Millimeter wave absorber and laminate

The millimeter wave absorber, made of carbon black, α-alumina, and silicone resin, addresses the challenges of weight, flexibility, and uniform dispersion, providing high absorption and thermal conductivity for electromagnetic waves, suitable for complex surfaces.

JP7551685B2Active Publication Date: 2024-09-17NITERRA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022073385
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-09-17
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

Existing electromagnetic wave absorbers face challenges in achieving high absorption performance while being lightweight, flexible, and ensuring uniform dispersion of fibrous materials in resin sheets, which can lead to non-uniform absorption and reduced flexibility.

Method used

A millimeter wave absorber composed of carbon black, α-alumina, and silicone resin, with specific weight percentages and particle sizes, ensuring high electromagnetic wave absorption, dielectric breakdown strength, thermal conductivity, and flexibility, allowing for uniform dispersion and ease of attachment to complex surfaces.

Benefits of technology

The absorber achieves high electromagnetic wave absorption, dielectric breakdown strength, and thermal conductivity, while maintaining flexibility, enabling effective attachment to various shapes and reducing weight compared to traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551685000007
    Figure 0007551685000007
  • Figure 0007551685000008
    Figure 0007551685000008
  • Figure 0007551685000005
    Figure 0007551685000005
Patent Text Reader

Abstract

To provide a millimeter-wave absorber that absorbs electromagnetic waves in a millimeter-wave band and a laminate including the millimeter-wave absorber that achieves high electromagnetic wave absorption capacity, dielectric breakdown strength, and thermal conductivity while reducing the weight of the millimeter-wave absorber.SOLUTION: In a millimeter wave absorber 10 that absorbs electromagnetic waves in a millimeter wave band, a carbon black 12 and α-alumina 14 are dispersed in a powder state in a silicone resin 16, one side is provided with an adhesive layer 18, the content of carbon black 18 is 10 to 50 wt%, the content of the α-alumina 14 is 10 to 70 wt%, and the content of the silicone resin 16 is 10 wt% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a millimeter wave absorber that absorbs electromagnetic waves in the millimeter wave band, and a laminate including the millimeter wave absorber. [Background technology]

[0002] In recent years, many electronic devices have been equipped with information and communication functions, and the number of devices that transmit and receive electromagnetic waves is increasing. In addition, with the increase in the amount of information exchanged between devices, the frequency band of electromagnetic waves used is gradually shifting to higher frequencies, and the use of the frequency band known as "millimeter waves" is progressing. With the spread of such devices, electromagnetic wave absorbers that absorb electromagnetic waves are being used to suppress the effects of electromagnetic waves emitted from the devices.

[0003] As electromagnetic wave absorbers, in addition to metal plates and sintered ferrite ceramics, electromagnetic wave absorbers made by mixing magnetic materials and resins are known. When the electromagnetic wave absorber is formed from a composition containing resin, it is easy to increase the degree of freedom in the shape of the electromagnetic wave absorber and reduce its weight. For example, Patent Document 1 discloses an electromagnetic wave absorbing sheet having an electromagnetic wave absorbing layer containing magnetic iron oxide, which is an electromagnetic wave absorbing material that magnetically resonates in a frequency band above the millimeter wave band, and a rubber binder. Patent Document 2 discloses an electromagnetic wave interference suppression sheet in which fibrous conductive carbon and carbonyl iron are contained in a resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-127039 A [Patent Document 2] JP 2007-288006 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the electromagnetic wave absorbing sheet described in Patent Document 1 uses magnetic iron oxide as the electromagnetic wave absorbing material, and iron oxide has a density of 5 g / cm 3 Since it is a relatively heavy material exceeding 1000 g / m², it may be difficult to reduce the weight of the electromagnetic wave absorber while improving the electromagnetic wave absorption performance. In addition, when a sheet is made by mixing a fibrous material with a resin, as in the electromagnetic interference suppression sheet described in Patent Document 2, the flexibility of the resin sheet is likely to decrease, and it may be difficult to increase the amount of the fibrous material mixed in the resin sheet. In addition, since it is generally relatively difficult to uniformly disperse fibrous materials in a resin, the electromagnetic wave absorption performance of the resin sheet may become non-uniform. Thus, in addition to high electromagnetic wave absorption performance, further performance improvements have been desired for electromagnetic wave absorbers (millimeter wave absorbers), including weight reduction and flexibility, thermal conductivity for dissipating heat generated by absorbing electromagnetic waves, and insulation for enabling installation near wiring. [Means for solving the problem]

