterial growing from the cathode within the cell.

[0016] Further aspects of the present invention will become apparent to those skilled in the art upon review of the detailed description of the various embodiments, together with the figures and brief description provided below. [Brief description of the drawings]

[0017] [Figure 1A] FIG. 1A is a block diagram of an electrolysis system for producing doped carbon nanomaterials from carbonates.

[0018] [Figure 1B] FIG. 1B is an illustration of several different techniques for producing carbon nanotubes and multiple morphologies of graphene carbon.

[0019] [Figure 2A] FIG. 2A shows an SEM image of the product and a graph of the electrolysis potential measured using an inert iridium anode and a Monel cathode.

[0020] [Figure 2B] FIG. 2B is an SEM image of the carbon nanotube product using copper or Monel anodes with more nickel powder added in a lithium carbonate (Li2CO3) electrolyte at 770° C.

[0021] [Figure 3A] FIG. 3A is an SEM image of product growth at the cathode-electrolyte interface under low nickel powder / iridium anode conditions, shown with the product peeled off from a Monel cathode.

[0022] [Figure 3B] FIG. 3B is an SEM image of the absence of a nucleating agent, in which nanostructures such as platelets rather than carbon nanotubes dominate the product formation.

[0023] [Figure 3C] FIG. 3C is an SEM image without the use of a nucleating agent, showing the growth of very thin graphene platelets and small carbon particles.

[0024] [Figure 4A]FIG. 4A shows different SEM images of carbon nanotubes and carbon nano-onions produced using a nickel-chromium anode and a Monel cathode.

[0025] [Figure 4B] FIG. 4B is an SEM image of the carbon nanotube containing nano-onion carbon product and hollow nanosphere product obtained without current cycling.

[0026] [Figure 4C] Figure 4C is an SEM image of nano-onion carbon obtained by adding zinc oxide to Li2CO3 electrolyte at 770 °C without cycling.

[0027] [Diagram 5] FIG. 5 is an SEM image of the boron doped carbon nanotube product.

[0028] [Figure 6] FIG. 6 shows SEM images of sulfur- or nitrogen-doped carbon nanotube products formed by electrolysis of Li2CO3 with either dissolved lithium sulfate (Li2SO4) or lithium phosphate (LiPO3), the respective sources of sulfur or phosphorus within the carbon nanotubes.

[0029] [Figure 7A] FIG. 7A is a table of experimental data showing that the carbonate electrolyte absorbs carbon dioxide at a rate sufficient to sustain maximum rates of molten electrolyte electrolysis and provides sufficient insulation so that molten carbonate electrolysis is self-heating and / or generates useful residual heat.

[0030] [Figure 7B] FIG. 7B is a plot of data obtained from the experimental data of FIG. 7A.

[0031] [Figure 7C]FIG. 7C is a graph showing that proper insulation retains most of the heat in the molten electrolysis chamber.

[0032] [Figure 7D] FIG. 7D is a graph showing that molten carbonate electrosynthesis is self-heating.

[0033] [Figure 8] FIG. 8 illustrates a synergistic pathway for doped or undoped carbon nanotube materials, including carbon nanotubes, graphene, carbon nano-onion, or hollow carbon nanosphere carbon nanomaterials.

[0034] While the invention is susceptible to various modifications and alternative forms, specific forms have been shown by way of example in the drawings and are described in detail herein. It should be understood, however, that the disclosure is not intended to be limited to the particular forms disclosed. Rather, the invention is intended to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the invention as defined by the appended claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The present invention can be embodied in many different forms. Representative examples are shown in the figures and described in detail herein. The present disclosure is an example or illustration of the principles of the present disclosure, and is not intended to limit the broad interpretation of the disclosure to the described examples. To that extent, elements or limitations disclosed, for example, in the excerpt, summary, and detailed description sections, but not expressly set forth in the claims, should not be incorporated into these claims, either by implication, inference, or otherwise, singular or collectively. Furthermore, for purposes of the detailed description, the singular includes the plural and vice versa, unless expressly stated otherwise, and the word "including" means "including without limitation." Furthermore, words that mean approximations, such as "about," "almost," "approximately," and "approximately," are used herein to mean, for example, "at, near, or in the vicinity of," or "within 3 to 5%," or "within acceptable manufacturing tolerances," or logical combinations thereof.

[0036] FIG. 1A is a block diagram of an example of a system 100 for producing doped carbon nanomaterials from carbonate materials. The system 100 includes a carbonate furnace 102, an electrolysis chamber 104, and a collector 106. Although the furnace 102, electrolysis chamber 104, and collector 106 are shown as separate components in FIG. 1A, they may be in the same physical structure. The electrolysis chamber 104 includes a chamber 110 (cell) that holds the molten carbonate electrolyte produced by the heated carbonate in the furnace 102, and further includes a morphology element 120 to maximize the production of carbon nanotubes compared to graphene, compared to nano-onions, compared to hollow nanospheres. The chamber 110 includes a doping element 122 to maximize product formation of doped carbon nanomaterials versus undoped carbon nanomaterials. The anode 112 and cathode 114 are coupled to a power source 116. The anode 112 and cathode 114 are inserted into the chamber 110. Carbon dioxide (CO2) from a CO2 source 118 is injected into the molten carbonate electrolyte. CO2 is optionally injected into the molten carbonate electrolyte to react with oxygen and renew the electrolyte rather than being consumed, and without CO2 injection, the electrolyte would be consumed and its level would drop during the electrolysis reaction, as CO2 is converted to O2 at the anode 112 and converted to carbon nanomaterials at the cathode 114 in the overall reaction of the electrolyte. The injection of CO2 can be active (e.g., bubbling), or passive (direct dissolution from the gas at the air / electrolyte interface), or a combination of the two (gas inflow or electrolyte mixing). A variety of CO2 sources may be the CO2 source 118.

[0037] The carbonate furnace chamber 102 heats carbonate electrolytes, such as pure lithium carbonate (Li2CO3), to their respective melting points to produce molten carbonate electrolyte. There may be various ways to power the carbonate furnace chamber 102, such as solar energy or a conventional power generator. A transition metal is added via a distributor to act as a catalyst. The molten carbonate electrolyte is electrolyzed by placing it between the anode 112 and cathode 114 in the electrolysis chamber 104.

[0038] FIG. 1B is an illustration of different techniques for producing carbon nanotube and graphene carbon morphologies using the example system 100 shown in FIG. 1A. FIG. 1B shows a first process 120 and a second process 130 for producing carbon nanotube carbon morphologies on the cathode 114. FIG. 1B shows a first process 140, a second process 150, and a third process 160 for producing graphene carbon morphologies on the cathode 114. The processes 120, 130, 140, 150, and 160 are not limited to the theory or mechanism of using the system of FIG. 1A. As can be seen with reference to the processes 120 and 130 of FIG. 1B, the reaction in the presence of nucleation seeds, such as those using certain transition metals, results in the separation of carbon from the carbonate, leaving carbon products, such as carbon nanotubes, on the cathode 114 from the nucleation sites. Such growth may occur as a tip growth mechanism as shown in process 120 of FIG. 1B, or as a root growth mechanism as shown in process 130. Of course, other growth mechanisms are also possible. As can be seen with reference to processes 140, 150, and 160 of FIG. 1B, in the absence of nucleation seeds of a given transition metal, a pulsed electrolysis current is added to the reaction to separate carbon from the carbonate, form carbon products, and combine into carbon nanotube morphologies, such as the graphene products shown. The first process 140 uses an unbiased cathode 114. As in the second process 150, the cathode 114 may be forward biased. In process 160 of FIG. 1B, carbon nanotube morphologies are extruded from the cathode 114 during the alternating current reversal period. The resulting carbon products are collected at the collector 106, while oxygen is produced at the anode 112. The separated carbon nanomaterial may be washed with a solvent or separated from the molten electrolyte by high temperature phase separation or filtration.

