Highly water-absorbent resin hydrogel atomizer

The hydrogel atomization device uses centrifugal force to minimize pressure on cut portions, reducing water-soluble components and enhancing particle size reduction in superabsorbent resin processing.

JP7551218B2Active Publication Date: 2024-09-17LG CHEM LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023521952
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-20
Filing Date
2022-06-20
Publication Date
2024-09-17
Estimated Expiration
2042-06-20

AI Technical Summary

Technical Problem

Conventional methods for pulverizing superabsorbent resin hydrogel apply excessive pressure to the cut portion, leading to increased water-soluble component content and reduced vortex efficiency.

Method used

A hydrogel atomization device utilizing centrifugal force to transfer hydrogel through a rotor/stator assembly with specific gap configurations, minimizing pressure on the cut portion and preventing vortex reduction.

Benefits of technology

Prevents damage to hydrogel particles, reduces water-soluble component content, and achieves finer particle sizes without vortex slowdown.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551218000013
    Figure 0007551218000013
  • Figure 0007551218000015
    Figure 0007551218000015
  • Figure 0007551218000011
    Figure 0007551218000011
Patent Text Reader

Abstract

The present invention provides an apparatus for atomizing hydrogel of a superabsorbent polymer. The atomization apparatus includes: a body having a transfer space for transferring hydrogel therein and a discharge space for discharging the pulverized hydrogel; a rotary shaft rotatably disposed in the transfer space and having at least one screw formed on its outer periphery for transferring the hydrogel along the longitudinal direction of the body; a rotor attached to the rotary shaft so as to rotate together with the rotary shaft and having a plurality of rotor blades and a plurality of rotor grooves formed on its outer periphery in an alternating manner along the circumferential direction; and a stator fixedly attached to the body, surrounding the rotor at a predetermined gap from the rotor, and having a plurality of stator blades and a plurality of stator grooves formed in an alternating manner along the circumferential direction. The hydrogel transferred to the rotor by the screw is transported radially outward by centrifugal force, passes through the rotor grooves, is cut / pulverized by the gap between the rotor and the stator, and is discharged to the discharge space through the stator grooves.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority to Korean Patent Application No. 10-2021-0079644, filed June 18, 2021, Korean Patent Application No. 10-2021-0080344, filed June 21, 2021, and Korean Patent Application No. 10-2022-0074876, filed June 20, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to an apparatus for atomizing a hydrogel of a superabsorbent resin, and more specifically, to an apparatus for atomizing a hydrogel of a superabsorbent resin that can prevent a decrease in vortex by preventing excessive pressure from being applied to a cut section and can prevent an increase in the water-soluble component content (E / C) of the particles. [Background technology]

[0003] Super absorbent polymer (SAP) is a white powdery polymeric material made by reacting acrylic acid with caustic soda, and can absorb 500 to 1,000 times its own weight in water. Super absorbent polymer is a synthetic polymeric material that changes into a jelly-like shape when it absorbs water, and has the ability to store water without releasing it even when a certain amount of pressure is applied from the outside.

[0004] Superabsorbent polymer molecules have a net-like structure, and the many holes between the molecules allow them to absorb water well. Due to the difference in ion concentration between the water and the superabsorbent polymer, water moves into the superabsorbent polymer (due to the osmotic pressure phenomenon). When water molecules flow into the superabsorbent polymer, the anions fixed inside try to occupy a certain amount of space due to repulsive forces, and the space in the polymer chains expands, allowing it to absorb more water (electrostatic repulsive forces).

[0005] Such superabsorbent polymers first came into practical use as sanitary products and are now widely used not only in sanitary products such as disposable diapers for babies, but also as soil water retention agents for horticulture, waterproofing materials for civil engineering and construction, seedling sheets, freshness-preserving agents in the food distribution sector, and materials for compresses.

[0006] Superabsorbent polymers are commercially available as powder products after drying and pulverizing hydrogels or hydrogel polymers obtained through polymerization reactions. In order to efficiently carry out the drying process, it is important to maximize the surface area of ​​the hydrogel polymer. Therefore, in order to maximize the surface area of ​​the hydrogel polymer before the drying process, a method of increasing the surface area of ​​the hydrogel polymer by pulverizing the hydrogel polymer polymerized by thermal polymerization or photopolymerization can be considered. As described above, in order to increase the surface area of ​​the hydrogel polymer, a process of primarily pulverizing the hydrogel polymer after polymerization has been disclosed.

[0007] In the primary crushing process of such hydrogels, a chopper is mainly used.

[0008] Such a chopper includes a screw for moving the hydrous gel, a cutter for cutting the hydrous gel, and a hole plate having a plurality of through holes formed therein through which the cut hydrous gel is discharged. According to a conventional chopper, when the screw transfers the hydrous gel to a cutting section including the cutter and the hole plate, the hydrous gel is cut by the hole plate and the cutter until it becomes smaller than the through holes, and the cut hydrous gel passes through the through holes and is discharged.

[0009] The screw continues to push the hydrogel into the cut section until it passes through the through holes, and the hydrogel continues to cut until it completely passes through the through holes, so strong pressure is applied to the cut section. This increases the damage to the hydrogel particles, increasing the water-soluble component content (E / C) of the particles, and slows down the vortex due to particle aggregation.

[0010] In order to reduce the pressure applied to the cut portion, the thickness of the hole plate must be reduced, but there is a limit to how much the thickness can be reduced because the pressure applied to the hole plate may damage the hole plate.

[0011] The contents described in this Background section are intended to deepen understanding of the background of the invention, and may include content that is not prior art already known to those having ordinary skill in the art to which this technology pertains. Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention provides an apparatus for atomizing a hydrogel of a superabsorbent resin, which prevents a decrease in vortex by preventing excessive pressure from being applied to the cutting section by utilizing centrifugal force to transport the hydrogel to the cutting section, and thus prevents an increase in the content (E / C) of water-soluble components in the particles. [Means for solving the problem]

[0013] The hydrogel atomization device of the present invention includes a body having a transfer space in which hydrogel is transferred and a discharge space in which pulverized hydrogel is discharged; a rotating shaft rotatably disposed in the transfer space and having at least one screw formed on its outer circumferential surface to transfer the hydrogel along the longitudinal direction of the body; a rotor attached to the rotating shaft so as to rotate together with the rotating shaft and having a plurality of rotor blades and a plurality of rotor grooves formed alternately in the circumferential direction on its outer circumferential surface; and a stator fixedly attached to the body, surrounding the rotor at a predetermined gap from the rotor, and having a plurality of stator blades and a plurality of stator grooves formed alternately in the circumferential direction, and the hydrogel transferred to the rotor by the screw is transferred radially outward by centrifugal force, passes through the rotor groove, is cut / pulverized by the gap between the rotor and the stator, and is discharged to the discharge space through the stator groove.

[0014] The width of the rotor groove may be greater than the width of the stator groove.

[0015] The gap between the rotor and the stator may be less than the width of the stator groove.

[0016] The gap between the rotor and the stator can be 0.1mm to 0.2mm, and the width of the stator groove can be 0.2mm to 3mm.

[0017] The width of the stator groove may at least partially increase radially outward.

[0018] The stator blades may be spaced apart from the body to define a radial exhaust space between the stator blades and the body.

[0019] The atomization device may further include at least one cutter attached to a rotating shaft between the screw and the rotor and rotating together with the rotating shaft; and at least one hole plate fixedly attached to a body at a set gap from the at least one cutter and having a plurality of through holes formed therein.

[0020] The diameter of the through hole may be smaller than the width of the rotor groove.