[0006] The present disclosure can be realized in the following forms. (1) According to one embodiment of the present disclosure, there is provided a millimeter wave absorber for absorbing electromagnetic waves in a millimeter wave band, the millimeter wave absorber including carbon black, α-alumina, and a silicone resin. According to the millimeter wave absorber of this embodiment, it is possible to realize high electromagnetic wave absorbing ability, high dielectric breakdown strength, and good thermal conductivity while making the millimeter wave absorber relatively lightweight. (2) In the millimeter wave absorber of the above embodiment, the content of the carbon black may be 10 to 50 wt %. With such a configuration, it becomes easy to ensure the electromagnetic wave absorbing ability of the millimeter wave absorber. (3) In the millimeter wave absorber of the above embodiment, the content of the α-alumina may be 10 to 70 wt %. With this configuration, it becomes easy to ensure the dielectric breakdown strength and thermal conductivity of the millimeter wave absorber. (4) In the millimeter wave absorber of the above embodiment, the content of the silicone resin may be 10 wt % or more. With this configuration, it is easy to reduce the Young's modulus of the millimeter wave absorber and increase the elongation rate. (5) In the millimeter wave absorber of the above embodiment, the Young's modulus may be 10 MPa or less and the elongation rate at room temperature may be 20% or more. With such a configuration, the flexibility and flexibility of the millimeter wave absorber can be increased, and therefore, by bending the millimeter wave absorber, the millimeter wave absorber can be easily disposed on the surface of a member of any shape. (6) In the millimeter wave absorber of the above embodiment, the dielectric breakdown strength may be 100 V / mm or more. With such a configuration, it becomes possible to use the millimeter wave absorber while suppressing dielectric breakdown even in the vicinity of electric wiring, etc. (7) The millimeter wave absorber of the above embodiment may exhibit a return loss of 10 dB or more for electromagnetic waves of 20 to 100 GHz. With such a configuration, good performance as a millimeter wave absorber can be ensured. (8) According to another aspect of the present disclosure, there is provided a laminate comprising: the millimeter wave absorber according to any one of (1) to (7) formed into a sheet shape; and a reflective layer provided in contact with one surface of the millimeter wave absorber and configured to reflect electromagnetic waves transmitted through the electromagnetic wave absorbing layer. According to this configuration of the laminate, it is possible to suppress diffuse reflection of the millimeter wave caused by the reflective layer, while blocking the transmission of the millimeter wave through the millimeter wave absorber. The present disclosure can be realized in various forms other than those described above, such as a millimeter wave absorbing sheet, a method for manufacturing a millimeter wave absorber, a housing including a millimeter wave absorber, a method for preventing the emission or intrusion of undesirable electromagnetic waves in electronic devices, and the like. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view illustrating a schematic configuration of a millimeter wave absorber according to a first embodiment. [Diagram 2] FIG. 2 is an explanatory diagram showing how electromagnetic waves are absorbed in a λ / 4 type electromagnetic wave absorber. [Diagram 3] FIG. 2 is an explanatory diagram showing how millimeter waves incident on a millimeter wave absorber are attenuated. [Figure 4] FIG. 5 is a schematic cross-sectional view illustrating a schematic configuration of a laminate according to a second embodiment. [Diagram 5] FIG. 1 is an explanatory diagram showing the composition and performance of a millimeter wave absorber. [Figure 6] FIG. 11 is an explanatory diagram showing the evaluation results of the millimeter wave absorber. [Figure 7] FIG. 13 is an explanatory diagram showing the radio wave absorption characteristics of sample S8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] A. First embodiment: 1 is a cross-sectional schematic diagram showing a schematic configuration of a millimeter wave absorber 10 in the first embodiment. The millimeter wave absorber 10 includes carbon black 12, alumina 14, and a silicone resin 16. In the millimeter wave absorber 10 of this embodiment, the carbon black 12 and the alumina 14 are dispersed in a powder state in the silicone resin 16. A millimeter wave generally refers to an electromagnetic wave in the 30 GHz band to 300 GHz band, but in this specification, the "millimeter wave" includes the 28 GHz band used in the 5G communication standard, and the millimeter wave absorber 10 attenuates electromagnetic waves in particular in the 10 to 100 GHz band.

[0009] As the carbon black 12, for example, furnace black, channel black, acetylene black, thermal black, etc. can be used, and two or more of these may be used. Carbon black 12 is a conductive material and exhibits electromagnetic wave absorption ability in a wide frequency band of the millimeter wave band. Specifically, it exhibits electromagnetic wave absorption ability at 24 GHz, 28 GHz, and 79 GHz.

[0010] The higher the content of carbon black 12 in the millimeter wave absorber 10, the higher the electromagnetic wave absorbing ability of the millimeter wave absorber 10. Therefore, from the viewpoint of ensuring the electromagnetic wave absorbing ability, the content of carbon black 12 in the millimeter wave absorber 10 is preferably 10 wt% or more, more preferably 20 wt% or more, and even more preferably 30 wt% or more. However, since the higher the content of carbon black 12, the more difficult it becomes to mix with the silicone resin 16, the content of carbon black 12 in the millimeter wave absorber 10 may be, for example, 70 wt% or less. In addition, the higher the content of carbon black 12, the lower the electrical resistance and dielectric breakdown strength of the entire millimeter wave absorber 10, the larger the Young's modulus (the lower the flexibility), and the smaller the elongation rate. Therefore, from the viewpoint of ensuring the dielectric breakdown strength, flexibility, and elongation rate of the entire millimeter wave absorber 10, the content of carbon black 12 in the millimeter wave absorber 10 is desirably 50 wt% or less.

[0011] The particle size (arithmetic mean particle size) of carbon black 12 is generally 10 nm or more and 200 nm or less. If the particle size of carbon black 12 is too small, the intermolecular forces are so great that the particles tend to aggregate with each other, and when such particles are mixed into a resin, the viscosity of the resin increases significantly, making kneading difficult. For this reason, the particle size of carbon black 12 is preferably, for example, 30 nm or more, and more preferably 50 nm or more.

[0012] The alumina 14 is composed of α-alumina having a stable crystal structure. The higher the content of alumina 14 in the millimeter wave absorber 10, the higher the electrical resistance, dielectric breakdown strength, and thermal conductivity of the entire millimeter wave absorber 10. In addition, by adding alumina 14 to the millimeter wave absorber 10, the gaps between the particles of the carbon black 12 are filled with alumina 14, and the strength of the millimeter wave absorber 10 can be increased. Furthermore, by adding alumina 14 to the millimeter wave absorber 10, the carbon black 12 can be crushed and the dispersion state of the carbon black 12 can be made uniform when the materials are kneaded during the manufacture of the millimeter wave absorber 10. As described above, in order to obtain the effects of adding alumina 14, such as improved dielectric breakdown strength and thermal conductivity, the content of alumina 14 in the millimeter wave absorber 10 is preferably 10 wt% or more. However, as the content of alumina 14 increases and the relative content of alumina 14 to carbon black 12 increases, the electromagnetic wave absorbing ability of the millimeter wave absorber 10 is suppressed. Furthermore, the higher the content of alumina 14, the more difficult it becomes to mix it with the silicone resin 16. Furthermore, the higher the content of alumina 14, the higher the Young's modulus of the entire millimeter wave absorber 10 (the lower the flexibility) and the lower the elongation. Therefore, from the viewpoint of ensuring the electromagnetic wave absorbing ability and flexibility of the millimeter wave absorber 10, the content of alumina 14 in the millimeter wave absorber 10 is, for example, preferably 70 wt% or less, more preferably 60 wt% or less, and even more preferably 50 wt% or less.

