Resin composition, prepreg, laminate, resin film, printed wiring board, semiconductor package, and method for producing resin composition
A resin composition combining polyphenylene ether derivatives, epoxy resins, and maleimide compounds with organometallic compounds addresses the limitations of existing compositions, providing superior dielectric and thermal performance for high-frequency electronic devices.
Patent Information
- Application Number
- JP2020038008
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-05
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-03-05
AI Technical Summary
Existing resin compositions for printed wiring boards exhibit insufficient high-frequency properties, adhesion with conductors, thermal stability, and flame retardancy, particularly in the GHz range, failing to meet the demands of advanced electronic devices such as 5G antennas and millimeter wave radars.
A resin composition comprising polyphenylene ether derivatives, epoxy resins, cyanate resins, and maleimide compounds, combined with organometallic compounds like organotitanium and zirconium, to enhance dielectric properties, adhesion, and thermal stability.
The composition achieves excellent dielectric properties in frequencies above 10 GHz, improved adhesion, and enhanced thermal stability, making it suitable for high-frequency electronic devices.
Smart Images

Figure 0007552037000025 
Figure 0007552037000012 
Figure 0007552037000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a prepreg, a laminate, a resin film, a printed wiring board, a semiconductor package, and a method for producing the resin composition. [Background technology]
[0002] In mobile communication devices such as mobile phones, their base station equipment, network infrastructure devices such as servers and routers, and large computers, the speed and capacity of signals used are increasing year by year. Accordingly, the printed wiring boards mounted on these electronic devices must be compatible with higher frequencies, and substrate materials with excellent dielectric properties (low dielectric constant and low dielectric tangent; hereinafter, sometimes referred to as "high frequency properties") in high frequency bands that enable reduction in transmission loss are in demand. In recent years, in addition to the electronic devices mentioned above, new systems that handle high frequency wireless signals have been put into practical use or are planned to be put into practical use in the ITS field (related to automobiles and traffic systems) and in the field of indoor short-range communication as applications that handle such high frequency signals, and it is expected that low transmission loss will also be required for printed wiring boards mounted on these devices in the future.
[0003] Conventionally, polyphenylene ether (PPE) resins have been used as heat-resistant thermoplastic polymers with excellent high-frequency characteristics for printed wiring boards that require low transmission loss. Specifically, resin compositions containing polyphenylene ether and epoxy resins (see, for example, Patent Document 1), resin compositions containing polyphenylene ether and cyanate resins that have a low dielectric constant among thermosetting resins (see, for example, Patent Document 2), etc. have been disclosed. However, the resin compositions described in Patent Documents 1 and 2 are generally insufficient in terms of high-frequency characteristics in the GHz range, adhesion to conductors, low thermal expansion coefficient, and flame retardancy, and the heat resistance is often reduced due to low compatibility between polyphenylene ether and thermosetting resins.
[0004] Under these circumstances, a resin composition containing one or more thermosetting resins selected from the group consisting of polyphenylene ether derivatives having a specific structure, epoxy resins, cyanate resins, and maleimide compounds, and a styrene-based thermoplastic elastomer has been proposed with the objective of providing a resin composition that has particularly good compatibility, dielectric properties in the high frequency band, high adhesion to conductors, excellent heat resistance, a high glass transition temperature, a low thermal expansion coefficient, and high flame retardancy (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 58-069046 [Patent Document 2] Special Publication No. 61-018937 [Patent Document 3] International Publication No. 2016 / 175326 Summary of the Invention [Problem to be solved by the invention]
[0006] The resin composition described in Patent Document 3 certainly has excellent dielectric properties in high frequency bands. However, in recent years, there has been a strong demand for the development of a resin composition with improved dielectric properties in the 10 GHz band or higher that can be used in fifth generation mobile communication system (5G) antennas that use radio waves in a frequency band exceeding 6 GHz and millimeter wave radars that use radio waves in a frequency band of 30 to 300 GHz. Furthermore, from the viewpoint of economic efficiency, there is a demand for a simple method to improve the dielectric properties without going through a complicated process.
[0007] In view of the current situation, an object of the present invention is to provide a resin composition which is economical and capable of exhibiting excellent dielectric properties in a high frequency band of 10 GHz or more, a method for producing the same, and a prepreg, a laminate, a resin film, a printed wiring board, and a semiconductor package which use the resin composition. [Means for solving the problem]
[0008] As a result of investigations conducted by the present inventors to solve the above problems, they have found that the problems can be solved by the present invention described below. That is, the present invention relates to the following [1] to
[13] . [1] (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof; (B) a polyphenylene ether resin; (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons an organometallic compound having a group; A resin composition comprising: [2] Above (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons The organometallic compound having a group is attached to the titanium atom. Through one oxygen atom Combine Hydrocarbons An organic titanium compound having a group and a zirconium atom Through one oxygen atom Combine Hydrocarbons The resin composition according to the above item [1], wherein the compound is one or more selected from the group consisting of organic zirconium compounds having a group. [3] Above (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons The resin composition according to the above [1] or [2], wherein the organometallic compound having a group is a compound represented by the following general formula (C-1) or the following general formula (C-2): [ka] (In the above general formulas (C-1) and (C-2), R C1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms; M C1 represents a titanium atom or a zirconium atom. C2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. [4] Above (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons The organometallic compound having a group is attached to the titanium atom. Through one oxygen atom Combine Hydrocarbons The resin composition according to the above item [2], wherein the compound is an organotitanium compound having a group. [5] The resin composition according to any one of the above [1] to [4], wherein the (B) polyphenylene ether resin has a number average molecular weight of 1,000 to 25,000. [6] The resin composition according to any one of the above [1] to [5], wherein the (B) polyphenylene ether resin has an ethylenically unsaturated bond-containing group. [7] Above (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons The resin composition according to any one of the above [1] to [6], wherein the content of the organometallic compound having a group is 0.01 to 20 parts by mass per 100 parts by mass of the (B) polyphenylene ether resin. [8] A prepreg comprising the resin composition according to any one of [1] to [7] above. [9] A laminate comprising the prepreg according to [8] above and a metal foil.
[10] A resin film comprising the resin composition according to any one of the above [1] to [7].
[11] A printed wiring board comprising at least one member selected from the group consisting of the prepreg described in [8] above, the laminate described in [9] above, and the resin film described in
[10] above.
[12] A semiconductor package comprising the printed wiring board according to
[11] above and a semiconductor element mounted thereon.
[13] A method for producing the resin composition according to any one of the above [1] to [7], (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof; (B) a polyphenylene ether resin; (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons an organometallic compound having a group; A method for producing a resin composition comprising mixing the above components. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition which is economical and capable of exhibiting excellent dielectric properties in a high frequency band of 10 GHz or more, a method for producing the same, and a prepreg, a laminate, a resin film, a printed wiring board, and a semiconductor package which use the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. In addition, the lower and upper limits of the numerical ranges may be arbitrarily combined with the lower or upper limit of other numerical ranges. In addition, each component and material exemplified in this specification may be used alone or in combination of two or more types, unless otherwise specified. In this specification, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. The present invention also includes any combination of the features described in this specification.
[0011] [Resin composition] The resin composition of the present embodiment is (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof [hereinafter, sometimes abbreviated as "maleimide compound (A)" or "component (A)"], (B) a polyphenylene ether resin (hereinafter sometimes abbreviated as "polyphenylene ether resin (B)" or "component (B)"); (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons an organometallic compound having a group (hereinafter, sometimes abbreviated as "organometallic compound (C)" or "component (C)"); The resin composition comprises: Each component will be described in detail below.
[0012] <Component (A); Maleimide compound (A)> The maleimide compound (A) is at least one selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof. Examples of the "derivative of a maleimide compound having two or more N-substituted maleimide groups" include an addition reaction product between the maleimide compound having two or more N-substituted maleimide groups and an amine compound such as the diamine compound (a2) described below. The maleimide compound (A) may be used alone or in combination of two or more kinds.
[0013] As the maleimide compound (A), from the viewpoints of compatibility with other resins, adhesion to conductors, and dielectric properties, (i) a maleimide compound (a1) having two or more N-substituted maleimide groups (hereinafter, sometimes simply referred to as "maleimide compound (a1)" or "component (a1)"); and (ii) A polyaminobismaleimide compound having a structural unit derived from a maleimide compound (a1) and a structural unit derived from a diamine compound (a2) [hereinafter, sometimes abbreviated as "polyaminobismaleimide compound (A1)" or "component (A1)".] One or more selected from the group consisting of are preferred.
[0014] (Maleimide compound (a1)) The component (a1) is not particularly limited as long as it is a maleimide compound having two or more N-substituted maleimide groups, and examples thereof include aromatic maleimide compounds having two N-substituted maleimide groups in the molecule, such as bis(4-maleimidophenyl)methane, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane; aromatic polymaleimide compounds having three or more N-substituted maleimide groups in the molecule, such as polyphenylmethane maleimide and biphenyl aralkyl maleimide; and aliphatic maleimide compounds, such as 1,6-bismaleimido-(2,2,4-trimethyl)hexane and pyrophosphate binder type long chain alkyl bismaleimide. Among these, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, and biphenyl aralkyl maleimide are preferred from the standpoints of compatibility with other resins, adhesion to conductors, heat resistance, low thermal expansion, and mechanical properties. The component (a1) may be used alone or in combination of two or more kinds.
[0015] The component (a1) is preferably a bismaleimide compound represented by the following general formula (a1-1).
[0016] [ka] (In the formula, X a1 is a divalent organic group.
[0017] X in the above general formula (a1-1) a1 is a divalent organic group, which corresponds to the residue of component (a1). The residue of component (a1) refers to the structure of the portion remaining after removing the N-substituted maleimide group from component (a1). X a1Examples of the divalent organic group represented by the formula include groups represented by the following general formula (a1-2), (a1-3), (a1-4), (a1-5) or (a1-6).
[0018] [ka] (In the formula, R a1 is an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. p1 is an integer of 0 to 4.
