How Graphene is Formed
The PECVD method for graphene formation on a substrate addresses the challenge of growing graphene at low temperatures, enhancing semiconductor device production by effectively adsorbing activated carbon onto the substrate surface.
Patent Information
- Application Number
- JP2019179332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-01
- Filing Date
- 2019-09-30
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-09-30
AI Technical Summary
The challenge is to develop a method for directly forming graphene on a substrate, particularly for use in semiconductor devices, where existing methods face issues with increased resistance due to shorter metal wiring and the need for new metal barrier materials.
A method involving plasma enhanced chemical vapor deposition (PECVD) is used, where the substrate surface is treated with a bias and plasma to create charges and activation sites for effective adsorption of activated carbon, allowing graphene to be grown directly on the substrate at relatively low temperatures.
This method enables the effective adsorption of activated carbon onto the substrate surface, enabling graphene growth at low temperatures, facilitating the production of semiconductor devices with graphene as a metal barrier material using a low-temperature process.
Smart Images

Figure 0007551284000010 
Figure 0007551284000004 
Figure 0007551284000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming graphene, and in particular to a method for forming graphene directly on a substrate. [Background technology]
[0002] In the field of semiconductor devices, research into graphene is being actively conducted to solve the problem of increased resistance as the width of metal wiring becomes shorter and the need to develop new metal barrier materials. Graphene is a material in which carbon atoms are two-dimensionally connected to form a hexagonal honeycomb structure, and has a very thin thickness at the atomic level. Compared to silicon (Si), graphene has the advantages of high electrical mobility, excellent thermal properties, chemical stability, and a large surface area. Summary of the Invention [Problem to be solved by the invention]
[0003] The problem to be solved by the present invention is to provide a method for forming graphene directly on a substrate. [Means for solving the problem]
[0004] In one aspect, treating a surface of a substrate disposed in a reaction chamber using plasma while applying a bias to the substrate; and growing graphene on the surface of the substrate by a plasma enhanced chemical vapor deposition (PECVD) process.
[0005] In the step of treating the surface of the substrate, at least one of charges and activation sites that induce adsorption of activated carbon may be formed on the surface of the substrate, and the activation sites may include at least one of roughness and defects.
[0006] The step of treating the surface of the substrate may include the steps of injecting a pre-treatment gas into the reaction chamber, applying the bias to the substrate, and generating the plasma in the reaction chamber while the bias is applied to the substrate.
[0007] The pretreatment gas may include at least one of an inert gas, hydrogen, oxygen, ammonia, chlorine, bromine, fluorine, and a fluorocarbon.
[0008] The bias power applied to the substrate is as high as 1 to 100 W.
[0009] The step of growing the graphene may include injecting a reaction gas containing a carbon source into the reaction chamber; and generating plasma in the reaction chamber to directly grow the graphene on a surface of the substrate.
[0010] The reaction gas may further include at least one of an inert gas and a hydrogen gas.
[0011] The steps of treating the surface of the substrate and growing the graphene may be performed at a process temperature of 1,000° C. or less.
[0012] The process pressure in the step of treating the surface of the substrate may be lower than the process pressure in the step of growing the graphene, and may be 0.02 to 5.0 Torr.
[0013] The plasma in the step of treating the surface of the substrate and the plasma in the step of growing the graphene are each generated by at least one RF (radio frequency) plasma generator or at least one MW (microwave) plasma generator.
[0014] The plasma power in the step of treating the surface of the substrate may be stronger than the plasma power in the step of growing the graphene. The plasma power in the step of treating the surface of the substrate may be 10 to 4,000 W.
[0015] The step of growing graphene may further include applying a bias to the substrate.
[0016] The substrate may include at least one of a Group IV semiconductor material, a semiconductor compound, a metal, and an insulating material, and may further include a dopant.
[0017] In another aspect, applying a bias to a substrate to treat a surface of the substrate; and growing graphene on the surface of the substrate.