[0039] In this example, carbon nanotube growth enhancing elements are added to the cell 110, which contains an anode 112, a cathode 114, and a carbonate electrolyte. The carbon nanotube growth enhancing elements may include nickel, copper, chromium, iron, brass, manganese, titanium, zirconium, molybdenum, tantalum, cobalt, silicon, carbon, and alloys and mixtures thereof. In the presence of transition metals such as nickel, which act as nucleation sites, carbon nanotube formation and growth occurs readily under a wide variety of conditions in a lithium carbonate mixed molten electrolyte. The transition metal is provided by dissolution of the anode during initial stabilization of the anode surface, or, in the case of an inert oxygen anode such as iridium, is added to the electrolyte as a metal or salt. As described below, the carbon nanotube growth enhancing elements may be transition metals or transition metal salts added to the cathode material, anode material, or electrolyte. In this example, the carbonate electrolyte at 770°C is lithium carbonate (Li2CO3), with a current of 0.1 A / cm 2 The electrolysis was carried out in a 1 wt% nickel metal powder for carbon nanotube growth that was initially added to a carbonate electrolyte. The cathode 114 was made of Monel or copper alloy.

[0040] FIG. 2A shows an SEM image of nanotube type product morphology with more nickel powder added to Li2CO3 electrolyte at 770° C. FIG. 2A also shows a graph 210 of the product and a graph of the electrolysis potential measured for the use of an inert iridium anode and a Monel cathode for the process. FIG. 2A shows an SEM image 200 of the carbon product where the electrolysis was carried out with an iridium anode. Iridium is very stable and does not release transition metal nucleation ions into the electrolyte. Even in this case, when nickel powder is instead added to the electrolyte to induce nucleation at the cathode, a uniform carbon nanotube product is observed in the SEM image 200.

[0041] FIG. 2B shows SEM images 220, 222, 224, and 226 of carbon nanotube production with copper or Monel anodes when more nickel powder was added to the Li2CO3 electrolyte at 770° C. Images 220 and 222 show the production from a copper cathode when an iridium anode was used with 0.5 wt% cobalt oxide (CoO) added to the electrolyte instead. Image 224 shows the production from a copper cathode when a nickel chromium anode was used with 1 wt% nickel addition. Image 226 shows the production from a Monel cathode when a nickel chromium anode was used with 1 wt% nickel addition.

[0042] The products in images 220, 222, 224, and 226 of FIG. 2B are from electrolysis with a nickel-chromium anode, not an iridium one. SEM images 220, 222, and 224 show uniform carbon nanotubes formed, and show short carbon nanotubes formed at the copper cathode. SEM image 226 shows long carbon nanotubes formed at the Monel cathode. As shown in images 220 and 222 of FIG. 2A, uniform carbon nanotube products are formed using an iridium anode without the addition of nickel powder, and with 0.5 wt% cobalt oxide CoO added to the electrolyte. Monel alloys are alloys of nickel, copper, and small amounts of iron, manganese, carbon, and silicon. Different carbonate electrolytes may also be used, such as lithium carbonate, sodium carbonate, potassium carbonate, strontium carbonate, rubidium carbonate, cesium carbonate, barium carbonate, and calcium carbonate.

[0043] Images 300 and 302 in FIG. 3A show product growth at the cathode-electrolyte interface under low nickel powder / iridium anode conditions using a product exfoliated from a Monel cathode. As shown in image 300, the sample includes layer 310, transition layer 312, and graphene layer 314. Images 300 and 302 show an example of limited availability of nucleation metals using an iridium anode with only 0.1 wt% nickel powder added in a Li2CO3 electrolyte at 770° C. The product in SEM image 300 is 5 cm 2 0.1A / cm2 on a Monel cathode 2 Figure 3 shows the product after extended (48 hours) molten carbonate CO2 electrolysis at 300°C, showing that the product consists of thin, multi-layered graphene. Thin, multi-layered graphene sheets are produced from electrolysis with low transition metal nucleation site inhibition. The electrolysis is further restricted to an iridium anode (which does not release transition metal ions into the electrolyte), low levels of nickel powder added to the electrolyte (0.1 wt% instead of 1 wt%), and a Monel sheet cathode. Upon cooling, the product is easily peeled off from the Monel cathode, and SEM image 302 shows the clean product. The electrode side of the peeled layer is clearly visible in the center of SEM image 302, and the contained product growth occurs to the right of the layer. The contained product consists of a mixture of partially formed carbon nanotubes mixed with multi-layered graphene sheets, and it is clear that restricting the nucleation seeding points promotes graphene formation compared to carbon nanotubes in the CO2 inhibited product.

[0044] Figure 3B shows SEM images 320, 322, 324, and 326, which show that in the absence of a nucleating agent, nanostructures such as platelets, rather than carbon nanotubes, dominate the product growth. Figure 3C shows SEM images 330, 332, 334, and 336, which show that in the absence of a nucleating agent, very thin graphene platelets and small carbon particles grow. SEM images 330 and 332 show the product formed with a Monel cathode, and SEM images 334 and 336 show the product formed with an iron cathode.

[0045] The products of images 320, 322, 324, and 326 of FIG. 3B and images 330, 332, 334, and 336 of FIG. 3C are 0.1 A / cm 2 The SEM image 320 shows that no carbon nanotube product morphology is formed when no transition metal nucleating agent is included in the electrolysis cell. The product in SEM image 320 was produced using a copper cathode combined with a nickel anode. This process is an extended pure Li2CO3 electrolysis at 770 °C, with a large 100 cm 2A planar copper cathode and nickel anode are used. With the same electrolyte, SEM image 322 shows the cathode product using an iron cathode and an iridium anode, without the addition of a (nickel) transition metal to the electrolyte. The eutectic mixed carbonate of lithium, sodium, and potassium, LiNaK, reduces the melting point of the carbonate below 400°C. Potassium carbonate significantly inhibits the formation of carbon nanotubes. The electrolysis product of the mixed potassium carbonate electrolyte is observed to start to show disordered nanostructure characteristics above 600°C, which increases with increasing temperature. However, LiNaK carbonate has not been observed to form carbon nanotubes in high yields. The electrolysis of LiNaK, but not pure lithium, produces only low yields of carbon nanotubes (less than 15%) under all electrolysis conditions. SEM image 324 shows the product formed in the mixed potassium carbonate (with lithium and sodium) electrolyte at 770°C. The product shown in SEM image 324 is complex, but the majority of the product consists of very thin, multi-layered graphite platelets, with the largest width observed being ~10 mm wide (not shown). SEM image 326 shows that at low temperatures, platelets form in the lithium carbonate, even with the addition of iron oxide and lithium oxide. SEM image 326 shows that Li2CO3 with 8 wt% lithium oxide (Li2O) and 0.4 wt% iron oxide (Fe2O3) at 730 °C exhibits a 0.1 A / cm 2 1 shows the products formed by electrolysis of 1,2-dichloroethane using a nickel anode and an iron cathode.