[0019] R a1 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. The aliphatic hydrocarbon group may be an aliphatic hydrocarbon group having 1 to 3 carbon atoms or may be a methyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. p1 is an integer of 0 to 4, and from the viewpoint of availability, may be an integer of 0 to 2, may be 0 or 1, or may be 0. When p1 is an integer of 2 or more, a plurality of R a1 They may be the same or different.
[0020] [ka] (In the formula, R a2 and R a3 Each of X is independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a2 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, a single bond, or a divalent group represented by the following general formula (a1-3-1): p2 and p3 each independently represent an integer of 0 to 4.
[0021] R a2 and R a3The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R a1 The aliphatic hydrocarbon group may be an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and may be a methyl group, an ethyl group, or an ethyl group. X a2 Examples of the alkylene group having 1 to 5 carbon atoms represented by include a methylene group, a 1,2-dimethylene group, a 1,3-trimethylene group, a 1,4-tetramethylene group, a 1,5-pentamethylene group, etc. From the viewpoints of compatibility with other resins, adhesion to a conductor, heat resistance, low thermal expansion, and mechanical properties, the alkylene group may be an alkylene group having 1 to 3 carbon atoms or a methylene group. X a2 Examples of the alkylidene group having 2 to 5 carbon atoms represented by include an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a pentylidene group, an isopentylidene group, etc. Among these, an isopropylidene group may be used from the viewpoints of compatibility with other resins, adhesion to a conductor, heat resistance, low thermal expansion, and mechanical properties. X a2 Among the above options, may be an alkylene group having 1 to 5 carbon atoms or an alkylidene group having 2 to 5 carbon atoms. p2 and p3 are each independently an integer of 0 to 4, and from the viewpoint of availability, may be either an integer of 0 to 2, or may be 0 or 2. When p2 or p3 is an integer of 2 or more, a plurality of R a2 Friends or R a3 They may be the same or different. In addition, X a2 The divalent group represented by general formula (a1-3-1) is as follows.
[0022] [ka] (In the formula, R a4 and R a5 Each of X is independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a3represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. p4 and p5 each independently represent an integer of 0 to 4.
[0023] R a4 and R a5 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R a1 This is explained in the same way as in the case of X a3 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by X a2 Examples of the alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by the formula (I) are the same as those represented by the formula (I). X a3 Among the above options, may be an alkylidene group having 2 to 5 carbon atoms or an isopropylidene group. p4 and p5 are each independently an integer of 0 to 4. From the viewpoint of availability, each may be an integer of 0 to 2, or may be 0 or 1, or may be 0. When p4 or p5 is an integer of 2 or more, a plurality of R a4 Friends or R a5 They may be the same or different.
[0024] [ka] (In the formula, p6 is an integer of 0 to 10.)
[0025] p6 may be an integer of 0 to 5, or an integer of 0 to 3, from the viewpoint of availability.
[0026] [ka] (In the formula, p7 is a number from 0 to 5.)
[0027] [ka] (In the formula, R a6 and R a7 are each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms. p8 is an integer of 1 to 8.
[0028] R a6 and R a7 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R a1 This is explained in the same way as in the case of p8 is an integer of 1 to 8, and may be an integer of 1 to 3, or may be 1. If p8 is an integer equal to or greater than 2, multiple R a6 Friends or R a7 They may be the same or different.
[0029] (Polyaminobismaleimide compound (A1)) The polyaminobismaleimide compound (A1) is a polyaminobismaleimide compound having a structural unit derived from a maleimide compound (a1) and a structural unit derived from a diamine compound (a2). The component (A1) may be used alone or in combination of two or more kinds.
[0030] Examples of the structural unit derived from the component (a1) include one or more types selected from the group consisting of groups represented by general formula (a1-7) and groups represented by general formula (a1-8) below.
[0031] [ka] (In the formula, X a1 is a divalent organic group, and * indicates the bonding position to other structures.)
[0032] X in the above general formula (a1-7) and general formula (a1-8) a1 The explanation for X in the above general formula (a1-1) is a1 This is the same as the explanation for . The content of the structural unit derived from the (a1) component in the polyaminobismaleimide compound (A1) is not particularly limited, but is preferably 5 to 95 mass%, more preferably 30 to 93 mass%, further preferably 60 to 90 mass%, and particularly preferably 75 to 90 mass%. When the content of the structural unit derived from the (a1) component is within the above range, the dielectric properties in the high frequency band of 10 GHz or more become better, and good film handling properties tend to be obtained.
[0033] There are no particular limitations on the component (a2) so long as it is a compound having two amino groups, and the amino groups are preferably primary amino groups. Examples of the component (a2) include 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ketone, 4,4'-diaminobiphenyl, 3,3'-dimethyl ... 2,2'-Dimethyl-4,4'-diaminobiphenyl, 3,3'-Dihydroxybenzidine, 2,2-Bis(3-amino-4-hydroxyphenyl)propane, 3,3'-Dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 2,2-Bis(4-aminophenyl)propane, 2,2-Bis[4-(4-aminophenoxy)phenyl]propane, 1,3-Bis[4-(4-aminophenoxy)phenyl]propane, bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 1,3-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 1,4-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 4,4'-[1,3 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline, 3,3'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, and 9,9-bis(4-aminophenyl)fluorene. The component (a2) may be used alone or in combination of two or more types.
[0034] Among these, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline are preferred as the (a2) component from the viewpoints of excellent solubility in organic solvents, reactivity with the (a1) component, and heat resistance. Also, 3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane is preferred as the (a2) component from the viewpoints of excellent dielectric properties and low water absorption. From the viewpoints of excellent mechanical properties such as high adhesion to the conductor, elongation, and breaking strength, the component (a2) is preferably 2,2-bis[4-(4-aminophenoxy)phenyl]propane. Furthermore, from the viewpoints of excellent solubility in the above organic solvents, reactivity during synthesis, heat resistance, high adhesion to the conductor, as well as excellent dielectric properties and low moisture absorption, the component (a2) is preferably 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline or 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline.
[0035] Examples of the structural unit derived from the component (a2) include one or more types selected from the group consisting of groups represented by the following general formula (a2-1) and groups represented by the following general formula (a2-2).
[0036] [ka] (In the formula, X a4 is a divalent organic group, and * indicates the bonding position to other structures.)
[0037] X in the above general formulae (a2-1) and (a2-2) a4 is a divalent organic group, which corresponds to the residue of component (a2). The residue of component (a2) refers to the structure of the portion of component (a2) excluding the functional group used in the bond, i.e., the amino group.
[0038] X in the above general formula (a2-1) and the above general formula (a2-2) a4 is preferably a divalent group represented by the following general formula (a2-3).
[0039] [ka] (In the formula, R a11 and R a12 are each independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. a5 is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, a fluorenylene group, a single bond, or a divalent group represented by the following general formula (a2-3-1) or (a2-3-2). q1 and q2 each independently represent an integer of 0 to 4.
[0040] [ka] (In the formula, R a13 and R a14 Each of X is independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a6 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an m-phenylenediisopropylidene group, a p-phenylenediisopropylidene group, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. q3 and q4 each independently represent an integer of 0 to 4.
[0041] [ka] (In the formula, R a15 Each of X is independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a7 and X a8are each independently an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. q5 is an integer of 0 to 4.
[0042] R in the above general formula (a2-3), (a2-3-1) or (a2-3-2) a11 , R a12 , R a13 , R a14 and R a15 The aliphatic hydrocarbon group having 1 to 5 carbon atoms or the halogen atom represented by R a1 The aliphatic hydrocarbon group may be an aliphatic hydrocarbon group having 1 to 3 carbon atoms, or may be a methyl group or an ethyl group. X in the above general formula (a2-3) a5 In the above general formula (a2-3-1), X a6 And X in the above general formula (a2-3-2) a7 and X a8 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by X in the above general formula (a1-3) are a2 This is explained in the same way as in the case of In the above general formula (a2-3), q1 and q2 are each independently an integer of 0 to 4. From the viewpoint of availability, each may be an integer of 0 to 2, or may be 0 or 2. When q1 or q2 is an integer of 2 or more, multiple R a11 Friends or R a12 They may be the same or different. In the above general formula (a2-3-1), q3 and q4 are each independently an integer of 0 to 4. From the viewpoint of availability, each may be an integer of 0 to 2, or may be 0 or 1, or may be 0. When q3 or q4 is an integer of 2 or more, multiple R a13 Friends or R a14 They may be the same or different. In the above general formula (a2-3-2), q5 is an integer of 0 to 4. From the viewpoint of availability, it may be an integer of 0 to 2, or may be 0. When q5 is an integer of 2 or more, a plurality of R a15 They may be the same or different.
[0043] The content of the structural unit derived from the (a2) component in the polyaminobismaleimide compound (A1) is not particularly limited, but is preferably 5 to 95 mass%, more preferably 7 to 70 mass%, further preferably 10 to 40 mass%, and particularly preferably 10 to 25 mass%. When the content of the structural unit derived from the (a2) component is within the above range, excellent dielectric properties, and better heat resistance, flame retardancy, and glass transition temperature tend to be obtained.
[0044] The total content of the structural units derived from the component (a1) and the structural units derived from the component (a2) in the polyaminobismaleimide compound (A1) is not particularly limited, but is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass%.
[0045] The content ratio of the structural unit derived from the component (a1) and the structural unit derived from the component (a2) in the polyamino bismaleimide compound (A1) is such that the equivalent ratio (Ta2 / Ta1) of the total equivalent (Ta2) of the groups (including -NH2) derived from the -NH2 group of the component (a2) in the polyamino bismaleimide compound (A1) to the total equivalent (Ta1) of the groups (including N-substituted maleimide groups) derived from the N-substituted maleimide group of the component (a1) in the polyamino bismaleimide compound (A1) is preferably 0.05 to 10, more preferably 1 to 5. When the equivalent ratio (Ta2 / Ta1) is within the above range, excellent dielectric properties, and better heat resistance, flame retardancy, and glass transition temperature tend to be obtained.