[0018] The step of treating the surface of the substrate may include the steps of injecting a predetermined pretreatment gas into a reaction chamber, applying the bias to the substrate, and generating plasma in the reaction chamber while the bias is applied to the substrate.
[0019] The step of growing the graphene may include injecting a reaction gas containing a carbon source into the reaction chamber; and generating plasma in the reaction chamber to directly grow the graphene on a surface of the substrate. Effect of the Invention
[0020] According to this embodiment, in the pretreatment step of the substrate, a bias is applied to the substrate and plasma is used to form charges and activation sites that can induce adsorption of activated carbon on the surface of the substrate. Therefore, in the graphene growth step, activated carbon can be more effectively adsorbed on the surface of the substrate, so that graphene can be grown and formed on the surface of the substrate at a relatively low temperature. In addition, in the graphene growth step, a bias is applied to the substrate, so that graphene can be selectively grown and formed on a desired surface of the substrate.
[0021] For example, when fabricating a semiconductor device including graphene, which can also be used as a metal barrier material, it is necessary to directly grow graphene on a non-catalytic substrate at a relatively low temperature of 700° C. or less. According to an exemplary embodiment, a pretreatment process capable of inducing adsorption of activated carbon on a surface of a substrate at a low temperature is performed, and graphene can be directly grown and formed on the surface of the pretreated substrate through a plasma enhanced chemical vapor deposition process, thereby making it possible to easily fabricate a semiconductor device including graphene through a low temperature process. [Brief description of the drawings]
[0022] [Figure 1] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Diagram 2] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Diagram 3] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 4A] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 4B] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Diagram 5] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 6] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 7] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 8] 1 is a diagram illustrating a method for forming graphene according to an example embodiment; [Figure 9] 1 is a graph showing a comparison of Raman spectra measured on the surface of a silicon substrate after graphene is grown on the surface of the silicon substrate in a pretreatment process of the silicon substrate, with and without a bias applied to the silicon substrate. [Figure 10] 1 is a graph showing a comparison of the amount of Si-C bonds formed on a surface of a silicon substrate after graphene is grown on the surface of the silicon substrate when a bias is applied to the silicon substrate and when a bias is not applied in a pretreatment process of the silicon substrate. [Figure 11] 1 is a diagram illustrating a method of forming graphene according to another exemplary embodiment; [Figure 12] 1 is a diagram illustrating a method of forming graphene according to another exemplary embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, exemplary embodiments will be described in detail with reference to the accompanying drawings. In the following drawings, the same reference numerals refer to the same components, and the size of each component in the drawings may be exaggerated for clarity and convenience of description. Meanwhile, the embodiments described below are merely exemplary, and various modifications are possible from such embodiments.
[0024] In the following, the terms "upper" and "above" may include not only those directly above in contact, but also those above without contact. A singular expression includes a plural expression unless the context clearly indicates otherwise. In addition, when a part "includes" a certain component, it does not mean to exclude other components, but means that the part may further include other components, unless otherwise specified to the contrary.
[0025] The use of the term "said" and similar directives refers to both the singular and the plural. Unless the steps constituting the method are explicitly stated in a sequence or are stated to the contrary, the steps are performed in any suitable sequence. The order of the steps described above is not necessarily limited to the above. The use of all examples or exemplary terms is merely for the purpose of explaining the technical idea in detail, and the scope is not limited by the above examples or exemplary terms, except as limited by the claims.
[0026] Graphene is a material in which carbon atoms are two-dimensionally connected to form a hexagonal honeycomb structure, and has a very thin thickness at the atomic level. Compared to silicon (Si), such graphene has advantages of high electrical mobility, excellent thermal properties, chemical stability, and a large surface area. In the following embodiments, a method for forming graphene will be described.
[0027] 1 to 8 are views illustrating a method for forming graphene according to an example embodiment.