[0013] The particle size of the alumina 14 is preferably such that the 90% diameter is 50 μm or less when the particle size abundance ratio is measured on a volume basis. By setting the particle size to such a value, it becomes easy to disperse the alumina 14 in the resin when kneading the materials in manufacturing the millimeter wave absorber 10, and as a result, it is possible to make the thermal conductivity and electrical resistance of the millimeter wave absorber 10 uniform. Furthermore, by setting the particle size as described above, it is possible to prevent the particles of the alumina 14 from interfering with the thinning of the millimeter wave absorber 10.

[0014] The closer the particle shape of the alumina 14 is to a sphere, the more the reduction in flexibility of the millimeter wave absorber 10 caused by the addition of the alumina 14 is suppressed, and the elongation rate of the millimeter wave absorber 10 can be increased. In addition, the closer the particle shape of the alumina 14 is to a sphere, the easier it is to disperse the alumina 14 in the resin when kneading the materials in the manufacture of the millimeter wave absorber 10, and as a result, the thermal conductivity and electrical resistance of the millimeter wave absorber 10 can be made uniform. Furthermore, the closer the particle shape of the alumina 14 is to a sphere, the easier it is to increase the amount of alumina 14 added to the millimeter wave absorber 10 (the easier it is to increase the filling rate of the alumina 14 in the silicone resin 16), and the thermal conductivity of the millimeter wave absorber 10 can be increased. However, as long as the dispersion state of the alumina 14, the flexibility of the millimeter wave absorber 10, the thermal conductivity of the millimeter wave absorber 10, and the like are within an acceptable range, the particle shape of the alumina 14 may be a shape other than a sphere, such as an irregular shape.

[0015] As described above, from the viewpoint of making the particle shape of the alumina 14 closer to a sphere, when the radius of the inscribed circle when the particle of the alumina 14 is viewed in cross section is R1 and the radius of the circumscribed circle is R2, the average value of the value of "R2 / R1" is preferably 1.3 or less, more preferably 1.1 or less. The closer "R2 / R1" is to 1.0, the closer the particle shape is to a true sphere (hereinafter, also referred to as high sphericity). The method of specifying the inscribed circle and the circumscribed circle, and the method of calculating "R2 / R1" are as follows. That is, the millimeter wave absorber 10 is cut and polished so that it can be viewed in cross section, and a field of view of 200 μm×200 μm is observed with a scanning electron microscope (SEM), and the shape of 10 particles of the alumina 14 is observed. Specifically, image analysis software WinROOF (manufactured by Mitani Shoji Co., Ltd.) or the like is used to measure R1 and R2, and R2 / R1 is calculated.

[0016] The silicone resin 16 is a resin layer of silicone resin in which powders of carbon black 12 and alumina 14 are mixed in a dispersed state. By using a silicone resin having excellent heat resistance and weather resistance, it becomes easy to ensure the durability of the millimeter wave absorber 10 even when the millimeter wave absorber 10 is used in a relatively high temperature environment or outdoors. From the viewpoint of ensuring the flexibility and elongation rate of the millimeter wave absorber 10, the content of the silicone resin 16 in the millimeter wave absorber 10 is preferably 10 wt% or more, and more preferably 30 wt% or more. In addition, from the viewpoint of ensuring the contents of the carbon black 12 and alumina 14 and ensuring the electromagnetic wave absorbing ability, insulating property, and conductivity of the millimeter wave absorber 10, the content of the silicone resin 16 in the millimeter wave absorber 10 is preferably 80 wt% or less.

[0017] The higher the molecular weight of the silicone resin 16, the higher the elongation of the millimeter wave absorber 10 can be, and the lower the crosslink density of the silicone resin 16, the lower the Young's modulus and the higher the elongation of the millimeter wave absorber 10. Therefore, the molecular weight and crosslink density of the silicone resin 16 can be appropriately selected depending on the desired elongation and Young's modulus to be realized in the millimeter wave absorber 10.

[0018] The silicone resin 16 may be either an addition curing type or a moisture curing type, and a catalyst that accelerates the curing reaction may be added as necessary. As the catalyst, various conventionally known catalysts may be used, such as platinum catalysts, rhodium catalysts, titanium catalysts, and bismuth catalysts. Of these, it is preferable to use a platinum catalyst, which has high reactivity. In the case of using an addition curing type silicone resin that uses a catalyst, it is preferable because it is possible to suppress the generation of outgassing as a by-product when the millimeter wave absorber 10 is used at high temperatures.

[0019] The millimeter wave absorber 10 desirably exhibits a return loss of 10 dB or more for electromagnetic waves of 20 to 100 GHz, more desirably exhibits a return loss of 20 dB or more, and further desirably exhibits a return loss of 30 dB or more. The return loss is the power ratio between the radio wave incident on the millimeter wave absorber and the radio wave reflected back, and represents the electromagnetic wave absorbing ability of the millimeter wave absorber. By setting the return loss of the millimeter wave absorber 10 to the above value, the electromagnetic wave absorbing ability of the millimeter wave absorber 10 can be ensured.