[0046] From the viewpoints of dielectric properties, solubility in organic solvents, high adhesion to conductors, and moldability of resin films, it is preferable that the polyaminobismaleimide compound (A1) contains a polyaminobismaleimide compound represented by the following general formula (a2-4):
[0047] [ka] (In the formula, X a1 and X a4 is as explained above.)
[0048] (Production method of polyaminobismaleimide compound (A1)) The component (A1) can be produced, for example, by reacting the component (a1) with the component (a2). The reaction between the components (a1) and (a2) is preferably carried out in an organic solvent, and a reaction catalyst can also be used as necessary. The reaction catalyst is not particularly limited, but examples thereof include acid catalysts such as p-toluenesulfonic acid, amines such as triethylamine, pyridine, tributylamine, imidazoles such as methylimidazole, phenylimidazole, phosphorus catalysts such as triphenylphosphine, etc. These may be used alone or in combination of two or more. The amount of the reaction catalyst is not particularly limited, but is, for example, 0.01 to 5 parts by mass per 100 parts by mass of the total amount of the components (a1) and (a2).
[0049] The polyaminobismaleimide compound is obtained by charging the (a1) component, the (a2) component, and other components, if necessary, in a synthesis vessel in predetermined amounts and reacting the (a1) component with the (a2) component. The reaction between the (a1) component and the (a2) component is a Michael addition reaction, and the reaction conditions are not particularly limited, but from the viewpoints of workability such as reaction rate and suppression of gelation during the reaction, the reaction temperature is preferably 50 to 160°C, and the reaction time is preferably 1 to 10 hours. In this step, the organic solvent can be added or concentrated to adjust the solid content concentration and solution viscosity of the reaction raw materials. The solid content concentration of the reaction raw materials is not particularly limited, but is preferably 10 to 90 mass%, more preferably 20 to 80 mass%. When the solid content concentration of the reaction raw materials is 10 mass% or more, the reaction rate does not become too slow, and there is a tendency that it is advantageous in terms of production costs. Furthermore, when the solid content concentration of the reaction raw materials is 90 mass% or less, better solubility is obtained, stirring efficiency is improved, and gelation tends to be less likely.
[0050] The number average molecular weight of the polyaminobismaleimide compound (A1) is not particularly limited, but is preferably 400 to 10,000, more preferably 500 to 5,000, further preferably 600 to 2,000, and particularly preferably 700 to 1,500. In this specification, the number average molecular weight means a value measured by gel permeation chromatography (GPC) in terms of polystyrene, and specifically, it can be measured by the method described in the examples.
[0051] The content of component (A) in the resin composition of this embodiment is not particularly limited, but from the viewpoint of dielectric properties and moldability in a high frequency band of 10 GHz or more, the content is preferably 10 to 90 parts by mass, more preferably 20 to 80 parts by mass, even more preferably 30 to 70 parts by mass, and particularly preferably 35 to 60 parts by mass, relative to 100 parts by mass of the total of the resin components in the resin composition. In this specification, the term "resin components" refers to components (A) and (B) as well as any resins that are optionally used. The optionally used resins are components (D), (E) and other resins, and components (C), (F) and (G) are not included in the resin components when calculating the content.
[0052] <Component (B): Polyphenylene ether resin (B)> The polyphenylene ether resin (B) is not particularly limited, but examples thereof include one or more types selected from the group consisting of polyphenylene ether and polyphenylene ether derivatives. The component (B) may be used alone or in combination of two or more types.
[0053] The component (B) preferably has a structural unit represented by the following general formula (B-1).
[0054] [ka] (In the formula, R B1 are each independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. B1 is an integer between 0 and 4.)
[0055] R in the above general formula (B-1) B1 are each independently an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. Examples of the aliphatic hydrocarbon group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, and an n-pentyl group. Examples of the aliphatic hydrocarbon group include an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and a methyl group is more preferable. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Among the above, R B1 is preferably an aliphatic hydrocarbon group having 1 to 5 carbon atoms. n B1 is an integer of 0 to 4, and may be an integer of 1 or 2, or may be 2. B1 If is 1 or 2, R B1 may be substituted at the ortho position on the benzene ring (based on the substitution position of the oxygen atom). B1 If is 2 or more, multiple R B1 They may be the same or different. The structural unit represented by the above general formula (B-1) may specifically be a structural unit represented by the following general formula (B-1').
[0056] [ka]
[0057] The number average molecular weight of the polyphenylene ether resin (B) is preferably 1,000 to 25,000. When the number average molecular weight of the polyphenylene ether resin (B) is 1,000 or more, the dielectric properties in a high frequency band of 10 GHz or more tend to be further improved, and when it is 25,000 or less, the compatibility of the resin composition is improved, and separation tends to be difficult even when left for a long period of time. From the same viewpoint, the number average molecular weight of the polyphenylene ether resin (B) is more preferably 2,000 to 20,000, further preferably 3,000 to 10,000, and particularly preferably 4,000 to 6,000.
[0058] The polyphenylene ether resin (B) is preferably a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group (hereinafter, the polyphenylene ether derivative having an ethylenically unsaturated bond-containing group may be abbreviated as "polyphenylene ether derivative (B1)" or "component (B1)"). In this specification, the term "ethylenically unsaturated bond" means a carbon-carbon double bond capable of undergoing an addition reaction and does not include double bonds in aromatic rings, and the term "ethylenically unsaturated bond-containing group" means a substituent containing the above-mentioned ethylenically unsaturated bond.
[0059] In the polyphenylene ether derivative (B1), the position of the ethylenically unsaturated bond-containing group is not particularly limited, and for example, it may be present at one terminal or at both terminals. The component (B1) may be a mixture of a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at one end and a polyphenylene ether derivative having ethylenically unsaturated bond-containing groups at both ends, but it preferably contains at least a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at one end, and more preferably is a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at one end itself. When the component (B) contains a polyphenylene ether derivative (B1) having an ethylenically unsaturated bond-containing group at one end, the content of the polyphenylene ether derivative (B1) having an ethylenically unsaturated bond-containing group at one end in the component (B) is not particularly limited, and may be 30 mass % or more, 45 mass % or more, 55 mass % or more, 70 mass % or more, 90 mass % or more, or substantially 100 mass %.
[0060] Examples of the ethylenically unsaturated bond-containing group contained in component (B1) include unsaturated aliphatic hydrocarbon groups such as vinyl groups, isopropenyl groups, allyl groups, 1-methylallyl groups, and 3-butenyl groups; and heteroatom-containing substituents such as maleimide groups and (meth)acryloyl groups. Among these, from the viewpoint of dielectric properties in high frequency bands of 10 GHz or more, unsaturated aliphatic hydrocarbon groups or maleimide groups are preferred, allyl groups or maleimide groups are more preferred, and allyl groups are even more preferred. In this specification, groups which contain an unsaturated aliphatic hydrocarbon group in part but cannot be considered an unsaturated aliphatic hydrocarbon group when viewed as a whole, such as a maleimide group, a (meth)acryloyl group, etc., are not included in the above-mentioned "unsaturated aliphatic hydrocarbon group".
[0061] The number of ethylenically unsaturated bond-containing groups that the component (B1) has in one molecule is not particularly limited, but from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more, it is preferably 2 or more, more preferably 4 or more, and may be 8 or less, or may be 6 or less. Furthermore, from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more, the number of ethylenically unsaturated bond-containing groups that the component (B1) has at one end is preferably 2 or more, more preferably 4 or more, and may be 8 or less, or may be 6 or less.
[0062] From the viewpoint of dielectric properties in the high frequency band of 10 GHz or more, the component (B1) preferably contains a structure represented by the following general formula (B-2).
[0063] [ka] (In the formula, R B2 are each independently an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. B2 is 1 or 2, n B3 is 0 or 1. * indicates the position of attachment to other structures.)
[0064] In the above general formula (B-2), R B2 Examples of the unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms represented by include a vinyl group, an isopropenyl group, an allyl group, a 1-methylallyl group, a 3-butenyl group, etc. Among these, from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more, an unsaturated aliphatic hydrocarbon group having 2 to 5 carbon atoms is preferred, and an allyl group is more preferred.
[0065] From the viewpoint of dielectric properties in the high frequency band of 10 GHz or higher, the component (B1) also preferably has a structure represented by the following general formula (B-3).
[0066] [ka] (In the formula, R B3 and R B4 are each independently an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. * indicates the bonding position to other structures.)
[0067] In the above general formula (B-3), R B3 and R B4 The unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms represented by R B2 The same as those mentioned above can be mentioned, and the same are preferred.
[0068] From the viewpoint of dielectric properties in the high frequency band of 10 GHz or more, the (B1) component more preferably contains a structure represented by any one of the following general formulas (B-4) to (B-6), and even more preferably contains a structure represented by the following general formula (B-6).
[0069] [ka] (In the formula, R B5 is an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. * indicates the bonding position to other structures.)
[0070] [ka] (In the formula, R B6 and R B7 are each independently an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. B1 is a divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms. * indicates the bonding position to other structures.)
[0071] [ka] (In the formula, R B8 ~R B11 are each independently an unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms. B2 is a divalent organic group. * indicates the bonding position to other structures.)
[0072] R in the above general formulas (B-4) to (B-6) B5 ~R B11 The unsaturated aliphatic hydrocarbon group having 2 to 10 carbon atoms represented by R B2 The same can be mentioned as in the above, and the preferred ones are also the same. X in the above general formula (B-5) B1Examples of the divalent aliphatic hydrocarbon group having 1 to 6 carbon atoms represented by include alkylene groups having 1 to 6 carbon atoms, such as a methylene group, an ethylene group, and a trimethylene group; and alkylidene groups having 2 to 6 carbon atoms, such as an isopropylidene group. Among these, a methylene group and an isopropylidene group are preferred, and an isopropylidene group is more preferred. X in the above general formula (B-6) B2 Examples of the divalent organic group represented by include an aliphatic hydrocarbon group which may contain a heteroatom in part, an alicyclic hydrocarbon group which may contain a heteroatom in part, an aromatic hydrocarbon group which may contain a heteroatom in part, and a group consisting of any combination of these. Examples of the heteroatom include an oxygen atom, a nitrogen atom, and a sulfur atom. X B2 The divalent organic group represented by is preferably a group containing no heteroatoms, more preferably an aliphatic hydrocarbon group containing no heteroatoms or an alicyclic hydrocarbon group containing no heteroatoms, and even more preferably a group consisting of a combination of an aliphatic hydrocarbon group containing no heteroatoms and an alicyclic hydrocarbon group containing no heteroatoms.