[0046] As shown in SEM images 330, 332, 334, and 336 in Figure 3C, when platinum or iridium anodes are used, limited or no nucleation metals are present, and little or no nickel is added to the Li2CO3 electrolyte at 770°C, no carbon nanotubes are observed and the product consists of very thin multi-layered graphene sheets. The electrolysis time was 0.5 h, iridium electrodes and Monel cathodes were used, and 0.1 A / cm 2When the electrolysis time is limited to 30 min with an iridium electrode, the product is uniform, multi-layered graphene sheets and no other carbon nanostructures. With a platinum electrode, a low electrolysis potential (1.2 V) and an iron cathode, the product is 0.1 A / cm 2 After 1.5 hours of electrolysis, small carbon particles are intermingled with the primary carbon platelet product, as shown in SEM image 330. Image 330 shows the product produced using an iridium anode and only 0.1 wt% nickel powder added to a Li2CO3 electrolyte at 770° C. SEM image 332 shows the product produced using a 5 cm 2 Monel cathode, 0.1A / cm 2 Figure 3 shows the product of extended (48 hours) molten carbonate CO2 electrolysis of 1000 sq. m. The resulting product has thin, multi-layered graphene. SEM images 334 and 336 show the product from an experiment without nickel. When a platinum anode is used, no nucleation metal is used, and no nickel is added to the electrolyte, no carbon nanotubes are observed, and the product consists of very thin multi-layered graphene sheets, and small carbon particles, as shown in SEM images 334 and 336. The product is 5 cm 2 iron cathode, Li2CO3 electrolyte at 770 °C, and 0.1 A / cm 2 It was produced by electrolysis at 400 K for 3 hours.

[0047] Figure 4A shows a current of 0.1 A / cm using a nickel-chromium anode and a Monel cathode. 24A shows an SEM image 400 of long carbon nanotube growth with a constant electrolysis current of 0.1 A / cm at a measured electrolysis potential of 1.6 V. FIG. 4A also shows an SEM image 402 of carbon nano-onions produced under the same conditions with the addition of a step of cycling the current. FIG. 4A also includes a graph 404 showing the cycling of the current to produce the carbon nano-onions in image 402, rather than the carbon nanotube product. That is, the SEM image 400 shows the results of electrolysis of CO2 in Li2CO3 at 770° C., aging for 24 hours (to obtain an equilibrated electrolyte), immersing a Monel cathode and a nickel-chromium anode, and then electrolysis at 0.1 A / cm at a measured electrolysis potential of 1.6 V. 2 Figure 1 shows the carbon nanotube wool product produced by applying a constant electrolysis current of 10 ... 2+ ), but enough of them are released into the electrolyte and redeposited on the cathode as carbon nanotube nucleation sites. 2It is observed that the carbon nanotube wool, which also works as an effective and stable anode when a high current (0.2 V increase at 1000 V) is required, releases both nickel and chromium into the electrolyte, and longer carbon nanotube products are formed upon extended electrolysis. These longer carbon nanotubes, or "carbon nanotube wool", reach long macroscopic (0.2 to 2 mm, visible) lengths while retaining nanoscale diameters when Monel (nickel-copper alloy) is used instead of iron, titanium or nickel as the cathode, and very small carbon nanotubes are synthesized when a copper cathode is used. Comparing the SEM images 220, 222, and 224 in FIG. 2B with the images 226 and 200 in FIG. 2A and the SEM image 400 in FIG. 4A, it can be seen that carbon nanotubes of various lengths may be uniformly produced; i.e., the lengths may be longer than 100 μm, between 1 and 100 μm, or less than 1 μm.

[0048] SEM image 402 shows that by varying the electrolysis current, rather than direct current, as shown in current graph 404, a completely different morphology of electrolysis product can be obtained. In this example, identical electrolysis conditions are applied to produce the product shown in image 400, except that the potential is kept below 1.2V and cycled, and instead of long carbon nanotube morphology, the product at the cathode is observed to be carbon "nano-onions" as shown in image 402. The observed nano-onion carbon morphology is a new product obtained from simple CO2 electrolysis by limiting the electrolysis to constant current density and cycling low potentials. The nano-onion carbon product could be worth over a million US dollars per ton if synthesized via the more expensive CVD method.

[0049] FIG. 4B shows the first image 440 of the carbon nanotube containing nano-onion carbon product obtained when zinc coated iron was used as the cathode or zinc oxide (ZnO) was added to the electrolyte and iridium was used as the anode without current cycling. SEM image 442 shows the hollow nanosphere product formed (along with the carbon nanotubes) with the lithium / magnesium mixed carbonate electrolyte. SEM image 444 shows the predominantly thin-walled carbon nanotube product with the lithium / calcium mixed carbonate electrolyte.

[0050] SEM image 440 shows larger carbon nano-onion products produced by applying DC rather than AC as the electrolysis current. Instead, a zinc-coated (galvanized) iron cathode and an iridium anode are used in the electrolysis. Zinc has a melting point of 420° C., which facilitates the production of these larger-looking carbon nano-onion products. However, when a low-current pre-electrolysis step is added, transition metal nucleation points begin to form on the cathode, and uniform carbon nanotube products predominate (not shown). This low-current pre-electrolysis step, along with replacing the pure Li2CO3 electrolyte with a mixture containing 5% lithium borate (LiBO2), 11.4% magnesium carbonate (MgCO3), 0.6% zinc oxide (ZnO), and 83 wt.% lithium carbonate (Li2CO3), results in the formation of a product of mostly hollow nanosphere products (along with carbon nanotubes), as shown in the washed product in SEM image 442. The product in SEM image 442 contains magnesium oxide (MgO) deposits (suggesting that, unlike lithium oxide (Li2O), MgO is highly soluble in Li2CO3). A similar mix of electrolyte with calcium carbonate (CaCO3) rather than magnesium carbonate (MgCO3) results in a primarily thin-walled carbon nanotube product, as shown in image 444.

[0051] FIG. 4C shows SEM images 460, 462, and 464 of nano-onion carbon products, instead of carbon nanotubes, obtained when zinc oxide was added to Li2CO3 electrolyte at 770° C. without cycling. SEM images 460, 462, and 464 show carbon nano-onion products formed from CO2 on a copper cathode in extended electrolysis. The electrolysis products in SEM images 460, 462, and 464 were obtained when zinc oxide was added to Li2CO3 electrolyte at 770° C., with a copper cathode and nickel anode, at 0.2 A / cm 2 By applying an average electrolysis potential of 1.2 V, extended electrolysis (19.5 h at 20 A, total charge 3.9 Ah / cm) was achieved. 2 ) to obtain uniform and larger (0.5 to 1 μm) carbon nano-onion products. These electrosyntheses were performed at 100 cm 2 This was performed with a planar electrode. Smaller carbon nano-onions (not shown) were formed with a shorter electrolytic charging time.