[0020] Moreover, it is desirable that the millimeter wave absorber 10 has a Young's modulus of 10 MPa or less. Furthermore, it is desirable that the millimeter wave absorber 10 has an elongation rate of 20% or more at room temperature. This ensures the flexibility of the millimeter wave absorber 10. By ensuring the flexibility of the millimeter wave absorber 10, it becomes easy to attach the millimeter wave absorber 10 along a shape different from a flat surface. For example, when the millimeter wave absorber 10 is attached to a part of the inner wall surface of a housing that houses a device that transmits and receives millimeter waves, it becomes possible to easily attach the millimeter wave absorber 10 even if the attachment portion is a curved surface. Furthermore, since the millimeter wave absorber 10 exhibits a high elongation rate as described above, it becomes possible for the millimeter wave absorber 10 to follow the thermal expansion of the housing when, for example, the millimeter wave absorber 10 is attached to a part of the inner wall surface of a housing that houses a device that transmits and receives millimeter waves.

[0021] Moreover, it is desirable that the millimeter wave absorber 10 has a dielectric breakdown strength of 100 V / mm or more. This makes it possible to suppress leakage current through the millimeter wave absorber 10 even when the millimeter wave absorber 10 is placed close to electrical wiring. Specifically, for example, in a so-called mild EV using a 48 V power supply, it becomes possible to use the millimeter wave absorber 10 while suppressing dielectric breakdown even when the millimeter wave absorber 10 is placed close to electrical wiring.

[0022] Moreover, it is desirable that the millimeter wave absorber 10 has a thermal conductivity of 0.50 W / (m·K) or more. When the millimeter wave absorber 10 absorbs electromagnetic waves, the energy of the electromagnetic waves is converted into heat in the carbon black 12, which is a conductive material, and the alumina 14, which is a dielectric material, and thus heat is generated. Therefore, by ensuring the thermal conductivity of the millimeter wave absorber 10 and enhancing the heat dissipation in the millimeter wave absorber 10 as described above, it becomes easy to maintain the performance of the millimeter wave absorber 10. Furthermore, when the millimeter wave absorber 10 is attached to a part of the inner wall surface of a housing that houses a device that transmits and receives millimeter waves, it becomes easy to maintain the performance of the device housed in the housing by enhancing the heat dissipation performance of the millimeter wave absorber 10 and suppressing overheating in the housing. In particular, when the millimeter wave absorber 10 is disposed in the vicinity of a heat-generating component such as a power semiconductor, it is desirable that the millimeter wave absorber 10 has high thermal conductivity and excellent heat dissipation performance.

[0023] The physical properties of the millimeter wave absorber 10, such as the return loss, Young's modulus, elongation, dielectric breakdown strength, and thermal conductivity, can be easily achieved by setting the composition of the millimeter wave absorber 10, i.e., the content of the carbon black 12, the alumina 14, and the silicone resin 16 constituting the millimeter wave absorber 10, within the above-mentioned ranges.

[0024] The thickness of the millimeter wave absorber 10 can be, for example, 0.1 mm to 1.5 mm. Here, the frequency band of electromagnetic waves in which the millimeter wave absorber 10 exhibits its absorbing ability is determined by the composition and thickness of the millimeter wave absorber 10. A method for setting the thickness of the millimeter wave absorber 10 according to the electromagnetic waves to be absorbed will be described below.

[0025] FIG. 2 is an explanatory diagram showing the state of electromagnetic wave absorption in a λ / 4 type electromagnetic wave absorber. The millimeter wave absorber 10 is a λ / 4 type electromagnetic wave absorber. In the case where an electromagnetic wave with a wavelength λ0 [mm] in the atmosphere changes to a wavelength λm [mm] inside the millimeter wave absorber 10, the condition in which the reflected waves from the front and back surfaces of the millimeter wave absorber 10 interfere with each other to reduce the electromagnetic wave can be expressed by the following formula (1) using an integer m (m=1, 2, 3, . . .). Note that λm is determined by λ0 and the permittivity and permeability of the millimeter wave absorber 10. For example, λm can be obtained from the frequency λ0 of the electromagnetic wave to be attenuated and the permittivity and permeability of the millimeter wave absorber 10, and the obtained λm can be substituted into formula (1) to derive the thickness t to be set as the thickness of the millimeter wave absorber 10. Note that the wavelength of the millimeter wave becomes shorter inside the millimeter wave absorber 10. In the following formula (2), "n" represents the ratio of the wavelength λ0 in the atmosphere to the wavelength λm inside the millimeter wave absorber 10.

[0026]

number

number

[0027] The above description of the λ / 4 type electromagnetic wave absorber assumes that the millimeter wave is reflected by the inner wall surface of the housing to which the millimeter wave absorber 10 is attached, but the millimeter wave absorber 10 can also attenuate the millimeter wave by utilizing attenuation within the medium in addition to reflection attenuation. The millimeter wave that penetrates the inside of the millimeter wave absorber 10 is attenuated according to the following formula (3). Formula (3) can be solved from the frequency and the complex dielectric constant of the millimeter wave absorber 10, and the millimeter wave can be attenuated by adjusting the thickness of the millimeter wave absorber 10 to a thickness that makes the electric field amplitude in the medium sufficiently small. In formula (3), E is the electric field amplitude within the medium (inside the millimeter wave absorber 10), E0 is the electric field amplitude of the electromagnetic wave (the millimeter wave incident on the millimeter wave absorber 10), α is the attenuation constant, β is the phase constant, and the millimeter wave travels in the Z direction.

[0028]

number

[0029] 3 is an explanatory diagram showing how a millimeter wave incident on the inside of the millimeter wave absorber 10 is attenuated according to the above formula (3). The horizontal axis represents the distance in the thickness direction from the incident surface on which the millimeter wave is incident, and the vertical axis represents the electric field amplitude within the medium.