[0073] More preferred embodiments of the structures represented by the above general formula (B-4), (B-5) or (B-6) are structures represented by the following formula (B-4'), (B-5') or (B-6'), respectively, from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more. Among these, from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more, the structures represented by the following formula (B-5') or (B-6') are more preferred, and the structure represented by the following formula (B-6') is even more preferred.
[0074] [ka] (In the formula, X B2 is X in the above general formula (B-6) B2 (The symbol * indicates the position of attachment to another structure.)
[0075] The component (B) may contain, as the component (B1), a polyphenylene ether derivative represented by any one of the following general formulas (B-7) to (B-9), and particularly preferably contains a polyphenylene ether derivative represented by the following general formula (B-8) or (B-9), and more preferably contains a polyphenylene ether derivative represented by the following general formula (B-9).
[0076] [ka] (In the formula, X B2 is X in the above general formula (B-6) B2 is the same as n B4 ~n B6 are each independently an integer of 1 to 200.
[0077] In the above general formulae (B-7) to (B-9), n B4 ~n B6 are each independently an integer of 1 to 200, and may be an integer of 1 or more, an integer of 10 or more, an integer of 20 or more, or an integer of 25 or more from the viewpoint of the dielectric properties in a high frequency band of 10 GHz or more and the compatibility of the resin composition. B4 ~n B6 may each independently be an integer of 150 or less, an integer of 120 or less, or an integer of 100 or less. In any of the above general formulas (B-7) to (B-9), n B4 ~n B6 It may be, and usually tends to be, a mixture of polyphenylene ether derivatives having different values of
[0078] [Method for producing component (B)] One embodiment of a method for producing the component (B) will be described below, however, the method for producing the component (B) is not particularly limited to the method described below. The polyphenylene ether resin (B) can be prepared, for example, by subjecting a raw material polyphenylene ether and a phenol compound to a redistribution reaction. The above-mentioned redistribution reaction is a reaction in which, for example, a phenol compound is mixed with a raw material polyphenylene ether already produced by polymerization in an organic solvent, and a reaction catalyst is added as necessary, so that an oxy radical of the phenol compound attacks a carbon atom to which an oxygen atom in the raw material polyphenylene ether is bonded, whereby the O-C bond is broken and the molecular weight is reduced. At that time, the oxy radical of the phenol compound that attacked bonds with the carbon atom whose bond is broken, and is incorporated into the structure of the polyphenylene ether. As the redistribution reaction, a known method can be used and applied. As the raw material polyphenylene ether, for example, polyphenylene ether having a number average molecular weight of 3,000 to 30,000 can be used.
[0079] The molecular weight of the polyphenylene ether resin (B) can be controlled by the amount of the phenol compound used, and the more the amount of the phenol compound used, the lower the molecular weight of the (B) component. In other words, the amount of the phenol compound used can be appropriately adjusted so that the number average molecular weight of the (B) component finally produced falls within a suitable range. The amount of the phenol compound used is not particularly limited, but for example, if the number average molecular weight of the raw material polyphenylene ether to be reacted with the phenol compound is 3,000 to 30,000, the phenol compound is used in an amount such that the number of hydroxyl groups per mole of the raw material polyphenylene ether is 1 to 10 moles, preferably 4 to 7 moles, to obtain component (B) having a number average molecular weight within the above-mentioned preferred range.
[0080] When preparing a polyphenylene ether derivative (B1) having an ethylenically unsaturated bond-containing group as the component (B), it is preferable to use, as the phenol compound, a phenol compound containing an unsaturated aliphatic hydrocarbon group, specifically, for example, a phenol compound containing a structure represented by any one of the above general formulas (B-2) to (B-6).
[0081] The organic solvent used in the production process of the polyphenylene ether resin (B) is not particularly limited, but examples thereof include alcohols such as methanol, ethanol, butanol, butyl cellosolve, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and mesitylene; esters such as methoxyethyl acetate, ethoxyethyl acetate, butoxyethyl acetate, and ethyl acetate; and nitrogen-containing compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These may be used alone or in combination of two or more.
[0082] In the process for producing the polyphenylene ether resin (B), a reaction catalyst can be used as necessary, as described above. As the reaction catalyst, for example, from the viewpoint of obtaining the component (B) having a stable number average molecular weight with good reproducibility, it is preferable to use an organic peroxide such as t-butylperoxyisopropyl monocarbonate in combination with a metal carboxylate such as manganese naphthenate or manganese octylate. The amount of the reaction catalyst used is not particularly limited, but from the viewpoint of the reaction rate and gelation suppression when producing the (B) component, for example, 0.5 to 5 parts by mass of the organic peroxide and 0.05 to 0.5 parts by mass of the metal carboxylate may be used per 100 parts by mass of the raw material polyphenylene ether to be reacted with the phenol compound.
[0083] The reaction conditions in the redistribution reaction, such as the reaction temperature and reaction time, may be appropriately adjusted depending on the raw materials used, the structure of the target polyphenylene ether, and the like. From the viewpoints of workability and suppression of gelation, and from the viewpoint of obtaining the component (B) having the desired number average molecular weight, for example, the reaction temperature may be set to 70 to 110°C and the reaction time to 1 to 8 hours.
[0084] The solids concentration during the reaction in the production process of component (B) [hereinafter also referred to as "reaction concentration"] is not particularly limited, but may be, for example, 10 to 60% by mass, or 20 to 50% by mass. If the reaction concentration is 10% by mass or more, the reaction rate does not become too slow and there is a tendency for it to be more advantageous in terms of production costs, and if it is 60% by mass or less, better solubility and low solution viscosity are obtained, stirring efficiency is good, and gelation tends to be less likely.
[0085] The solution of the polyphenylene ether resin (B) produced as described above may be concentrated to remove a part of the organic solvent, or may be diluted by adding an organic solvent, if necessary.
[0086] The content of the (B) component in the resin composition of the present embodiment is not particularly limited, but from the viewpoint of dielectric properties in the high frequency band of 10 GHz or more, it is preferably 1 to 20 parts by mass, more preferably 1.5 to 10 parts by mass, and even more preferably 2 to 5 parts by mass per 100 parts by mass of the total of the resin components in the resin composition.
[0087] The content ratio of the (A) component to the (B) component [(B) / (A)] (mass ratio) is not particularly limited, but is preferably 1 / 99 to 80 / 20, more preferably 2 / 98 to 75 / 25, even more preferably 3 / 97 to 70 / 30, even more preferably 4 / 96 to 50 / 50, particularly preferably 4 / 96 to 20 / 80, and most preferably 4 / 96 to 10 / 80. When the content ratio [(B) / (A)] is 1 / 99 or more, excellent dielectric properties tend to be obtained in high frequency bands of 10 GHz or more, and when it is 80 / 20 or less, heat resistance, moldability, and processability tend to be excellent.
[0088] <(C) component; organometallic compound (C)> The organometallic compound (C) is Through one oxygen atom Bonds to metal atoms Hydrocarbons It is an organometallic compound having a group. The resin composition of the present embodiment contains the organometallic compound (C), and thus can exhibit excellent dielectric properties in the high frequency band of 10 GHz or higher. Although the reason for this is unclear, the component (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons Since the component (C) has a group, A hydrocarbon bonded to a metal atom via one oxygen atom It is believed that a ligand exchange reaction occurs between the hydroxyl group of the (B) component and the hydroxyl group of the (B) component in the (C) group, and the hydroxyl group of the (B) component is modified by the (C) component. Since the hydroxyl group has a relatively high polarity in the system, it is believed that the dielectric tangent of the cured product is reduced by modifying the hydroxyl group. As described above, the resin composition of the present embodiment is also economical in that excellent dielectric properties can be easily achieved by simply blending the (C) component. In this embodiment, when a hydrocarbon group forms a chelate bond with a metal atom via two oxygen atoms, the group is A hydrocarbon bonded to a metal atom via one oxygen atom The chelate bond herein means a bond of a compound having two or more coordinating atoms in one molecule, which are coordinated to surround a metal atom to form a ring structure. The organometallic compound (C) may be used alone or in combination of two or more kinds.
[0089] Examples of the metal atom contained in the organometallic compound (C) include titanium, zirconium, and aluminum atoms. Among these, from the viewpoint of further improving the dielectric properties in the high frequency band of 10 GHz or more, titanium or zirconium atoms are preferred, and titanium atoms are more preferred. That is, the component (C) is a compound containing titanium atoms. Through one oxygen atom Combine Hydrocarbons An organic titanium compound having a group and a zirconium atom Through one oxygen atom Combine Hydrocarbons The compound is preferably one or more selected from the group consisting of organic zirconium compounds having a group, Through one oxygen atom Combine Hydrocarbons More preferably, it is an organotitanium compound having a group.
[0090] (C) Component has A hydrocarbon bonded to a metal atom via one oxygen atom Examples of the group include a group represented by the following general formula (C-3).
[0091] [ka] (In the formula, R C1 represents a hydrocarbon group having 1 to 10 carbon atoms, and * represents the bonding position to the metal atom.)
[0092] In the above general formula (C-3), R C1 The hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) preferably has 2 to 8 carbon atoms, and more preferably has 3 to 6 carbon atoms. R C1 Examples of the hydrocarbon group having 1 to 10 carbon atoms represented by include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl; alkenyl groups such as vinyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, and acetylacetonate; and alkynyl groups. These hydrocarbon groups may be substituted with heteroatoms such as oxygen and nitrogen atoms, or may not be substituted. Among the above-mentioned hydrocarbon groups, the hydrocarbon groups having 3 or more carbon atoms may be linear or branched. Among these, from the viewpoints of reactivity and dielectric properties in a high frequency band of 10 GHz or more, an alkyl group or an alkenyl group is preferred, a propyl group or an acetylacetonate group is more preferred, and an isopropyl group is even more preferred.