[0021] The atomization device may further include an inlet formed in an upper portion of one longitudinal side of the body, connected to the transfer space, through which the hydrogel is introduced; and an outlet formed in a lower portion of the other longitudinal side of the body, connected to the discharge space, through which the hydrogel is discharged.

[0022] A transfer space may be formed on one longitudinal side of the body, and a discharge space may be formed on the other longitudinal side of the body, and the rotor and the stator may define a boundary between the transfer space and the discharge space. Effect of the Invention

[0023] According to the present invention, the hydrogel is transferred to the cutting section by using centrifugal force, so that excessive pressure is not applied to the cutting section, and therefore, a decrease in vortex and an increase in E / C of particles can be prevented.

[0024] In addition, the width of the stator recess through which the cut hydrous gel passes increases toward the radially outward direction, thereby preventing damage to the hydrous gel.

[0025] In addition, the gap between the stator and the rotor can be reduced, and the hydrous gel particles can be made smaller.

[0026] Other advantages that are obtained or expected by the embodiments of the present invention are directly or implicitly disclosed in the detailed description of the present invention, i.e., various advantages that are expected by the embodiments of the present invention are disclosed in the detailed description below.

[0027] The embodiments herein can be better understood by reference to the following description in conjunction with the accompanying drawings, where like reference numbers indicate identical or functionally similar elements and wherein: [Brief description of the drawings]

[0028] [Figure 1] 1 is a cross-sectional view of an apparatus for atomizing a hydrogel of a highly water-absorbent resin according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view showing one example of a cutting section of the hydrogel atomization device according to the embodiment of the present invention. [Diagram 3] 2 is a perspective view of one side of the rotor of a rotor / stator assembly according to an embodiment of the present invention; FIG. [Figure 4] 2 is a perspective view of the rotor / stator assembly according to the embodiment of the present invention, seen from the other side of the rotor. FIG. [Diagram 5] FIG. 2 is a perspective view from one side of a stator of a rotor / stator assembly according to an embodiment of the present invention. [Figure 6]2 is a perspective view of the other side of the stator of the rotor / stator assembly according to the embodiment of the present invention. FIG. [Figure 7] FIG. 2 is a perspective view of a portion of a rotor / stator assembly according to an embodiment of the present invention.

[0029] The above-referenced drawings are not necessarily drawn to scale and should be understood as presenting somewhat simplified representations of various preferred features illustrating the underlying principles of the present invention. For example, the specific design features of the present invention, including specific size, orientation, location, and shape, are determined in part by the particular intended application and environment of use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The terms used herein are merely for the purpose of describing particular embodiments and are not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. It can be understood that the terms "comprise" and / or "contain" as used herein specify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more of other features, integers, steps, operations, elements, components, and / or groups thereof. As used herein, the term "and / or" includes any one or all combinations of the associated listed items.

[0031] The term "polymer" or "polymeric polymer" used in the present specification means a state in which a water-soluble ethylenically unsaturated monomer is polymerized, and may include any range of water content or particle size. Among the above polymers, a polymer having a water content (water content) of about 40% by weight or more in a state after polymerization and before drying may be referred to as a hydrogel polymer.

[0032] In addition, the term "super absorbent polymer" refers to the polymer or base resin itself depending on the context, or is used to encompass all of the polymers or base resins that have been subjected to additional processes such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, etc. to be made into a state suitable for commercialization.

[0033] The term "fine powder" refers to superabsorbent resin particles having a particle size of less than 150 μm. The particle size of such resin particles can be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 220.3 method.

[0034] The term "chopping" refers to cutting the hydrogel polymer into small pieces on the order of millimeters to increase drying efficiency, and is used to distinguish from grinding to micrometer or normal particle levels.

[0035] Moreover, the term "micronizing" or "micronization" refers to pulverizing a hydrogel polymer into particles having a particle size of several tens to several hundreds of micrometers, and is used to distinguish it from "chopping."

[0036] The apparatus for atomizing hydrogel of superabsorbent resin according to the embodiment of the present invention uses centrifugal force to transfer the hydrogel to the cutting section, thereby preventing excessive pressure from being applied to the cutting section, thereby preventing a decrease in vortex and an increase in the water-soluble component content (E / C) of the particles.

[0037] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an apparatus for atomizing hydrogel of a highly water-absorbent resin according to an embodiment of the present invention will be described in detail with reference to the accompanying drawings.

[0038] The apparatus for producing a superabsorbent resin according to an embodiment of the present invention includes a polymerization reactor, a pulverizer, a dryer, a pulverizer, and a surface cross-linking device.

[0039] In the polymerization reactor, a polymerization reaction of the monomer composition occurs in the presence of an internal crosslinking agent and a polymerization initiator to form a hydrous gel polymer.

[0040] The polymerization reaction is a reaction for forming a hydrogel polymer, and is a reaction for forming a polymer in which the water-soluble ethylenically unsaturated monomer having an acidic group and the internal crosslinking agent are crosslinked by carrying out polymerization on a monomer composition including the water-soluble ethylenically unsaturated monomer having an acidic group, an internal crosslinking agent, and a polymerization initiator (Step 1).

[0041] The water-soluble ethylenically unsaturated monomer constituting the crosslinked polymer may be any monomer commonly used in the manufacture of superabsorbent resins. As a non-limiting example, the water-soluble ethylenically unsaturated monomer may be a compound represented by the following formula 1:

[0042] [Chemical formula 1] R 1 -COOM 1

[0043] In the above formula 1, R 1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, and M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.

[0044] Preferably, the monomer may be one or more selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts of these acids. In this way, when acrylic acid or its salt is used as the water-soluble ethylenically unsaturated monomer, it is advantageous to obtain a highly water-absorbent resin with improved water absorption. In addition, the monomer may be maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid or 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, (N,N)-dimethylaminoethyl (meth)acrylate, (N,N)-dimethylaminopropyl (meth)acrylamide, etc.

[0045] Here, the water-soluble ethylenically unsaturated monomer has an acidic group. In the conventional production of a superabsorbent resin, a monomer in which at least a part of the acidic groups has been neutralized with a neutralizing agent is cross-linked to form a hydrogel polymer. Specifically, at least a part of the acidic groups of the water-soluble ethylenically unsaturated monomer is neutralized in a step of mixing the water-soluble ethylenically unsaturated monomer having the acidic group, an internal cross-linking agent, a polymerization initiator, and a neutralizing agent.

[0046] However, according to one embodiment of the present invention, the water-soluble ethylenically unsaturated monomer is polymerized in a state where the acid group is not neutralized to form a polymer.

[0047] Water-soluble ethylenically unsaturated monomers (e.g., acrylic acid) in which the acid group is not neutralized are in a liquid state at room temperature and have high miscibility with the solvent (water) and exist in the form of a mixed solution in the monomer composition. However, water-soluble ethylenically unsaturated monomers in which the acid group is neutralized are in a solid state at room temperature and have different solubility depending on the temperature of the solvent (water), with the solubility decreasing as the temperature decreases.

[0048] As described above, the water-soluble ethylenically unsaturated monomer in which the acid group is not neutralized has a higher solubility or miscibility in a solvent (water) than a monomer in which the acid group is neutralized, and is not precipitated even at a low temperature, which is advantageous for long-term polymerization at low temperatures. As a result, a polymer having a higher molecular weight and a uniform molecular weight distribution can be stably formed by performing long-term polymerization using the water-soluble ethylenically unsaturated monomer in which the acid group is not neutralized.

[0049] In addition, it is possible to form a polymer with a longer chain, and the content of water-soluble components that are in an incompletely polymerized or incompletely crosslinked state and are not crosslinked can be reduced.