[0030] 1 shows a state where an adhesive layer 18 is further provided on one surface of the millimeter wave absorber 10. The adhesive layer is a structure for attaching the millimeter wave absorber 10 to a location where it is desired to place the millimeter wave absorber 10, such as the inner wall surface of a housing that houses the above-mentioned device that transmits and receives millimeter waves. The adhesive layer 18 can be formed by applying an adhesive such as a silicone resin, an acrylic resin, or an epoxy resin. Note that when the millimeter wave absorber 10 is arranged by being mechanically fixed using a fastener, for example, instead of being attached, the adhesive layer 18 may not be provided.

[0031] Furthermore, when the millimeter wave absorber 10 is disposed by adhesion, for example, an alkoxide such as a silane coupling agent may be added to the silicone resin 16, and the millimeter wave absorber 10 may be used as an adhesive sheet without providing the adhesive layer 18. In this case, after preparing the millimeter wave absorber 10 in a state in which a part of the silicone resin 16 is cured, the millimeter wave absorber 10 can be bonded to the adherend by attaching the millimeter wave absorber 10 to a desired location (adherend) and thermally curing the millimeter wave absorber 10. The silane coupling agent to be added to the silicone resin 16 is not particularly limited, and can be appropriately selected from conventionally known silane coupling agents, such as those having any one of a vinyl group, an epoxy group, a methacryl group, an amino group, a mercapto group, and an isocyanate group as an organic reactive group.

[0032] The silicone resin 16 may contain other additives instead of or in addition to the silane coupling agent. Examples of other additives include aluminum nitride, boron nitride, spinel ferrite, hexagonal ferrite, pure iron powder, silicon steel powder, permalloy powder, sendust powder, amorphous iron powder, and Fe-Si-Cr alloy magnetic powder. By adding such additives, the millimeter wave absorber 10 can be given performance according to the additive used. The content of the additive in the millimeter wave absorber 10 may be, for example, 40 wt% or less. It is sufficient that the effect of improving the millimeter wave absorption performance realized by the carbon black 12, the effect of ensuring the electrical resistance and thermal conductivity realized by the alumina 14, and the effect on the flexibility of the millimeter wave absorber 10 are within an acceptable range.

[0033] The millimeter wave absorber 10 of the present embodiment configured as described above includes the carbon black 12, the alumina 14, and the silicone resin 16. In this manner, since carbon black, which has a lower density than ferrite (metal oxide, which is a magnetic material) and the like, which has been conventionally used in electromagnetic wave absorbers, is used as a component that mainly exhibits millimeter wave absorbing performance, it becomes easy to reduce the weight of the millimeter wave absorber 10. In addition, by using a combination of the carbon black 12, which has high electromagnetic wave absorbing ability and relatively low electrical resistance, and the alumina 14, which is inferior to the carbon black 12 in millimeter wave absorbing performance but has high electrical resistance and good thermal conductivity, it becomes possible to realize high electromagnetic wave absorbing ability, high dielectric breakdown strength, and good thermal conductivity as the entire millimeter wave absorber 10.

[0034] By disposing such a millimeter wave absorber 10 to absorb millimeter waves, undesirable effects of millimeter waves can be suppressed. For example, by attaching the millimeter wave absorber 10 to a part of the inner wall surface of a housing that houses a device that transmits millimeter waves, it is possible to suppress the transmission of unnecessary electromagnetic waves in undesirable directions. Also, by attaching the millimeter wave absorber 10 to the inner wall surface of a housing that houses a device that receives millimeter waves, it is possible to suppress the input of unnecessary electromagnetic waves to the above-mentioned device. Here, since the millimeter wave absorber 10 is configured as a composition in which powders of carbon black 12 and alumina 14 are dispersed in silicone resin 16, it is easy to ensure the flexibility and flexibility of the millimeter wave absorber 10. Therefore, it is possible to dispose the millimeter wave absorber on the wall surface of a housing of any shape by bending the millimeter wave absorber 10, for example.

[0035] When the millimeter wave absorber 10 is disposed on a metal member such as the body of a vehicle as an adherend, the adherend acts as a reflective layer and reflects millimeter waves that cannot be absorbed by the millimeter wave absorber 10, thereby blocking the transmission of electromagnetic waves through the millimeter wave absorber 10. Here, the metal member as the adherend can block the transmission of millimeter waves, but can also cause diffuse reflection of millimeter waves. By using the millimeter wave absorber 10 of this embodiment, which has excellent electromagnetic wave absorption ability, as the millimeter wave absorber, diffuse reflection of millimeter waves caused by the millimeter waves being reflected on the surface of the metal member can be suppressed.

[0036] B. Second embodiment: 4 is a cross-sectional schematic diagram showing a schematic configuration of a laminate 120 of the second embodiment. The laminate 120 of the second embodiment includes a millimeter wave absorber 10 similar to that of the first embodiment, and also includes a reflective layer 119 on one surface (the surface in contact with an adherend) of the millimeter wave absorber 10.

[0037] The reflective layer 119 is a layer that reflects electromagnetic waves that have passed through the millimeter wave absorber 10. The reflective layer 119 may be formed of any metal that can reflect millimeter waves, such as copper, nickel, iron, stainless steel, precious metals such as gold and silver, and aluminum. The reflective layer 119 may be formed, for example, by attaching a metal film that has been prepared in advance to one surface of the millimeter wave absorber 10. At this time, the reflective layer 119 and the millimeter wave absorber 10 may be attached to each other using an adhesive, or a silane coupling agent or the like may be added to the silicone resin 16 to make the millimeter wave absorber 10 into an adhesive sheet, and the reflective layer 119 and the millimeter wave absorber 10 may be joined together. In addition, when a metal that can form a plated film is used as the material for the reflective layer 119, the reflective layer 119 may be formed by performing plating treatment such as electrolytic plating or electroless plating on the surface of the millimeter wave absorber 10.