[0093] From the viewpoint of dielectric properties in the high frequency band of 10 GHz or higher, it is preferable that the component (C) does not have a hydroxyl group in the molecule.
[0094] From the viewpoint of dielectric properties in the high frequency band of 10 GHz or more, the component (C) is preferably a compound represented by the following general formula (C-1) or the following general formula (C-2).
[0095] [ka] (In the above general formulas (C-1) and (C-2), R C1 is as explained above. C1 represents a titanium atom or a zirconium atom. C2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.
[0096] R in the above general formula (C-1) and general formula (C-2) C1 The explanation for formula (C-3) is as above, and the preferred embodiments are also the same. R in the above general formula (C-2) C2 The hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) preferably has 2 to 8 carbon atoms, and more preferably has 3 to 6 carbon atoms. R C2 Examples of the hydrocarbon group having 1 to 10 carbon atoms represented by include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl; alkenyl groups such as vinyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, and decenyl; and alkynyl groups. These hydrocarbon groups may be substituted with heteroatoms such as oxygen and nitrogen atoms, or may not be substituted. Among the above hydrocarbon groups, the hydrocarbon groups having 3 or more carbon atoms may be linear or branched. Among these, alkyl groups and alkenyl groups are preferred, alkyl groups are more preferred, and methyl or ethyl groups are even more preferred. M in the above general formula (C-1) and general formula (C-2) C1 is a titanium atom or a zirconium atom, and is preferably a titanium atom.
[0097] Examples of the (C) component include organic titanium compounds such as tetraethoxytitanium, tetraisopropoxytitanium, tetra n-propoxytitanium, tetrabutoxytitanium, tetramethoxytitanium, titanium diisopropoxybis(acetylacetonate), titanium diisopropoxybis(ethylacetoacetate), and titanium tetraacetylacetonate; and organic zirconium compounds such as tetraethoxyzirconium, tetraisopropoxyzirconium, tetra n-propoxyzirconium, tetrabutoxyzirconium, tetramethoxyzirconium, zirconium diisopropoxybis(acetylacetonate), zirconium diisopropoxybis(ethylacetoacetate), and zirconium tetraacetylacetonate. Among these, titanium diisopropoxybis(acetylacetonate) and titanium tetraacetylacetonate are preferred from the viewpoint of improving reactivity and dielectric properties in the high frequency band.
[0098] The content of the (C) component in the resin composition of this embodiment is not particularly limited, but is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 1 to 5 parts by mass, per 100 parts by mass of the (B) component.
[0099] <Other ingredients> The resin composition of the present embodiment may further contain other components. Examples of the other components include one or more selected from a styrene-based thermoplastic elastomer (D) [hereinafter, sometimes abbreviated as "component (D)"], a crosslinking agent (E) [hereinafter, sometimes abbreviated as "component (E)"], a curing accelerator (F) [hereinafter, sometimes abbreviated as "component (F)"], a flame retardant (G) [hereinafter, sometimes abbreviated as "component (G)"], and an inorganic filler (H) [hereinafter, sometimes abbreviated as "component (H)"]. By including these, it is possible to further improve various properties when the laminate is formed. However, the resin composition of the present embodiment may not include one or more selected from the component (D), the component (E), the component (F), the component (G), and the component (H) depending on the desired performance. These components are described in detail below.
[0100] <Component (D): Styrene-based thermoplastic elastomer (D)> By including the styrene-based thermoplastic elastomer (D) in the resin composition of this embodiment, the balance of the dielectric properties in the high frequency band of 10 GHz or more, moldability, adhesion to a conductor, solder heat resistance, glass transition temperature, thermal expansion coefficient, and flame retardancy tends to be improved. Examples of the component (D) include thermoplastic elastomers having a structural unit derived from a styrene-based compound represented by the following general formula (D-1) (see below), and the structural unit derived from styrene (R D1 = hydrogen atom, k=0).
[0101] [ka] (In the formula, R D1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and R D2 is an alkyl group having 1 to 5 carbon atoms. k is an integer of 0 to 5.
[0102] R D1 and R D2 Examples of the alkyl group having 1 to 5 carbon atoms represented by include a methyl group, an ethyl group, and an n-propyl group, and the alkyl group may be an alkyl group having 1 to 3 carbon atoms or a methyl group. k may be an integer of 0 to 2, or may be 0 or 1, or may be 0.
[0103] Examples of structural units contained in the component (D) other than those derived from styrene-based compounds include structural units derived from butadiene, structural units derived from isoprene, structural units derived from maleic acid, and structural units derived from maleic anhydride. The component (D) may be used alone or in combination of two or more types. The butadiene-derived structural unit and the isoprene-derived structural unit may be hydrogenated. When hydrogenated, the butadiene-derived structural unit is a structural unit having a mixture of ethylene units and butylene units, and the isoprene-derived structural unit is a structural unit having a mixture of ethylene units and propylene units.
[0104] As the (D) component, from the viewpoints of dielectric properties in the high frequency band of 10 GHz or more, adhesion to conductors, heat resistance, glass transition temperature, and thermal expansion coefficient, one or more types selected from the group consisting of hydrogenated styrene-butadiene-styrene block copolymers (SEBS, SBBS), hydrogenated styrene-isoprene-styrene block copolymers (SEPS), and styrene-maleic anhydride copolymers (SMA) are preferred, one or more types selected from the group consisting of hydrogenated styrene-butadiene-styrene block copolymers (SEBS) and hydrogenated styrene-isoprene-styrene block copolymers (SEPS) are more preferred, and hydrogenated styrene-butadiene-styrene block copolymers (SEBS) are even more preferred.
[0105] In the above SEBS, the content of structural units derived from styrene [hereinafter sometimes abbreviated as "styrene content"] is preferably 5 to 80 mass%, more preferably 10 to 75 mass%, further preferably 15 to 70 mass%, and particularly preferably 20 to 50 mass%, from the viewpoints of dielectric characteristics in a high frequency band of 10 GHz or more, adhesion to a conductor, heat resistance, glass transition temperature, and thermal expansion coefficient. Examples of commercially available SEBS products include the Tuftec (registered trademark) H series and M series manufactured by Asahi Kasei Corporation, the Septon (registered trademark) series manufactured by Kuraray Co., Ltd., and the Kraton (registered trademark) G Polymer series manufactured by Kraton Polymer Japan, Ltd.
[0106] The weight average molecular weight (Mw) of the component (D) is not particularly limited, but is preferably 12,000 to 1,000,000, more preferably 20,000 to 500,000, still more preferably 30,000 to 100,000, and particularly preferably 40,000 to 70,000. The weight average molecular weight (Mw) is measured in terms of polystyrene by gel permeation chromatography (GPC).
[0107] When the resin composition of the present embodiment contains the (D) component, the content of the (D) component is not particularly limited, but from the viewpoint of the dielectric properties, adhesion to the conductor, heat resistance, glass transition temperature, and thermal expansion coefficient in the high frequency band of 10 GHz or more, it is preferably 5 to 60 parts by mass, more preferably 10 to 55 parts by mass, even more preferably 15 to 50 parts by mass, particularly preferably 20 to 45 parts by mass, and most preferably 25 to 40 parts by mass, relative to 100 parts by mass of the total of the resin components in the resin composition. When the content of the (D) component is 5 parts by mass or more, the dielectric properties and moisture absorption resistance in the high frequency band of 10 GHz or more tend to be better, and when it is 60 parts by mass or less, the heat resistance, moldability, processability, and flame retardancy tend to be better.
[0108] <Component (E); Crosslinking agent> By containing the crosslinking agent (E), the resin composition of the present embodiment tends to have even more excellent heat resistance and dielectric properties. The crosslinking agent (E) may be used alone or in combination of two or more kinds.
[0109] The crosslinking agent (E) may, for example, be a compound having two or more ethylenically unsaturated bonds. The ethylenically unsaturated bond is, for example, an unsaturated bond contained in an unsaturated aliphatic hydrocarbon group such as a vinyl group, an isopropenyl group, an allyl group, a 1-methylallyl group, a 3-butenyl group, etc.; or a heteroatom-containing substituent such as a maleimide group, a (meth)acryloyl group, etc. Among these, the crosslinking agent (E) is preferably one having a vinyl group as the ethylenically unsaturated bond, from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more. The number of ethylenically unsaturated bonds that the crosslinking agent (E) has in one molecule is preferably 3 or more, more preferably 5 or more, and even more preferably 10 or more, from the viewpoint of obtaining excellent heat resistance.
[0110] As the crosslinking agent (E), from the viewpoints of compatibility with other resins, dielectric properties, low thermal expansion and heat resistance, a polymer having two or more ethylenically unsaturated bonds as vinyl groups is preferred, polybutadiene having two or more 1,2-vinyl groups and butadiene-styrene copolymer having two or more 1,2-vinyl groups are more preferred, and polybutadiene having two or more 1,2-vinyl groups is even more preferred.
[0111] When the crosslinking agent (E) is a polybutadiene having two or more 1,2-vinyl groups, the content of structural units having a 1,2-vinyl structure with respect to all structural units derived from butadiene constituting the polybutadiene [hereinafter sometimes abbreviated as vinyl group content] is not particularly limited, but is preferably 50 mol% or more, more preferably 60 mol% or more, even more preferably 70 mol% or more, particularly preferably 80 mol% or more, and most preferably 85 mol% or more. From the same viewpoint, the polybutadiene having two or more 1,2-vinyl groups is preferably a 1,2-polybutadiene homopolymer.
[0112] The number average molecular weight of a polymer having two or more ethylenically unsaturated bonds, preferably a polybutadiene having two or more 1,2-vinyl groups, is preferably 500 to 10,000, more preferably 800 to 5,000, and even more preferably 1,000 to 3,500, from the viewpoint of compatibility with other resins, dielectric properties, low thermal expansion, and heat resistance. From the viewpoint of compatibility, it may be 3,000 or less, or may be 2,500 or less. The number average molecular weight of a polymer having two or more ethylenically unsaturated bonds can be measured by the method described in the Examples.