[0050] In addition, when the polymerization is carried out first in a state where the acidic groups of the monomers are not neutralized, a polymer is formed, and after neutralization, the polymer is micronized in the presence of a surfactant, or the acidic groups present in the polymer are neutralized simultaneously with the micronization, whereby the surfactant is present in a large amount on the surface of the polymer, and can adequately play a role in reducing the tackiness of the polymer.

[0051] The concentration of the water-soluble ethylenically unsaturated monomer in the monomer composition can be appropriately adjusted in consideration of the polymerization time, reaction conditions, etc., and can be about 20 to about 60% by weight, or about 40 to about 50% by weight.

[0052] The term "internal crosslinking agent" used in this specification is a term used to distinguish it from a surface crosslinking agent for crosslinking the surface of a superabsorbent resin particle described later, and plays a role of introducing a crosslinking bond between the unsaturated bonds of the water-soluble ethylenically unsaturated monomer described above to form a polymer containing a crosslinked structure.

[0053] The crosslinking in this step is performed without distinction between the surface and the inside, but when the surface crosslinking process of the superabsorbent resin particles described below is performed, the surface of the finally produced superabsorbent resin particles may include a new crosslinked structure by the surface crosslinking agent, and the inside of the superabsorbent resin particles may maintain the structure crosslinked by the internal crosslinking agent.

[0054] According to an embodiment of the present invention, the internal crosslinking agent may include at least one of a multifunctional acrylate-based compound, a multifunctional allyl-based compound, and a multifunctional vinyl-based compound.

[0055] Non-limiting examples of the polyfunctional acrylate compound include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, pentaerythritol, Examples of the acrylates include dipentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin di(meth)acrylate, and glycerin tri(meth)acrylate, and these may be used alone or in combination of two or more.

[0056] Non-limiting examples of polyfunctional allyl compounds include ethylene glycol diallyl ether, diethylene glycol diallyl ether, triethylene glycol diallyl ether, tetraethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, tripropylene glycol diallyl ether, polypropylene glycol diallyl ether, butanediol diallyl ether, butylene glycol diallyl ether, hexanediol diallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol diallyl ether, dipentaerythritol triallyl ether, dipentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, glycerin diallyl ether, and glycerin triallyl ether. These may be used alone or in combination of two or more.

[0057] Non-limiting examples of polyfunctional vinyl compounds include ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, tetraethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, tripropylene glycol divinyl ether, polypropylene glycol divinyl ether, butanediol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, pentaerythritol divinyl ether, pentaerythritol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol divinyl ether, dipentaerythritol trivinyl ether, dipentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, trimethylolpropane divinyl ether, trimethylolpropane trivinyl ether, glycerin divinyl ether, and glycerin trivinyl ether, which may be used alone or in a mixture of two or more. Preferably, pentaerythritol triallyl ether can be used.

[0058] The above-mentioned polyfunctional allyl compounds or polyfunctional vinyl compounds can form a crosslinked structure during the polymerization process by bonding two or more unsaturated groups contained in the molecule with the unsaturated bonds of the water-soluble ethylenically unsaturated monomer or with the unsaturated bonds of other internal crosslinking agents, and unlike acrylate compounds containing an ester bond (-(C=O)O-) in the molecule, the crosslinked bonds can be more stably maintained even during the neutralization process after the above-mentioned polymerization reaction.

[0059] Therefore, the gel strength of the produced superabsorbent resin is increased, the process stability during the extrusion process after polymerization is improved, and the amount of water-soluble matter can be minimized.

[0060] The crosslinking polymerization of the water-soluble ethylenically unsaturated monomer in the presence of such an internal crosslinking agent can be carried out in the presence of a polymerization initiator, and optionally a thickener, a plasticizer, a storage stabilizer, an antioxidant, etc.

[0061] In the monomer composition, the internal crosslinking agent can be used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be used in an amount of 0.01 parts by weight or more, or 0.05 parts by weight or more, or 0.1 parts by weight or more, and 5 parts by weight or less, or 3 parts by weight or less, or 2 parts by weight or less, or 1 part by weight or less, or 0.7 parts by weight or less based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the internal crosslinking agent is too low, crosslinking does not occur sufficiently, making it difficult to achieve strength above an appropriate level, and if the content of the internal crosslinking agent is too high, the internal crosslinking density increases, making it difficult to achieve the desired water retention ability.

[0062] The polymer formed using such an internal crosslinking agent has a three-dimensional network structure in which the main chain formed by polymerization of the water-soluble ethylenically unsaturated monomer is crosslinked by the internal crosslinking agent. When the polymer has a three-dimensional network structure, the water retention capacity and pressure absorption capacity, which are general physical properties of the superabsorbent resin, can be significantly improved compared to a two-dimensional linear structure that is not additionally crosslinked by an internal crosslinking agent.

[0063] According to one embodiment of the present invention, the step of polymerizing the monomer composition to form a polymer may be performed in a batch type reactor.

[0064] In the conventional manufacturing method of superabsorbent resin, the polymerization method is largely divided into thermal polymerization and photopolymerization depending on the polymerization energy source. In general, thermal polymerization can be carried out in a reactor having a stirring shaft such as a kneader, and photopolymerization can be carried out in a reactor equipped with a movable conveyor belt or in a vessel with a flat bottom.

[0065] Meanwhile, the above polymerization methods generally have a short polymerization reaction time (eg, 1 hour or less), so that the molecular weight of the polymer is not large and the polymer has a broad molecular weight distribution.

[0066] When photopolymerization is carried out in a reactor equipped with a movable conveyor belt or a vessel with a flat bottom, the obtained hydrogel polymer is usually in the form of a sheet having the width of the belt. The thickness of the polymer sheet varies depending on the concentration of the monomer composition injected and the injection speed or amount, but is usually about 0.5 to about 5 cm.

[0067] However, if a monomer composition is supplied such that the thickness of the sheet-like polymer is too thin, the production efficiency is low, which is undesirable, and if the thickness of the sheet-like polymer is increased for the sake of productivity, the polymerization reaction does not occur evenly throughout the entire thickness, making it difficult to form a high-quality polymer.

[0068] In addition, in the polymerization in the reactor having a reactor agitator equipped with a conveyor belt, the polymerization product is moved while new monomer composition is supplied to the reactor, and the polymerization is carried out in a continuous manner. Therefore, polymers with different polymerization rates are mixed, and therefore, it is difficult to carry out uniform polymerization throughout the monomer composition, resulting in a deterioration of the overall physical properties.

[0069] However, according to one embodiment of the present invention, the polymerization is carried out in a stationary batch reactor, so that there is little risk of polymers with different polymerization rates being mixed together, and therefore, a polymer with uniform quality can be obtained.

[0070] In addition, the polymerization step is carried out in a batch reactor having a predetermined volume, and the polymerization reaction is carried out for a longer period of time, for example, 6 hours or more, than in the case of a continuous polymerization in a reactor equipped with a conveyor belt. Despite the long polymerization reaction time, since the polymerization is carried out on unneutralized water-soluble ethylenically unsaturated monomer, the monomer does not precipitate well even if the polymerization is carried out for a long time, and therefore it is advantageous for long-term polymerization.

[0071] In the present invention, since the polymerization in the batch reactor is carried out by a thermal polymerization method, a thermal polymerization initiator is used as the polymerization initiator.

[0072] The thermal polymerization initiator may be one or more selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8), and examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, and the like. dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. More diverse thermal polymerization initiators are described in detail in Odian's book "Principle of Polymerization" (Wiley, 1981), p. 203, and are not limited to the above examples.

[0073] The polymerization initiator can be used in an amount of 2 parts by weight or less per 100 parts by weight of the water-soluble ethylenically unsaturated monomer. That is, if the concentration of the polymerization initiator is too low, the polymerization rate is slowed down, and a large amount of monomer remaining in the final product may be extracted, which is not preferable. On the other hand, if the concentration of the polymerization initiator is higher than the above range, the polymer chains forming the network become shorter, the content of water-soluble components increases, and the physical properties of the resin, such as the compression absorption capacity, may decrease, which is not preferable.