[0038] When the millimeter wave absorber 10 of the second embodiment is disposed on a desired adherend, for example, the reflective layer 119 attached to the millimeter wave absorber 10 and the adherend may be fixed using an adhesive. Since the reflective layer 119 is a conductive member, when the millimeter wave absorber 10 is disposed on the adherend, it is desirable to further provide an insulating layer between the reflective layer 119 and the adherend. This makes it possible to suppress the occurrence of a short circuit, even when the millimeter wave absorber 10 is disposed near an electric wiring.

[0039] With such a configuration, the same effect as that of the millimeter wave absorber 10 of the first embodiment can be obtained, and by providing the reflective layer 119 overlapping the millimeter wave absorber 10, it is possible to block the transmission of millimeter waves in the millimeter wave absorber 10. That is, not only are millimeter waves absorbed by the millimeter wave absorber 10, but the reflective layer 119 can also reflect millimeter waves that cannot be completely absorbed by the millimeter wave absorber 10.

[0040] C. Other embodiments: In each of the above-described embodiments, the millimeter wave absorber is formed in a sheet shape, but may be formed in a different shape, however, forming the millimeter wave absorber in a sheet shape makes it easy to arrange the millimeter wave absorber along the surface of an adherend of any shape. EXAMPLES

[0041] FIG. 5 is an explanatory diagram showing the results of preparing 12 types of millimeter wave absorbers from sample S1 to sample S12 and examining their compositions and performance. FIG. 6 is an explanatory diagram showing the results of evaluating the millimeter wave absorbers from sample S1 to sample S12. The configuration and manufacturing method of each sample, and the results of evaluating the performance are described below. Each sample differs in the type of material used and the mixing ratio of the materials. Samples S9 to S12 are comparative examples that do not satisfy the conditions related to carbon black, alumina, and silicone resin described in the embodiment.

[0042] <Preparation of each sample> [Sample S1] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to carbon black (arithmetic mean particle size: about 120 nm), alumina (volume mean particle size: about 10 μm), and a silicone resin (molecular weight about 70,000) having a vinyl group as a functional group, and mixed with a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape by a doctor blade method so as to have a thickness of 700 μm and 1000 μm, and heat cured at a temperature of 100 ° C. or higher to obtain a millimeter wave absorber of sample S1. The volume mean particle size of the alumina mentioned above was a value measured using a laser diffraction / scattering type particle size distribution measuring device (MT3300, manufactured by Microtrack Bell Co., Ltd.).

[0043] The carbon black and alumina used in each sample described below are the same materials as those used in the above-mentioned sample S1.

[0044] [Sample S2] A silane coupling agent, a crosslinking agent, and a small amount of water were further added to the carbon black and alumina described above, and the silicone resin (molecular weight approximately 30,000) having a hydroxyl group as a functional group, and mixed with a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into sheets by the doctor blade method to have thicknesses of 700 μm and 1000 μm, and heat cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S2.

[0045] [Samples S3, S4] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to the carbon black and alumina described above, and a silicone resin (molecular weight approximately 30,000) having a vinyl group as a functional group, and mixed using a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape by a doctor blade method so as to have a thickness of 700 μm and 1000 μm, and heat cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S3 or sample S4. Sample S3 and sample S4 use the same materials, but have different compositions (contents of carbon black, alumina, and silicone resin) as shown in Figures 5 and 6.

[0046] [Sample S5] A silane coupling agent, a crosslinking agent, a metal catalyst, and toluene as a solvent were further added to the carbon black and alumina described above, and the silicone resin (molecular weight approximately 30,000) having a vinyl group as a functional group, and mixed by a ball mill to obtain a paste. The obtained paste was formed into a sheet shape by a doctor blade method so as to have a thickness of 700 μm and 1000 μm, and after volatilizing the toluene at a temperature of 80° C. or less, it was thermally cured at a temperature of 100° C. or more to obtain a millimeter wave absorber of sample S5.

[0047] [Samples S6, S7] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to the carbon black and alumina described above, and a silicone resin (molecular weight approximately 60,000) having a vinyl group as a functional group, and mixed using a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape by a doctor blade method so as to have a thickness of 700 μm and 1000 μm, and heat cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S6 or sample S7. Sample S6 and sample S7 use the same materials, but have different compositions (contents of carbon black, alumina, and silicone resin) as shown in Figures 5 and 6.

[0048] [Sample S8] The above-mentioned carbon black and alumina, and the silicone resin (molecular weight about 60000) having a vinyl group as a functional group were further added with a silane coupling agent, a crosslinking agent, a metal catalyst, and toluene as a solvent, and mixed by a ball mill to obtain a paste. The obtained paste was formed into a sheet shape by a doctor blade method so as to have a thickness of 700 μm and 1000 μm, and after volatilizing the toluene at a temperature of 80° C. or less, it was thermally cured at a temperature of 100° C. or more to obtain a millimeter wave absorber of sample S8.

[0049] [Sample S9] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to the above-mentioned alumina and silicone resin (molecular weight approximately 60,000) having a vinyl group as a functional group, and mixed by a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into sheets by the doctor blade method to have thicknesses of 700 μm and 1000 μm, and heat-cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S9.

[0050] [Sample S10] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to the above-mentioned alumina and silicone resin (molecular weight approximately 70,000) having a vinyl group as a functional group, and mixed by a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was formed into sheets by the doctor blade method to have thicknesses of 700 μm and 1000 μm, and heat-cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S10.

[0051] [Sample S11] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to the carbon black and the silicone resin (molecular weight approximately 60,000) having a vinyl group as a functional group, and mixed by a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was molded into sheets by the doctor blade method to have thicknesses of 700 μm and 1000 μm, and heat cured at a temperature of 100° C. or higher to obtain a millimeter wave absorber of sample S11.