[0113] When the resin composition of the present embodiment contains the (E) component, the content of the (E) component is not particularly limited, but from the viewpoint of obtaining excellent heat resistance and from the viewpoint of dielectric properties in a high frequency band of 10 GHz or more, the content of the (E) component is preferably 5 to 60 parts by mass, more preferably 7 to 40 parts by mass, even more preferably 10 to 30 parts by mass, and particularly preferably 13 to 20 parts by mass, relative to 100 parts by mass of the total of the resin components in the resin composition.
[0114] <Component (F); Curing accelerator (F)> By adding the curing accelerator (F) to the resin composition of the present embodiment, the curability of the resin composition is improved, and the dielectric properties, heat resistance, adhesion to a conductor, elastic modulus, and glass transition temperature in a high frequency band of 10 GHz or more tend to be improved. Examples of the (F) component include acid catalysts such as p-toluenesulfonic acid; amine compounds such as triethylamine, pyridine, and tributylamine; imidazole compounds such as methylimidazole, phenylimidazole, and isocyanate-masked imidazole (for example, an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); tertiary amine compounds; quaternary ammonium compounds; phosphorus compounds such as triphenylphosphine; organic peroxides such as dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, and α,α'-bis(t-butylperoxy)diisopropylbenzene; and carboxylates such as manganese, cobalt, and zinc. These may be used alone or in combination of two or more. Among these, from the viewpoints of heat resistance, glass transition temperature, and storage stability, imidazole compounds, organic peroxides, and carboxylates may be used, and from the viewpoints of heat resistance, glass transition temperature, elastic modulus, and thermal expansion coefficient, imidazole compounds and organic peroxides may be used in combination. As the imidazole compound, isocyanate-masked imidazole is preferred, and as the organic peroxide, α,α'-bis(t-butylperoxy)diisopropylbenzene is preferred.
[0115] When the resin composition of the present embodiment contains the (F) component, the content of the (F) component is not particularly limited, but is, for example, preferably 0.01 to 10 parts by mass, more preferably 0.05 to 8 parts by mass, further preferably 0.1 to 6 parts by mass, and particularly preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total of the resin components in the resin composition. When the (F) component content is within the above range, better heat resistance and storage stability tend to be obtained.
[0116] <(G) Ingredient; Flame retardant (G)> By including a flame retardant (G) in the resin composition of this embodiment, the flame retardancy of the resin composition tends to be improved. Examples of the (G) component include phosphorus-based flame retardants, metal hydrates, and halogen-based flame retardants. From the viewpoint of environmental issues, phosphorus-based flame retardants and metal hydrates are also acceptable. The flame retardant (G) may be used alone or in combination of two or more. Furthermore, a flame retardant assistant may be included as necessary.
[0117] - Phosphorus-based flame retardants - The phosphorus-based flame retardant is not particularly limited as long as it contains phosphorus atoms among those generally used as flame retardants, and may be an inorganic phosphorus-based flame retardant or an organic phosphorus-based flame retardant. From the viewpoint of environmental issues, it is preferable that it does not contain halogen atoms. From the viewpoints of dielectric properties in a high frequency band of 10 GHz or more, adhesion to a conductor, heat resistance, glass transition temperature, thermal expansion coefficient, and flame retardancy, it may be an organic phosphorus-based flame retardant. Examples of inorganic phosphorus-based flame retardants include red phosphorus; ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate; inorganic nitrogen-containing phosphorus compounds such as phosphoric acid amide; phosphoric acid; and phosphine oxide. Examples of organic phosphorus-based flame retardants include aromatic phosphate esters, mono-substituted phosphonic acid diesters, di-substituted phosphinic acid esters, metal salts of di-substituted phosphinic acid, organic nitrogen-containing phosphorus compounds, and cyclic organic phosphorus compounds. Among these, aromatic phosphate ester compounds and metal salts of di-substituted phosphinic acid are preferred. Here, the metal salt may be any of lithium salts, sodium salts, potassium salts, calcium salts, magnesium salts, aluminum salts, titanium salts, and zinc salts, or may be aluminum salts. In addition, aromatic phosphate esters are preferred among organic phosphorus-based flame retardants.
[0118] Examples of aromatic phosphate esters include triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, resorcinol bis(diphenyl phosphate), 1,3-phenylene bis(di-2,6-xylenyl phosphate), bisphenol A bis(diphenyl phosphate), and 1,3-phenylene bis(diphenyl phosphate). Examples of the mono-substituted phosphonic acid diester include divinyl phenylphosphonate, diallyl phenylphosphonate, and bis(1-butenyl) phenylphosphonate. Examples of the disubstituted phosphinate ester include phenyl diphenylphosphinate and methyl diphenylphosphinate. Examples of metal salts of disubstituted phosphinic acids include metal salts of dialkylphosphinic acids, metal salts of diallylphosphinic acids, metal salts of divinylphosphinic acids, metal salts of diarylphosphinic acids, etc. These metal salts may be any of lithium salts, sodium salts, potassium salts, calcium salts, magnesium salts, aluminum salts, titanium salts, and zinc salts, and aluminum salts may be selected. Examples of the organic nitrogen-containing phosphorus compound include phosphazene compounds such as bis(2-allylphenoxy)phosphazene and dicresylphosphazene; melamine phosphate; melamine pyrophosphate; melamine polyphosphate; and melam polyphosphate. Examples of the cyclic organic phosphorus compound include 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and the like. Among these, aromatic phosphate esters and disubstituted phosphines are preferred, and 1,3-phenylenebis(di-2,6-xylenyl phosphate) and aluminum salts of dialkylphosphinic acid are more preferred.
[0119] -Metal hydrate- Examples of metal hydrates include aluminum hydroxide hydrates and magnesium hydroxide hydrates. These may be used alone or in combination of two or more. The metal hydroxides may also be inorganic fillers, but if they are materials that can impart flame retardancy, they are classified as flame retardants. -Halogen-based flame retardants- Examples of halogen-based flame retardants include chlorine-based flame retardants, bromine-based flame retardants, etc. Examples of chlorine-based flame retardants include chlorinated paraffin, etc.
[0120] When the resin composition of the present embodiment contains a phosphorus-based flame retardant as component (G), the content of the phosphorus-based flame retardant in the resin composition is not particularly limited, but is preferably 0.2 to 5 parts by mass, more preferably 1 to 4 parts by mass, and even more preferably 2 to 3.5 parts by mass, calculated as phosphorus atoms, relative to 100 parts by mass of the total of the resin components in the resin composition. When the content of phosphorus atoms is 0.2 parts by mass or more, better flame retardancy tends to be obtained, and when it is 5 parts by mass or less, better moldability, high adhesion to a conductor, excellent heat resistance, and high glass transition temperature tend to be obtained.
[0121] <(H) component; Inorganic filler (H)> By including the inorganic filler (H) in the resin composition of this embodiment, it tends to be possible to further improve the low thermal expansion coefficient, high elastic modulus, heat resistance, and flame retardancy. The (H) component is not particularly limited, and examples thereof include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), talc, aluminum borate, silicon carbide, etc. These may be used alone or in combination of two or more. Among these, silica, alumina, mica, and talc are preferred, silica and alumina are more preferred, and silica is even more preferred, from the viewpoints of thermal expansion coefficient, elastic modulus, heat resistance, and flame retardancy. Examples of silica include precipitated silica produced by a wet method and having a high water content, and dry method silica produced by a dry method and containing almost no bound water, etc., and examples of dry method silica include crushed silica, fumed silica, and fused silica (fused spherical silica) depending on the production method. There is no particular restriction on the shape and particle size of the inorganic filler (H). For example, the particle size is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm. Here, the particle size refers to the average particle size, and is the particle size at the point corresponding to 50% volume when the cumulative frequency distribution curve of the particle size is calculated with the total volume of the particles being 100%. The particle size of the inorganic filler (H) can be measured by a particle size distribution measuring device using a laser diffraction scattering method.
[0122] When the resin composition of the present embodiment contains the (H) component, the content of the (H) component in the resin composition is not particularly limited, but from the viewpoints of thermal expansion coefficient, elastic modulus, heat resistance, and flame retardancy, the content is preferably 10 to 200 parts by mass, more preferably 30 to 170 parts by mass, even more preferably 50 to 150 parts by mass, particularly preferably 70 to 130 parts by mass, and most preferably 90 to 110 parts by mass, per 100 parts by mass of the total of the resin components in the resin composition.
[0123] In addition, when the (H) component is used, a coupling agent may be used in combination as necessary for the purpose of improving the dispersibility of the (H) component and the adhesion between the (H) component and the organic component in the resin composition. The coupling agent is not particularly limited, and for example, a silane coupling agent or a titanate coupling agent may be appropriately selected and used. The coupling agent may be used alone or in combination of two or more. The amount of the coupling agent used is also not particularly limited, and may be, for example, 0.1 to 5 parts by mass or 0.5 to 3 parts by mass relative to 100 parts by mass of the (H) component. If the content of the (H) component is within the above range, there is little deterioration in various properties, and the above-mentioned features of the (H) component tend to be effectively exhibited. When a coupling agent is used, the so-called integral blending method may be used in which the coupling agent is added after the (H) component is blended into the resin composition, but it is preferable to use an inorganic filler that has been surface-treated in advance with a coupling agent by a dry or wet method. By adopting this method, the characteristics of the (H) component can be more effectively expressed.
[0124] When the (H) component is used in this embodiment, in order to improve the dispersibility of the (H) component in the resin composition, the (H) component may be used as a slurry in which the (H) component is dispersed in an organic solvent in advance, as necessary. As the organic solvent used when forming the (H) component into a slurry, for example, the above-mentioned organic solvents can be used. These may be used alone or in combination of two or more. Among these, from the viewpoint of dispersibility, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone are preferable. The solid content (non-volatile content) concentration of the slurry is not particularly limited, but may be, for example, 50 to 80 mass %, or 60 to 80 mass %, from the viewpoint of sedimentation and dispersibility of the inorganic filler (H).