[0028] The method for forming graphene according to the present embodiment includes a substrate pre-treatment process and a graphene growth process. Figures 1 to 4D are views for explaining the substrate pre-treatment process, and Figures 5 to 8 are views for explaining the graphene growth process.
[0029] First, the substrate pretreatment process will be described below with reference to FIGS. 1 to 4D.
[0030] Referring to FIG. 1, a pre-treatment gas is injected into a reaction chamber (not shown) in which a substrate 110 is disposed.
[0031] The substrate 110 may include, for example, a semiconductor material. The semiconductor material may include, for example, a group IV semiconductor material or a semiconductor compound. As a specific example, the group IV semiconductor material may include Si, Ge, or Sn. And, the semiconductor compound may include, for example, a material in which at least two elements selected from the group consisting of Si, Ge, C, Zn, Cd, Al, Ga, In, B, N, P, S, Se, As, Sb, and Te are combined.
[0032] The substrate 110 may include a metal. The metal may include at least one of Cu, Mo, Ni, Al, W, Ru, Co, Mn, Ti, Ta, Au, Hf, Zr, Zn, Y, Cr, and Gd. The substrate 110 may also include an insulating material. The insulating material may include, for example, an oxide, a nitride, or a carbide. However, the above-mentioned materials of the substrate 110 are merely exemplary, and the substrate 110 may include various other materials. Meanwhile, the substrate 110 may further include a dopant.
[0033] In the pre-treatment process of the substrate 110, the pre-treatment gas injected into the reaction chamber may include at least one of an inert gas, hydrogen, oxygen, ammonia, chlorine, bromine, fluorine, and fluorocarbon. Here, the inert gas may include at least one of an argon gas, a neon gas, a nitrogen gas, a helium gas, a krypton gas, and a xenon gas. FIG. 1 illustrates an example in which hydrogen is used as the pre-treatment gas.
[0034] Next, a bias is applied to the substrate 110 via a bias supply 120. The bias applied to the substrate 110 may be, for example, a radio frequency (RF) bias or a direct current (DC) bias. Thus, a predetermined (+) bias voltage or (-) bias voltage is applied to the substrate 110. To this end, a bias power of a predetermined magnitude is applied to the substrate 110. For example, in the pre-treatment process of the substrate 110, the bias power applied to the substrate 110 may be about 1 to 100 W. However, this is merely an example, and the bias power applied to the substrate 110 may be modified in various ways.
[0035] 2, while a bias is applied to the substrate 110, power for generating plasma is applied from a plasma power source (not shown) to the inside of the reaction chamber. The plasma power applied in the pre-treatment process of the substrate 110 is stronger than the plasma power applied in the graphene growth process described below. However, this is not necessarily limited thereto, and the plasma power applied in the pre-treatment process of the substrate 110 may be variously changed depending on the graphene growth conditions. For example, the plasma power applied in the pre-treatment process of the substrate 110 may be, for example, about 10 to 4,000 W.
[0036] As the plasma power source, for example, an RF plasma generator or a MW (microwave) plasma generator is used. The RF plasma generator can generate an RF plasma having a frequency range of, for example, about 3 to 100 MHz, and the MW plasma generator can generate an MW plasma having a frequency range of, for example, about 0.7 to 2.5 GHz. However, such frequency ranges are merely exemplary, and other frequency ranges may also be used. Meanwhile, as such a plasma power source, a plurality of RF plasma generators or a plurality of MW plasma generators may also be used.
[0037] 3, when plasma power is applied to the reaction chamber while a bias is applied to the substrate 110, a gas plasma (e.g., hydrogen plasma) is generated within the reaction chamber. When gas plasma is generated within the reaction chamber while a bias is applied to the substrate 110, a predetermined charge 131 is formed on the surface 110a of the substrate 110. For example, when a (-) bias voltage is applied to the substrate 110, a (+) charge 131 may be formed on the surface 110a of the substrate 110 as shown in FIG. Also, when a (+) bias voltage is applied to the substrate 110, a (-) charge may be formed on the surface 110a of the substrate 110.