[0074] Meanwhile, in one embodiment of the present invention, the polymerization can be initiated by adding the initiator and a reducing agent which forms a redox couple together.

[0075] Specifically, when the initiator and the reducing agent are added to the polymer solution, they react with each other to form radicals.

[0076] The formed radicals react with the monomer, and the oxidation-reduction reaction between the initiator and the reducing agent is highly reactive, so polymerization can be initiated even with only a small amount of initiator and reducing agent added, making it possible to perform low-temperature polymerization without the need to increase the process temperature, and minimizing changes in the physical properties of the polymer solution.

[0077] The polymerization reaction using the oxidation-reduction reaction can be smoothly carried out at or below room temperature (25° C.). For example, the polymerization reaction can be carried out at a temperature of 5° C. to 25° C., or 5° C. to 20° C.

[0078] In one embodiment of the present invention, when a persulfate initiator is used as the initiator, the reducing agent may be at least one selected from the group consisting of sodium metabisulfite (Na2S2O5); tetramethylethylenediamine (TMEDA); a mixture of iron(II) sulfate and EDTA (FeSO4 / EDTA); sodium formaldehyde sulfoxylate; and disodium 2-hydroxy-2-sulfinoacteate.

[0079] For example, potassium persulfate can be used as the initiator and disodium 2-hydroxy-2-sulfinoacetate can be used as the reducing agent; ammonium persulfate can be used as the initiator and tetramethylethylenediamine can be used as the reducing agent; or sodium persulfate can be used as the initiator and sodium formaldehyde sulfoxylate can be used as the reducing agent.

[0080] In another embodiment of the present invention, when a hydrogen peroxide-based initiator is used as the initiator, the reducing agent may be at least one selected from the group consisting of ascorbic acid; sucrose; sodium sulfite (Na2SO3), sodium metabisulfite (Na2S2O5); tetramethylethylenediamine (TMEDA); a mixture of iron(II) sulfate and EDTA (FeSO4 / EDTA); sodium formaldehyde sulfoxylate; disodium 2-hydroxy-2-sulfinoacteate; and disodium 2-hydroxy-2-sulfoacteate.

[0081] The monomer composition may further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.

[0082] The monomer composition containing the monomer may be in a solution state dissolved in a solvent such as water, and the solid content in the monomer composition in such a solution state, i.e., the concentration of the monomer, the internal crosslinking agent, and the polymerization initiator, may be appropriately adjusted in consideration of the polymerization time, reaction conditions, etc. For example, the solid content in the monomer composition may be 10 to 80% by weight, or 15 to 60% by weight, or 30 to 50% by weight.

[0083] In this case, the solvent that can be used is not limited in composition as long as it can dissolve the above-mentioned components. For example, one or more selected from water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, and N,N-dimethylacetamide can be used in combination.

[0084] The polymer obtained by such a method can form a polymer having a high molecular weight and a uniform molecular weight distribution as described above by polymerizing an unneutralized ethylenically unsaturated monomer, and can reduce the content of water-soluble components.

[0085] The polymer obtained by such a method may be in a hydrogel polymer state and may have a water content of 30 to 80% by weight. For example, the water content of the polymer may be 30% by weight or more, 45% by weight or more, or 50% by weight or more, and 80% by weight or less, 70% by weight or less, or 60% by weight or less.

[0086] If the moisture content of the polymer is too low, it may be difficult to ensure a suitable surface area in the subsequent crushing step, and the polymer may not be crushed effectively. If the moisture content of the polymer is too high, the pressure applied in the subsequent crushing step may increase, making it difficult to crush the polymer to a desired particle size.

[0087] Meanwhile, the term "moisture content" in the present specification refers to the amount of moisture contained in the total weight of the polymer, and is calculated by subtracting the weight of the polymer in a dry state from the weight of the polymer. Specifically, it is defined as a value calculated by measuring the weight loss due to the evaporation of moisture in the polymer during the process of increasing the temperature of the crumb-state polymer by infrared heating and drying it. Here, the drying conditions are to increase the temperature from room temperature to about 180°C and then maintain it at 180°C, and the total drying time is set to 40 minutes, including 5 minutes for the temperature increase step, and the moisture content is measured.

[0088] Next, a step (step 2) is carried out in which at least some of the acidic groups of the polymer are neutralized.

[0089] In this case, as the neutralizing agent, a basic substance capable of neutralizing the acidic group, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide, etc., can be used.

[0090] In addition, the degree of neutralization, which refers to the degree to which the acidic groups in the polymer are neutralized by the neutralizing agent, may be 50 to 90 mol%, or 60 to 85 mol%, or 65 to 85 mol%, or 65 to 75 mol%. The range of the degree of neutralization may vary depending on the final physical properties, but if the degree of neutralization is too high, the absorption capacity of the superabsorbent resin may decrease, and the concentration of carboxyl groups on the particle surface may be too low, making it difficult to perform surface crosslinking in the subsequent process, and the absorption characteristics or liquid permeability under pressure may decrease. Conversely, if the degree of neutralization is too low, not only will the absorption capacity of the polymer decrease significantly, but it may also exhibit properties similar to elastic rubber, which are difficult to handle.

[0091] Simultaneously with step 2, or before or after carrying out step 2, a step of atomizing the polymer in the presence of a surfactant to produce water-containing superabsorbent resin particles is carried out (step 3).

[0092] This step is a step of atomizing the polymer in the presence of a surfactant, where the polymer is not chopped into millimeter sizes but is simultaneously chopped and aggregated, and the polymer is given an appropriate adhesiveness to produce secondary aggregate particles in which the chopped primary particles are aggregated. The secondary aggregate particles produced in this step have a significantly increased surface area and can have a significantly improved absorption speed.

[0093] In this manner, after mixing the polymer and the surfactant, the polymer is atomized in the presence of the surfactant to produce hydrous superabsorbent resin particles in the form of secondary agglomerated particles in which the superabsorbent resin particles and the surfactant are chopped and agglomerated in a mixed state.

[0094] Here, the "water-containing superabsorbent resin particles" are particles having a water content (moisture content) of about 30% by weight or more, and since the polymer is chopped and aggregated in particulate form without a drying process, it can have a moisture content of 30 to 80% by weight, similar to the polymer.

[0095] According to one embodiment of the present invention, the surfactant may be a compound represented by the following Chemical Formula 2 or a salt thereof, but the present invention is not limited thereto:

[0096] [ka]

[0097] In the above Chemical Formula 2, A1, A2 and A3 each independently represent a single bond, carbonyl,

[0098] [ka]

[0099] where at least one of these is carbonyl or

[0100] [ka]

[0101] wherein m1, m2, and m3 each independently represent an integer from 1 to 8;

[0102] [ka]

[0103] are each linked to an adjacent oxygen atom,

[0104] [ka]

[0105] are connected to adjacent R1, R2 and R3, respectively;

[0106] R1, R2, and R3 are each independently hydrogen, linear or branched alkyl having 6 to 18 carbon atoms, or linear or branched alkenyl having 6 to 18 carbon atoms; n is an integer from 1 to 9.

[0107] The surfactant is added so that it can be mixed with the polymer to facilitate the atomization step without agglomeration.