[0125] The resin composition of the present embodiment may further contain, as necessary, resin materials such as thermoplastic resins and elastomers other than the above-mentioned components, as well as coupling agents, antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, pigments, colorants, flame retardant assistants, lubricants, etc., which are appropriately selected and contained. These may be used alone or in combination of two or more. The amount of these used is not particularly limited, and may be used within a range that does not impair the effects of the present invention.
[0126] <Organic solvent> The resin composition of the present embodiment may contain an organic solvent from the viewpoint of facilitating handling by dilution and from the viewpoint of facilitating production of a prepreg, which will be described later. A resin composition containing an organic solvent is generally referred to as a resin varnish or varnish. The organic solvent used in the varnish is not particularly limited, but examples thereof include alcohol-based solvents such as ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethyl sulfoxide; and ester-based solvents such as γ-butyrolactone. Among these, from the viewpoint of solubility, alcohol solvents, ketone solvents, and nitrogen atom-containing solvents are preferred, ketone solvents are more preferred, acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone are further preferred, and methyl ethyl ketone is particularly preferred. The organic solvent may be used alone or in combination of two or more kinds.
[0127] When the resin composition of the present embodiment contains an organic solvent, the solid content concentration is, for example, 30 to 90% by mass, may be 35 to 80% by mass, or may be 40 to 60% by mass. When the solid content concentration is within the above range, the handling becomes easy, and the impregnation into the substrate and the appearance of the produced prepreg tend to be good. Furthermore, the solid content concentration of the resin in the prepreg described later becomes easy to adjust, and the production of a prepreg having a desired thickness tends to be easier.
[0128] <Method of producing resin composition> The resin composition of the present embodiment is (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof; (B) a polyphenylene ether resin; (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons an organometallic compound having a group; The composition can be produced by a method of mixing the above. When mixing, other components other than the components (A) to (C) may also be mixed in as necessary. The method for mixing is not particularly limited, and a known method using a mixer or the like can be used. Each component may be dissolved or dispersed in an organic solvent, or may be kneaded without a solvent. The mixing conditions, such as the order of mixing, temperature, and time, are not particularly limited and may be appropriately adjusted depending on the types of raw materials used, etc.
[0129] <Physical properties of cured resin composition> The dielectric constant (Dk) at 10 GHz of the cured product of the resin composition of this embodiment (a laminate and a cured product of a resin film not including a fiber substrate such as glass cloth) is preferably 3.0 or less, more preferably 2.9 or less. The smaller the dielectric constant (Dk), the better, and there is no particular limitation on the lower limit, but in consideration of the balance with other physical properties, it may be, for example, 2.4 or more, or 2.6 or more. The dielectric loss tangent (Df) at 10 GHz of the cured product of the resin composition of this embodiment (a laminate and a cured product of the resin film not including a fiber substrate such as glass cloth) is preferably 0.0024 or less, more preferably 0.0023 or less. The smaller the dielectric loss tangent (Df), the better, and the lower limit is not particularly limited, but may be, for example, 0.0015 or more, or 0.0020 or more, taking into consideration the balance with other physical properties. The dielectric constant (Dk) and the dielectric loss tangent (Df) are values based on the cavity resonator perturbation method, and more specifically, are values measured by the method described in the Examples. In this specification, the term "dielectric constant" simply refers to the relative dielectric constant.
[0130] [Prepreg] The present invention also provides a prepreg containing the resin composition of the present embodiment. The prepreg of this embodiment contains, for example, the resin composition of this embodiment and a sheet-like fiber reinforced substrate, and can be produced by impregnating or coating the resin composition of this embodiment into a sheet-like fiber reinforced substrate and drying it. More specifically, for example, the prepreg of this embodiment can be produced by heating and drying in a drying oven at a temperature of 80 to 200°C for 1 to 30 minutes and semi-curing (B-stage). The amount of the resin composition used is not particularly limited, but is, for example, an amount such that the solid content derived from the resin composition in the prepreg after drying is 30 to 90 mass%. When the solid content derived from the resin composition is within the above range, better moldability tends to be obtained when the laminate is formed.
[0131] As the sheet-like fiber reinforcement substrate of the prepreg, a known one used in various laminates for electrical insulating materials is used. Examples of the material of the sheet-like fiber reinforcement substrate include inorganic fibers such as E glass, D glass, S glass, and Q glass; organic fibers such as polyimide, polyester, and tetrafluoroethylene; and mixtures thereof. These sheet-like fiber reinforcement substrates have shapes such as woven fabric, nonwoven fabric, roving, chopped strand mat, and surfacing mat. The thickness of the sheet-like fiber reinforcement substrate is not particularly limited, but is, for example, 0.02 to 0.5 mm. In addition, from the viewpoints of impregnation of the resin composition, heat resistance, moisture absorption resistance, and processability when made into a laminate, those that have been surface-treated with a coupling agent or the like, and those that have been mechanically opened can be used.
[0132] As a method for impregnating or coating the resin composition on the sheet-like fiber-reinforced substrate, for example, a hot melt method, a solvent method, or the like can be used. The hot melt method is a method in which the resin composition does not contain an organic solvent, and (1) the resin composition is first coated onto a coated paper that has good peelability from the resin composition, and then the coated paper is laminated onto a sheet-like fiber-reinforced substrate, or (2) the resin composition is directly coated onto a sheet-like fiber-reinforced substrate using a die coater. On the other hand, the solvent method is a method in which a sheet-shaped fiber-reinforced substrate is immersed in a resin varnish in which an organic solvent is added to a resin composition, and then dried, thereby impregnating the sheet-shaped fiber-reinforced substrate with the resin composition.
[0133] [Resin film] The present invention also provides a resin film containing the resin composition of the present embodiment. The resin film of the present embodiment can be produced, for example, by applying a resin composition containing an organic solvent, that is, a resin varnish, to a support and drying it by heating. Examples of the support include polyolefin films such as polyethylene, polypropylene, and polyvinyl chloride; polyester films such as polyethylene terephthalate (hereinafter also referred to as "PET") and polyethylene naphthalate; and various plastic films such as polycarbonate films and polyimide films. In addition, metal foils such as copper foil and aluminum foil, release paper, and the like may be used as the support. The support may be subjected to a surface treatment such as a matte treatment or a corona treatment. In addition, the support may be subjected to a release treatment using a silicone resin-based release agent, an alkyd resin-based release agent, a fluororesin-based release agent, or the like. The thickness of the support is not particularly limited, but is preferably 10 to 150 μm, and more preferably 25 to 50 μm.
[0134] The method for applying the resin varnish to the support is not particularly limited, and for example, a coating device known to those skilled in the art can be used, such as a comma coater, a bar coater, a kiss coater, a roll coater, a gravure coater, a die coater, etc. These coating devices may be appropriately selected in consideration of the desired thickness of the resin film, etc. The drying temperature and drying time may be appropriately determined depending on the amount of organic solvent used and the boiling point of the organic solvent used. For example, in the case of a resin varnish containing about 40 to 60 mass % of organic solvent, a resin film can be suitably formed by drying at 50 to 150°C for about 3 to 10 minutes.
[0135] [Laminate] The present invention also provides a laminate comprising the prepreg of this embodiment and a metal foil. The laminate of this embodiment can be produced, for example, by disposing a metal foil on one or both sides of a single prepreg of this embodiment, or by disposing a metal foil on one or both sides of a prepreg obtained by stacking two or more prepregs of this embodiment, and then molding the prepreg under heat and pressure. A laminate having a metal foil is sometimes called a metal-clad laminate. The metal of the metal foil is not particularly limited as long as it is used in electrical insulating material applications. From the viewpoint of electrical conductivity, the metal may be copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, or an alloy containing one or more of these metal elements, with copper and aluminum being preferred, and copper being more preferred. The conditions for hot and pressure molding are not particularly limited, but may be, for example, a temperature of 100 to 300° C., a pressure of 0.2 to 10 MPa, and a time of 0.1 to 5 hours. In addition, the hot and pressure molding may employ a method in which a vacuum state is maintained for 0.5 to 5 hours using a vacuum press or the like.
[0136] [Printed wiring board] The printed wiring board of this embodiment contains one or more selected from the group consisting of the prepreg of this embodiment, the resin film of this embodiment, and the laminate of this embodiment. The printed wiring board of this embodiment can be manufactured by performing a circuit formation process and a multi-layer adhesion process by a known method using one or more selected from the group consisting of the prepreg of this embodiment, the resin film of this embodiment, and the laminate of this embodiment.
[0137] [Semiconductor package] The semiconductor package of this embodiment is formed by mounting a semiconductor on the printed wiring board of this embodiment. The semiconductor package of this embodiment can be manufactured by mounting a semiconductor chip, a memory, etc. at predetermined positions on the printed wiring board of this embodiment.
[0138] The resin composition, prepreg, laminate, resin film, printed wiring board, and semiconductor package of the present embodiment can be suitably used in electronic devices that handle high-frequency signals of 10 GHz or more. In particular, the printed wiring board is useful as a printed wiring board for millimeter-wave radar.
[0139] Although the preferred embodiments of the present invention have been described above, these are merely examples for the purpose of explaining the present invention, and the scope of the present invention is not limited to these embodiments. The present invention can be embodied in various forms different from the above-described embodiments without departing from the gist of the present invention. EXAMPLES
[0140] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples.