[0052] FIG. 5 shows two SEM images 500 and 502 of boron doped carbon nanotubes (BNTs) formed during electrosynthesis in Li2CO3 electrolyte with 9 wt% additive at 770° C. In 5 g (grams) of lithium metaborate (LiBO2) and 50 g of lithium carbonate (Li2CO3), 5 cm 2The characteristics of boron doped carbon nanotubes formed at 1 Ah (ampere hour) with a cathode of 1000 mAh are shown in SEM images 500 and 502. The effect of increasing the LiBO2 concentration on the product in images 500 and 502 is shown by a shift in the Raman spectrum shown in spectrograph 510 and an increase in the electrical conductivity of the carbon product shown in graph 512. Graph 512 shows increasing the concentration of LiBO2 dissolved in Li2CO3 electrolyte and the electrical conductivity of the carbon nanotube product. Spectrograph 510 shows the Raman spectrum of boron doped carbon nanotubes. Graph 512 shows the spectrum from bottom (black) to top (gray) for the electrosynthesis of 1.5 g, 3 g, 5 g, and 8 g of LiBO2 added to 50 g of Li2CO3.

[0053] Pure boron oxide (B2O3) has a melting point of 450°C, is white, but is transparent when melted, and the melt is a glass insulator. However, when molten B2O3 contains dissolved lithium oxide (Li2O) (melting point 1438°C, white, transparent when melted), it becomes an electrochemically conductive liquid. The binary system of B2O3 and Li2O has a complex phase diagram, with a wide range of homogeneous liquid phases above 767°C. Here, lithium metaborate, LiBO2 (melting point 849°C, white), a chemically bonded salt of the oxides of boron and lithium, is very soluble in Li2CO3 (melts transparent), retains very high electrochemical conductivity, and is a good additive for the one-pot synthesis of boron-doped highly electrically conductive carbon nanotubes (boron-doped highly electrically conductive carbon nanotubes).

[0054] The carbonate electrolysis method for converting CO2 into doped carbon nanotubes is straightforward and, without being bound by any theory, involves a single step in which the desired dopant is added during synthesis, e.g., in carbonate electrolysis, this occurs simultaneously with the production of oxygen and dissolved lithium oxide. Li2CO3(liquid)+dopant→C(CNT doped) + Li2O(dissolved) + O2(gas) (1) Li2CO3 is consumed by electrolysis, but is constantly replenished by reacting this excess Li2O, which is formed as a product in the electrolysis reaction (1), with CO2 from the air (or with high concentrations of CO2 obtained from the exhaust). Li2O(dissolved)+CO2(gas)→Li2CO3(liquid) (2) The final reaction (combination of reactions (1) and (2)) is: CO2(gas)+dopant→C(CNT doped ) + O2(gas) (3)

[0055] The washed and boron-doped product (B-doped product) is shown in images 500 and 502. Higher levels of LiBO2 (greater than 10% by mass) added lead to increased levels of non-uniform impurities in the carbon nanotube product (not shown). In particular, very high quality, straight carbon nanotubes were formed in systems containing 50 g Li2CO3 plus less than 10% by mass of LiBO2, e.g., 1.5 g, 3 g, or 5 g LiBO2, respectively. However, as can be inferred from SEM images 500 and 502, amorphous carbon nanoparticles were present in the product, within the range of 10%. When 5 g of LiBO2 was added, a distribution of carbon nanotube diameters (200 to 500 nm (nanometers)) was observed, which was somewhat larger than that observed when no LiBO2 was added at all. When 8 g LiBO2 (>10%) was added, the diameters of the carbon nanotubes were very widely distributed, ranging from 150 nm to 1.5 μm, indicating that they became heterogeneous with the addition of more LiBO2. High levels of LiBO2 may change the macroenvironment of reduction at the cathode and / or deposition of boron on the nickel nuclei may lead to the formation of nickel boride (NiB) instead of pure nickel, resulting in less nanostructures and a more heterogeneous growth pattern. When 17 wt% LiBO2 was added to the Li2CO3 electrolyte, particulates rather than nanotubes became the major product.

[0056] To determine whether the resulting carbon nanotubes were boron doped or a mixture of boron and pure carbon nanotubes, Raman spectra were recorded using a 532 nm incident laser and are shown in graph 510 of FIG. 5. For conventional (boron-free) electrosynthesized carbon nanotubes produced from pure lithium carbonate electrolyte, E 2g The G band associated with graphite in the planar mode of symmetry is at 1575 cm -1However, in the samples with added LiBO2, the G band shifts to higher wavenumbers. This upshift indicates that holes (hole carriers) are transferred from boron to the carbon nanotubes. The charge transfer shortens the C-C bonds, increasing the force constant and enhancing the lattice frequency of the carbon nanotubes. Thus, the shift of the G band to higher frequencies is attributed to the deformation of the graphite structure due to the increased boron concentration. As seen in images 500 and 502, when either 1.5 g, 3 g, 5 g, or 8 g of LiBO2 were added to the electrolyte before electrosynthesis, after synthesis, the G band of the product was at 1583, 1587, 1589, and 1600 cm, respectively. -1 According to the linear relationship between the G band shift and the boron doping level in Ishii et al.'s study, the boron content was estimated to be about 0.7 to about 2 at% (atomic percent). Furthermore, the DG ratio, which is the intensity ratio of the D band associated with irregular and amorphous graphite to the G band of graphite, increases with increasing added LiBO2. This indicates that the number of defects increases with increasing boron doping level. Boron doping is a process that increases the number of defects in the B X C Y Generate domains, e.g. low doping levels 34 BC3, high doping levels of B4C, B 13There are C2 domains and increased defects in the carbon nanotubes. Each of these features in the spectrum indicates that the resulting sample is a boron-doped carbon nanotube, rather than a mixture of elemental boron and pure carbon nanotubes. It should be noted that the boron content in the boron-doped carbon nanotubes is significantly different from the boron / carbon ratio (B / Cratio) in the electrolyte. For example, when 50 g Li2CO3 and 8 g LiBO2 are added, the boron / carbon ratio in the electrolyte is 31 at% but the resulting boron in the carbon nanotube sample product is only about 2%. There is no indication that excess LiBO2 in the electrolyte is detrimental (other than increased conductivity, as will be shown further), and this large difference between the percentage of boron added to the electrolyte and the percentage of boron in the product is related to the reduction voltage of lithium metaborate to elemental boron, which, according to thermodynamic calculations of the reaction (4) from the entropies and enthalpies of the individual species, is less than 2.15 V at 770 °C (1043 K). This is higher than the reduction of carbonate to carbon, which is less than 1.6 V, and would favor the formation of carbon over boron at the cathode if they were to be simultaneously deposited (depending on the reaction rate) at the cathode. 2LiBO2 → 2B+Li2O+3 / 2O2(4)

[0057] Boron doping is known to produce metallic carbon nanotubes and to increase the conductivity of carbon nanotubes (synthesized by CVD). To investigate the effect of boron dopant on the conductivity of carbon nanotubes synthesized by molten carbonate synthesis, samples with increasing boron dopant levels were prepared and compared to the products shown in images 500 and 502 of Figure 5. For comparison, the conductivity of amorphous carbon nanoparticles, straight carbon nanotubes, and entangled carbon nanotubes electrosynthesized from Li2CO3 melt was also measured. Carbon nanotubes synthesized in 9 wt% LiBO2 electrolyte showed an order of magnitude higher conductivity than straight carbon nanotubes (formed in pure Li2CO3) and 30 times higher conductivity than amorphous carbon nanoparticles or electrosynthesized entangled carbon nanotubes (addition of oxides, e.g., 4 m Li2O (10.7 wt%) in Li2CO3 electrolyte, adds defects and results in entangled carbon nanotubes). Among the boron doped samples, the conductivity first increased with the addition of 1.5 g LiBO2 to the composite electrolyte, up to 5 g LiBO2, and then decreased with increasing concentrations of LiBO2 added. Although boron doping improves the conductivity, too much boron (more than 10 wt% in the electrolyte) leads to degradation (reduced amount of carbon nanotubes and increased nanoparticles), and thus a maximum in conductivity was observed with the addition of LiBO2.