[0038] By applying plasma power while a bias is applied to the substrate 110, charges 131 formed on the surface 110a of the substrate 110 can serve to induce adsorption of activated carbon 140 (FIG. 7) in the graphene growth process described below.
[0039] On the other hand, if plasma power is applied to generate gas plasma while a bias is applied to the substrate 110, activation sites 132 (FIG. 4A) that can induce adsorption of activated carbon 140 (FIG. 7) are formed on the surface 110a of the substrate 110.
[0040] FIG. 4A illustrates a state in which activation sites are formed on the surface 110a of the substrate 110 by applying plasma power while a bias is applied to the substrate 110. Referring to FIG. 4A, when plasma power is applied to generate gas plasma while a bias is applied to the substrate 110, a certain charge 131 moves toward the substrate 110 inside the reaction chamber and collides with the surface 110a of the substrate 110. As a result, activation sites 132 that can serve to induce adsorption of activated carbon 140 (FIG. 7) in the graphene growth process described below are formed on the surface 110a of the substrate 110. Here, the activation sites 132 may include, for example, roughness or defects. FIG. 4A illustrates roughness as an example of the activation sites 132.
[0041] In addition, when a bias is applied to the substrate 110 and plasma power is applied to generate gas plasma, charges 131 and activation sites 132 capable of inducing adsorption of activated carbon 140 (FIG. 7) are both formed on the surface 110a of the substrate 110.
[0042] 4B illustrates how charges 131 and activation sites 132 are formed on the surface of the substrate 110 by applying plasma power while a bias is applied to the substrate 110. Referring to FIG. 4B, when plasma power is applied to generate gas plasma while a bias is applied to the substrate 110, certain charges 131 move toward the substrate inside the reaction chamber. In the process, some of the charges 131 are formed on the surface 110a of the substrate 110, and other charges 131 collide with the surface 110a of the substrate 110 to form activation sites 132. Here, the activation sites 132 may include, for example, roughness or defects.
[0043] In such a pretreatment process of the substrate 110, the process temperature and process pressure in the reaction chamber are variously changed according to the graphene growth conditions. For example, the pretreatment process of the substrate 110 may be performed at a relatively low temperature. For example, the pretreatment process of the substrate 110 may be performed at a process temperature of about 1,000° C. or less. As a specific example, the pretreatment process of the substrate 110 may be performed at a process temperature of about 700° C. or less (more specifically, 400° C. or less). In addition, the process pressure at which the pretreatment process of the substrate 110 is performed is lower than the process pressure at which the graphene growth process described below is performed. However, the process pressure is not necessarily limited thereto, and the process pressure at which the pretreatment process of the substrate 110 is performed may be variously changed according to the graphene growth conditions. For example, the process pressure at which the pretreatment process of the substrate 110 is performed may be about 0.02 to 5.0 torr.
[0044] Through the above-described pretreatment process of the substrate 110, at least one of charges 131 and activation sites 132 capable of inducing adsorption of activated carbon 140 (FIG. 7) is formed on the surface 110a of the substrate 110. Due to the charges 131 or activation sites 132 formed on the surface 110a of the substrate 110, the activated carbon 140 (FIG. 7) is effectively adsorbed onto the surface 110a of the substrate 110 in the graphene growth process described below, so that graphene 150 (FIG. 8) is directly grown and formed on the surface 110a of the substrate 110 even at a relatively low temperature, for example, below 700° C.