[0052] [Sample S12] A silane coupling agent, a crosslinking agent, and a metal catalyst were further added to a silicone resin (molecular weight approximately 70,000) having a vinyl group as a functional group, and mixed using a blade stirrer and a three-roll mill to obtain a paste. The obtained paste was molded into sheets with thicknesses of 700 μm and 1000 μm by the doctor blade method, and thermally cured at a temperature of 100°C or higher to obtain a millimeter wave absorber of sample S12.

[0053] <Measurement of the composition of millimeter wave absorbers> The composition of each sample, i.e., the content of carbon black, alumina, and silicone resin (content in each sample) was examined using a sample with a thickness of 1000 μm. The carbon black content was measured by carbon component analysis. The alumina and silicone resin contents were calculated by measuring the density of the millimeter wave absorber by Archimedes' method, and then calculating the content and specific gravity of the carbon black measured previously, and the specific gravity of the alumina and silicone resin. Here, the content of the platinum catalyst contained in some samples was very small compared to the total amount of the sample, so it was ignored as an error in the calculation.

[0054] <Measurement of Young's modulus and elongation rate> The Young's modulus and elongation were measured at room temperature using a tensile tester (Shimadzu Autograph (AG-IS)) using a sample with a thickness of 700 μm. Each sample was cut into a rectangular test piece with a width of 1 cm and a length of 7 cm, and a tensile test was performed on the middle part with a length of 3 cm while holding the test piece with a jig at a position 2 cm from both ends. The Young's modulus and elongation were obtained from the SS curve (stress-strain curve). Specifically, the change in the sample length and the load was measured over time while pulling each test piece until it broke. At this time, the tensile stress was calculated by dividing the measured load by the cross-sectional area of ​​the test piece before the tensile test. The Young's modulus was calculated as the slope in the elastic deformation region in a graph (stress-strain curve) with the strain calculated by the following formula (4) on the horizontal axis and the tensile stress on the vertical axis. The elongation percentage was calculated by pulling each test piece until it broke, subtracting the original sample length (the intermediate length of 3 cm in the above sample) from the sample length at the time of breakage, and then dividing the result by the original sample length. The formula for calculating the elongation percentage is shown below as formula (5).

[0055] Strain (%) = [sample length during tension – original sample length] / original sample length (4) Elongation (%) = [sample length at break – original sample length] / original sample length (5)

[0056] <Measurement of dielectric breakdown strength> The dielectric breakdown strength was measured using a millimeter wave absorber with a thickness of 1000 μm in accordance with JIS C 2110-1: 2016. Here, the "effect of increasing the insulation properties of the millimeter wave absorber and enabling the use of the millimeter wave absorber near wiring" was evaluated using the dielectric breakdown strength.

[0057] <Measurement of return loss> The return loss was measured by the free space method (JIS R 1679:2007) at room temperature. The attenuation was measured in the frequency range of 18 GHz to 110 GHz, and the value at which the attenuation was maximum in the frequency range of 20 GHz to 100 GHz was taken as the attenuation. Even if the peak of the attenuation was different from the target frequency, if there was a peak of attenuation in the frequency range of 20 GHz to 100 GHz, that value was taken as the attenuation. The return loss was measured using both a sample with a thickness of 700 μm and a sample with a thickness of 1000 μm, and the value with the greater degree of attenuation was used.

[0058] Fig. 7 is an explanatory diagram showing the radio wave absorption characteristics of sample S8 having a thickness of 1000 μm as an example. Fig. 7 shows how sample S8 significantly attenuates electromagnetic waves of 45 GHz (see the arrow in Fig. 7).

[0059] <Thermal conductivity> The thermal conductivity was measured using a thermal conductivity measuring device TCi (manufactured by Rigaku Corporation) that uses a non-stationary flat heat source. For the measurement, each sample molded to a thickness of 1000 μm was used.

[0060] <Evaluation method> As shown in Figure 6, each item was evaluated by comparing it with the standard value. For "carbon content," if the carbon black content in each sample was within the range of 10wt% to 50wt%, it was marked "○," and if it was outside the above range, it was marked "×." For "alumina content," if the alumina content in each sample was within the range of 10wt% to 70wt%, it was marked "○," and if it was outside the above range, it was marked "×." For "silicone content," if the silicone resin content in each sample was 10wt% or more, it was marked "○."

[0061] For "Young's modulus," samples were rated "○" if their Young's modulus was 10 MPa or less. For "elongation," samples were rated "○" if their elongation was 20% or more, and "×" if their elongation was less than 20%. For "dielectric breakdown strength," samples were rated "○" if their dielectric breakdown strength was 100 V / mm or more, and "×" if their dielectric breakdown strength was less than 100 V / mm.

[0062] For "return loss," if the return loss of each sample was 10 dB or more, it was marked as "○," if it was 2 dB or more and less than 10 dB, it was marked as "△," and if it was less than 2 dB, it was marked as "×." For "thermal conductivity," if the thermal conductivity of each sample was 0.50 W / (m·K) or more, it was marked as "○," if it was 0.30 W / (m·K) or more and less than 0.50 W / (m·K), it was marked as "△," and if it was less than 0.30 W / (m·K), it was marked as "×."

[0063] FIG. 6 further shows the results of the overall evaluation. The "overall evaluation" was marked as "X" when there were two or more evaluation items marked as "X" in the above-mentioned evaluation items of Young's modulus, elongation, dielectric breakdown strength, return loss, and thermal conductivity, or when the return loss could not be confirmed (it was less than 2 dB, which is the detection limit). In addition, when the overall evaluation was other than "X" and there was one evaluation item marked as "X", it was marked as "△". In addition, when the overall evaluation was other than "X" and there was no evaluation item marked as "X", it was marked as "O".

[0064] <Evaluation Results> Sample S1 contains carbon black, alumina, and silicone resin, but because the amounts of carbon and alumina are relatively small, both the return loss and thermal conductivity are relatively low, which is thought to be why the overall evaluation was "△".