[0108] The surfactant represented by the formula 2 is a nonionic surfactant, and has excellent surface adsorption performance due to hydrogen bonding even with unneutralized polymers, and is therefore suitable for achieving the desired aggregation control effect. On the other hand, in the case of an anionic surfactant, rather than a nonionic surfactant, when mixed with a polymer neutralized with a neutralizing agent such as NaOH or Na2SO4, the ionized Na in the carboxyl group substituent of the polymer is easily absorbed. + When the compound is adsorbed via ions and mixed with an unneutralized polymer, there is a problem that the adsorption efficiency to the polymer is relatively reduced due to competition with the anions of the carboxyl group substituents of the polymer.

[0109] Specifically, the hydrophobic functional groups in the surfactant represented by the above chemical formula 2 are the terminal functional groups R1, R2, and R3 (if not hydrogen), and the hydrophilic functional groups are the glycerol-derived portion in the chain and the terminal hydroxyl group (A n is a single bond and at the same time R n When is hydrogen, n=1 to 3) is further included, but the glycerol-derived portion and the terminal hydroxyl group serve as hydrophilic functional groups to improve the adsorption performance to the polymer surface. Therefore, the aggregation of the superabsorbent resin particles can be effectively suppressed.

[0110] In the above formula 2, the hydrophobic functional groups R1, R2, and R3 (when not hydrogen) are each independently a linear or branched alkyl having 6 to 18 carbon atoms or a linear or branched alkenyl having 6 to 18 carbon atoms. In this case, when the R1, R2, and R3 (when not hydrogen) are alkyl or alkenyl having less than 6 carbon atoms, there is a problem that the chain length is short and the aggregation control of the pulverized particles is not effectively performed, and when the R1, R2, and R3 (when not hydrogen) are alkyl or alkenyl having more than 18 carbon atoms, there is a problem that the mobility of the surfactant is reduced and it is not effectively mixed with the polymer, and the unit price of the composition is high due to the increase in the cost of the surfactant.

[0111] Preferably, R1, R2, and R3 are hydrogen, or when they are linear or branched alkyl having 6 to 18 carbon atoms, they can be 2-methylhexyl, n-heptyl, 2-methylheptyl, n-octyl, n-nonyl, n-decanyl, n-undecanyl, n-dodecanyl, n-tridecanyl, n-tetradecanyl, n-pentadecanyl, n-hexadecanyl, n-heptadecanyl, or n-octadecanyl, or when they are linear or branched alkenyl having 6 to 18 carbon atoms, they can be 2-hexenyl, 2-heptenyl, 2-octenyl, 2-nonenyl, n-dekenyl, 2-undekenyl, 2-dodekenyl, 2-tridekenyl, 2-tetradekenyl, 2-pentadekenyl, 2-hexadekenyl, 2-heptadekenyl, or 2-octadekenyl.

[0112] The surfactant is selected from the compounds represented by the following formulas 2-1 to 2-14:

[0113] [ka] [ka]

[0114] Meanwhile, the surfactant can be used in an amount of 0.01 to 10 parts by weight based on 100 parts by weight of the polymer. If the surfactant is used too little, it may not be evenly adsorbed on the polymer surface, and re-aggregation of particles may occur after pulverization. If the surfactant is used too much, various physical properties of the final superabsorbent resin may be deteriorated. For example, the surfactant can be used in an amount of 0.01 parts by weight or more, 0.015 parts by weight or more, or 0.1 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less based on 100 parts by weight of the polymer.

[0115] The method of mixing such a surfactant with a polymer is not particularly limited as long as it can be uniformly mixed with the polymer, and can be appropriately selected and used. Specifically, the surfactant can be mixed in a dry state, dissolved in a solvent and then mixed in a solution state, or melted and then mixed.

[0116] Among these, for example, the surfactant may be mixed in a state of solution dissolved in a solvent. In this case, any type of solvent may be used without limitation, whether it is an inorganic solvent or an organic solvent, but water is the most suitable in consideration of the ease of the drying process and the cost of the solvent recovery system. In addition, the solution may be mixed by putting the surfactant and the polymer in a reaction vessel, putting the polymer in a mixer and injecting the solution, or continuously supplying the polymer and the solution to a continuously operating mixer and mixing them.

[0117] Meanwhile, according to one embodiment of the present invention, the step of neutralizing at least a portion of the acidic groups of the polymer (step 2) and the step of atomizing the polymer in the presence of a surfactant (step 3) may be carried out sequentially, alternately, or simultaneously.

[0118] That is, a neutralizer is added to the polymer to neutralize the acidic groups first, and then a surfactant is added to the neutralized polymer to atomize the polymer mixed with the surfactant (performed in the order of step 2 → step 3), or a neutralizer and a surfactant are added to the polymer at the same time to neutralize and atomize the polymer (performed in the order of step 2 and step 3 simultaneously). Alternatively, the surfactant can be added first, and the neutralizer can be added later (performed in the order of step 3 → step 2). Alternatively, the neutralizer and the surfactant can be added alternately. Alternatively, the surfactant can be added first to atomize, and then the neutralizer can be added to neutralize, and the surfactant can be further added to the neutralized hydrogel polymer to perform an additional atomization process.

[0119] On the other hand, in order to ensure uniform neutralization of the entire polymer, it is preferable to allow a certain time lag between the addition of the neutralizing agent and the atomization step.

[0120] At least a portion or a substantial amount of the surfactant may be present on the surface of the water-loaded superabsorbent polymer particles.

[0121] Here, the presence of the surfactant on the surface of the water-containing superabsorbent resin particles means that at least a part or a substantial amount of the surfactant is adsorbed or bound to the surface of the water-containing superabsorbent resin particles. Specifically, the surfactant may be physically or chemically adsorbed to the surface of the superabsorbent resin. More specifically, the hydrophilic functional group of the surfactant is physically adsorbed to the hydrophilic portion of the surface of the superabsorbent resin by intermolecular forces such as dipole-dipole interaction. In this way, the hydrophilic portion of the surfactant is physically adsorbed to the surface of the superabsorbent resin particles and surrounds the surface, and the hydrophobic portion of the surfactant is not adsorbed to the surface of the resin particles, so that the resin particles are coated with the surfactant in the form of a kind of micelle structure. This is because the surfactant is added not during the polymerization process of the water-soluble ethylenically unsaturated monomer but during the microparticulation step after the formation of the polymer, and therefore the surfactant can faithfully fulfill its role as a surfactant compared to the case where the surfactant is added during the polymerization process and exists inside the polymer, and particles with a large surface area can be obtained in the form of aggregates of fine particles due to the simultaneous pulverization and aggregation.

[0122] According to one embodiment of the present invention, the step of preparing water-containing superabsorbent resin particles by atomizing the polymer may be carried out two or more times.

[0123] According to one embodiment of the present invention, the atomization step is performed by an atomization device as described below.

[0124] When the polymer mixed with the surfactant is pulverized using a micronizer, a smaller particle size distribution is realized and the subsequent drying and pulverization processes can be carried out under milder conditions, thereby preventing the generation of fine powder and improving the physical properties of the superabsorbent resin.

[0125] Hereinafter, the apparatus 20 for atomizing hydrogel of a superabsorbent resin according to the embodiment of the present invention will be described in more detail with reference to Figs.

[0126] FIG. 1 is a cross-sectional view of an apparatus for atomizing a hydrogel of a highly water-absorbent resin according to an embodiment of the present invention.

[0127] As shown in FIG. 1, an apparatus 20 for atomizing a hydrogel of a superabsorbent resin according to an embodiment of the present invention includes a body 120, a driving motor 100, and cutting units (130, 132, 140, 142, 150).

[0128] The body 120 has a transfer space 126 into which the hydrogel is transferred and a discharge space 128 into which the pulverized hydrogel is discharged. The transfer space 126 is formed on one side of the body 120 in the longitudinal direction, and the discharge space 128 is formed on the other side of the body 120 in the longitudinal direction. Cut portions (130, 132, 140, 142, 150) are disposed inside the body 120 between the transfer space 126 and the discharge space 128. That is, the cut portions (130, 132, 140, 142, 150) can define the boundary between the transfer space 126 and the discharge space 128.