[0058] A successful and straightforward route for the one-pot electrosynthesis of boron-doped carbon nanotubes from carbon dioxide via the addition of soluble lithiated dopants to a molten carbonate electrolyte has been demonstrated here, suggesting that similar routes are possible for the synthesis of other doped carbon nanotubes, such as nitrogen, phosphorus or sulfur doped nanotubes. Inserting different dopants at different concentrations into carbon nanomaterials changes both their physical and chemical properties.

[0059] Boron and nitrogen have been the most studied carbon dopants due to their close size (and atomic number) to carbon. The common polyatomic anions, metaphosphates, nitrates, and sulfates, in which lithium is the cation (lithium metaphosphate (LiPO3), lithium nitrate (LiNO3) or lithium sulfate (Li2SO4)), are soluble in molten lithium electrolyte. The 3e required to form elemental boron as a dopant from lithium metaborate - In comparison with the reduction of LiBO2, LiPO3, and LiNO3, 5e is needed to form phosphorus or nitrogen elements, respectively. - Reduction is required, and Li2SO4 requires 6e to form sulfur. - is required for the reduction of carbon. Boron, phosphorus and nitrogen are less electronegative (negatively charged) than carbon, while sulfur is more electronegative (negatively charged). Thus, as a rough estimate (based on electronegativity, without any prediction of competing chemical reactions), carbon may be easier to form electrolytically from its oxide than boron, phosphorus or nitrogen, making the latter oxides good candidates as co-reduced elemental dopants in the electrosynthesis of carbon nanotubes, while sulfur may be a thermodynamically favorable reduction product for carbon nanotubes and may suppress their formation in sulfate-containing electrolytes.

[0060] 6 shows SEM images 600 and 602 of sulfur and nitrogen doped carbon nanotube products formed by electrolysis of Li2CO3 containing either dissolved Li2SO4 or LiPO3 as a source of either sulfur or phosphorus in the carbon nanotubes. SEM image 600 shows a long (300 to 600 μm) product of P-type heteroatoms, with a current density of 0.03 A / cm 2 Low current density in the middle of 0.8Ah / cm 2The nanotubes were produced electrolytically using a conventional (nickel 200) anode with no nickel powder added to the electrolyte, with a charge of 10 ...

[0061] SEM image 602 shows carbon nanotubes containing sulfur, from molten carbonate electrolysis with 0.1 mol% sulfate, followed by 2 hours of electrolysis at 1 A (using a conventional galvanized steel cathode and a nickel 200 wire anode, without the addition of nickel metal powder). Electron dispersive analysis of the carbon nanotube product measured 0.1 mol% sulfur in the carbon nanotube product. As in previous experiments, nucleation on the cathode was promoted by applying successively increasing low constant currents (10 min each) from 0.05, 0.10, 0.25 to 0.5 A, followed by extended electrolysis at higher currents. During the first 10 min, the lowest current electrolysis occurred at potentials of 0.4 to 0.5 V, consistent with expected nucleation with nickel on the cathode, and subsequent constant current increments occurred by increasing the potential between 1 and 2 V, respectively. In electrolysis of high sulfate concentrations, such as 1 mol% (or 3 or 5 mol%) Li2SO4 in Li2CO3 at 770 °C, no formation of carbon products (carbon nanotubes or otherwise) was observed at the cathode. The potential at which a current of 1 A was measured was lower with increasing Li2SO4 (lower than the 1-2 V electrolysis potential measured without Li2SO4). The lack of carbon nanotube formation at higher sulfate concentrations is due to the electronegativity of sulfur compared to carbon, which favors the thermodynamic formation of the former compared to the latter. Reducing the sulfate concentration (relative to carbonate) to improve the energetics of carbon formation creates a pathway for the formation of sulfur-containing carbon nanotubes.

[0062] Carbon nanotube products have also been observed from the electrolysis of LiNO3 in Li2CO3 electrolyte at 770 °C. In this case, carbon nanotube yields are improved with 5 mol% lithium nitrate dissolved in the electrolyte compared to 1 mol%. The added dissolved lithium nitrate is believed to be in equilibrium with the lithium nitrate in the molten electrolyte. This is similar to the known solid-state thermal decomposition for LiNO3 solid, which occurs above 500 °C. LiNO3 → LiNO2 + 1 / 2O2 (5) Electron dispersive analysis indicates the presence of nitrogen in the carbon nanotube product after electrolysis.

[0063] The dopants have been shown to be introduced by dissolving an oxide containing the dopant in the electrolyte during electrolysis. It is clear that pure elements or other salts can also be used to introduce the dopant additives. Examples of such additives include, by way of illustration and without limitation, sulfur, boron, thionyl chloride, sulfur chloride, silicon chloride, boron chloride, boron chlorate, thionyl nitrate, silicon nitrate and nitride, boron nitride, and boron nitrate.

[0064] This example shows that dopants may be injected into the electrolyte in the gas phase, rather than by dissolution of a solid or liquid in the electrolyte. The separation of the molten carbonate carbon dioxide electrolyte occurs easily (high current density) and with low energy (low electrolysis potential), with either low or high temperature inlet gas, which may be 0.04% (air), 5 to 13% (natural gas or coal-fired power flue gas), 33% (cement flue gas), or 100% CO2 concentration. Here, the gases are mixed to simulate coal plant flue gases containing average concentrations of sulfur dioxide (SO2) and nitrogen oxides (NOx). NOx, SO2 and CO2 are added continuously in the correct ratio to air through the blower duct inlet before entering the carbonate electrolyser. The CO2 inlet rate is measured and controlled to 76 L / min (equivalent to 200 kg of CO2 converted to carbon nanomaterials daily) by a calibrated Omega mass flow controller (MA5400 / 500) with an upper limit of 131 L / min. NOX is produced in the laboratory by the reaction of copper metal with nitric acid, the ratio being controlled by the strength of the acid and the relative thickness of the copper. A low concentration of nitric acid (4 mol of nitric oxide (NO)) produces more NO, while a high concentration of nitric acid forms pure brown nitrogen dioxide (NO2). Copper ions (Cu 2+ ) enters the electrolytic cell, the 4 moles of nitric acid gradually changes from colorless to blue. Similarly, sulfur dioxide (SO2) is produced by the direct reaction of sulfur powder with sulfuric acid. The inlet gas flow rate is monitored by an in-line Digi-Sense Hot Wire, a thermoanemometer with NIST traceable calibration. NOX and SO2 injected into the electrolytic cell at low ppm levels had no effect on the physical and chemical characteristics or formation of the observed carbon nanotubes.