[0045] Hereinafter, a process of growing graphene 150 (FIG. 8) on the surface 110a of the substrate 110 on which the pretreatment process has been performed as described above will be described with reference to FIGS. 5 to 8. As described above, at least one of charges 131 and activation sites 132 capable of inducing adsorption of activated carbon 140 (FIG. 7) is formed on the surface 110a of the substrate 110 through the pretreatment process of the substrate 110. For convenience, the charges 131 and activation sites 132 formed on the surface 110a of the substrate 110 through the pretreatment process are not shown in FIGS. 5 to 8.
[0046] 5 to 8 illustrate a process of growing and forming graphene 150 on a surface 110a of a substrate 110 by a plasma enhanced chemical vapor deposition (PECVD) process.
[0047] 5, after the pretreatment process of the substrate 110 is completed, a reaction gas for growing the graphene 150 is injected into the reaction chamber. Here, the reaction gas may include a carbon source. Here, the carbon source also serves as a source that supplies carbon for the growth of the graphene 150.
[0048] The carbon source may include at least one of a hydrocarbon gas and a vapor of a liquid precursor containing carbon. Here, the hydrocarbon gas may include, for example, methane, ethylene gas, acetylene gas, or propylene gas. And, the liquid precursor containing carbon may include, for example, benzene, toluene, xylene, anisole, hexane, octane, isopropyl alcohol, or ethyl alcohol. However, the carbon source materials mentioned above are merely exemplary, and various other materials may be used as the carbon source material.
[0049] The reaction gas may further include at least one of an inert gas and a hydrogen gas. The inert gas may include at least one of an argon gas, a neon gas, a nitrogen gas, a helium gas, a krypton gas, and a xenon gas. FIG. 5 illustrates an example in which the reaction gas includes a carbon source, an inert gas, and a hydrogen gas, and acetylene gas is used as the carbon source and argon gas is used as the inert gas. Meanwhile, the mixture ratio of the reaction gas injected into the reaction chamber may be variously changed according to the growth conditions of the graphene 150.
[0050] 6, power for generating plasma is applied from a plasma power source (not shown) to the inside of the reaction chamber. The plasma power applied in the growth process of graphene 150 is lower than the plasma power applied in the pretreatment process of the substrate 110. However, this is not necessarily limited thereto, and the plasma power applied in the growth process of graphene 150 may be variously changed depending on the growth conditions of graphene 150.
[0051] As the plasma power source, for example, an RF plasma generator or an MW plasma generator is used. The RF plasma generator can generate an RF plasma having a frequency range of, for example, about 3 to 100 MHz, and the MW plasma generator can generate an MW plasma having a frequency range of, for example, about 0.7 to 2.5 GHz. However, such frequency ranges are merely exemplary, and other frequency ranges may also be used. Meanwhile, a plurality of RF plasma generators or a plurality of MW plasma generators may also be used as the plasma power source.
[0052] When power for generating plasma is applied from the plasma power source to the inside of the reaction chamber, plasma of the reaction gas is generated inside the reaction chamber, and activated carbon 140 (FIG. 7), specifically, activated carbon source radicals, are formed inside the reaction chamber by the plasma of the reaction gas.
[0053] 7, carbon 140 activated by the plasma of the reaction gas, i.e., carbon source radicals, are adsorbed onto the surface 110a of the substrate 110. As described above, at least one of charges 131 (FIG. 3) and activation sites 132 (FIG. 4A) capable of inducing adsorption of activated carbon 140 is formed on the surface 110a of the substrate 110 by the pretreatment process of the substrate 110, and thus the activated carbon 140 is more effectively adsorbed onto the surface 110a of the substrate 110 due to the charges 131 and activation sites 132.
[0054] 8, as described above, the activated carbon 140 is continuously absorbed into the surface 110a of the substrate 110, so that the graphene 150 is grown and formed on the surface 110a of the substrate 110. In this case, the surface 110a of the substrate 110 in contact with the graphene 150 may have carbide formed by bonding the substrate material with carbon.