[0129] An inlet 122 connected to a transfer space 126 is formed at an upper portion of one side of the body 120, and the hydrogel discharged from a polymerization reactor (not shown) is introduced into the inside of the body 120, i.e., into the transfer space 126 through the inlet 122. An outlet 124 connected to a discharge space 128 is formed at a lower portion of the other side of the body 120, and the hydrogel crushed by the cutting units (130, 132, 140, 142, 150) is discharged to the outside of the body 120 through the outlet 124.

[0130] A driving motor 100 is disposed on one side of the body 120, and a rotating shaft 110 is rotatably disposed in a transfer space 126 of the body 120 and connected to the driving motor 100. That is, one end of the rotating shaft 110 disposed in the transfer space 126 is connected to the driving motor 100 by penetrating one side of the body 120.

[0131] At least one screw 112 is formed on the outer circumferential surface of the rotating shaft 110. When the driving motor 100 provides a driving force to the rotating shaft 110 to rotate the rotating shaft 110, the screw 112 rotates together with the rotating shaft 110 to transport the hydrous gel in the transport space 126 to the other side in the longitudinal direction toward the cutting units (130, 132, 140, 142, 150).

[0132] FIG. 2 is a perspective view showing an example of a cutting section of the hydrogel atomization device according to the embodiment of the present invention.

[0133] As shown in FIG. 2, the cutting units ( 130 , 132 , 140 , 142 , 150 ) crush the hydrogel transported by the screw 112 and discharge it into the discharge space 128 .

[0134] In one example, the cutting section (130, 132, 140, 142, 150) may include first and second cutters 130, 140, first and second hole plates 132, 142, and a rotor / stator assembly 150. Here, it is shown that the cutting section includes two cutters / hole plates and one rotor / stator assembly 150, but the number of cutters / hole plates and rotor / stator assemblies 150 is not particularly limited. For example, the cutting section may include one cutter / hole plate and one rotor / stator assembly 150, or may include at least one rotor / stator assembly 150 without a cutter / hole plate. However, in order to prevent excessive pressure from being applied to the cutting section, the cutting section must include one rotor / stator assembly 50 disposed closest to the discharge space 128.

[0135] In one example, the rotor / stator assembly 150 is disposed at the other end of the rotating shaft 110, and the first and second cutters 130, 140 and the first and second hole plates 132, 142 are disposed between the screw 112 and the rotor / stator assembly 150.

[0136] The first and second hole plates 132, 142 are fixedly mounted inside the body 120 at a distance from each other, and the first and second cutters 130, 140 are rotatably disposed on one side of the first and second hole plates 132, 142, respectively.

[0137] A plurality of first through holes 134 are formed in the first hole plate 132 in the longitudinal direction, and a plurality of second through holes 144 are formed in the second hole plate 142 in the longitudinal direction. The diameter of the second through holes 144 may be smaller than the diameter of the first through holes 134 so that the hydrogel is transported in the longitudinal direction by the screw 112 and further crushed into small pieces.

[0138] The first cutter 130 is disposed on one side of the first hole plate 132 with a first gap therebetween. The first cutter 130 is provided with a plurality of first cutter knife blades and is mounted on the rotating shaft 112 to rotate together with the rotating shaft 112. The second cutter 140 is disposed on one side of the second hole plate 142 with a second gap therebetween. The second cutter 140 is provided with a plurality of second cutter knife blades and is mounted on the rotating shaft 112 to rotate together with the rotating shaft 112. The second gap may be smaller than the first gap so that the hydrogel is transported in the longitudinal direction by the screw 112 and further crushed into smaller pieces.

[0139] The hydrous gel transferred to the cutting section by the screw 112 is primarily crushed / cut by the first cutter 130 and the first hole plate 132, and passes through the first through hole 134. The hydrous gel that has passed through the first through hole 134 is secondarily crushed / cut by the second cutter 140 and the second hole plate 142, and passes through the second through hole 144. The hydrous gel is then transferred to the rotor / stator assembly 150.

[0140] The rotor / stator assembly 150 finally crushes / cuts the hydrogel that has been secondarily crushed / cut, and discharges it to the discharge space 128. The rotor / stator assembly 150 includes a rotor 160 that is attached to the rotating shaft 110 and rotates together with the rotating shaft 110, and a stator 170 that is fixedly attached to the body 120, surrounding the rotor 160 while being spaced radially outward from the rotor 160 by a set gap.

[0141] FIG. 3 is a perspective view of a rotor / stator assembly according to an embodiment of the present invention as viewed from one side of the rotor, and FIG. 4 is a perspective view of a rotor / stator assembly according to an embodiment of the present invention as viewed from the other side of the rotor.

[0142] 3 and 4, the rotor 160 is generally cylindrical and includes a disk portion 162, a plurality of rotor blades 164, and a plurality of rotor grooves 166. In one example, the inner circumferential surface of the rotor 160 is splined to the rotating shaft 110, thereby allowing the rotor 160 to rotate together with the rotating shaft 110.

[0143] The disk portion 162 is formed at the other end in the longitudinal direction of the cylindrical rotor 160. One surface of the disk portion 162 (the surface of the disk portion 162 facing the second hole plate 142) is formed with a curvature, and can guide the hydrous gel rotating on the cylindrical portion of the rotor 160 to move radially outward due to centrifugal force.

[0144] The rotor blades 164 are arranged along the circumferential direction on the outer periphery of one surface of the disc portion 162. The rotor blades 164 are extended to one side in the longitudinal direction on the outer periphery of one surface of the disc portion 162, and rotor grooves 166 are formed between adjacent rotor blades 164. That is, the rotor blades 164 and the rotor grooves 166 are alternately formed along the circumferential direction. Since the width of the rotor grooves 166 is larger than the diameter of the second through holes 144, the hydrous gel that has passed through the second through holes 144 can pass through the rotor grooves 166. Therefore, the hydrous gel that has moved radially outward by centrifugal force continues to move radially outward through the rotor grooves 166.

[0145] FIG. 5 is a perspective view of a stator of a rotor / stator assembly according to an embodiment of the present invention as viewed from one side, and FIG. 6 is a perspective view of a stator of a rotor / stator assembly according to an embodiment of the present invention as viewed from the other side.

[0146] As shown in FIGS. 5 and 6, the stator 170 is generally cylindrically formed and includes an outer circumferential surface 172, a number of stator blades 174, and a number of stator grooves 176.

[0147] The outer circumferential surface 172 is fixed to the body 120, and a plurality of stator blades 174 extend on one side of the outer circumferential surface 172 in the longitudinal direction, and stator grooves 176 are formed between adjacent stator blades 174. That is, the stator blades 174 and the stator grooves 176 are alternately formed along the circumferential direction.

[0148] Further, the plurality of stator blades 174 are formed radially inward from the outer circumferential surface 172. When the outer circumferential surface 172 is fixed to the body 120, the plurality of stator blades 174 are radially spaced apart from the body 120, and a discharge space 128 is formed radially between the plurality of stator blades 174 and the body 120. Therefore, the hydrous gel that has passed through the stator grooves 176 is discharged into the discharge space 128.

[0149] FIG. 7 is a perspective view of a portion of a rotor / stator assembly according to an embodiment of the present invention.

[0150] 7, stator 170 surrounds rotor 160 with a gap (G1) set radially outward from rotor 160. In addition, the width of rotor groove 166 is greater than the width (t1) of stator groove 176. The width (t1) of stator groove 176 at least partially increases radially outward. That is, the width of the inner circumferential surface of stator groove 176 is smaller than the width of the outer circumferential surface of stator groove 176.