[0065] This example shows that the carbonate electrolyte can absorb carbon dioxide at a rate sufficient to sustain the highest rates of molten carbonate electrolysis, and that with sufficient insulation, molten carbonate electrolysis can self-heat and / or generate useful excess heat. FIG. 7 is a data table 700 that shows the extremely rapid rates of carbon dioxide absorption from the gas phase into molten lithium carbonate and molten lithium carbonate mixtures, as measured and recorded experimentally. Even at the lowest carbon dioxide concentration studied (0.04% carbon dioxide using typical air), the absorption rate was 0.1 A / cm. 2 During electrolysis, which was performed at a constant current density of 1000 volts, the current density was sufficient to maintain and renew all of the molten lithium carbonate in an open air system. During electrolysis, lithium oxide is co-produced at the cathode and continuously reacts with carbon dioxide to renew the electrolyte. FIG. 7B shows a graph 710 representing the rate of carbon dioxide absorption from the data in data table 700. As shown in data table 700 in FIG. 7A, the absorption rate of even a small amount (50 g) of molten lithium carbonate bubbled into it does not limit the rate of absorption of carbon dioxide gas until the carbon dioxide inflow rate is well above 0.3 L per minute, and as expected (not shown), it further increases with the addition of lithium oxide concentration (as it is produced by the faster electrolysis rate). The cumulative carbon dioxide absorbed, on the vertical axis, is limited to just below 100% due to the natural lithium carbonate concentration that occurs at equilibrium in the lithium carbonate electrolyte. The fastest electrolysis experimented here was at 1 amp / cm. 2 and the CO2-containing gas must be bubbled through the electrolyte otherwise the electrolyte will be consumed and the electrolyte level will drop appreciably relative to the electrolyte when the mass of the electrolyte is held constant by bubbling.

[0066] 7C is a graph 720 showing that the majority of the heat is retained within the molten electrolysis chamber with sufficient insulation. In a kiln built using 9×4.4×2.4 inch refractory bricks with 24×9×4 inch refractory bricks (purchased from BNZ Materials) and heating elements and control circuitry from a commercial Paragon Caldera kiln, a custom radiant heat shield cut from 0.034 inch thick mirror-finished 304 stainless steel (purchased from onlinemetals.com) was added as an intermediate vessel to the kiln, and heat retention was seen to improve with increasing levels of insulation. A one-inch thick, highly insulating, rigid ceramic insulation was installed as a thermal protection barrier on all sides, with a high temperature resistance and very low heat flow (0.28K at 800°C, part number 6841K5 ultra-high temperature ceramic insulation purchased from Mcmaster.com), and is visible as a white outer border on the kiln cover during construction, in addition to the gray furnace chamber mortar. Before adding the carbonate electrolysis chamber, a fourth layer of insulation (in addition to the brick, radiant barrier, and ceramic insulation) was added to the kiln in the form of mineral insulation (lime-green, Mcmaster.com product No. 9328K43, 2-inch thick, 65-C mineral wool insulation sheet for extra high temperatures), and finally, an exterior coat of pink R-30 Home Depot insulation was added as the final insulation against heat loss, as seen in the photo below (before reinserting the electrolysis chamber). R-30 exterior insulation (purchased from Home Depot as general household insulation) was finally added before adding the outermost layer of the kiln.

[0067] FIG. 7D is a graph 730 showing that molten electrolyte electrosynthesis is self-heating. The major breakthrough is reaching the limit of thermal equilibrium where, despite the high temperatures of the molten salt process, the molten carbonate process does not require any external heating. A custom-built kiln with a carbonate electrolysis chamber was heated to 725° C. (higher than the melting point of lithium carbonate electrolyte), then all heating power switches in the kiln were turned off and the kiln was unplugged. 0.1 / cm 2 In constant electrolysis of , the carbon dioxide to carbon nanotube process was independently maintained at a constant temperature of 727 °C. According to the expected exothermic nature of the reaction of CO2 with Li2O, which constantly renews the electrolyte (and absorbs CO2), it is observed that this temperature rises to 737 °C when CO2 (unheated, pure) is bubbled in at a very precise rate that matches the rate at which CO2 is consumed by electrolysis. This temperature is reached when the current density (proportional to the flow rate of CO2) is 0.5 A / cm 2 If the current density is increased to 0.3 A / cm, the temperature rises to 787°C. 2 750° C. when the current was reduced to 0.3 A / cm 2 The graph shows the electrolysis performance at a constant current density of 750°C, which was maintained constant throughout the electrolysis. An outlier measurement during the experiment was not included in graph 720 due to a poor thermocouple connection, which has been corrected.

[0068] One-step molten carbonate electrosynthesis of doped carbon nanotubes is demonstrated for carbon nanotubes doped with boron, nitrogen, sulfur, and phosphorus. In a similar manner, numerous dopant source materials and types allow electrosynthesis of carbon nanotubes with numerous dopants, and by applying this straightforward synthesis approach to a wide variety of simple additives, electrosynthesis allows for a broader portfolio of doped carbon nanomaterials, including boron, silicon, germanium, nitrogen, phosphorus, arsenic, antimony, sulfur, selenium, tellurium, gold, alkali or alkaline earth metals, nickel, copper, iron, manganese, titanium, zinc, zirconium, molybdenum, tantalum, platinum, iridium, cobalt, silicon, and (C 12 The present invention also includes doped carbon nanomaterials, which include one or more substances having a carbon isotope other than 10 ...

[0069] If the material to be deposited with the carbon nanomaterial requires a higher electrolysis potential than that required to deposit carbon from carbonates, it is possible to deposit the material by a two-step molten carbonate synthesis. As an example, a one-step 770 °C electrolysis of Li2CO3 with nickel powder and lithium silicate (Li4SiO4) does not contain silicon in the deposited product. A two-step electrosynthesis process can deposit the desired material. The first step is to carry out the electrolysis in an electrolyte of 0.42 g nickel powder and 52 g Li2CO3 (without Li4SiO4). Then, in the second step, the electrodes are moved into a second electrolyte consisting of 18.4 g Li4SiO4 and 40.2 g Li2CO3 (without nickel powder) and the electrolysis continues. The observed electrolysis potentials are 1.4 V for the first step and 2.3 V for the second step. The washed final product shows carbon nanotubes as observed in SEM images. In the resulting nanotubes, silicon-based carbon was observed, as determined by electron dispersive spectroscopy and Raman spectroscopy at 480 cm -1This was evidenced by both the formation of a new silicon peak at 1000 nm.

[0070] 8 is a schematic diagram of known and new synergistic pathways for one-step electrolysis of molten carbonate 800 to form nucleated carbon nanotubes or carbon nano-onions, graphene, or hollow carbon nanospheres, which may be doped or undoped, without being bound by any theory or pathway. FIG. 8 shows known synthetic sequence pathways 810 and 820.

[0071] In FIG. 8, route 820 does not use a nucleating agent and provides a facile route to form nano-onions, graphene, or hollow carbon nanospheres. In route 821, zinc oxide (ZnO) or magnesium oxide (MgO) is added to the carbonate electrolyte to induce the formation of carbon nano-onions, graphene, or hollow carbon nanospheres, respectively. In route 823, an alternating rather than direct electrolysis current is applied between the anode and cathode to form graphene or carbon nano-onions (by having ZnO in the electrolyte or zinc cobalt on the cathode). In route 825, potassium carbonate (K2CO3) induces the formation of graphene platelets on the cathode.