[0055] In the graphene growth process, the process temperature and process pressure inside the reaction chamber may be variously changed depending on the graphene growth conditions. For example, the graphene growth process may be performed at a relatively low temperature similar to the pretreatment process of the substrate 110. For example, the graphene growth process may be performed at a process temperature of about 1,000° C. or less. As a specific example, the graphene growth process may be performed at a process temperature of about 700° C. or less.
[0056] The process pressure at which the graphene growth process is performed is, for example, higher than the process pressure at which the pretreatment process of the substrate 110 is performed. However, the process pressure is not necessarily limited thereto, and may be variously changed depending on the graphene growth conditions.
[0057] As described above, in the pretreatment step of the substrate 110, a bias is applied to the substrate 110 to generate plasma, thereby forming charges 131 and activation sites 132 capable of inducing adsorption of activated carbon 140 on the surface 110a of the substrate 110. Therefore, such charges 131 and activation sites 132 allow the activated carbon 140 to be more effectively adsorbed on the surface 110a of the substrate 110 in the graphene growth step, and thus graphene 150 can be formed by being directly grown on the surface 110a of the substrate 110 at a relatively low temperature.
[0058] For example, when fabricating a semiconductor device including graphene, which is also used as a metal barrier material, it is necessary to directly grow graphene on a non-catalytic substrate at a relatively low temperature of 700° C. or less. According to an exemplary embodiment, a pretreatment process capable of inducing adsorption of activated carbon 140 on a surface 110a of a substrate 110 at a low temperature is performed, and graphene 150 can be directly grown and formed on the surface of the pretreated substrate 110 through a plasma enhanced chemical vapor deposition process, so that a semiconductor device including graphene can be easily fabricated in a low temperature process.
[0059] Figure 9 shows a comparison of Raman spectra measured on the surface of a silicon substrate after graphene was grown on the surface of the silicon substrate in the pretreatment process of the silicon substrate, with (A) no bias applied to the silicon substrate and (B) a bias applied to the silicon substrate. Figure 9 shows the results when a bias power of 25 W was applied to the silicon substrate for 5 minutes.
[0060] 9, it can be seen that when a bias is applied to the silicon substrate in the pretreatment process of the silicon substrate (B), the Raman peak is higher than when a bias is not applied to the silicon substrate (A). Therefore, it can be seen that when a bias is applied to the silicon substrate in the pretreatment process of the silicon substrate, graphene can be directly grown on the surface of the silicon substrate even at a relatively low temperature, for example, below 700° C.
[0061] Figure 10 shows a comparison of the amount of Si-C bonds formed on the surface of a silicon substrate after graphene is grown on the surface of the silicon substrate when a bias is not applied to the silicon substrate (C) and when a bias is applied to the silicon substrate (D) in the pretreatment process of the substrate. Figure 10 shows the results when a bias power of 25 W is applied to the silicon substrate for 5 minutes.
[0062] 10, it can be seen that when a bias is applied to the silicon substrate in the pretreatment process (D), more Si-C bonds are formed on the surface of the substrate than when a bias is not applied to the silicon substrate (C). This shows that when a bias is applied to the substrate in the pretreatment process of the silicon substrate, the bonding strength between the silicon substrate and graphene is increased.
[0063] 11 and 12 are views illustrating a method of forming graphene according to another exemplary embodiment.
[0064] The method for forming graphene according to the present embodiment includes a substrate pretreatment process and a graphene growth process. Here, the substrate pretreatment process is the same as the substrate pretreatment process shown in Figs. 1 to 4D, so a detailed description thereof will be omitted. However, in the present embodiment, for example, a trench having a predetermined shape is formed in the substrate 210. As described above, when the substrate 210 pretreatment process is performed, at least one of charges and activation sites capable of inducing adsorption of activated carbon is formed on the surface of the substrate 210.