[0065] Sample S2 had a good return loss because it contained more carbon than Sample S1. However, it had a relatively small amount of alumina, which resulted in a relatively low dielectric breakdown strength and thermal conductivity, which is thought to be why the overall evaluation was "△".

[0066] Sample S3 has a larger amount of alumina than Sample S1, so both the dielectric breakdown strength and thermal conductivity were good, and the overall evaluation was "○". However, by increasing the amount of alumina, the Young's modulus increased and the elongation decreased, and a decrease in flexibility and elongation was confirmed.

[0067] Sample S4 has a higher carbon content than Sample S3, which resulted in an improved return loss value. However, the total amount of powder added to the silicone resin increased, which further reduced the elongation value, resulting in the overall evaluation of "△".

[0068] Sample S5 has a higher carbon content than Sample S4, and the return loss value is improved. Also, the alumina content is lower than Sample S4, and the elongation value is improved. However, it is thought that the increase in carbon content caused the dielectric breakdown strength to decrease, resulting in the overall evaluation of "△".

[0069] Samples S6 to S8 had a good balance between the carbon black and alumina contents, and showed relatively good values ​​for each of the Young's modulus, elongation, dielectric breakdown strength, return loss, and thermal conductivity, and were overall evaluated as "good."

[0070] Sample S9 did not contain carbon black, so the return loss could not be confirmed and the overall evaluation was "X." However, because the amount of alumina was relatively large, the dielectric breakdown strength and thermal conductivity were good.

[0071] Sample S10, like sample S9, does not contain carbon black, so the return loss could not be confirmed and the overall evaluation was "X." Furthermore, the amount of alumina was less than that of sample S9, so the thermal conductivity was also low.

[0072] Sample S11 had a good return loss because it contained a sufficient amount of carbon. However, because it did not contain alumina, it had low dielectric breakdown strength and thermal conductivity, and was given an overall rating of "X."

[0073] Sample S12 did not contain either carbon black or alumina, and therefore the return loss could not be confirmed. In addition, the thermal conductivity was low, and the overall evaluation was "X".

[0074] The present disclosure is not limited to the above-mentioned embodiments, etc., and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features in the embodiments corresponding to the technical features in each form described in the Summary of the Invention column can be appropriately replaced or combined in order to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted.

[0075] The present disclosure can also be realized in the following forms. [Application example 1] A millimeter wave absorber that absorbs electromagnetic waves in a millimeter wave band, The composition is characterized by comprising carbon black, α-alumina, and a silicone resin. Millimeter wave absorber. [Application example 2] The millimeter wave absorber according to Application Example 1, The carbon black content is 10 to 50 wt %. Millimeter wave absorber. [Application example 3] The millimeter wave absorber according to Application Example 1 or 2, The content of the α-alumina is 10 to 70 wt%. Millimeter wave absorber. [Application example 4] The millimeter wave absorber according to any one of Application Examples 1 to 3, The silicone resin content is 10 wt % or more. Millimeter wave absorber. [Application example 5] The millimeter wave absorber according to any one of Application Examples 1 to 4, The Young's modulus is 10 MPa or less, and the elongation at room temperature is 20% or more. Millimeter wave absorber. [Application Example 6] The millimeter wave absorber according to any one of Application Examples 1 to 5, Characterized by a dielectric breakdown strength of 100 V / mm or more Millimeter wave absorber. [Application Example 7] The millimeter wave absorber according to any one of Application Examples 1 to 6, It is characterized by a return loss of 10 dB or more for electromagnetic waves of 20 to 100 GHz. Millimeter wave absorber. [Application Example 8] A laminate comprising: The millimeter wave absorber according to any one of Application Examples 1 to 7 formed into a sheet shape; a reflecting layer provided in contact with one surface of the millimeter wave absorber and configured to reflect the electromagnetic wave transmitted through the electromagnetic wave absorbing layer; A laminate comprising: [Explanation of symbols]

[0076] 10...Millimeter wave absorber 12…Carbon black 14...Alumina 16...Silicone resin 18…Adhesive layer 119...Reflection layer 120...Laminate

Claims

1. A millimeter wave absorber that absorbs electromagnetic waves in a millimeter wave band, Carbon black, α-alumina, and a silicone resin; The carbon black content is 35 to 50 wt %, The Young's modulus is 2 MPa or less, and the elongation at room temperature is 100% or more. Millimeter wave absorber.

2. The millimeter wave absorber according to claim 1, The content of the α-alumina is 10 to 70 wt %. Millimeter wave absorber.

3. The millimeter wave absorber according to claim 1, The silicone resin content is 10 wt % or more. Millimeter wave absorber.

4. The millimeter wave absorber according to claim 1, Characterized by a dielectric breakdown strength of 100 V / mm or more Millimeter wave absorber.

5. The millimeter wave absorber according to claim 1, It is characterized by showing a return loss of 10 dB or more for electromagnetic waves of 20 to 100 GHz. Millimeter wave absorber.

6. A laminate comprising: The millimeter wave absorber according to any one of claims 1 to 5 formed in a sheet shape; a reflective layer provided in contact with one surface of the millimeter wave absorber and configured to reflect electromagnetic waves transmitted through the millimeter wave absorber; A laminate comprising:

Citation Information

Patent Citations

  • Electromagnetic wave absorbing material composition and electromagnetic wave absorber

    JP2004059832A

  • Electromagnetic wave multi-functional PC board and sheathed type electromagnetic wave shield building constituted thereof

    JP2004116100A

  • Electromagnetic wave absorbing thermal conductive sheet

    JP2004200534A

  • Millimeter wave absorber

    JP2004296758A

  • Electromagnetic wave noise suppressor and its manufacturing method

    JP2005327930A