[0072] In FIG. 8, route 810 uses nucleating agents to provide a facile route to forming carbon nanotubes and carbon nanofibers. Nucleating agents are specific transition metals, or combinations thereof, that may be dissolved in the electrolyte, released from the anode, or included in the cathode to form nucleation sites for carbon nanotube or carbon nanofiber growth from the cathode. In route 811, specific nucleating agents, such as copper, induce short carbon nanotubes. In route 815, specific nucleating agents, such as nickel and chromium, induce long carbon nanotube growth. In route 813, increased levels of dissolved oxygen are added to the carbonate electrolyte to produce high levels of SP 3 The defects cause the carbon nanotubes to be measured and are observed to be tangled rather than straight. In route 812, a thin-walled agent such as calcium carbonate (CaCO3) is added to reduce the solubility of oxygen in the carbonate electrolyte, resulting in thin-walled carbon nanotubes. In route 814, natural abundance carbon nanotubes are added to the carbonate electrolyte, resulting in thin-walled carbon nanotubes. 12 C is 13 C, leading to the production of carbon nanotubes with buried or closed cores, thick-walled, thin-core carbon nanotubes, or solid carbon nanofibers.

[0073] 8 also shows synthesis sequences 830 and 840, characterized by the addition of a dopant source to the molten carbonate electrolyte in sequence 830 without a dopant and in sequence 840. This allows for the selection of either the inherent (undoped) or doped pathways for pathways 811-815 and pathways 821-825. Carbon nanomaterial products, including a portfolio of either doped or undoped carbon nanotube morphologies, may be derived from pathways 811 to 815, or may be either doped carbon nano-onions, graphene or hollow nanospheres derived from pathways 821 to 835.

[0074] In FIG. 8, pathway 830 shows that omitting the dopant source from the molten carbonate electrolyte leads to the production of pristine (intrinsic, undoped) carbon nanomaterial formed at the cathode.

[0075] In Figure 8, pathway 840 shows that a dopant source for the molten carbonate electrolyte can be used to produce doped (e.g., boron, sulfur, nitrogen or phosphorus doped) carbon nanomaterials at the cathode. In Figure 8, pathway 840, the desired dopant source can be used as a variety of individual or combined sources in molten carbonate electrolysis. The dopant source (source) can be added directly to the electrolyte as a salt, covalent compound or elemental compound containing the dopant in solid, liquid or gas form, or can be added as a dopant using materials contained in the anode or cathode electrodes.

[0076] Nucleation factors may be combined synergistically, one or more transition metals may be added in specific types and concentrations, oxides may be added or removed, carbon isotopes may be added or removed, and these may be used in conjunction with carbonate configuration, electrolysis, charge, time and temperature to produce carbon nanotubes with different morphologies.

[0077] On the other hand, a new route 840 allows for the formation of non-native doped carbon nanomaterials by adding a source containing a dopant directly during molten carbonate electrolysis, providing doped carbon materials with specific, desirable, different chemical and physical properties, and further, the electrolysis can be performed directly and without the need for post-treatment doping.

[0078] Furthermore, one or more new routes from route 820, however, can directly form new and unique (non-carbon nanotube) carbon nanomaterial morphologies in molten carbonate electrolysis without the use of nucleating agents. New routes 821, 823 and 825, and synergistic combinations of these routes, form cathode products such as carbon nano-onions, graphene, or hollow nanospheres.

[0079] The dopant atoms introduced during molten carbonate electrolysis are directly incorporated into the construction of carbon nanomaterials at the cathode during electrolysis to form non-intrinsically doped carbon nanomaterials with specific, desirable, different chemical and physical properties, and the electrolysis is performed directly without the need for post-treatment doping. These processes may produce carbon nanomaterials of various morphologies (albeit uniform, depending on the specific route used for synthesis) that can be easily synthesized in high yields, with low energy, and doped. These nanomaterials have high conductivity, high strength, high charge storage, high explosion resistance, unique functionality as catalysts, and pollutant adsorption capabilities. Molten carbonate electrolysis synthesis removes atmospheric and / or anthropogenic carbon dioxide from the environment. The great effect of the electrolysis configuration and conditions on the carbon morphology, doping (addition of trace impurities), Raman spectroscopy and SEM, and on the electrical conductivity of carbon nanotubes have been shown. The same activation behavior as plated (zinc-plated) ones is achieved without the zinc coating, paving the way for the investigation of various alternatives for uncoated cathode electrodes. The doping is achieved directly through the addition of dopant content, and morphology control is achieved through several techniques, including the removal of nucleating agents from the electrolyte.

[0080] Carbon nanomaterials are highly conductive, and may be made in round, solid or hollow, flat, thin or thick-walled, long or short morphologies, and with a variety of chemical and physical properties. The expanding portfolio of inexpensively synthesized molten carbonate electrolysis products is useful in similar applications with other materials, such as metals, composites, woven or embedded in wires, cables, wires or cloth, textiles, batteries, catalysts, optical devices, packaging materials, lightweight, shatter-resistant, blast-resistant building and ceramic materials, and electronic devices.

[0081] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. As used herein, the singular references "a," "an," and "the" are intended to include the plural references as well, unless the context clearly indicates otherwise. Furthermore, to the extent that the words "include," "includes," "a," "having," "with," and similar words are used in either the detailed description and / or claims, these terms are intended to be equivalent to the term "comprising."

[0082] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly used by those skilled in the art. Furthermore, terms defined in commonly used dictionaries should be interpreted in a manner consistent with their meaning in the context of the relevant art, and unless expressly defined herein, such terms should not be interpreted in an idealized or overly formal manner.

[0083] Described herein is a method for producing carbon nanomaterials, the method including: (1) heating a carbonate electrolyte to obtain a molten carbonate electrolyte; (2) disposing the molten carbonate electrolyte between an anode and a cathode in a cell; (3) including a carbon nanomaterial doping component in the cell; (3) including a nanomaterial selection component in the cell; (4) passing a current through the cathode and the anode in the cell; and (5) collecting doped carbon nanomaterial growth from the cathode in the cell. The nanomaterial component may be free of transition metals, and the method may further include passing an alternating electrolysis current through the electrolyte. The electrolysis current may be selected for carbon nano-onion product growth. The method may further include adding zinc oxide to the electrolyte, and the electrolysis current may be selected for graphene platelet product growth. The method may further include adding magnesium oxide to the electrolyte, and the electrolysis current may be selected for hollow carbon nanosphere product growth. The nanomaterial selection component may disperse a transition metal, and the nanomaterial selection component may be selected for carbon nanotube product growth. The doping component may be free of doping additives, and the doping component may be selected for intrinsic nanomaterial growth from the cathode. The doping component may include at least one of a solid electrolyte additive, a liquid electrolyte additive, a gas electrolyte additive, a cathode material, or an anode material. The doping component may be a solid salt, element, or covalent mixture, and the doping component may be dissolved, reacted, or suspended in the electrolyte. The doping component may include at least one material that includes a Group 3 element.The doping component may include at least one material including a group 1 element, or at least one material including a group 2 element, or at least one material including a group 4 element other than carbon, or at least one material including a group 5 element, or at least one material including a group 6 chalcogenide element, or at least one material including gold, platinum, iridium, iron, or other 4th, 5th, or 6th period (row) metal. The doping component may include species using oxygen atoms, or halogen atoms, or one or more of sulfates, nitrates, phosphates, thiophosphates, silicates, borates, thionyl chloride, sulfur chloride, silicon chloride, boron chloride, or borochlorates, thiophosphates, thionyl nitrate, silicon nitrate, and nitrites, boron nitride, and boron nitride salts, or sulfur dioxide, or nitrous oxide gas. The doping component may include at least one doping element. The cathode and anode may comprise at least one material or alloy selected from the group consisting of nickel, copper, chromium, iron, manganese, titanium, zinc, zirconium, molybdenum, tantalum, platinum, iridium, cobalt, silicon, and pure carbon metal. The doping component may comprise a coating on the cathode or anode. The carbon nanomaterial may be a carbon nanotube, the carbon nanomaterial may be graphene, the carbon nanomaterial may be a carbon nanoonion, or the carbon nanosphere may be a hollow carbon nanosphere.