[0065] Hereinafter, a graphene growth process performed after the substrate pretreatment process will be described with reference to Figures 11 and 12. Figures 11 and 12 illustrate a process of growing and forming graphene 250 on a substrate 210 by a plasma enhanced chemical vapor deposition (PECVD) process. Charges and activation sites formed on the surface of the substrate 210 by the pretreatment process are not shown in Figures 11 and 12 for convenience.
[0066] 11, after the pretreatment process of the substrate 210 is completed, a reaction gas for growing graphene 250 (FIG. 12) is injected into the reaction chamber. Here, the reaction gas may include a carbon source. The carbon source may include at least one of a hydrocarbon gas and vapor of a liquid precursor containing carbon.
[0067] The reaction gas may further include at least one of an inert gas and a hydrogen gas. The inert gas may include at least one of an argon gas, a neon gas, a nitrogen gas, a helium gas, a krypton gas, and a xenon gas. Fig. 11 illustrates an example in which the reaction gas includes a carbon source, an inert gas, and a hydrogen gas, in which acetylene gas is used as the carbon source and argon gas is used as the inert gas.
[0068] Next, a bias is applied to the substrate 210 through the bias power supply 220. The bias applied to the substrate 210 may be, for example, an RF bias or a DC bias. Here, the bias power applied to the substrate 210 may be modified in various ways. Thus, a predetermined (+) bias voltage or (-) bias voltage is applied to the substrate 210. Next, while the bias is applied to the substrate 210, power for generating plasma is applied to the inside of the reaction chamber from a plasma power supply (not shown). Here, for example, an RF plasma generator or an MW plasma generator is used as the plasma power supply. Meanwhile, a plurality of RF plasma generators or a plurality of MW plasma generators may be used as the plasma power supply.
[0069] When power for generating plasma is applied from the plasma power source to the inside of the reaction chamber, plasma of the reaction gas is generated inside the reaction chamber, and activated carbon 240, specifically, activated carbon source radicals are formed inside the reaction chamber by the plasma of the reaction gas.
[0070] Activated carbon 240, i.e., carbon source radicals, generated by the plasma of the reactive gas are adsorbed on the surface of the substrate 210. In this case, since a bias is applied to the substrate 210, the activated carbon 240 generated by the plasma of the reactive gas has linearity and can move toward the substrate 210. As a result, the activated carbon 240 can be attached to a desired region of the substrate 210. For example, as shown in FIG. 11, since the activated carbon 240 has linearity and moves toward the substrate 210, the activated carbon 240 is selectively adsorbed to the bottom surface 210a of the trench, not the inclined surface 210b of the trench.
[0071] Meanwhile, due to the pretreatment process of the substrate 210, charges or activation sites capable of inducing adsorption of the activated carbon 240 are formed on the surface of the substrate 210, so that the activated carbon 240 is more effectively adsorbed to the bottom surface 210a of the trench.
[0072] Referring to FIG. 12, activated carbon 240 is continuously absorbed on a surface of a substrate 210, for example, on a bottom surface 210a of a trench, so that graphene 250 is selectively grown and formed on the bottom surface 210a of the trench.
[0073] In the process of growing graphene 250, the process temperature and process pressure inside the reaction chamber may be variously changed according to the graphene growth conditions. For example, the graphene growth process may be performed at a process temperature of about 1,000° C. or less (more specifically, 700° C. or less).
[0074] As described above, in the graphene growth process, by generating plasma of the reactive gas while applying a bias to the substrate 210, activated carbon 240 can be selectively adsorbed only onto a desired surface of the substrate 210, for example, the bottom surface 210a of the trench, thereby growing graphene 250.
[0075] As described above, according to the exemplary embodiment, in the substrate pretreatment step, a bias is applied to the substrate and plasma is used to form charges and activation sites on the surface of the substrate that can induce adsorption of activated carbon. Therefore, in the graphene growth step, activated carbon can be more effectively adsorbed on the surface of the substrate, so that graphene can be grown and formed on the surface of the substrate at a relatively low temperature. In addition, in the graphene growth step, a bias is applied to the substrate, so that graphene can be selectively grown and formed on a desired surface of the substrate.