[0151] The gap (G1) between the rotor 160 and the stator 170 may be smaller than the width (t1) of the stator groove 176 so that the hydrous gel cut / crushed by the rotor 160 and the stator 170 can pass through the stator groove 176. In one example, the gap (G1) between the rotor 160 and the stator 170 may be about 0.1 mm to about 0.2 mm, and the width (t1) of the stator groove 176 may be about 0.2 mm to about 3.0 mm.

[0152] The hydrous gel that has passed through the second through-holes 144 is transferred to the cylindrical portion of the rotor 160, rotates on the cylindrical portion of the rotor 160, and moves radially outward by centrifugal force. As described above, the width of the rotor groove 166 is larger than the diameter of the second through-holes 144, so the hydrous gel (X1) that has moved radially outward passes through the rotor groove 166 and continues to move radially outward until it reaches the inner circumferential surface of the stator 170.

[0153] The hydrous gel (X1) is finely crushed / cut by the gap (G1) between the rotor 160 and the stator 170. As described above, since the gap (G1) between the rotor 160 and the stator 170 is smaller than the width (t1) of the stator groove 176, the size of the hydrous gel crushed / cut by the gap (G1) between the rotor 160 and the stator 170 is smaller than the width (t1) of the stator groove 176, and the hydrous gel (X1) can pass through the stator groove 176.

[0154] At this time, the hydrous gel (X1) passes through the stator groove 176 by centrifugal force, not by the transport force of the screw 112, and since the width (t1) of the stator groove 176 increases toward the radially outward side, strong pressure is not applied to the hydrous gel passing through the stator groove 176. Therefore, damage to the hydrous gel is prevented, and thus a decrease in vortex and an increase in E / C of the particles can be prevented.

[0155] In addition, since no strong pressure is applied to the hydrous gel passing through the stator groove 176, the hydrous gel particles can be further reduced in size. Therefore, the subsequent crushing process can be omitted, and the vortex can be prevented from slowing down.

[0156] The hydrous gel that has passed through the stator groove 176 is discharged into the discharge space 128 and then discharged to the outside of the body 120 via the outlet 124 .

[0157] Thereafter, the atomized hydrogel is dried to produce dried superabsorbent resin particles (Step 4).

[0158] This step is a step of drying water from water-containing superabsorbent resin particles, which are polymers obtained by neutralizing at least a portion of the acid groups of the polymer and atomizing the polymer in the presence of a surfactant.

[0159] In a typical method for producing a superabsorbent polymer, the drying step is generally performed until the moisture content of the superabsorbent polymer becomes less than 10% by weight, but according to one embodiment of the present invention, the superabsorbent polymer is dried so that the moisture content becomes 10% by weight or more, for example, about 10 to about 20% by weight, or about 10 to about 15% by weight, but the present invention is not limited thereto.

[0160] For this reason, the temperature in the dryer used in the drying step can be about 150° C. or less, for example, about 80° C. to about 150° C., and can be relatively low. If the temperature in the dryer is too low, the drying time becomes too long, and if the drying temperature is too high, a superabsorbent resin having a moisture content lower than the desired moisture content is obtained.

[0161] In this case, the drying is performed in a moving type, which is different from static drying in that the material moves during drying.

[0162] The moving type drying is a method of drying materials while mechanically stirring them. In this case, the direction in which the hot air passes through the materials may be the same as or different from the direction in which the materials circulate. Alternatively, the materials may be circulated inside the dryer, and a heat transfer fluid (heat medium flow) may be passed through a separate pipe outside the dryer to dry the materials.

[0163] On the other hand, static drying is a method in which the material to be dried is suspended at the bottom of a perforated iron plate through which air passes, and hot air passes from bottom to top to dry the material.

[0164] Therefore, in this step, it is preferable to dry the water-containing superabsorbent polymer by a fluidized drying method, since it is possible to complete uniform drying within a short period of time.

[0165] As an apparatus capable of drying by such a fluidized drying method, a horizontal-type mixer, a rotary kiln, a paddle dryer, a steam tube dryer, or a commonly used fluidized dryer can be used.

[0166] Next, the dried superabsorbent resin particles are pulverized to prepare superabsorbent resin particles (Step 5).

[0167] Specifically, the pulverization step is performed by pulverizing the dried superabsorbent resin particles to have a particle size on the normal particle level, that is, a particle size of 150 μm to 850 μm.

[0168] The pulverizer used for this purpose may be, specifically, a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, or a disc cutter, and is not limited to the above-mentioned examples.

[0169] Alternatively, the grinding machine may be a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, a jog mill, or the like, but is not limited to the above examples.

[0170] Meanwhile, in the manufacturing method of the present invention, it is possible to realize superabsorbent resin particles with a smaller particle size distribution in the atomization step than in the conventional chopping step, and when a moving type drying is performed, the moisture content after drying is maintained relatively high at 10% by weight or more. Therefore, even if the grinding is performed under mild conditions with less grinding force, it is possible to form a superabsorbent resin with a very high content of normal particle sizes of 150 μm to 850 μm, and the ratio of fine powder generation can be significantly reduced.

[0171] The superabsorbent resin particles produced as described above may contain superabsorbent resin particles having a particle size of 150 μm to 850 μm, i.e., normal particles, at a ratio of 80% by weight or more, 85% by weight or more, 89% by weight or more, 90% by weight or more, 92% by weight or more, 93% by weight or more, 94% by weight or more, or 95% by weight or more. The particle size of such resin particles may be measured according to the EDANA WSP 220.3 method of the European Disposables and Nonwovens Association (EDANA) standard.

[0172] In addition, the superabsorbent resin particles may contain about 20% by weight or less, or about 18% by weight or less, or about 15% by weight or less, or about 13% by weight or less, or about 12% by weight or less, or about 11% by weight or less, or about 10% by weight or less, or about 9% by weight or less, or about 8% by weight or less, or about 5% by weight or less of fine powder having a particle size of less than 150 μm based on the total weight. This is in contrast to the conventional manufacturing method for producing superabsorbent resin, which contains more than about 20% by weight to about 30% by weight of fine powder.

[0173] After the step of pulverizing the superabsorbent resin particles, the method may further include a step of classifying the pulverized superabsorbent resin particles according to particle size.

[0174] In addition, the method may further include a step of forming a surface cross-linked layer on at least a part of the surface of the superabsorbent resin particles in the presence of a surface cross-linking agent after crushing and / or classifying the superabsorbent resin particles, whereby the cross-linked polymer contained in the superabsorbent resin particles is additionally cross-linked by the surface cross-linking agent, and a surface cross-linked layer is formed on at least a part of the surface of the superabsorbent resin particles.

[0175] Example 1 In a 2L glass container equipped with a stirrer and a thermometer, 100g of acrylic acid and 0.30g of pentaerythritol triallyl ether (P-30) as an internal crosslinking agent were added, and 226g of water was mixed while stirring. At this time, the reaction temperature was maintained at 5°C, and 1000cc / min of nitrogen was flowed into the resulting mixture for 1 hour. Then, 1.3g of 0.3% hydrogen peroxide aqueous solution, 1.5g of 1% ascorbic acid aqueous solution, 3.0g of 2% 2,2'-azobisamidinopropane dihydrochloride aqueous solution, and 1.5g of 0.01% iron sulfate aqueous solution were added and mixed. After the polymerization reaction started in the resulting mixture and the temperature of the polymer reached 85°C, the mixture was polymerized in an oven at 90±2°C for about 6 hours to produce a hydrogel polymer.