[0084] Also disclosed is a method for producing doped carbon nanomaterials, which includes: (1) providing a carbonate electrolyte containing a doping component between an anode and a cathode in a cell; (2) heating the carbonate electrolyte to a molten state; (3) passing a current between the cathode and the anode through the carbonate electrolyte disposed between the anode and the cathode; and (4) collecting carbon nanomaterial growth from the cathode of the cell. The doping component may be molten, reacted, or suspended in the electrolyte. The doping component may include at least one material containing one of boron, silicon, germanium, nitrogen, phosphorus, arsenic, antimony, sulfur, selenium, tellurium, gold, platinum, iridium, or iron. The cathode or the anode may comprise at least one metal or alloy selected from the group consisting of nickel, copper, chromium, iron, manganese, titanium, zinc, zirconium, molybdenum, tantalum, platinum, iridium, cobalt, silicon, and carbon. The carbon nanomaterial growth may comprise at least one of carbon nanotubes, graphene, carbon nano-onions, and hollow carbon nanospheres. The carbonate may comprise at least one of an alkali or alkaline earth carbonate, or may comprise at least one metal oxide additive, or may comprise at least one of lithium, barium, calcium, magnesium, or zinc oxide. The nanomaterial may have a length of at least 100 μm, the nanomaterial may have a length of 1 to 100 μm, or the nanomaterial may have a length of less than 1 μm.

[0085] Also disclosed is a system for producing carbon nanomaterials, the system comprising a current source, a cell holding a molten carbonate electrolyte between an anode and a cathode, and a doping component of carbon nanomaterial within the cell, the current source capable of passing a current through the cathode and the anode within the cell, producing a doped carbon nanomaterial from the cathode of the cell.

[0086] While various embodiments of the present invention have been described above, it should be understood that these embodiments are presented for illustrative purposes only, and not limiting. Many modifications can be made to the disclosed embodiments in accordance with the disclosure herein without departing from the spirit and scope of the present invention. Thus, the breadth and scope of the present invention should not be limited to the embodiments described above. Rather, the scope of the present invention should be defined in accordance with the following claims and their equivalents.

[0087] While the present invention has been shown and described in one or more embodiments, equivalent alterations and modifications (alternatives) are possible and will become apparent to those skilled in the art upon reading and understanding this specification and the accompanying figures. Moreover, although one particular feature of the invention may be disclosed in connection with one of several implementations, such feature may be combined with one or more features of other implementations, as may be known or suitable or desirable for a particular application. [Explanation of symbols]

[0088] 100 systems, 110 chambers (cells)

Claims

1. A method for producing carbon nanomaterials including carbon nano onions, comprising: heating the carbonate electrolyte to obtain a molten carbonate electrolyte; disposing the molten carbonate electrolyte between an anode and a cathode in a cell; containing a nano-onion selection component within said cell; removing the nucleating agent from within the cell; applying a current to the cathode and the anode in the cell; and collecting carbon nano-onion growths from the cathode in the cell.

2. In claim 1, The method, wherein the step of including the nano-onion selective ingredient comprises adding zinc to the molten carbonate electrolyte.

3. In claim 2, The method of claim 1, wherein the nano-onion selective ingredient is zinc oxide added to the molten carbonate electrolyte.

4. In claim 2, The method, wherein the step of including the nano-onion selective component comprises using the cathode comprising zinc.

5. In claim 4, The method according to claim 1, wherein the cathode comprises cobalt zinc.

6. In claim 4, The method wherein the cathode comprises zinc coated iron.

7. In claim 2, The method wherein the anode comprises an inert oxygen anode where oxygen is produced without releasing transition metal nucleation ions into the molten carbonate electrolyte.

8. In claim 7, The method wherein the inert oxygen anode comprises iridium.

9. In claim 1 or 2, The method, wherein the step of applying a current comprises applying an alternating current.

10. In claim 1, The cathode comprises copper and the current has a current density of at least 0.2 A / cm 2 That is, the method.

11. In claim 10, The method according to claim 1, wherein the anode comprises nickel.

12. In claim 1, The method further comprising the step of applying an electric current to the cell and adding carbon dioxide to the molten carbonate electrolyte between the anode and the cathode.

13. In claim 1, The method, wherein the cathode and the anode are flat and the step of passing a current comprises passing a current for at least 15 hours.

14. In claim 10, The cathode and the anode are each a flat 100 cm 2 The method includes a surface area of.

15. In claim 1, The nano-onion selective component comprises magnesium.

16. In claim 15, The nano-onion selective component comprises magnesium oxide.

17. In claim 1, The method further includes adding a nanomaterial doping component to at least one of a solid electrolyte additive, a liquid electrolyte additive, a gas electrolyte additive, a cathode material, and an anode material prior to and during the current passing step; The method, wherein the carbon nano-onion growths include doped carbon nano-onions.

18. In claim 17, The method, wherein the nanomaterial doping component comprises at least one material comprising a Group 3A element, or at least one material comprising a non-carbon Group 4A element, or at least one material comprising a Group 5A element, or at least one material comprising a Group 6A chalcogenide element, or at least one material comprising gold, platinum, iridium, iron, or other Period 4, 5 or 6 metal.

19. In claim 17, The doped carbon nano-onion comprises desirable chemical and physical properties different from undoped carbon nano-onion, the desirable chemical properties comprising catalytic properties, the catalytic properties comprising heterogeneous catalytic properties, homogeneous catalytic properties, fuel cell catalytic properties, aerobic oxidation catalyst, reaction promotion properties and combinations thereof.

20. In claim 17, The method, wherein the nanomaterial doping component comprises a solid salt, an element, or a covalent bond, and the doping component is dissolved, reacted, or suspended in the electrolyte.

21. In claim 17, The method, wherein the step of adding a nanomaterial doping component comprises adding at least one nanomaterial doping component.

Citation Information

Patent Citations

  • System of manufacturing carbon nano tube by electrolyzing CO2 at high temperature

    CN105506665A

  • New production of carbon cluster compound doped with metal atom

    JP1994321686A

  • How synthetic diamonds are produced

    JP2016505490A

  • Electrolytic generation of graphite

    US20140202874A1

  • Methods and systems for carbon nanofiber production

    WO2016138469A1