[0141] In each example, the number average molecular weight was measured by the following procedure. (Method of measuring number average molecular weight) The number average molecular weight was calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene. The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Type; A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation, product name]. The measurement conditions for GPC are shown below. Equipment: High-speed GPC equipment HLC-8320GPC Detector: UV-8320 ultraviolet absorption detector [manufactured by Tosoh Corporation] Column: Guard column: TSK Guardcolumn SuperHZ-L + Column: TSKgel SuperHZM-N + TSKgel SuperHZM-M + TSKgel SuperH-RC (all product names manufactured by Tosoh Corporation) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column) Eluent: Tetrahydrofuran Sample concentration: 10mg / 5mL Injection volume: 25μL Flow rate: 1.00mL / min Measurement temperature: 40℃
[0142] [Production Example 1: Production of polyaminobismaleimide compound (A-1)] Into a 1 L glass flask equipped with a thermometer, a reflux condenser, and a stirrer and capable of being heated and cooled, 50 parts by mass of 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 50 parts by mass of 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 14 parts by mass of 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, and 50 parts by mass of propylene glycol monomethyl ether were added, and the liquid temperature was kept at 120°C. The mixture was reacted for 3 hours with stirring, and then cooled and filtered through a 200 mesh filter to produce a polyamino bismaleimide compound (A-1) having a number average molecular weight of 800.
[0143] [Production Example 2: Production of polyphenylene ether derivative (B-1)] Toluene, raw material polyphenylene ether "Zylon (registered trademark) S203A" (trade name, manufactured by Asahi Kasei Corporation, number average molecular weight: 12,000), and an allyl group-containing compound represented by the following general formula (B-10) were added to a glass flask with a volume of 2 L equipped with a thermometer, a reflux condenser, and a stirrer, and dissolved while stirring at 90 to 100 ° C. The amount of the allyl group-containing compound was set so that the hydroxyl group equivalent derived from the allyl group-containing compound was 6 (equivalent ratio) relative to the hydroxyl group equivalent of the raw material polyphenylene ether. The amount of toluene used was set so that the reaction concentration was 35 mass %.
[0144] [ka] (In the formula, X B2 is a divalent organic group, and X in the above general formula (B-6) B2 It is explained similarly to the above.)
[0145] After visually confirming that the allyl group-containing compound had dissolved, 2 parts by mass of t-butylperoxyisopropyl monocarbonate per 100 parts by mass of raw polyphenylene ether and 0.11 parts by mass of manganese octylate per 100 parts by mass of raw polyphenylene ether were added, and the solution was subjected to a redistribution reaction at a solution temperature of 90 to 100°C for 6 hours, and then cooled to 40°C to obtain a polyphenylene ether derivative (B-1) having an allyl group at the molecular end. A small amount of this reaction solution was taken out and subjected to GPC measurement, and the double peak derived from the allyl group-containing compound became a single peak, and the number average molecular weight of the polyphenylene ether derivative (B-1) was 4,200.
[0146] [Preparation of resin composition] Examples 1 to 3, Comparative Example 1 Each component shown in Table 1 was stirred and mixed while heating at room temperature or at 50 to 80°C according to the compounding amount (unit: parts by mass) shown in Table 1 to prepare a resin composition having a solids (non-volatile content) concentration of approximately 50% by mass. The resin composition obtained in each example was applied to a PET film (manufactured by Teijin Limited, product name: G2-38) having a thickness of 38 μm, and then heated and dried at 170° C. for 5 minutes to produce a resin film in a B-stage state. This resin film was peeled off from the PET film and then crushed to produce a resin powder. Next, the above-mentioned resin powder was put into a Teflon (registered trademark) sheet cut into a size of 1 mm thick x 50 mm long x 35 mm wide, and low-profile copper foils having a thickness of 18 μm (manufactured by Furukawa Electric Co., Ltd., product name: BF-ANP18) were placed on the top and bottom of the Teflon (registered trademark) sheet so that the M side was in contact with the put-in resin powder, and the resin composition was cured by heating and pressing under conditions of a temperature of 230° C., a pressure of 2.0 MPa, and a time of 120 minutes to produce a resin plate with copper foils on both sides (resin plate thickness: 1 mm).
[0147] [Evaluation and measurement methods] The resin sheets with copper foil on both sides obtained in the above Examples and Comparative Examples were subjected to measurements and evaluations according to the following methods. The results are shown in Table 1.
[0148] (Evaluation of dielectric properties (dielectric constant and dielectric tangent) of resin boards) The resin board with copper foil on both sides obtained in each example was immersed in a 10 mass % solution of ammonium persulfate (manufactured by Mitsubishi Gas Chemical Company, Inc.) as a copper etching solution to remove the copper foil, and from this evaluation board, a 2 mm x 50 mm evaluation board was produced. The dielectric constant (Dk) and dielectric loss tangent (Df) of the evaluation substrate were measured in the 10 GHz band in accordance with the cavity resonator perturbation method.
[0149] (Method of measuring glass transition temperature and thermal expansion coefficient) The thermal expansion coefficient (thickness direction, temperature range: 30 to 120°C) and glass transition temperature (Tg) were measured using a 5 mm square test piece made by etching the copper foil on both sides of a double-sided copper foil-covered resin sheet, using a thermomechanical analyzer (TMA) [Model Q400, manufactured by TA Instruments Japan, Inc.] in accordance with the IPC (The Institute for Interconnecting and Packaging Electronic Circuits) standard.
[0150] (Method of measuring copper foil peel strength) The copper foil peel strength was measured for the resin sheet with copper foil on both sides obtained in each example, in accordance with JIS C 6481, a copper-clad laminate test standard, by measuring the peel strength between the resin sheet and the copper foil.
[0151] [Table 1]
[0152] The materials in Table 1 are as follows. [Component (A): Maleimide compound (A)] Polyaminobismaleimide compound (A-1): The polyaminobismaleimide compound (A-1) produced in Production Example 1 was used.
[0153] [Component (B): Polyphenylene ether resin (B)] Polyphenylene ether derivative (B-1): The polyphenylene ether derivative (B-1) produced in Production Example 2 was used.
[0154] [(C) Component: Organometallic compound (C)] Organometallic Compound (C-1): Titanium diisopropoxybis(acetylacetonate) Organometallic Compounds (C-2): Titanium tetraacetylacetonate
[0155] [Component (D): Styrene-based thermoplastic elastomer (D)] Kraton (registered trademark) G1726: Hydrogenated styrene-based thermoplastic elastomer (SEBS) (product name, manufactured by Kraton Polymer Japan Co., Ltd.)
[0156] [Component (E); Crosslinking agent (E)] B-1000: Polybutadiene, number average molecular weight: 1,200, vinyl group content: 85% or more (product name, manufactured by Nippon Soda Co., Ltd.)
[0157] [Component (F); Curing accelerator (F)] α,α'-Bis(t-butylperoxy)diisopropylbenzene G-8009L: Isocyanate masked imidazole (addition product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole) (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name)
[0158] [Component (G); Flame retardant (G)] OP935: aluminum dialkylphosphinic acid salt, metal salt of disubstituted phosphinic acid, phosphorus content: 23.5% by mass (manufactured by Clariant, product name) 1,3-phenylenebis(di-2,6-xylenyl phosphate), phosphorus content: 9.0% by mass
[0159] [(H) component; inorganic filler (H)] Silica: Spherical fused silica, average particle size: 0.5 μm
[0160] As is clear from the results shown in Table 1, the cured products obtained from the resin compositions of Examples 1 to 3 of this embodiment have excellent dielectric properties in the high frequency band of 10 GHz or higher. These results show that in the resin composition of this embodiment, (C) Through one oxygen atom Bonds to metal atoms Hydrocarbons It is clear that the dielectric properties of the cured product can be improved by the simple method of blending an organometallic compound having a group. [Industrial Applicability]
[0161] The laminate produced from the resin composition of this embodiment has excellent dielectric properties in high frequency bands of 10 GHz or more, and is therefore useful for multilayer printed wiring boards used in fifth generation mobile communication system (5G) antennas that use radio waves in a frequency band exceeding 6 GHz and millimeter wave radars that use radio waves in a frequency band of 30 to 300 GHz.
Claims
1. (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof; (B) a polyphenylene ether resin; (C) an organometallic compound having a hydrocarbon group bonded to a metal atom via one oxygen atom; Contains the component (A) is a polyaminobismaleimide compound having a structural unit derived from a maleimide compound (a1) having two or more N-substituted maleimide groups and a structural unit derived from a diamine compound (a2), The resin composition, wherein the (C) organometallic compound having a hydrocarbon group bonded to a metal atom via one oxygen atom is a compound represented by the following general formula (C-1) or the following general formula (C-2): 【Chemistry 1】 (In the above general formulas (C-1) and (C-2), each R C1 independently represents a hydrocarbon group having 1 to 10 carbon atoms, and each M C1 independently represents a titanium atom or a zirconium atom. In the above general formula (C-2), each R C2 independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms.)
2. The resin composition according to claim 1, wherein the polyphenylene ether resin (B) has a number average molecular weight of 1,000 to 25,000.
3. 3. The resin composition according to claim 1, wherein the polyphenylene ether resin (B) has an ethylenically unsaturated bond-containing group.
4. The resin composition according to any one of claims 1 to 3, wherein the content of the organometallic compound (C) having a hydrocarbon group bonded to a metal atom via one oxygen atom is 0.01 to 20 parts by mass relative to 100 parts by mass of the polyphenylene ether resin (B).
5. A prepreg comprising the resin composition according to any one of claims 1 to 4.
6. A laminate comprising the prepreg according to claim 5 and a metal foil.
7. A resin film comprising the resin composition according to any one of claims 1 to 4.
8. A printed wiring board comprising at least one member selected from the group consisting of the prepreg according to claim 5, the laminate according to claim 6, and the resin film according to claim 7.
9. A semiconductor package comprising the printed wiring board according to claim 8 and a semiconductor element mounted thereon.
10. A method for producing the resin composition according to any one of claims 1 to 4, comprising the steps of: (A) one or more compounds selected from the group consisting of maleimide compounds having two or more N-substituted maleimide groups and derivatives thereof; (B) a polyphenylene ether resin; (C) an organometallic compound having a hydrocarbon group bonded to a metal atom via one oxygen atom; A method for producing a resin composition comprising mixing the above components.
Citation Information
Patent Citations
Laminated board and its molding method
JP1983069046A
Lighting device of industrial telecamera
JP1986018937A
Curable polyphenylene ether and preparation thereof
JP1989069628A
Novel curable polyphenylene ether and preparation thereof
JP1989069629A
Curable resin composition and flame-retardant laminate
JP1995238128A