[0176] The hydrogel polymer produced above was mixed in the form of an aqueous solution with hot water in an amount of 0.3 parts by weight of glycerol monolaurate (GML) having the following structure as a surfactant relative to 100 parts by weight of the hydrogel polymer, and then the mixture was atomized using a hydrogel atomization device 20. The hydrogel atomization device 20 included a rotor / stator assembly 150, which atomized the obtained hydrogel polymer. Here, the gap (G1) between the rotor 160 and the stator 170 was 0.1 mm, and the width (t1) of the stator groove 176 was 0.2 mm.

[0177] [ka]

[0178] Then, a 50% NaOH aqueous solution was added to the micronized water-containing superabsorbent resin particles to neutralize some of the acidic groups of the polymer, and the mixture was placed in a rotary mixer and dried at 150°C and 100 rpm for 60 minutes while stirring to obtain superabsorbent resin particles (base resin).

[0179] Examples 2 to 4 and Comparative Example 3 A hydrogel polymer was obtained in the same manner as in Example 1, and the obtained hydrogel polymer was atomized in the hydrogel atomizer 20 and then dried to produce a highly water-absorbent resin.

[0180] However, in Example 2, the gap (G1) between the rotor 160 and the stator 170 was 0.1 mm, and the width (t1) of the stator groove 176 was 3.0 mm; in Example 3, the gap (G1) between the rotor 160 and the stator 170 was 0.2 mm, and the width (t1) of the stator groove 176 was 0.4 mm; in Example 4, the gap (G1) between the rotor 160 and the stator 170 was 0.2 mm, and the width (t1) of the stator groove 176 was 3.0 mm; and in Comparative Example 3, the gap (G1) between the rotor 160 and the stator 170 was 0.2 mm, and the width (t1) of the stator groove 176 was 0.1 mm.

[0181] Comparative Example 1 and Comparative Example 2 A hydrous gel polymer was obtained in the same manner as in Example 1, and the obtained hydrous gel polymer was atomized using a conventional chopper, and then dried to produce a superabsorbent resin. Here, the chopper includes a hole plate having a plurality of through holes formed therein and a cutter disposed near the hole plate.

[0182] However, in Comparative Example 1, the size of each of the through holes was 16 mm, and in Comparative Example 2, the size of each of the through holes was 4 mm.

[0183] <Experimental Example> The properties of the superabsorbent resins produced in the above Examples and Comparative Examples were evaluated by the following methods.

[0184] Unless otherwise specified, all of the following physical property evaluations were performed at constant temperature and humidity (23±1°C, relative humidity 50±10%), and physiological saline or salt water refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.

[0185] Moreover, unless otherwise specified, the physical property evaluations were performed on resins having particle sizes of 300 μm to 400 μm classified using sieves according to ASTM standards.

[0186] (1) Absorption speed (Vortex time) The vortex time was measured in seconds according to the method described in WO 1987 / 003208.

[0187] Specifically, 2 g of superabsorbent resin (particle size 300-400 μm) was placed in 50 mL of saline at 23°C to 24°C, and the solution was stirred at 600 rpm with a magnetic bar (diameter 8 mm, length 30 mm), and the time until the vortex disappeared was measured in seconds to calculate the value.

[0188] (2) Water-soluble components (Extractable Contents, wt%) The water-soluble components were measured for 2 g of the superabsorbent resin after swelling for 1 hour according to EDANA method WSP 270.3.

[0189] The results of the vortex and water-soluble components measured by the above-mentioned method are shown in Table 1 below.

[0190] [Table 1]

[0191] As shown in Table 1, in Examples 1 to 4 in which the gap (G1) between the rotor 160 and the stator 170 is 0.1 mm to 0.2 mm and the width (t1) of the stator groove 176 is 0.2 mm to 3 mm, the vortex is relatively small at 25 seconds or less, and the water-soluble component is maintained relatively small at 3.5 wt%.

[0192] In contrast, in Comparative Example 1 and Comparative Example 2 using a conventional chopper, the vortex is relatively large at 28 seconds or more, and the water-soluble component is relatively large at 4.2 wt%. In Comparative Example 3, in which the gap (G1) between the rotor 160 and the stator 170 is 0.2 mm, but the width (t1) of the stator groove 176 is 0.1 mm, which is smaller than the gap (G1), the vortex is relatively large at 32 seconds, and the water-soluble component is relatively large at 4.6 wt%.

[0193] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and includes all modifications that can be easily modified from the embodiments of the present invention by a person having ordinary skill in the art to which the invention pertains and are deemed to be equivalent.

Claims

1. A body having a transfer space in which the hydrogel is transferred and a discharge space in which the pulverized hydrogel is discharged; A rotating shaft that is rotatably disposed in the transfer space and has at least one screw formed on its outer circumferential surface to transfer the hydrogel along the longitudinal direction of the body; a rotor attached to the rotary shaft so as to rotate together with the rotary shaft, the rotor having a plurality of rotor blades and a plurality of rotor grooves formed alternately on an outer periphery thereof along a circumferential direction; a stator fixedly attached to the body, surrounding the rotor at a predetermined gap from the rotor in a radial direction, the stator having a plurality of stator blades and a plurality of stator grooves alternately formed in a circumferential direction; The hydrous gel transferred to the rotor by the screw is transferred radially outward by centrifugal force, passes through the rotor groove, is cut / crushed by the gap between the rotor and the stator, and is discharged to the discharge space through the stator groove; A hydrogel atomization device for a superabsorbent resin, wherein the gap between the rotor and the stator is smaller than the width of the stator groove.

2. 2. The apparatus for atomizing hydrogel of a highly water-absorbent resin according to claim 1, wherein the width of said rotor groove is greater than the width of said stator groove.

3. The gap between the rotor and the stator is 0.1 mm to 0.2 mm; 2. The apparatus for atomizing hydrogel of a highly water-absorbent resin according to claim 1, wherein the width of the stator groove is 0.2 mm to 3 mm.

4. 2. The apparatus for atomizing hydrogel of a highly water-absorbent resin according to claim 1, wherein the width of the stator groove at least partially increases as it moves radially outward.

5. 2. The apparatus for atomizing hydrogel of a highly water-absorbent resin according to claim 1, wherein the stator blades are spaced apart from the body to form a discharge space in a radial direction between the stator blades and the body.

6. At least one cutter attached to a rotating shaft between the screw and the rotor and rotating together with the rotating shaft; at least one hole plate fixedly attached to the body at a predetermined gap from the at least one cutter, the hole plate having a plurality of through holes formed therein; The apparatus for atomizing a hydrogel of a highly water-absorbent resin according to claim 1, further comprising:

7. 7. The apparatus for atomizing hydrogel of a highly water-absorbent resin according to claim 6, wherein the diameter of the through-hole is smaller than the width of the rotor groove.

8. an inlet formed at an upper portion of one longitudinal side of the body and connected to the transfer space through which the hydrogel is introduced; an outlet formed at a lower portion of the other longitudinal side of the body and connected to the discharge space to discharge the hydrogel; The apparatus for atomizing a hydrogel of a highly water-absorbent resin according to claim 1, further comprising:

9. 9. The apparatus for atomizing a hydrogel of a superabsorbent resin according to claim 8, wherein a transfer space is formed on one side of the body in the longitudinal direction, and a discharge space is formed on the other side of the body in the longitudinal direction, and the rotor and the stator define a boundary between the transfer space and the discharge space.

Citation Information

Patent Citations

  • Production of water-absorbable resin

    JP1999188726A

  • Method for making water-containing gel-like crosslinked polymer granules

    JP2000063527A

  • Stirrer

    JP2020175379A

  • Method for producing absorbent resin particles

    KR1020210013101A

  • Dispersion and grinding machine

    WO2013161229A1