[0076] For example, when fabricating a semiconductor device including graphene, which can also be used as a metal barrier material, it is necessary to directly grow graphene on a non-catalytic substrate at a relatively low temperature of 700° C. or less. According to an exemplary embodiment, a pretreatment process capable of inducing adsorption of activated carbon on a surface of a substrate at a low temperature is performed, and graphene can be directly grown and formed on the surface of the pretreated substrate through a plasma enhanced chemical vapor deposition process, thereby making it possible to easily fabricate a semiconductor device including graphene through a low temperature process. [Industrial Applicability]
[0077] The graphene formation method of the present invention can be effectively applied to, for example, technical fields related to electronic devices. [Explanation of symbols]
[0078] 110,210 Board 110a Surface of substrate 120,220 Bias power supply 131 Charge 132 Activation Site 140,240 Activated carbon source radicals 150,250 Graphene 210a Bottom of trench 210b Trench slope
Claims
1. treating a surface of a substrate disposed in a reaction chamber using plasma while applying a bias to the substrate; and directly growing graphene on the surface of the substrate by a plasma enhanced chemical vapor deposition (PECVD) process, The substrate includes at least one of a Group IV semiconductor material, a semiconductor compound, and an insulating material; The step of growing graphene includes: injecting a reaction gas containing a carbon source into the reaction chamber; generating a plasma in the reaction chamber to directly grow the graphene on the surface of the substrate; 2. The method for forming graphene, wherein a plasma power in the step of treating a surface of the substrate is stronger than a plasma power in the step of growing graphene.
2. 2. The method of claim 1, wherein in the treating the surface of the substrate, at least one of charges and activation sites that induce adsorption of activated carbon is formed on the surface of the substrate.
3. The method of claim 2 , wherein the activation sites include at least one of roughness and defects.
4. The step of treating the surface of the substrate includes: injecting a pre-treatment gas into the reaction chamber; applying the bias to the substrate; The method for forming graphene according to claim 1 , further comprising: generating the plasma in the reaction chamber while the bias is applied to the substrate.
5. 5. The method of claim 4, wherein the pre-treatment gas comprises at least one of an inert gas, hydrogen, oxygen, ammonia, chlorine, bromine, fluorine, and a fluorocarbon.
6. 6. The method for forming graphene according to claim 4, wherein a bias power applied to the substrate is 1 to 100 W.
7. The method for forming graphene according to claim 1 , wherein the reaction gas further includes at least one of an inert gas and a hydrogen gas.
8. 8. The method of claim 1, wherein the steps of treating the surface of the substrate and growing the graphene are performed at a process temperature of 1,000° C. or less.
9. 9. The method of claim 1, wherein a process pressure in the step of treating the surface of the substrate is lower than a process pressure in the step of growing the graphene.
10. 10. The method of claim 1, wherein a process pressure in treating the surface of the substrate is 0.02 to 5.0 Torr.
11. 11. The method of claim 1 , wherein the plasma in the step of treating the surface of the substrate and the plasma in the step of growing the graphene are generated by at least one RF plasma generator or at least one MW plasma generator, respectively.
12. 12. The method of claim 1, wherein the plasma power in the step of treating the surface of the substrate is 10 to 4,000 W.
13. The method of claim 1 , wherein the step of growing the graphene further comprises applying a bias to the substrate.
14. The method of claim 1 , wherein the substrate further comprises a dopant.
Citation Information
Patent Citations
Method for realizing controllable orientated growth of graphene and graphene prepared by using method
CN104163418A
Process of preparing graphene
CN105585011A
Method for laminating polycrystal material on silicon base substrate
JP1999080962A
Base material for forming carbon nanotube, carbon nanotube orientedly grown on the base material and their production method
JP2010077007A
Method for producing graphene
JP2014231455A